High temperature annealed laminated can lid material
By preheating and annealing the metal strips, combined with the lamination and annealing technology of polymer films, the discoloration, feathering and whitening of metal can lids in pasteurization and acid testing were solved, and the low feathering and The effect of low whitening improves the acid resistance of the can lid material.
Patent Information
- Application Number
- CN202410809132.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2016-05-10
- Filing Date
- 2017-05-05
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art is difficult to keep the protective layer of the metal can cover material from discoloration during pasteurization, and exhibits high elongation and whiteness in acid tests, which cannot meet the strict requirements for amorphous polymer film coating.
The metal strips are preheated to below 250°C, and then the polymer film is laminated onto the metal strips and annealed at an annealing temperature above the melting temperature of the polymer film to ensure that the polymer film is amorphous and if necessary When adjusting the surface roughness and selecting appropriate conversion layer parameters to control feathering and bleaching performance.
The protective layer does not change color during pasteurization and exhibits low elongation and low whitening in the 3% acetic acid test, meeting the strict requirements for amorphous polymer film coating and improving the can lid material acid resistance.
Smart Images

Figure CN118906579A_ABST
Abstract
Description
[0001] This application is a divisional application of the invention patent application with application number 201780028978.0, application date May 5, 2017, and invention name “Laminated can cover material after high temperature annealing”. Technical Field
[0002] The present disclosure relates generally to metal processing, and more particularly to laminating and pre-treating metal strips. Background Art
[0003] Certain metal products, such as aluminum beverage cans, may require a protective layer, such as a polymer coating between the metal and its contents. For example, beverage cans generally must provide adequate protection between the metal of the beverage can and the beverage contained therein to avoid damage to the metal by stimulant beverages such as soda and cola, as well as to avoid adverse effects on the beverage such as discoloration or changes in taste.
[0004] There are often requirements with respect to the basic properties of the protective layer. It may be desirable to produce a laminated metal product that meets various requirements. In some cases, it may be desirable to laminate a metal product rather than paint it.
[0005] For example, certain can end stocks (CES) used in beverage cans must have a protective layer that has less than a maximum amount of feathering and less than a maximum amount of blushing. Feathering can refer to the elongation and delamination of the protective layer, especially when the metal breaks, such as the hole created when the beverage can is opened. Blushing can refer to the discoloration of the protective layer, which may occur when the metal is subjected to high temperatures in a specific media after coating, such as during a pasteurization or sterilization process. It can be expected that there will be no discoloration during the pasteurization process. In some cases, the protective layer must withstand an acid test, such as an acetic acid test. The metal strip may need to meet one or more of these and other requirements after coating.
[0006] In order to ensure that the metal sheets laminated with polymers meet the desired requirements, it has been asserted that certain restrictions must be placed on the selection of materials and pre-forming processes. These restrictions may include restrictions on polymer selection, strict temperature regulation with a small window of error, and other such restrictions.
[0007] U.S. 5,582,319 describes a process for producing polymer film coated metal sheets, noting that the use of an amorphous polymer is undesirable because it is too elastic and will produce excessive feathering when opening a can, and it will blush too easily, for example, during pasteurization due to the crystallization mechanism of the polymer. The process described involves maintaining the annealing process temperature below the melting point of the primary polymer layer to achieve compliance with CES requirements such as feathering and blushing after pasteurization. In addition, the aluminum alloy disclosed in the '319 patent has a low Mg content range that falls outside the standard industrial alloy for AA5182, which in turn has an impact on product attributes.
[0008] It would be desirable to provide a laminated metal product that meets or exceeds desired requirements. It would be desirable to produce such a laminated metal product using an amorphous polymer. Summary of the invention
[0009] The term embodiment and similar terms are intended to broadly refer to all subject matter of the present disclosure and the following [. Statements containing these terms should be understood not to limit the subject matter described herein or to limit the meaning or scope of the following [. The embodiments of the present disclosure covered herein are defined by the following [ and not by this disclosure. This disclosure is a high-level overview of various aspects of the present disclosure and introduces some concepts that are further described in the following detailed description section. This disclosure is not intended to identify key or essential features of the claimed subject matter, nor is it intended to be used alone to determine the scope of the claimed subject matter. The subject matter should be understood by reference to appropriate portions of the entire specification of the present disclosure, any or all of the drawings, and each [.
[0010] Embodiments of the present disclosure include a method for preparing a can cover material, the method comprising: preheating a metal strip to a first temperature below 250°C; laminating a polymer film to a first side of the metal strip to produce a laminated metal strip, wherein a main component of the polymer film has a melting temperature higher than the first temperature; and annealing the laminated metal strip at an annealing temperature, wherein the annealing temperature is higher than the melting temperature of the polymer film.
[0011] In some cases, the metal strip is an aluminum strip, such as AA5182 aluminum alloy. In some cases, the method may include applying a conversion coating to the metal strip, wherein laminating the polymer film to the first side of the metal strip includes laminating the polymer film to the conversion coating. In some cases, laminating the polymer film includes laminating a polyethylene terephthalate film to the metal strip. In some cases, the method includes applying a paint layer or another polymer film to the second side of the metal strip, wherein the first side of the metal strip corresponds to the inner side of the can lid formed by the metal strip, and wherein the second side of the metal strip corresponds to the outer side of the can lid formed by the metal strip. In some cases, annealing the laminated metal strip includes raising the temperature of the polymer film for a duration sufficient to melt the polymer film into the surface texture of the metal strip. In some cases, annealing the laminated metal strip includes raising the temperature of the polymer film to at least 250°C. In some cases, annealing the laminated metal strip comprises raising the temperature of the polymer film to at least 265° C. In some cases, annealing the laminated metal strip comprises raising the temperature of the polymer film to at least 280° C. In some cases, the method may comprise cooling the laminated metal strip after annealing the laminated metal strip to ensure that the polymer film remains amorphous. In some cases, the method may comprise applying a lubricant to the laminated metal strip after annealing the laminated metal strip. In some cases, the method may comprise selecting a conversion layer parameter from a plurality of conversion layer parameter candidates based on the tested performance and applying a conversion layer to the metal strip according to the conversion layer parameter before laminating the polymer film to the first side of the metal strip. In some cases, the tested performance is a blushing performance.
[0012] An embodiment of the present disclosure includes a method for determining conversion layer parameters, the method comprising: determining a plurality of conversion layer parameter candidates; preparing a can cover material sample for each of the plurality of conversion layer parameter candidates according to the aforementioned method; evaluating the whitening performance of each of the can cover material samples; and selecting conversion layer parameters from the plurality of conversion layer parameter candidates based on the evaluated whitening performance.
[0013] In some cases, the method may include adjusting the surface roughness of the metal strip before laminating the polymer film to the first side of the metal strip. In some cases, adjusting the surface roughness includes reducing the height of the surface roughness to a value below the thickness of the contact layer of the polymer film. In some cases, laminating the polymer film to the first side of the metal strip includes: pressing the polymer film against the first side of the metal strip using a coating roller having a compressible layer surrounding a hollow metal core; and passing a fluid through the hollow metal core to control the temperature of the compressible layer. In some cases, the method may include preheating the compressible layer before laminating the polymer film to the first side of the metal strip. In some cases, passing the fluid through the hollow metal core includes cooling the fluid to extract heat from the inner surface of the compressible layer to induce a thermal gradient between the inner surface of the compressible layer and the outer surface of the compressible layer. In some cases, cooling the fluid comprises reducing the temperature of the fluid sufficiently to maintain an internal temperature at the inner surface of the compressible layer below a maximum set point and to maintain an external temperature at the outer surface of the compressible layer above a minimum set point. In some cases, the method may comprise determining a temperature of the compressible layer; and adjusting a temperature or a volumetric flow rate of the fluid based on the temperature of the compressible layer.
[0014] Embodiments of the present disclosure include can end stock products prepared according to the aforementioned methods. Embodiments of the present disclosure include beverage cans, the beverage cans comprising a body and a cap, wherein the cap is formed from the can end stock prepared according to the aforementioned methods.
[0015] Embodiments of the present disclosure include a system comprising: a preheating furnace for receiving a metal strip and preheating the metal strip to a preheating temperature; a laminating system located downstream of the preheating furnace, for receiving the metal strip at the preheating temperature and applying a polymer film to a first side of the metal strip, wherein the preheating temperature is lower than the melting temperature of a main component of the polymer film; and an annealing furnace located downstream of the laminating system, for receiving the laminated metal strip and heating the laminated metal strip to an annealing temperature, wherein the annealing temperature is higher than the melting temperature of the main component of the polymer film.
