Ceramic microcrystal grinding wheel
By using low-temperature sintering bonding agent, the problem of degradation of ceramic microcrystalline abrasives at high temperatures is solved, and a ceramic microcrystalline grinding wheel with good compatibility is prepared, which improves the grinding performance and service life, and meets the needs of modern automated grinding processes. .
Patent Information
- Application Number
- CN202411037814.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The existing ceramic grinding wheel bonding agents cause the performance of ceramic microcrystalline abrasives to decline when sintered at high temperatures, and the quality differences of conventional bonding agents are difficult to ensure the quality of unified products and cannot meet the needs of modern automated grinding processes.
A low-temperature sintering bonding agent is used, and the sintering temperature is between 800 and 1000℃, and consists of SiO2, Al2O3, B2O3, alkali metal oxide and alkaline earth metal oxide. Through the optimization of the formulation and preparation method, a ceramic microcrystal grinding wheel with good compatibility is prepared.
It improves the grinding performance and service life of ceramic microcrystalline grinding wheels, ensures consistency of product quality and adaptability to automated grinding processes.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of abrasive materials and grinding tools, in particular to a ceramic microcrystalline grinding wheel. Background Art
[0002] The grinding wheel manufacturing industry is a traditional industry that can be traced back more than 100 years ago. It is a necessity in the industrial field and is also known as the "teeth" of industry. With the emergence of more and more difficult-to-grind materials, the common abrasives used before, such as brown corundum, white corundum, chrome corundum, and single crystal corundum, are difficult to meet the processing requirements of new materials. The emerging ceramic microcrystalline corundum has the characteristics of high toughness and strong self-sharpening due to its microcrystalline structure. It is particularly suitable for the processing of difficult-to-grind materials, has high processing efficiency and is not easy to burn the workpiece, and has become a hot spot in current research.
[0003] The quality of the grinding wheel mainly depends on the performance of the binder itself, as well as the wettability between the binder and the abrasive particles, the compatibility of the thermal expansion coefficient, and the bonding strength. Therefore, the screening of the binder is an important factor in obtaining high-quality grinding wheels. For ceramic microcrystalline abrasives, conventional high-temperature binders (generally referring to binders sintered at a sintering temperature above 1100°C) cannot be used to manufacture grinding tools. This is attributed to the fact that the microcrystalline structure of the ceramic microcrystalline abrasive is kept at a high temperature of more than 1100°C for more than 4 hours, and the original microcrystals will gradually grow and the performance will drop significantly. At the same time, conventional ceramic grinding wheel binders are composed of materials such as clay, feldspar and glass powder. These materials are subject to quality differences and it is difficult to guarantee uniform product quality. They are no longer suitable for modern automated grinding processes with preset processing parameters.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a ceramic microcrystalline grinding wheel.
[0006] The technical solution adopted by the present invention is:
[0007] The present invention provides a ceramic microcrystalline grinding wheel, which is composed of ceramic microcrystalline abrasive and a low-temperature sintering binder;
[0008] The sintering temperature of the low-temperature sintering binder and the ceramic microcrystalline abrasive is 800-1000°C.
[0009] The invention provides a ceramic microcrystalline grinding wheel, wherein the low-temperature sintering binder has the characteristic of low sintering temperature, so that the prepared ceramic microcrystalline grinding wheel has excellent grinding performance, can increase the grinding wheel dressing cycle, and greatly increase the service life of the grinding wheel.
[0010] Preferably, the ceramic microcrystalline abrasive is ceramic microcrystalline corundum.
[0011] Preferably, the low temperature sintering binder is composed of the following raw materials in percentage by mass: 40-60% SiO 2 、10~20%Al 2 O 3 , 9~20%B 2 O 3 , 9~21% alkali metal oxide (M1) 2 O, 1.5-2% alkaline earth metal oxide (M2) O, wherein M1 is Li, Na and K, and M2 is Ca or Mg.
[0012] More preferably, the SiO 2 Derived from quartz powder;
[0013] The Al 2 O 3 Derived from Al(OH) 3 ;
[0014] B 2 O 3 Derived from H 3 BO 3 ;
[0015] The Li, Na and K are derived from Li 2 CO 3 、Na 2 CO 3 and K 2 CO 3 ;
[0016] The Ca or Mg is derived from CaCO 3 or MgCO 3 .