[0016] In some cases, the metal strip is an aluminum strip, such as AA5182 aluminum alloy. In some cases, the system includes a conversion coating application system for applying a conversion coating to the metal strip, wherein the laminating system is configured to apply the polymer film to the conversion coating. In some cases, the laminating system is coupled to a supply of polyethylene terephthalate film. In some cases, the system includes a paint application system for applying a paint layer to the second side of the metal strip. In some cases, the laminating system is configured to apply an additional polymer film to the second side of the metal strip opposite to the first side. In some cases, the annealing furnace has a length sufficient to increase the temperature of the polymer film for a duration sufficient to melt the polymer film into the surface texture of the metal strip. In some cases, the annealing furnace is configured to provide heat sufficient to increase the temperature of the polymer film to at least 250°C. In some cases, the annealing furnace is configured to provide heat sufficient to increase the temperature of the polymer film to at least 265°C. In some cases, the annealing furnace is configured to provide heat sufficient to raise the temperature of the polymer film to at least 280°C. In some cases, the system includes a conversion layer applicator for applying a conversion layer to the metal strip according to conversion layer parameters selected from a plurality of conversion layer parameter candidates based on tested performance. In some cases, the system includes a surface roughness adjuster for adjusting the surface roughness of the metal strip, wherein the surface roughness adjuster is located upstream of the lamination system. In some cases, the surface roughness adjuster is configured to reduce the height of the surface roughness to a value below the thickness of the contact layer of the polymer film. In some cases, the lamination system includes: a coating roller, the coating roller including a compressible layer surrounding a hollow metal core; and a coolant source, the coolant source for providing a coolant to a channel of the hollow metal core to control the temperature of the compressible layer. In some cases, the system includes an external heater, the external heater being located near the compressible layer to preheat the compressible layer. In some cases, the lamination system further includes a controller coupled to the coolant source for adjusting the volume flow rate or temperature of the coolant provided by the coolant source to maintain a temperature gradient across the inner surface of the compressible layer and the outer surface of the compressible layer. In some cases, the lamination system further includes a temperature sensor coupled to the controller for providing a temperature signal associated with the temperature of the compressible layer. In some cases, the lamination system further includes a data storage containing a model, and wherein the controller is coupled to the data storage to control the coolant source based on the model.In some cases, the lamination system further includes a controller coupled to the coolant source for adjusting the volumetric flow rate or temperature of the coolant provided by the coolant source to maintain the internal temperature of the inner surface of the compressible layer below a maximum set point and maintain the external temperature of the outer surface of the compressible layer above a minimum set point.
[0017] Embodiments of the present disclosure include methods for laminating metal, the method comprising: pressing a polymer film against a first side of a preheated metal strip using a coating roller having a compressible layer surrounding a hollow metal core; and passing a fluid through the hollow metal core to control the temperature of the compressible layer. In some cases, the method includes preheating the compressible layer before laminating the polymer film to the first side of the metal strip. In some cases, preheating the compressible layer includes passing a heated fluid through the hollow metal core. In some cases, preheating the compressible layer includes externally heating the compressible layer. In some cases, passing the fluid through the hollow metal core includes cooling the fluid to extract heat from an inner surface of the compressible layer to induce a thermal gradient between the inner surface of the compressible layer and an outer surface of the compressible layer. In some cases, cooling the fluid includes sufficiently reducing the temperature of the fluid to maintain an internal temperature at the inner surface of the compressible layer below a maximum set point and an external temperature at the outer surface of the compressible layer above a minimum set point. In some cases, the method includes determining a temperature of the compressible layer; and adjusting a temperature or a volumetric flow rate of the fluid based on the temperature of the compressible layer. In some cases, wherein determining the temperature of the compressible layer includes receiving a temperature measurement of the compressible layer from a temperature sensor. In some cases, determining the temperature of the compressible layer includes receiving a temperature measurement of an element near the compressible layer from a temperature sensor. In some cases, determining the temperature of the compressible layer includes accessing a model. In some cases, the method includes sensing a change in a linear velocity of the preheated metal strip; and adjusting a temperature or a volumetric flow rate of the fluid based on the change in the linear velocity.
[0018] The present disclosure relates to the following contents.
[0019] [1] A method for preparing a can cover material, comprising:
[0020] preheating the metal strip to a first temperature below 250°C;
[0021] laminating a polymer film to the first side of the metal strip to produce a laminated metal strip, wherein a major component of the polymer film has a melting temperature higher than the first temperature; and
[0022] The laminated metal strips are annealed at an annealing temperature, wherein the annealing temperature is higher than the melting temperature of the polymer film.
[0023] [2] The method according to [1], wherein the metal strip is an aluminum strip.
[0024] [3] The method according to [1], wherein the metal strip is AA5182 aluminum alloy.
[0025] [4] The method of [1] further comprising applying a conversion coating to the metal strip, wherein laminating the polymer film to the first side of the metal strip comprises laminating the polymer film to the conversion coating.
[0026] [5] The method according to [1], wherein laminating the polymer film includes laminating a polyethylene terephthalate film to the metal strip.
[0027] [6] The method according to [1] further includes applying a paint layer or another polymer film to the second side of the metal strip, wherein the first side of the metal strip corresponds to the inner side of the can cover formed by the metal strip, and wherein the second side of the metal strip corresponds to the outer side of the can cover formed by the metal strip.
[0028] [7] The method of [1], wherein annealing the laminated metal strip comprises raising the temperature of the polymer film for a duration sufficient to melt the polymer film into the surface texture of the metal strip.
[0029] [8] The method of [1], wherein annealing the laminated metal strips comprises raising the temperature of the polymer film to at least 250°C.
[0030] [9] The method of [1], wherein annealing the laminated metal strips comprises raising the temperature of the polymer film to at least 265°C.
[0031]
[10] The method of [1], wherein annealing the laminated metal strips comprises raising the temperature of the polymer film to at least 280°C.
[0032]
[11] The method according to [1] further comprises cooling the laminated metal strips after annealing the laminated metal strips to ensure that the polymer film remains amorphous.
[0033]
[12] The method according to [1] further includes applying a lubricant to the laminated metal strip after annealing the laminated metal strip.
[0034]
[13] The method according to [1] further comprises:
[0035] selecting a translation layer parameter from a plurality of translation layer parameter candidates based on the tested performance; and
[0036] Prior to laminating the polymer film to the first side of the metal strip, a conversion layer is applied to the metal strip according to the conversion layer parameters.
[0037]
[14] The method according to
[13] , wherein the property tested is whitening property.
[0038]
[15] A method for determining conversion layer parameters, comprising:
[0039] determining a plurality of conversion layer parameter candidates;
[0040] According to the method described in [1], a can cover material sample is prepared for each of the plurality of conversion layer parameter candidates;
[0041] evaluating each of the can end stock samples for blush performance; and
[0042] A conversion layer parameter is selected from the plurality of conversion layer parameter candidates based on the evaluated blush performance.
[0043]
[16] The method according to [1] further comprises:
[0044] Prior to laminating the polymer film to the first side of the metal strip, the surface roughness of the metal strip is adjusted.
[0045]
[17] The method according to
[16] , wherein adjusting the surface roughness includes reducing the height of the surface roughness to a value lower than the thickness of the contact layer of the polymer film.
[0046]
[18] The method of [1], wherein laminating the polymer film to the first side of the metal strip comprises:
[0047] pressing the polymer film against the first side of the metal strip using a coating roller having a compressible layer surrounding a hollow metal core; and
[0048] A fluid is passed through the hollow metal core to control the temperature of the compressible layer.
[0049]
[19] The method according to
[18] further comprises:
[0050] Prior to laminating the polymer film to the first side of the metal strip, the compressible layer is preheated.
[0051]
[20] The method of
[18] , wherein passing the fluid through the hollow metal core includes cooling the fluid to extract heat from the inner surface of the compressible layer to induce a thermal gradient between the inner surface of the compressible layer and the outer surface of the compressible layer.
[0052]
[21] A method according to
[20] , wherein cooling the fluid comprises sufficiently reducing the temperature of the fluid to maintain the internal temperature at the inner surface of the compressible layer below a maximum set point and maintaining the external temperature at the outer surface of the compressible layer above a minimum set point.
[0053]
[22] The method according to
[18] , further comprising:
[0054] determining a temperature of the compressible layer; and
[0055] A temperature or volumetric flow rate of the fluid is adjusted based on the temperature of the compressible layer.
[0056]
[23] A can end material product prepared according to the method described in [1].
[0057]
[24] A beverage can comprising a body and a cap, wherein the cap is formed from the can cap stock prepared according to the method described in [1].
[0058]
[25] A system comprising:
[0059] a preheating furnace for receiving the metal strip and preheating the metal strip to a preheating temperature;
[0060] a laminating system located downstream of the preheating furnace for receiving the metal strip at the preheating temperature and applying a polymer film to a first side of the metal strip, wherein the preheating temperature is below a melting temperature of a major component of the polymer film; and
[0061] An annealing furnace located downstream of the lamination system is configured to receive the laminated metal strips and heat the laminated metal strips to an annealing temperature, wherein the annealing temperature is above the melting temperature of the major component of the polymer film.
[0062]
[26] The system according to
[25] , wherein the metal strip is an aluminum strip.
[0063]
[27] The system of
[25] , wherein the metal strip is AA5182 aluminum alloy.
[0064]
[28] The system of
[25] further comprises a conversion coating application system for applying a conversion coating to the metal strip, wherein the lamination system is configured to apply the polymer film to the conversion coating.
[0065]
[29] The system of
[25] , wherein the lamination system is coupled to a supply of polyethylene terephthalate film.
[0066]
[30] The system according to
[25] also includes a paint coating system for applying a paint layer to the second side of the metal strip.
[0067]
[31] The system of
[25] , wherein the lamination system is configured to apply an additional polymer film to a second side of the metal strip opposite the first side.
[0068]
[32] The system of
[25] , wherein the annealing furnace has a length sufficient to raise the temperature of the polymer film for a duration sufficient to melt the polymer film into the surface texture of the metal strip.
[0069]
[33] The system of
[25] , wherein the annealing furnace is configured to provide heat sufficient to raise the temperature of the polymer film to at least 250°C.
[0070]
[34] The system of
[25] , wherein the annealing furnace is configured to provide heat sufficient to raise the temperature of the polymer film to at least 265°C.
[0071]
[35] The system of
[25] , wherein the annealing furnace is configured to provide heat sufficient to raise the temperature of the polymer film to at least 280°C.
[0072]
[36] The system according to
[25] further includes a conversion layer coater for coating the conversion layer to the metal strip according to conversion layer parameters selected from a plurality of conversion layer parameter candidates based on tested performance.
[0073]
[37] The system according to
[25] further includes a surface roughness adjuster for adjusting the surface roughness of the metal strip, wherein the surface roughness adjuster is located upstream of the lamination system.
[0074]
[38] The system according to
[37] , wherein the surface roughness adjuster is configured to reduce the height of the surface roughness to a value lower than the thickness of the contact layer of the polymer film.
[0075]
[39] The system according to
[25] , wherein the lamination system comprises:
[0076] a coating roller comprising a compressible layer surrounding a hollow metal core; and
[0077] A coolant source is provided for providing a coolant to the passages of the hollow metal core to control the temperature of the compressible layer.
[0078]
[40] The system according to
[39] , further comprising:
[0079] An external heater is positioned adjacent to the compressible layer to preheat the compressible layer.
[0080]
[41] A system according to
[39] , wherein the lamination system further includes a controller coupled to the coolant source for adjusting the volume flow rate or temperature of the coolant provided by the coolant source to maintain a temperature gradient across the inner surface of the compressible layer and the outer surface of the compressible layer.
[0081]
[42] The system of
[41] , wherein the lamination system further comprises a temperature sensor coupled to the controller for providing a temperature signal associated with the temperature of the compressible layer.
[0082]
[43] The system of
[41] , wherein the lamination system further comprises a data storage device comprising a model, and wherein the controller is coupled to the data storage device to control the coolant source based on the model.
[0083]
[44] A system according to
[39] , wherein the lamination system further includes a controller coupled to the coolant source for adjusting the volume flow rate or temperature of the coolant provided by the coolant source to maintain the internal temperature of the inner surface of the compressible layer below a maximum set point and maintain the external temperature of the outer surface of the compressible layer above a minimum set point.
[0084]
[45] A method for laminating metal, comprising:
[0085] pressing the polymer film against the first side of the preheated metal strip using a coating roller having a compressible layer surrounding a hollow metal core; and
[0086] A fluid is passed through the hollow metal core to control the temperature of the compressible layer.
[0087]
[46] The method according to
[45] further comprises:
[0088] Prior to laminating the polymer film to the first side of the metal strip, the compressible layer is preheated.
[0089]
[47] The method of
[46] , wherein preheating the compressible layer comprises passing a heated fluid through the hollow metal core.
[0090]
[48] The method according to
[46] , wherein preheating the compressible layer includes externally heating the compressible layer.
[0091]
[49] A method according to
[45] , wherein passing the fluid through the hollow metal core includes cooling the fluid to extract heat from the inner surface of the compressible layer to induce a thermal gradient between the inner surface of the compressible layer and the outer surface of the compressible layer.
[0092]
[50] A method according to
[49] , wherein cooling the fluid comprises sufficiently reducing the temperature of the fluid to maintain the internal temperature at the inner surface of the compressible layer below a maximum set point and maintaining the external temperature at the outer surface of the compressible layer above a minimum set point.
[0093]
[51] The method according to
[45] , further comprising:
[0094] determining a temperature of the compressible layer; and
[0095] A temperature or volumetric flow rate of the fluid is adjusted based on the temperature of the compressible layer.
[0096]
[52] The method of
[51] , wherein determining the temperature of the compressible layer includes receiving a temperature measurement of the compressible layer from a temperature sensor.
[0097]
[53] The method of
[51] , wherein determining the temperature of the compressible layer includes receiving temperature measurements of elements near the compressible layer from a temperature sensor.
[0098]
[54] The method of
[51] , wherein determining the temperature of the compressible layer includes accessing a model.
[0099]
[55] The method according to
[45] further comprises:
[0100] sensing a change in the linear speed of the preheated metal strip; and
[0101] The temperature or volumetric flow rate of the fluid is adjusted based on the change in the linear velocity. BRIEF DESCRIPTION OF THE DRAWINGS
[0102] The description refers to the following drawings, in which the same reference numerals are used in different drawings to indicate the same or similar components.
[0103] Figure 1 is a schematic diagram of a system for preparing can end stock (CES) according to certain aspects of the present disclosure.
[0104] Figure 2 yes Figure 1 Close-up side view of a can cover material.
[0105] Figure 3A is a can end stock sheet according to certain aspects of the present disclosure.
[0106] Figure 3B According to certain aspects of the present disclosure, the Figure 3A Sheet material for can cover.
[0107] Figure 3C According to certain aspects of the present disclosure, Figure 3A A group of can end blanks produced from sheets of can end material.
[0108] Figure 3D According to certain aspects of the present disclosure, a Figure 3C The can end blank is formed into a can end for a beverage can.
[0109] Figure 4 is an isometric cutaway view of multiple layers depicting a cross section of a can end stock according to certain aspects of the present disclosure.
[0110] Figure 5 is a flow chart depicting a process for laminating metal strips according to certain aspects of the present disclosure.
[0111] Figure 6 is a partial top view depicting a portion of the opening of a can lid exhibiting feathering.
[0112] Figure 7 is a partial top view depicting a portion of an opening of a can lid that does not exhibit feathering, according to certain aspects of the present disclosure.
[0113] Figure 8 is a schematic diagram of a lamination system according to certain aspects of the present disclosure.
[0114] Fig. 9 is a flow chart depicting a process for determining desired conversion layer properties for laminated metal strips according to certain aspects of the present disclosure.
[0115] Fig.10 is a highly enlarged partial cross-sectional view of a portion of a metal strip having a film laminated thereon, according to certain aspects of the present disclosure.
[0116] Fig.11 is a partial side cross-sectional view of a lamination system according to certain aspects of the present disclosure.
[0117] Fig.12 is a schematic diagram depicting a control system for a coating roller of a laminating system according to certain aspects of the present disclosure.
[0118] Fig.13is a graph depicting temperature as a function of radial distance from the axis of rotation of a coating roller of a lamination system according to certain aspects of the present disclosure.
[0119] Fig.14 is a flow chart depicting a process for controlling the temperature of a coating roller during a lamination process according to certain aspects of the present disclosure.
[0120] Fig.15 is a graphic matrix depicting a set of laminated aluminum metal samples 1500 that were processed and tested according to certain aspects of the present disclosure. DETAILED DESCRIPTION
[0121] Certain aspects and features of the present disclosure relate to aluminum can endstock (CES) having a laminated, amorphous polymer coating that exhibits low feathering, low blushing, and high performance in an acetic acid test. The laminated metal strip may include a laminated polymer coating on the inner side (e.g., product side) and a painted coating on the outer side (e.g., consumer side). The process may include heating the bare metal strip to a temperature below the melting point of the main polymer component of the polymer film, applying a crystalline polymer to the inner side of the strip, and heating the combined strip and polymer to an annealing temperature above the melting point of the polymer. In some cases, the polymer film laminated to the metal strip may be a biaxially oriented polymer, such as an amorphous polyethylene terephthalate (PET) film from a continuous production line. During the annealing process, the polymer film may be made amorphous. The polymer film may include only a main component (e.g., a PET layer), or may include a main component and one or more supplementary components (e.g., an adhesive layer). As used herein, unless otherwise specified, the melting temperature of a polymer or polymer film refers to the melting temperature of the main component.