[0017] More preferably, the Al 2 O 3 The molar percentage is 8 to 12%;
[0018] B 2 O 3 The molar percentage is 11.5 to 18.1%.
[0019] More preferably, the boron anomaly coefficient of the low temperature sintering binder is between 0 and 0.15, and the boron anomaly coefficient is the total free oxygen and the B 2 O 3 The total free oxygen is the sum of the free oxygen provided by each oxide, and the free oxygen provided by each oxide is the product of the free oxygen coefficient of the oxide and the molar percentage of the oxide.
[0020] Preferably, the mass percentage of the low-temperature sintering binder is 15-25%. DETAILED DESCRIPTION
[0021] In order to better understand the above technical scheme, exemplary embodiments of the present invention will be described in more detail below. However, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a clearer and more thorough understanding of the present invention, and to be able to fully convey the scope of the present invention to those skilled in the art.
[0022] The embodiment of the present invention provides a ceramic microcrystalline grinding wheel, which is composed of a ceramic microcrystalline abrasive and a low-temperature sintered binder;
[0023] The sintering temperature of the low-temperature sintering binder and the ceramic microcrystalline abrasive is 800-1000°C.
[0024] In the present invention, for example, the sintering temperature can be any value among 800°C, 830°C, 860°C, 890°C, 920°C, 950°C, 980°C, 1000°C, etc., but is not limited to the above-mentioned values. At the same time, the present invention has no particular restrictions on the preparation method of the ceramic microcrystalline grinding wheel. For example, the ceramic microcrystalline abrasive and the low-temperature sintering binder are mixed in a certain ratio and then pressed into a green body, and sintered at 800-1000°C, and then cooled to obtain the green body.
[0025] In a preferred embodiment of the present invention, the ceramic microcrystalline abrasive is ceramic microcrystalline corundum. In the present invention, the grain size of the ceramic microcrystalline corundum is less than 1 μm, the abrasive grains are high in strength, and have micro-crushing properties. The grinding wheel prepared with the ceramic microcrystalline corundum as the abrasive has good self-sharpening properties, no clogging, good toughness, and low wear.
[0026] In a preferred embodiment of the present invention, the low temperature sintering binder is composed of the following raw materials in percentage by mass: 40-60% SiO 2 、10~20%Al 2 O 3 , 9~20%B 2 O 3 , 9~21% alkali metal oxide (M1) 2 O, 1.5-2% alkaline earth metal oxide (M2) O, wherein M1 is Li, Na and K, and M2 is Ca or Mg.
[0027] In the present invention, by studying the composition and dosage of the basic low-temperature sintering binder, a high-strength, low-melting-point low-temperature sintering binder is provided. 2 It is the most important network former in glass, ensuring the basic hardness and strength of the binder. 2The content of Al should not be too high, otherwise it will cause the melting point of the binder to be too high. 2 O 3 Can improve the strength and heat resistance of glass, but Al 2 O 3 It should not be excessive, otherwise it will increase the melting point of the binder. 2 O 3 It can significantly reduce the melting point of glass. 2+ In the case of [BO 4 ] structural units enter the spatial network structure of the glass to improve the strength of the glass, but B 2 O 3 Insufficient B will result in a high melting point of the glass. 2 O 3 Too much, without enough 2+ In the case of [BO 3 ] layered structure into the glass network, but reduce the strength of the glass. Among alkali metal oxides, Li 2 O in glass can reduce the thermal expansion coefficient, improve chemical stability, act as a flux, improve production efficiency, and improve alkali resistance. 2 O.K 2 The role of O in glass mainly includes lowering the melting point of glass, enhancing the heat resistance and chemical stability of glass, and improving the stress resistance of glass. However, its content should not be too high, otherwise it will reduce the mechanical strength, chemical stability, thermal stability, etc. of the glass. 2 O、Na 2 O and K 2 The amount of O is preferably 3-7%. Among alkaline earth metal oxides, CaO mainly reduces the high-temperature viscosity of glass at high temperatures, promotes the melting and clarification of glass liquid, and increases the chemical stability and mechanical strength of glass. However, excessive CaO may enhance the crystallization tendency of glass, reduce thermal stability, and increase annealing temperature. The role of MgO is similar to that of CaO, which will not be described here. In addition, the low-temperature sintering binder used in the present invention belongs to the soda-lime-silica glass system, and its linear expansion coefficient is 8.2×10 -6 / ℃, which is similar to the thermal expansion coefficient of abrasive ceramic microcrystalline corundum (the thermal expansion coefficient in the range of room temperature to 1000℃ is 8.4×10 -6 / ℃), all of which have low expansion coefficients and good compatibility; at the same time, the main phase of the low-temperature sintering binder of the present invention is SiO 2 、Al 2 O 3 and B 2 O 3 , and the main component of the abrasive Al 2 O 3They are all inorganic non-metals, have no mutual repulsion and good compatibility.
[0028] In a more preferred embodiment of the present invention, SiO 2 Derived from quartz powder;
[0029] Al 2 O 3 Derived from Al(OH) 3 ;
[0030] B 2 O 3 Derived from H 3 BO 3 ;
[0031] Li, Na and K are derived from Li 2 CO 3 、Na 2 CO 3 and K 2 CO 3 ;
[0032] Ca or Mg are derived from CaCO 3 or MgCO 3 .
[0033] In the present invention, there is no particular limitation on the preparation method of the low-temperature sintering binder. For example, the raw materials are weighed and sieved according to the sources and amounts of the above-mentioned formula components (quartz powder is sieved through a 600-mesh sieve, Al(OH) 3 Pass through 320 mesh sieve, H 3 BO 3 Pass through 120 mesh sieve, Li 2 CO 3 Pass through 800 mesh sieve, Na 2 CO 3 and K 2 CO 3 Pass through 220 mesh sieve, CaCO 3 After all the raw materials are mixed evenly, they are heated to 1300°C in a glass melting furnace. The molten glass flows into a pool filled with water for water quenching. The quenched glass fragments are dried and ball-milled in a ball mill to 220 mesh and sieved to obtain a low-temperature sintering binder.
[0034] In a more preferred embodiment of the present invention, Al 2 O 3 The molar percentage is 8 to 12%;
[0035] B 2 O 3 The molar percentage is 11.5 to 18.1%.
[0036] The hardness and strength of glass mainly depend on its chemical composition and structure. Generally speaking, network-forming ions increase the strength of glass, while network-external ions reduce the strength of glass. However, boron anomaly and boron-aluminum anomaly are also very important in the strength-composition relationship. 2 O 3 and B 2 O 3 All transformed into tetrahedral [AlO 4 ] and [BO 4 ] participates in the network formation, which is better than the simple [SiO 4 ] The network structure is more dense, and the mechanical properties of the glass are the best. When there is too much or too little free oxygen, the mechanical properties of the glass will decrease. 2 O 3 It is a spatial network intermediate. In the presence of excess free oxygen, it changes from coordination 6 to coordination 4 and enters the network. Its network body [AlO 4 ] takes precedence over [BO 4 ]Enter the network, so in Li + 、Na + , K + , Ca 2+ Mg 2+ When providing free oxygen, [AlO 4 ], and then supply the excess free oxygen to B 2 O 3 , so that the layered structure [BO 3 ] to [BO 4 ] enter the network structure. When free oxygen is insufficient, B 2 O 3 Cannot convert all to [BO 4 ] enters the spatial network, so the mechanical properties of the binder decrease; and when there is too much free oxygen, it will break the network and also reduce the mechanical properties of the binder. 2 O 3 and B 2 O 3 The molar percentage range is conducive to meeting the requirements of the boron anomaly and boron aluminum anomaly principles and obtaining a binder with better performance.
[0037] In a more preferred embodiment of the present invention, the boron anomaly coefficient of the low temperature sintering binder is between 0 and 0.15, and the boron anomaly coefficient is the total free oxygen and B 2 O 3 The ratio of mole percentage, the total free oxygen is the sum of the free oxygen given by each oxide, and the free oxygen given by each oxide is the product of the free oxygen coefficient of the oxide and the mole percentage of the oxide.