[0122] Through significant trial and experimentation, techniques have been discovered to produce laminated can end stocks having low feathering in the acetic acid test (e.g., 0.8 mm or less overhanging coating around the score line of the open end as defined by specific customer specifications), low blushing, and high performance. These techniques may include applying a polymer to a metal strip that has been heated to a first temperature (T1), where T1 is below the melting temperature (T2) of the polymer, prior to heating the combined strip and polymer to an annealing temperature (T2). m ) and T2 is higher than T m In some cases, T2 is equal to or greater than 250°C, 255°C, 257°C, 260°C, 265°C, 270°C, 275°C, or 280°C. In some cases, annealing occurring at a temperature above the melting temperature of the polymer can improve adhesion sufficiently to provide enhanced performance in the acid resistance test. During annealing at a temperature above the melting point of the film, the film is allowed to flow into the topography of the metal strip, thereby improving adhesion between the metal strip and the film through mechanical bonding.
[0123] In some cases where the film has a given color or gray shade, the blushing properties after pasteurization are not impaired by the amorphous state of the polymer after treatment at temperature T2.
[0124] In some cases, the metal strips can be laminated on two faces. In some cases, the metal strips can be laminated on one face and painted on the opposite face. For example, the metal strips can be laminated on the inner face and painted on the outer face, although other configurations can be used. This mixed laminated / painted metal strip can provide improved functional performance on the inside of the can cover material by using PET laminates, while maintaining high cosmetic properties on the outside of the can cover material by using lacquers, which may not be easy to whitish during pasteurization. In some cases, the PET film can include additives that provide a slight coloring for the film that does not change during pasteurization.
[0125] In some cases, the laminated metal material enters the annealing process (e.g., into an annealing furnace) directly from the lamination process. In some cases, the laminated metal material enters the paint coating system directly from the lamination process and then enters the annealing process (e.g., into an annealing furnace).
[0126] Through trials and experiments, it has been found that amorphous films can provide improved feathering performance when the adhesion between the film and the metal strip can be controlled. Trials and experiments have shown that adhesion can be controlled by controlling the annealing temperature (e.g., higher annealing temperatures can lead to improved adhesion, up to a point), controlling substrate properties (e.g., texture and chemistry), and film chemistry.
[0127] Conventional laminated metal strips typically score low in the 3% acetic acid test. However, through trials and experiments, it was found that laminates annealed at a temperature above the melting point of the polymer performed better in the 3% acetic acid test. As used herein, the 3% acetic acid test may include an evaluation of the coating's resistance to a dilute acidic medium at about 100°C for 30 minutes. The test may include cutting a cross-hatched mark into a sample and placing the sample in a 3% acetic acid solution at about 100°C for 30 minutes, then removing and cooling the sample, then performing an additional set of cross-cuts on each sample, with the tape placed over the cross-hatched area before and after the acid bath, and steadily removing the tape at an angle of about 60° within 0.5 to 1 second. The test results (e.g., based on the presence and strength of delamination) can be used to determine whether the metal strip is acceptable or unacceptable at a given desired specification. In some cases, the annealed, laminated can lid stock disclosed herein passes the 3% acetic acid test without delamination. In some cases, the annealed, laminated can end stocks disclosed herein achieve more favorable results in the 3% acetic acid test (eg, no delamination or low delamination) than standard, painted can end stocks.
[0128] These illustrative examples are given to introduce the reader to the general subject matter discussed herein and are not intended to limit the scope of the disclosed concepts. The following section describes various additional features and examples with reference to the accompanying drawings, wherein like numbers represent like elements and directional descriptions are used to describe the illustrative embodiments, but, similar to the illustrative embodiments, should not be used to limit the present disclosure. The elements contained in the illustrations herein may not be drawn to scale.
[0129] In some cases, aspects and features of the present disclosure are particularly useful with aluminum AA5182, although other types of aluminum may be used.
[0130] Figure 11 is a schematic diagram of a system 100 for preparing can end stock (CES) according to certain aspects of the present disclosure. A metal strip 102 enters a preheating furnace 112, which heats the metal strip 102 to a preheating temperature (T1). The preheating temperature T1 is much lower than the melting temperature of a polymer film 124 to be laminated to the metal strip 102. In some cases, the preheating temperature T1 is equal to or lower than 250°C, 240°C, 220°C, 200°C, 190°C, 180°C, 170°C, and 150°C. In some cases, the preheating temperature T1 is within a range of 120°C and 250°C, within a range of 170°C and 240°C, or within a range of 190°C and 220°C. The preheated metal strip 104 can enter a laminating system 114. The metal strip 102 as the preheated metal strip 104 passes through the laminating system 114, which applies a polymer film 124 to one side of the metal strip 102. In some cases, a polymer film may be applied to both sides of metal strip 102. Lamination system 114 may be any suitable system for laminating polymer film 124 to metal strip 102. Laminated metal strip 106 exits lamination system 114, combining metal strip 102 with polymer film 124.
[0131] In some cases, the laminated metal strips 106 can enter a paint coating system 118. Paint 120 is applied to the metal strips 102 by the paint coating system 118. The paint coating system 118 can be any suitable system for applying the paint 120 to the metal strips 102. The paint coating system 118 can include an oven for heating or curing the paint 120 onto the metal strips 102. In some cases, the paint coating system 118 is downstream of (e.g., after) the laminating system 114. In some cases, the paint coating system 118 is upstream of (e.g., before) the annealing oven 116. In some cases, the paint coating system 118 is upstream of the laminating system 114 or the preheating oven 112. In some cases, the paint coating system 118 is downstream of both the laminating system 114 and the annealing oven 116. As shown in FIG. Figure 1 As shown in FIG. 1 , the paint coating system 118 is located between the laminating system 114 and the annealing furnace 116 . The laminated, painted metal strip 108 can exit the paint coating system 118 .
[0132] When an upstream paint coating system 118 is used, the laminated, painted metal strips 108 may enter the annealing lehr 116. In some cases, where a paint coating system 118 is not used between the lamination system 114 and the annealing lehr 116, the laminated metal strips 106 may enter the annealing lehr.
[0133] The annealing oven 116 can be located downstream of (e.g., after) the laminating system 114 and optionally downstream of (e.g., after) the paint coating system 118. In some cases, the annealing oven 116 is located near the downstream of the paint coating system 118 so that the painted, laminated metal strip 108 exiting the paint coating system 118 enters the annealing oven 116 before entering or contacting other machines or systems.
[0134] The annealing furnace 116 raises the temperature of the painted, laminated metal strip 108 to an annealing temperature (T2). The annealing temperature T2 is higher than the melting temperature (T m ). In some cases, T2 is equal to or greater than 250° C., 255° C., 257° C., 260° C., 265° C., 270° C., 275° C., or 280° C. Thus, during the annealing process, the polymer film 124 is able to flow into the mechanical features (e.g., surface texture) of the metal strip 102 and become amorphous. The painted, laminated metal strip 108 spends a sufficient duration in the annealing furnace 116 to impart desired properties to the painted, laminated metal strip 108, including annealing of the metal strip 102 and desired adhesion of the polymer film 124. The duration in the annealing furnace 116 can be based on the furnace length and the speed of the metal strip. In some cases, the duration can be in the range of about 2 seconds to about 30 seconds, about 9 seconds to about 15 seconds, about 10 seconds to about 14 seconds, or about 12 seconds. In some cases, the duration can be adjusted as needed (e.g., by adjusting the metal strip speed) to compensate for temperature changes in the annealing furnace 116.
[0135] After leaving the annealing furnace 116, the can lid material 110 (e.g., annealed, painted, and laminated metal strips) can be optionally quenched, such as in a certain amount of quenching liquid or by applying a coolant to the can lid material 110. The can lid material 110 can be cooled immediately after leaving the annealing furnace 116 by quenching or other means at a rate sufficient to avoid a large amount of recrystallization of the amorphous polymer. In some cases, the can lid material 110 is cooled to less than about 150°C within a desired duration of about 30 seconds, 25 seconds, 20 seconds, 15 seconds, 10 seconds, 5 seconds, or 2 seconds or less. In some cases, the can lid material 110 is cooled to less than about 150°C within a duration of about 2 seconds to 15 seconds. Avoiding a large amount of recrystallization can avoid whitening of the polymer. It can be expected to have a weight fraction of 30%, 25%, 20%, or 15% of the recrystallizable portion of the recrystallized polymer that is equal to or less than. It may further be desirable to form crystals equal to or less than about 100 nm.
[0136] like Figure 1 and Figure 2As shown in , in some cases, the can end stock 110 produced by the system 100 can include a metal strip 102, wherein a paint layer 120 has been applied to a first side and a layer of laminated polymer film 124 has been applied to a second side. The metal strip 102 of the can end stock 110 can be annealed and the metal strip can include a crystalline polymer film 124 laminated thereto before being heated to a temperature above the melting temperature of the polymer film 124 for a sufficient duration to allow the polymer film 124 to melt to the surface texture of the metal strip 102 and become amorphous. As used herein, the duration sufficient to allow the polymer film 124 to melt to the surface texture of the metal strip 102 can be assessed by the polymer film 124 being sufficiently adhered to the metal strip 102 to result in an overhang coating around a score line of 0.8 mm or less, 0.7 mm or less, 0.6 mm or less, or 0.5 mm or less on the open end after pasteurization.