[0038] The inventors analyzed the effects of various chemical components in glass, combined with the network space structure theory of glass, introduced the free oxygen ion theory, and used the boron anomaly coefficient as the judgment standard to further simplify the steps of obtaining the optimal ratio of the formula. The inventors found that the boron anomaly coefficient must be between 0 and 0.15. First, the total free oxygen in the glass system must satisfy > 0, otherwise the lack of free oxygen in the glass system will make the melting point of the glass system high; at the same time, according to the boron anomaly theory, the free oxygen supply provided by alkali metal and alkaline earth metal oxides [AlO 4 ], there is excess free oxygen to supply B 2 O 3 The layered structure [BO 3 ] to [BO 4 ] enters the network structure. Under this condition, the boron anomaly coefficient gradually increases, indicating that the transformation into [BO 4 ] increases, the strength of the glass also increases, but the glass strength begins to decrease after the boron anomaly coefficient reaches an extreme value of 0.15. The ability of each oxide to give free oxygen is measured by the free oxygen coefficient K, see Table 1.
[0039] Table 1
[0040]
[0041]
[0042] In a preferred embodiment of the present invention, the mass percentage of the low temperature sintering binder is 15-25%. In the present invention, controlling the amount of the low temperature sintering binder and the ceramic microcrystalline abrasive is beneficial to improving the wettability between the binder and the abrasive particles, the compatibility of the thermal expansion coefficient, and the bonding strength, thereby obtaining a ceramic microcrystalline grinding wheel with better comprehensive performance.
[0043] Example 1
[0044] A ceramic microcrystalline grinding wheel, which is composed of 80% ceramic microcrystalline abrasive (ceramic microcrystalline corundum) and 20% low-temperature sintered binder by mass percentage;
[0045] The sintering temperature of the low temperature sintering binder and the ceramic microcrystalline abrasive is 960°C.
[0046] The low temperature sintering binder is composed of the following raw materials by mass percentage: 55% SiO 2 、18%Al 2 O 3 (mol percentage is 11.43%), 12.5% B 2 O 3 (mol percentage is 11.56%), 3% Li 2 O, 6.5% Na 2O, 3% K 2 O, 2% CaO.
[0047] SiO 2 Derived from quartz powder;
[0048] Al 2 O 3 Derived from Al(OH) 3 ;
[0049] B 2 O 3 Derived from H 3 BO 3 ;
[0050] Li 2 O、Na 2 O.K 2 O is derived from Li 2 CO 3 、Na 2 CO 3 and K 2 CO 3 ;
[0051] CaO comes from CaCO 3 .
[0052] The boron anomaly coefficient is the total free oxygen and B 2 O 3 The molar percentage ratio, the total free oxygen is the sum of the free oxygen given by each oxide, and the free oxygen given by each oxide is the product of the free oxygen coefficient of the oxide and the molar percentage of the oxide. The boron anomaly coefficient of this embodiment is 0.09, and the specific calculation is shown in Table 2.
[0053] Table 2
[0054]
[0055]
[0056] The low-temperature sintering binder is prepared by the following method: weigh the raw materials according to the source and amount of the formula components and sieve them (quartz powder is sieved through a 600-mesh sieve, Al(OH) 3 Pass through 320 mesh sieve, H 3 BO 3 Pass through 120 mesh sieve, Li 2 CO 3 Pass through 800 mesh sieve, Na 2 CO 3 and K 2 CO 3 Pass through 220 mesh sieve, CaCO 3After all the raw materials are mixed evenly, they are heated to 1300°C in a glass melting furnace. The molten glass flows into a pool filled with water for water quenching. The quenched glass fragments are dried and ball-milled in a ball mill to 220 mesh and sieved to obtain a low-temperature sintering binder.
[0057] Example 2
[0058] The difference between this embodiment and embodiment 1 is that the amount of raw materials used in the low-temperature sintering binder is different. The low-temperature sintering binder is composed of the following raw materials in percentage by mass: 55% SiO 2 、18.5%Al 2 O 3 (molar percentage is 11.75%), 12.5% B 2 O 3 (mol percentage is 11.56%), 3% Li 2 O, 6% Na 2 O, 3% K 2 O, 2% CaO. The rest of the steps remain unchanged.
[0059] The boron anomaly coefficient of this embodiment is 0.017, and the specific calculation is shown in Table 3.