[0137] As described herein, a standard feathering test for can lids may include immersing the can lid in a deionized water bath at about 75°C for thirty minutes, rinsing the can lid in cooled deionized water to return the can lid to room temperature, and then immediately opening the end label of the can lid. Feathering may be observed and measured on a scored plate or pour hole opening. In some cases, feathering tests may be performed on a flat metal plate, such as a flat plate of can lid stock. In this case, the feathering test may include immersing the sample in demineralized water at 80°C for forty minutes, after which the sample is allowed to cool to room temperature and the sample may be cut and the metal strip may be separated by pulling the strip in a direction away from the cut. Other feathering tests may be used.
[0138] In some examples, laminated metal strips annealed at a temperature of 280°C provided an average feathering of 0.41 mm with a standard deviation of 0.28, while laminated metal strips annealed at a temperature of 265°C provided an average feathering of 1.08 mm with a standard deviation of 0.69. Through experimentation, it has been shown that at temperatures equal to or above the metallization temperature of the polymer film, such as at or above 250°C, improvements in feathering and delamination may be significant. This feathering may be located at certain indicated locations along the hole of the opened can lid. Through experimentation, it has been shown that the feathering of the film also depends on the cutting, forming and punching tooling design of the product.
[0139] In some cases, the metal strip 102 may include one or more conversion layers that are pre-applied prior to entering the preheating oven 112 or lamination system 114, as described in further detail below.
[0140] In some cases, a lubricant may be further applied to the can end stock 110 after exiting the annealing furnace 116 .
[0141] Figure 2 yes Figure 1A close-up side view of a can end stock 110 is shown in FIG. The can end stock 110 comprises a metal strip 102 sandwiched between a lacquer layer 120 and a laminated polymer film 124.
[0142] In some cases, to prepare the aluminum to provide enhanced adhesion and blushing properties, one or more conversion layers 202 may be coated on the bare aluminum. In some cases, this layer 202 may include a composition of chromium (III) and phosphate. This layer 202 may provide enhanced adhesion in the acetic acid test, low blushing after pasteurization, and good corrosion performance. In some cases, the metal strip 102 may include one or more conversion layers 202 located between the paint layer 120 and one or both of the laminated polymer films 124. The properties of the conversion layer 202 may be selected to provide optimal blushing after pasteurization, such as with respect to Fig. 9 described in further detail.
[0143] Figures 3A to 3D is an isometric depiction of can end stock 302 in various stages of production. In some cases, can end stock 302 is a can end stock as described herein, including a laminated amorphous polymer and lacquer as described herein.
[0144] Figure 3A is a sheet of can cover material 302 according to certain aspects of the present disclosure. The sheet of can cover material 302 may be Figure 1 The can end stock 110 depicted in FIG. 1 , or a similar can end stock. Figure 3B Describes the cut Figure 3A The sheet of can lid stock 302 can be die cut, stamped or otherwise cut to produce a can lid stock 302 such as Figure 3C Can end blank 306 is visible in FIG. Figure 3C Depicted by Figure 3A A set of can end blanks 306 are produced from sheets of can end stock. Figure 3D Describes the Figure 3C The can end blank 306 is formed into a beverage can 310 with a can end 308 .
[0145] The can lid 308 includes an outer portion (e.g., Figure 3D 310) and an inner side (e.g., toward the interior of beverage can 310). As described herein, can lid 308 can be formed such that the paint layer appears on the outer side and the laminated polymer film appears on the inner side, although this is not required.
[0146] Figure 4 4 is a multi-layer isometric cross-sectional view depicting a cross section of a can end stock 400 according to certain aspects of the present disclosure. The can end stock 400 may include a metal layer 404, such as aluminum surrounded by a paint layer 402, and a polymer film layer 406. The can end stock 400 may be Figure 1Can cover material 110.
[0147] Figure 5 is a flow chart depicting a process 500 for manufacturing can cover stock according to certain aspects of the present disclosure. At block 502, a metal strip is provided. At an optional block at block 503, the surface roughness of the metal strip may be increased, as described below with reference to Fig.10 The metal strip may be an aluminum strip suitable for forming a can cover material. At frame 504, the metal strip is preheated to a preheating temperature T1. At frame 506, the metal strip is laminated with a PET polymer film. At frame 508, the laminated metal strip is annealed at an annealing temperature T2, wherein the annealing temperature T2 is higher than the melting temperature of the PET polymer film. At frame 510, the annealed metal strip is optionally quenched. At frame 512, a lubricant may be optionally applied to one or both sides of the metal strip.
[0148] Figure 6 602 is a partial top view depicting a portion of a can lid stock 602. According to certain aspects of the present disclosure, the can lid stock 602 includes an unannealed polymer film layer 606. The can lid stock 602 has been separated along the score line 604. It can be seen that the polymer film 606 is feathered outward from the score line 604. It can be considered Figure 6 The can cover stock 602 has poor feathering.
[0149] Figure 7 FIG. 1 is a partial top view of a portion of a can cover stock 702 according to certain aspects of the present disclosure. The can cover stock 702 includes a polymer film layer that has been annealed according to certain aspects of the present disclosure, such as the can cover stock 302 of FIG. 3 . The can cover stock 702 has been separated along the score line 704. The polymer film has not feathered outward from the score line 704. It can be considered Figure 7 The can cover stock 702 has good feathering (eg, feathering of less than 0.8 mm) or no feathering.
[0150] Figure 8 is a schematic diagram of a lamination system 814 according to certain aspects of the present disclosure. The lamination system 814 may be Figure 1 The lamination system 114, or another lamination system, is shown in exaggerated scale. Figure 8 Certain elements depicted in the drawings are for illustration purposes only.
[0151] The laminating system 814 can include a pair of rollers 852 through which the preheated metal strip 804 can pass. The preheated metal strip 804 can include the metal strip 802 that has been preheated, such as by Figure 1 In some cases, the preheated metal strip 804 includes one or more conversion layers 803.
[0152] While passing through roller 852, polymer film 824 can be pressed against preheated metal strip 804 to produce laminated metal strip 806. In some cases, single lamination system 814 can include an additional set of rollers to apply a second polymer film to the side of preheated metal strip 804 opposite polymer film 824. In some cases, roller 852 can additionally apply a second polymer film to the side of preheated metal strip 804 opposite polymer film 824.
[0153] Fig. 9 is a flow chart depicting a process 900 of determining desired conversion layer properties for a laminated metal strip according to certain aspects of the present disclosure. The blushing of certain products, such as CES materials, has traditionally been associated with poor performance or defects in the paint layer of the material. With respect to blushing properties, the properties of the conversion layer have not been considered. The conversion layer typically has a thickness on the nanometer scale, which is typically one or more orders of magnitude thinner than the paint layer or film layer. However, it has been unexpectedly discovered that the properties of the conversion layer can provide a significant and controllable effect on the blushing properties of a metal product (e.g., an aluminum CES material) having a laminated film layer (e.g., a laminated PET film). The metal product can be any suitable metal product, such as the laminated metal strip disclosed above. The properties of the conversion layer (e.g., chemical properties, thickness, or texture) have a significant effect on the blushing properties of the film layer applied to the conversion layer. The blushing properties of the metal product having the laminated film layer are the result of a different mechanism than the standard blushing associated with the metal product after painting. Further, annealing the metal product having the laminated film layer can further affect the blushing properties by a mechanism different from the standard blushing associated with the metal product after painting. It has been discovered that by manipulating the conversion layer properties, the blushing performance of a metal product having a laminated film layer with or without subsequent annealing can be controlled. Process 900 can be used to test the blushing performance of different conversion layer parameter candidates for a given combination of substrate (e.g., aluminum metal strip), film (e.g., PET film), and process step (e.g., post-lamination annealing), so that one or more optimal conversion layer parameters (e.g., combination of substrate, film, and process step) for a particular use case can be selected prior to mass production.
[0154] At block 902, one or more conversion layer parameter candidates may be determined. The conversion layer parameters may be any suitable parameters of the conversion layer or its coating process, such as the type of the conversion layer, the depth of the conversion layer, the parameters of the coating process of the conversion layer (e.g., the type of conversion solution, coating time, processing temperature, drying time, or coating thickness), or other such parameters. Changing one or more parameters of the conversion layer may result in a conversion layer with different characteristics. In some cases, determining one or more conversion layer parameter candidates may include determining a set of conversion solutions with different properties, which result in a set of conversion layers with different characteristics (e.g., thickness, texture, chemical composition, or other characteristics). For example, the set of conversion materials may include chromium phosphate conversion solutions using different concentrations of chromic acid, phosphoric acid, and hydrofluoric acid. In some cases, determining one or more conversion layer parameter candidates may include determining a set of parameters that result in a set of conversion layers with different thicknesses. In some cases, a single parameter candidate will be determined at block 902, and process 900 may still test multiple parameters by determining new conversion layer parameter candidates at optional block 916, as described in further detail below. In some cases, determining translation layer parameter candidates at block 902 may include accessing a set of predetermined parameters that are likely to produce the desired result.