[0060] Table 3
[0061] Binder Name <![CDATA[SiO 2 ]]> <![CDATA[Al 2 THE 3 ]]> CaO <![CDATA[Na 2 The]]> <![CDATA[K 2 The]]> <![CDATA[Li 2 The]]> <![CDATA[B 2 THE 3 ]]> total Mass percentage wt% 55 18.5 2 6 3 3 12.5 100 Molecular weight 60 102 56 62 94 30 70 Number of moles 0.92 0.18 0.04 0.10 0.03 0.10 0.18 1.54 Mole percentage % 59.36 11.75 2.31 6.27 2.07 6.48 11.56 Free oxygen coefficient -1.0 0.7 1.0 1.0 0.3 Free oxygen -0.117 0.016 0.063 0.021 0.019 0.002 Boron anomaly coefficient 0.017
[0062] Example 3
[0063] The difference between this embodiment and embodiment 1 is that the amount of raw materials used in the low-temperature sintering binder is different. The low-temperature sintering binder is composed of the following raw materials in percentage by mass: 51.5% SiO 2 、14.8%Al 2 O 3 (molar percentage is 9.40%), 19.5% B 2 O 3 (mol percentage is 18.04%), 3% Li 2 O, 6% Na 2 O, 3.2% K 2 O, 2% CaO. The rest of the steps remain unchanged.
[0064] The boron anomaly coefficient of this embodiment is 0.146, and the specific calculation is shown in Table 4.
[0065] Table 4
[0066]
[0067]
[0068] Comparative Example 1
[0069] The difference between this comparative example and Example 1 is that the amount of raw materials used in the low-temperature sintering binder is different. The low-temperature sintering binder is composed of the following raw materials in percentage by mass: 55% SiO 2 、19.5%Al 2 O 3 (molar percentage is 12.38%), 12.5%B 2 O 3 (mol percentage is 11.56%), 3% Li 2 O, 6% Na 2 O, 2% K 2 O, 2% CaO. The rest of the steps remain unchanged.
[0070] The boron anomaly coefficient of this comparative example is -0.10 (total free oxygen < 0), and the specific calculation is shown in Table 5.
[0071] Table 5
[0072] Binder Name <![CDATA[SiO 2 ]]> <![CDATA[Al 2 THE 3 ]]> CaO <![CDATA[Na 2 The]]> <![CDATA[K 2 The]]> <![CDATA[Li 2 The]]> <![CDATA[B 2 THE 3 ]]> total Mass percentage wt% 55.0 19.5 2.0 6.0 2.0 3.0 12.5 100.0 Molecular weight 60 102 56 62 94 30 70 Number of moles 0.92 0.19 0.04 0.10 0.02 0.10 0.18 1.54 Mole percentage % 59.36 12.38 2.31 6.27 1.38 6.48 11.56 Free oxygen coefficient -1.0 0.7 1.0 1.0 0.3 Free oxygen -0.124 0.016 0.063 0.014 0.019 -0.01 Boron anomaly coefficient -0.10
[0073] From the boron anomaly coefficients of Examples 1-3 and Comparative Example 1, it can be seen that the performance effects of the low-temperature sintering binders prepared by each formulation are: Example 3> Example 1> Example 2> Comparative Example 1. According to the free oxygen theory, the boron anomaly coefficient of Comparative Example 1 is less than 0 (i.e., total free oxygen is less than 0), indicating that there is insufficient free oxygen, the melting point of the glass system is too high, and the mechanical properties are insufficient, and it is not suitable for the preparation of low-temperature sintering binders; although the boron anomaly coefficient of Example 2 is greater than 0, the value is too small, indicating that the boron anomaly coefficient used to supply B 2 O 3 Convert it to [BO 4 ] enters the glass network structure too little, and the performance of the prepared low-temperature sintering binder is better than that of Comparative Example 1, but the improvement is not enough; and the boron anomaly coefficient of Examples 2 and 3 is close to 0.15, indicating that most of the B 2 O 3 All transformed into [BO 4 ] Entering into the glass network structure, the performance of the prepared low-temperature sintering binder can meet the actual needs. Among them, the boron anomaly coefficient of Example 3 is closest to 0.15, so the performance of the low-temperature sintering binder prepared in Example 3 is the best.
[0074] The low-temperature sintered binder of Example 3 was subjected to sintering experiments and grinding wheel performance tests, and the results are recorded in Tables 6 to 9.
[0075] (1) Low temperature sintering binder melting test
[0076] Test method: Weigh 0.5g of the low-temperature sintering binder powder of Example 3. The mold is pressed into a tablet shape and placed in Al2 O 3 The sintering test was carried out on the board, and the temperature curve setting was shown in Table 6.