[0155] At block 904, one or more conversion layers are applied to one or more surfaces of one or more metal strips based on the desired conversion layer parameter candidates. In some cases, the conversion layers may be applied to a continuous metal strip or a single metal billet. In some cases, all conversion layers may be applied to different locations of a single metal strip or metal billet, while in other cases, each metal strip or metal billet is treated with a single conversion layer.
[0156] Applying the conversion layer to the surface of the metal strip or billet can include degreasing the surface (e.g., by applying hydrofluoric acid), drying the surface, applying a wet film of a conversion material (e.g., a chromium-based conversion material in a water-based solution) (e.g., by roller coating or other suitable mechanism), and drying the surface to allow the conversion layer to form. In some cases, when multiple conversion layers are tested on a single metal strip or metal billet, the parameters of the conversion layer coating process can be manipulated across one or more dimensions of the surface of the single metal strip or metal billet. For example, the thickness of the wet film can be adjusted with respect to the horizontal distance across the surface of the metal strip or metal billet so that various portions of the metal strip or metal billet at different horizontal locations will have different conversion layer characteristics. In another example, different conversion solutions can be applied at different locations on a single metal strip or metal billet.
[0157] At block 906, a polymer film may be applied to the surface of the metal strip or metal blank having the conversion layer. The polymer film may be applied in any suitable manner, as described above, including with reference to Figure 1 , Figure 5 and Figure 8 .
[0158] At optional block 908, the one or more laminated metal strips or metal blanks may be annealed, as described above, including reference to Figure 1 and Figure 5 .
[0159] At block 910, a pasteurization process may be performed on the one or more laminated metal strips or metal blanks. In some cases, a pasteurization-like process may be performed, which may include performing a process different from pasteurization, but designed to produce a blanching effect similar to a standard pasteurization process. In some cases, a sterilization process may occur instead of a pasteurization process. In some cases, another process that may potentially cause blanching of the one or more laminated metal strips or metal blanks may be performed instead of a pasteurization process. In an example, the one or more laminated metal strips or metal blanks may be placed in water heated to a desired temperature (e.g., a temperature suitable for pasteurization) for a desired duration (e.g., a duration suitable for pasteurization).
[0160] At box 912, each of the one or more laminated metal strips or metal blanks can be tested for blushing properties. The blushing test can be performed using a subjective or objective characterization of the blushing properties of the surface of the metal strip or metal blank. For example, the objective characterization can include measuring blushing using a camera, a light sensor, or other suitable sensor. As an example, the subjective characterization can include having an individual perform a visual inspection of the surface of the metal strip or metal blank and rank the obvious blushing properties. In some cases, a sample that has been processed at box 910 (e.g., pasteurized) can be compared to a sample that has been immersed in water at room temperature for the same duration as the sample immersed in heated water at box 910 to determine the amount of blushing attributable to the process at box 910.
[0161] When multiple conversion layer parameter candidates have been selected at block 904, the testing at block 912 may include testing the blanching properties of multiple samples. At block 914, one or more desired conversion layer parameters may be selected based on the blanching properties tested at block 912. For example, of all conversion layer parameter candidates tested, the conversion layer parameters of the best performing sample (e.g., the sample showing the least amount of blanching) may be selected as the desired conversion layer parameters.
[0162] In some cases, after testing the blanching property at block 912, one or more new conversion layer parameter candidates may be determined at block 916. The one or more new conversion layer parameter candidates may be used to prepare and test one or more new samples having one or more new conversion layers at blocks 904, blocks 906, blocks 908, and blocks 910. When multiple iterations of blocks 904, blocks 906, blocks 908, and blocks 910 are performed (e.g., when block 916 is performed), selecting one or more desired conversion layer parameters at block 914 may include comparing the results of the current iteration of block 912 with the results from the previous iteration of block 912.
[0163] The one or more conversion layer parameters selected at block 914 may be used for mass production. For example, when different conversion layer parameter candidates involve using chromium phosphate conversion solutions having different concentrations of its components, the particular conversion solution selected at block 914 may be provided to a production line for mass production of a final laminated product (e.g., laminated can end stock).
[0164] about Fig.15 Process 900 is described in further detail.
[0165] Fig.10 is a highly enlarged partial cross-sectional view of a portion of a metal strip 1002 having a film 1004 laminated thereon, in accordance with certain aspects of the present disclosure. Fig.10 Certain elements depicted in the drawings are for illustrative purposes only. A metal strip or metal blank may have a surface having a surface roughness. The ability of a film such as a PET film to adhere to the surface of a metal strip or metal blank may be affected by the surface roughness of the metal. The surface roughness may affect not only the adhesion of the film to the metal during lamination, but also the continued adhesion of the film to the metal during the life of the final product. Adhesion may be determined in various ways, as disclosed above. The roughness of the PET film is much lower than the standard surface roughness of the metal strip used for CES, so it can be assumed that a lower roughness that increases the direct contact area during the lamination process will be beneficial. However, it has been unexpectedly determined that a low roughness of the metal surface is detrimental to some properties of the laminated metal product related to adhesion. Therefore, it may be desirable to have a metal surface having a roughness equal to or higher than a minimum threshold roughness for film lamination coating. In some cases, it may also be desirable for the metal surface to have a roughness equal to or lower than a maximum threshold roughness.
[0166] The metal strip 1002 may have a surface roughness 1006 defined by the protrusions and depressions present in the metal surface. The lower surface roughness 1006 may be defined by fewer or less pronounced protrusions and depressions in the metal surface, and thus the surface of the metal is smoother. In addition, the surface roughness 1006 may be defined by the height 1008 between the lowest depression and the highest protrusion of the metal surface (e.g., in a localized area of the metal surface). The metal strip 1002 may have a conversion layer 1010 on the surface. The conversion layer 1010 may generally be small enough not to have a visible or significant effect on the surface roughness 1006 of the metal strip 1002.
[0167] The film 1004 (e.g., PET film) may be applied to the metal strip 1002 as described herein, as described with reference to Figure 1 , Figure 5 and Figure 8 . The film 1004 can be a multilayer film and can include at least a main layer 1012 and a contact layer 1014 (e.g., a heat-matching layer), however the film 1004 can include additional layers. The contact layer 1014 can be a layer that is in direct contact with the surface of the metal strip 1002. The contact layer 1014 can have a melting point that is lower than the melting point of the main layer 1012. During the lamination process, the heat and / or pressure from the lamination process can cause the contact layer 1014 to melt before the main layer 1012, if the main layer 1012 is completely melted, and the contact layer 1014 can melt to the surface topology of the metal strip 1002. The contact layer 1014 can have a thickness 1016. The thickness 1016 of the contact layer 1014 can be equal to or greater than the height 1008 of the surface roughness 1006. If the contact layer 1014 has a thickness 1016 that is too thin, a void may be formed from the contact layer 1014, which melts into the depression and separates from the main layer 1012 supported above the contact layer 1014 by the high protrusion. The contact layer 1014 may have a thickness 1016 that is at least 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, or 55% greater than the height 1008. The contact layer 1014 may have a thickness of 1 micron or 1%, 2%, 3%, 4%, 5%, 10%, 15%, or 20% of 1 micron. The height 1008 of the surface roughness 1006 may be less than 1 micron, less than 0.9 microns, less than 0.8 microns, or less than 0.7 microns. In some cases, height 1008 of surface roughness 1006 may be at least 0.25 microns, 0.5 microns, or 0.6 microns.
[0168] In some cases, the metal strips may be treated to increase their surface roughness prior to lamination. For example, Figure 1The system 100 may include additional roughening equipment upstream of the lamination system 114 for measuring and / or increasing the surface roughness of the metal prior to lamination. In some cases, the metal strip to be laminated may be rolled using rollers designed to impart the desired surface roughness.
[0169] Fig.11 is a partial side cross-sectional view of a lamination system 1114 according to certain aspects of the present disclosure. The lamination system 1114 may be Figure 1 The lamination system 114, or another lamination system, is shown in exaggerated scale. Fig.11 Certain elements depicted in the drawings are for illustration purposes only.
[0170] The laminating system 1114 can include a coating roller 1150 opposite a backing roller 1152 of the metal strip 1102. The preheated metal strip 1104 can pass through a gap formed between the coating roller 1150 and the backing roller 1152. The preheated metal strip 1104 can include the metal strip 1102 that has been preheated, such as by Figure 1 In some cases, the preheated metal strip 1104 comprises one or more conversion layers 1103.
[0171] While passing through coating roller 1150, polymer film 1124 can be pressed against preheated metal strip 1104 to produce laminated metal strip 1106. In some cases, single lamination system 1114 can include additional roller sets to apply a second polymer film to the side of preheated metal strip 1104 opposite polymer film 1124. In some cases, backing roller 1152 can be replaced with an additional coating roller to simultaneously apply a second polymer film to the side of preheated metal strip 1104 opposite polymer film 1124.
[0172] Coating roller 1150 can include a compressible layer 1154 (e.g., a rubber coating) around a metal core 1156. Compressible layer 1154 can be adhered (e.g., by glue) or mechanically fixed to core 1156. Metal core 1156 can be made of any suitable metal such as steel. Compressible layer 1154 can be made of any suitable compressible material such as foam or rubber. In some cases, compressible layer 1154 has a thickness within 1%, 2%, 3%, 4%, 5%, 10%, 15%, or 20% of 2 cm, although other thicknesses can be used. The compressibility of compressible layer 1154 can be selected to achieve the desired lamination result. For example, the type of rubber selected for compressible layer 1154 can include hard rubber, soft rubber, or any rubber therebetween.
[0173] The compressible layer 1154 can help apply the polymer film 1124 to the surface of the metal strip 1102 without the presence of entrapped air. Even a small amount of entrapped air can cause blistering during subsequent processes, such as post-lamination annealing. For example, during post-lamination annealing, entrapped air can blow out the film and cause the film to rupture. Entrained air and bubbles can affect adhesion and blushing, as well as other characteristics of the laminated product. Therefore, the presence of entrapped air and / or bubbles can result in an undesirable product.
[0174] In some cases, the coating roller 1150 can include a mechanism for controlling the temperature of the compressible layer 1154. For example, heat can be extracted from the compressible layer 1154 to ensure that the compressible layer 1154 does not become so hot that it performs poorly, such as by causing it to lose its ability to rebound when the compressive force is released or lose its adhesion to the metal core 1156, thereby causing it to slip off. For example, if the temperature of the compressible layer 1154 at the metal core 1156 (e.g., where the adhesive may be located) reaches a sufficiently high temperature, such as a temperature equal to or exceeding 120° C., the rubber compressible layer 1154 can be delaminated from the metal core 1156. In some cases, the compressible layer 1154 can be cooled externally, such as by applying a coolant fluid (e.g., cold air) to the outer surface of the compressible layer 1154, or by direct conduction with a cooling roller in contact with the outer surface of the compressible layer 1154.
[0175] However, it has been discovered that internal cooling of the compressible layer 1154 can have unexpected benefits. The compressible layer 1154 can be internally cooled by passing a coolant through the channels 1158 within the hollow metal core 1156 of the coating roller 1150. Any suitable coolant can be used, including fluids such as air and water. The coolant can be pumped using any suitable pumping source. The coolant can be temperature controlled by a heat exchanger. The coolant can be designed to pass through the channels 1158 at a desired temperature, which can be higher or lower than ambient room temperature, higher or lower than the temperature of the compressible layer 1154, and higher or lower than the temperature of the preheated metal strip 1104. Therefore, the coolant can act to increase or decrease the temperature of the compressible layer 1154. When the hollow metal core 1156 is used to provide temperature control of the compressible layer 1154, the core 1156 can be made of a material with high thermal conductivity. The compressible layer 1154 may be selected to have a high or low thermal conductivity, however improved results may be obtained when using a compressible layer 1154 that does not have a high thermal conductivity.
[0176] In some cases, a heated coolant may be passed through the channels 1158 prior to the lamination process to heat the compressible layer 1154 so that the compressible layer 1154 is hot enough to ensure that the contact layer of the polymer film 1124 is melted or semi-melted when it is pressed against the preheated metal strip 1104, thereby allowing the contact layer to melt into the protrusions and depressions of the metal strip 1104. In some cases, a cooled coolant (e.g., lower than the temperature of the preheated metal strip 1104) may be passed through the channels 1158 during the lamination process to remove heat from the compressible layer 1154. Because the compressible layer 1154 is continuously heated by the environment of the lamination process (e.g., heat from the preheated metal strip 1104) and any other heating elements near the lamination nip (e.g., the space between the coating roll 1150 and the backing roll 1152), the outer surface of the compressible layer 1154 is pulled toward the high temperature. However, the inner surface of the compressible layer 1154 is cooled by conduction with the hollow metal core 1156 and the coolant passing therethrough. Thus, the use of the hollow metal core 1156 can ensure that the inner surface of the compressible layer 1154 is maintained at a suitable temperature (e.g., to avoid delamination of the compressible layer 1154) despite the higher temperature at its outer surface. Thus, a radial temperature gradient is induced in the compressible layer 1154.
[0177] Further, by forming the compressible layer 1154 from a material having a suitable low thermal conductivity and internally cooling the compressible layer 1154 through the use of a hollow metal core 1156, the temperature of the outer surface of the compressible layer 1154 can be maintained at a higher temperature without having to worry about the inner surface delaminating from the metal core 1156.
[0178] The ability to maintain the compressible layer 1154 at a higher temperature (e.g., higher than if internal cooling were not used) has a number of benefits. The higher temperature of the outer surface of the compressible layer 1154 can allow the metal strip 1102 to be preheated to a lesser extent, thereby saving energy. For example, the higher temperature of the outer surface of the compressible layer 1154 can be used to melt the contact layer of the polymer film 1124, thus eliminating the need to rely too much on heat from the preheated metal strip 1104 to melt the contact layer of the polymer film 1124. In addition, the ability to have a larger window of available temperatures for preheating the metal strip 1102 by being able to support a larger window of temperature of the outer surface of the compressible layer 1154 allows additional upstream and downstream processes to be more easily customized to work with a lamination system, such as the lamination system 1114.
[0179] For example, a downstream process may require a metal strip at about 200° C. Typically, without an internally cooled compressible layer 1154, the external temperature of the compressible layer would be maintained at no greater than about 70° C., thus requiring the metal strip to be preheated to about 220° C. Therefore, the preheated metal strip would need to be cooled before entering the downstream process. However, when an internally cooled compressible layer 1154 is used, the external temperature of the compressible layer can be set to about 90° C., thereby allowing the metal strip 1102 to be preheated to about 200° C., allowing the metal strip 1102 to enter the downstream process more quickly and more efficiently overall.
[0180] Additionally, allowing the outer surface of the compressible layer 1154 to reach a higher temperature may allow the lamination system 1114 to operate at a faster speed, and thus may allow the entire processing line to operate at a faster speed.
[0181] Fig.12 is a schematic diagram illustrating a control system 1200 for a coating roller 1208 of a laminating system according to certain aspects of the present disclosure. The coating roller 1208 may be Fig.11 The coating roller 1150. The control system 1200 may include a controller 1202, which may be any suitable controller or processor. The controller 1202 may be coupled to a data storage 1204 for storing programming instructions, collected data, models, predicted data, presets, and other information. The controller 1202 may be coupled to a coolant source 1206 for providing and / or circulating a coolant through the coating roller 1208. The controller 1202 may transmit a command signal to the coolant source 2106 so that the coolant source 2106 adjusts the amount of cooling or heating to a desired level. The command signal may cause the coolant source 2106 to adjust the volume flow rate of the coolant, the temperature of the coolant, or other characteristics of the coolant or its flow through the coating roller 1208. The coolant may pass through a conduit 1212, a conduit 1214 between the coolant source 1206 and the coating roller 1208. The coolant source 1206 may include a pressurized source (eg, a pump), a heat exchanger, an optional storage tank, and any other suitable elements for providing control of the flow of the coolant or the coolant through the coating roller 1208 .
[0182] The controller 1202 may be coupled to one or more sensors, including one or more temperature sensors 1210. The temperature sensor 1210 may be located within, near, adjacent to, or spaced apart from the coating roller 1208 to measure a temperature associated with the coating roller 1208. For example, the temperature sensor may measure an internal coolant temperature, a temperature of a metal core, a temperature of an inner surface of a compressible layer, or a temperature of an outer surface of a compressible layer. Any suitable temperature sensor 1210 may be used, including contact and non-contact temperature sensors. In some cases, the temperature sensor 1210 may measure the temperature of an element near the coating roller 1208 (e.g., a polymer film, a metal strip, or other element) to infer the temperature of the coating roller 1208. Signals from the one or more temperature sensors 1210 may provide feedback to the controller 1202 to help the controller 1202 ensure the desired operation of the coating roller 1208 (e.g., to ensure a sufficiently low temperature of the inner surface of the compressible layer or a sufficiently high temperature of the outer surface of the compressible layer).