[0077] Table 6
[0078] stage Starting temperature End temperature Time / Hour Warming up 20℃ 960℃ 6 hours Insulation 960℃ 960℃ 4 hours Cooling 960℃ Natural cooling
[0079] The equivalent diameter after sintering measured by the above method is The fluidity is relatively good, which indicates that the low-temperature sintering binder of Example 3 of the present invention has good wetting performance on ceramic microcrystalline corundum.
[0080] (2) Ceramic microcrystalline grinding wheel manufacturing performance test
[0081] Test method: According to the formula of Example 3 and the conventional grinding wheel production process, the following specifications of the product are produced, the product size is 183mm outer diameter×18mm thickness×33mm inner diameter, 5 pieces of each specification of grinding wheel are produced, and after the sample grinding wheel is produced, the grinding wheel density and sandblasting hardness are tested, compared with the standard, the grinding wheel size is measured, and the shrinkage performance of the grinding wheel production is tested. The results are shown in Table 7.
[0082] Table 7
[0083]
[0084] From the results in Table 7, it can be seen that the sintered density, sandblasting hardness and shrinkage performance of the ceramic microcrystalline grinding wheel prepared in Example 3 meet the requirements of grinding wheel production and manufacturing, which also shows that the low-temperature sintering binder of Example 3 of the present invention has good manufacturing performance.
[0085] (3) Ceramic microcrystalline grinding wheel customer test
[0086] Test method: According to the formula of Example 3, a ceramic microcrystalline grinding wheel was manufactured by conventional production method for customer testing. The grinding wheel size was 280 mm in outer diameter×160 mm in thickness×115 mm in inner diameter. The results are recorded in Tables 8 and 9.
[0087] Table 8
[0088]
[0089] Table 9
[0090]
[0091] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A ceramic microcrystalline grinding wheel, characterized in that: It is composed of ceramic microcrystalline abrasive and low temperature sintered binder; The sintering temperature of the low-temperature sintering binder and the ceramic microcrystalline abrasive is 800-1000°C.
2. The ceramic microcrystalline grinding wheel according to claim 1, characterized in that: The ceramic microcrystalline abrasive is ceramic microcrystalline corundum.
3. The ceramic microcrystalline grinding wheel according to claim 1, characterized in that: The low-temperature sintering binder is composed of the following raw materials in percentage by mass: 40-60% SiO2, 10-20% Al2O3, 9-20% B2O3, 9-21% alkali metal oxide (M1)2O, 1.5-2% alkaline earth metal oxide (M2)O, wherein M1 is Li, Na and K, and M2 is Ca or Mg.
4. The ceramic microcrystalline grinding wheel according to claim 3, characterized in that: The SiO2 is derived from quartz powder; The Al2O3 is derived from Al(OH)3; The B2O3 is derived from H3BO3; The Li, Na and K are derived from Li2CO3, Na2CO3 and K2CO3 respectively; The Ca or Mg is derived from CaCO3 or MgCO3, respectively.
5. The ceramic microcrystalline grinding wheel according to claim 3, characterized in that: The molar percentage of Al2O3 is 8-12%; The molar percentage of B2O3 is 11.5-18.1%.
6. The ceramic microcrystalline grinding wheel according to claim 5, characterized in that: The boron anomaly coefficient of the low-temperature sintering binder is between 0 and 0.15, and the boron anomaly coefficient is the ratio of total free oxygen to the molar percentage of B2O3. The total free oxygen is the sum of the free oxygen given by each oxide, and the free oxygen given by each oxide is the product of the free oxygen coefficient of the oxide and the molar percentage of the oxide.
7. The ceramic microcrystalline grinding wheel according to claim 1, characterized in that: The mass percentage of the low-temperature sintering binder is 15-25%.
Citation Information
Patent Citations
Bonding agent for low-melting high-strength microcrystalline alumina ceramic grinding tool and preparation method thereof
CN102729156A
Blade part efficient and precise grinding microcrystal ceramic corundum grinding wheel and machining method thereof
CN104015131A
Ceramic microcrystal fused alumina grinding wheel for crankshaft grinding and manufacturing method thereof
CN104759993A
Microcrystalline glass ceramic binding agent, preparing method thereof, SG grinding wheel and preparing method thereof
CN105252435A
Glass-ceramics ceramic bond and method for preparing CBN grinding wheel with the same
CN109551382A