[0183] In some cases, the controller 1202 can instruct the coolant source 1206 to pump heated coolant through the coating roller 1208 to raise the temperature of the outer surface of the compressible layer of the coating roller 1208 to a minimum desired temperature. The controller 1202 can then pump the cooled coolant to maintain the temperature of the outer surface of the compressible layer within a desired range during the lamination process (e.g., as the hotter preheated metal strip conducts heat into the coating roller 1208). The "cooled coolant" may be cooler than the preheated metal strip, but may still be warmer than the ambient room temperature. In some cases, the controller 1202 can control the optional external heater 1216 to preheat the coating roller 1208, instead of or in addition to pumping heated coolant through the coating roller 1208.
[0184] In some cases, the controller 1202 can operate based on feedback from the one or more temperature sensors 1210 and / or other sensors. In some cases, the controller 1202 can operate based on a model (e.g., a thermal model) stored in the data storage 1204, instead of or in addition to sensors such as the one or more temperature sensors 1210 and / or other sensors. For example, the controller 1202 can automatically increase the amount of cooling provided to the coating roller 1208 whenever the line speed increases.
[0185] Fig.13 13 is a graph 1300 depicting temperature as a function of radial distance from the axis of rotation of a coating roller of a laminating system according to certain aspects of the present disclosure. The coating roller may be Fig.111150 of a coating roller. The graph depicts a temperature curve 1302 at various radial distances from the axis of rotation (e.g., the center) of the coating roller. The graph 1300 and its elements, including the curve 1302 and the depicted area, are not drawn to scale and are shown without cells for illustrative purposes. In a direction outward from the center of the coating roller, the coating roller can include a coolant zone, a metal core zone, and a rubber coating zone. The film can be placed near the coating roller so that in the same direction, the film includes a main layer and a contact layer. The film can be pressed against the metal strip.
[0186] The preheated metal strip may be provided at a temperature 1304 (e.g., 200° C.). However, a coolant may be provided at a temperature 1306, which may be substantially cooler than the preheated metal strip. Thus, there is a temperature gradient between the coolant and the metal strip, approximating curve 1302. The coolant 1306 will absorb heat from the inner surface 1310 of the compressible layer, attempting to pull the temperature of the inner surface 1310 downward toward temperature 1306. At the same time, the higher temperature 1304 of the preheated metal strip will be directed through the membrane and will attempt to raise the temperature of the outer surface 1312 of the compressible layer. Thus, there is a temperature gradient within the compressible layer, which defines a temperature gap 1308 between the inner surface 1310 and the outer surface 1312. This temperature gap 1308 may be controlled by selecting a material for the compressible layer that has a desired thermal conductivity. This temperature gap 1308 may be further controlled by adjusting the temperature 1306 of the coolant 1306 and the temperature 1305 of the preheated metal strip. The temperature gap 1308 can be controlled so that the temperature of the inner surface 1310 is maintained below a maximum set point 1314 (e.g., the highest temperature before the risk of delamination or other failure becomes unacceptably high, such as the melting temperature of a glue used to adhere the compressible layer to the metal core) and so that the temperature of the outer surface 1312 is maintained above a minimum set point 1316 (e.g., the lowest temperature to ensure proper melting of the contact layer of the polymer film during lamination).
[0187] Fig.14 is a flow chart depicting a process 1400 for controlling the temperature of a coating roller during a lamination process according to certain aspects of the present disclosure. The process 1400 may be used Fig.11 The coating roller 1150 and laminating system 1114. At optional block 1402, the compressible layer of the coating roller can be preheated. As described herein, the compressible layer can be preheated using a heated cooling fluid and / or an external heater. Other mechanisms can be used to preheat the compressible layer (e.g., a resistive heater embedded in a metal core).
[0188] At block 1404, a compressive force is applied between the preheated metal strip and the coating roller. The compressive force may be applied to firmly adhere the polymer film to the metal strip.
[0189] At box 1406, a temperature associated with the surface of the compressible layer can be determined. The temperature can include the temperature of the inner surface or the outer surface of the compressible layer. Determining the temperature can include directly measuring the temperature of the compressible layer, measuring the temperature of nearby elements, and inferring the temperature of the compressible layer, or using a model with or without input from other sensors. At box 1408, the parameters of the coolant source can be adjusted based on the temperature determined at box 1406. At box 1410, the parameters of the coolant source can adjust the amount of cooling or heating provided to the compressible layer from the coolant passing through the coating roller. The parameters of the coolant source can include parameters associated with pressure sources, valves, heat exchangers, and other such parameters. Adjusting the parameters of the coolant source can result in changes in the volume flow rate or temperature of the coolant, as well as other characteristics.
[0190] At block 1410, the coolant is passed through the coating roller. The coolant may be passed according to the parameters set at block 1408 or according to previously set parameters. Passing the coolant through the coating roller may include inducing a temperature gradient in the coating roller. The temperature gradient may be induced such that the temperature of the inner surface of the compressible layer is maintained below a maximum set point and the temperature of the outer surface of the compressible layer is maintained above a minimum set point.
[0191] During continuous lamination, the coolant may continuously flow through the coating roller at block 1410 while applying a compressive force between the coating roller and the preheated metal strip at block 1404. During continuous lamination, the temperature of the surface of the compressible layer may be continuously or repeatedly determined at block 1406 to provide continuous or repeated adjustments to the parameters of the coolant source at block 1408.
[0192] In some cases, process 1400 may be performed without block 1406 if inference or models are used to determine appropriate parameters for the coolant source.
[0193] In some cases, reference Figure 11 to Figure 14 The described systems and methods can laminate films to metal strips at high speeds and with greatly reduced risk of air entrainment or blistering. In some cases, these systems and methods can be used to control the amount of air entrainment or blistering to produce certain desired results. For example, for certain use cases where lower thermal conductivity or a rougher surface is desired, increased air entrainment or blistering may be preferred. In some cases, these systems and methods can be used to advantage when the laminated metal strip is to be annealed, but these systems and methods can also be used to provide a laminated metal strip that is not thereafter annealed.
[0194] Fig.15is a graphical matrix depicting a group of laminated aluminum metal samples 1500 that have been processed and tested according to certain aspects of the present disclosure. The group 1500 is arranged vertically according to the pre-treatment method used (e.g., as the conversion layer applied according to process 900), and the group is arranged horizontally according to the annealing temperature used (e.g., T2 at block 508 of process 500). Fig.15 As seen in , testing and comparing samples can inform the determination of which one or more combinations of one or more pretreatment methods and one or more annealing temperatures will produce the desired results. Separate from the different pretreatments and anneals, each of the samples in group 1500 contains aluminum panels that have been laminated with the same type of film.
[0195] Each sample of group 1500 shows the result of similar test procedure, including acid bath test and delamination test.For acid bath test, about lower two-thirds of each sample is immersed in 3% acetic acid bath at 100 ℃ for 30 minutes.Some degree of blushing can be seen in each sample, and some samples have more or less blushing than other samples.According to visual inspection, the blushing level is scored on a scale of 1 to 10, wherein 7 is the expected critical line, and 10 is the best performance (e.g., minimum blushing).For delamination test, each sample is scratched in all directions with a material having a hardness greater than that of aluminum metal strip (e.g., greater than aluminum itself and / or greater than the conversion layer of the metal strip).Usually, delamination test includes diagonal scratch pattern and vertical-horizontal scratch pattern.Record the delamination presented by each sample and the amount of delamination determined.The presence of delamination can be easily seen, especially in vertical-horizontal scratch pattern.The amount of delamination can be determined based on visual inspection.
[0196] The first row of samples, including samples 1502, 1504, 1506, 1508, and 1510, were all pretreated with a silane-based (e.g., tetrahydrosilane-based) pretreatment. The second row of samples, including samples 1512, 1514, 1516, 1518, and 1520, were all pretreated with a chromium III-based (e.g., chromium hexaoxide-based) pretreatment. The third row of samples, including samples 1522, 1524, 1526, 1528, and 1530, were all pretreated with a titanium / zirconium-based pretreatment.
[0197] All first column samples, including samples 1502, 1512, and 1522, were prepared without post-lamination annealing (e.g., without performing block 508 of process 500). All second column samples, including samples 1504, 1514, and 1524, were annealed at 245° C. after lamination (e.g., T2=245° C. during block 508 of process 500). All third column samples, including samples 1506, 1516, and 1526, were annealed at 250° C. after lamination (e.g., T2=250° C. during block 508 of process 500). All fourth column samples, including samples 1508, 1518, and 1528, were annealed at 275° C. after lamination (e.g., T2=275° C. during block 508 of process 500). All fifth column samples, including sample 1510 , sample 1520 , and sample 1530 , are annealed at 290° C. (eg, T2 = 290° C. during block 508 of process 500 ) after lamination.
[0198] like Fig.15 As can be seen in the Figures, samples 1508, 1510, 1518, 1520, 1528, and 1530 annealed at a temperature equal to or higher than 275° C., such as higher than 250° C. after lamination performed well in the delamination test, with little or no noticeable delamination of the film after the test. In the case of no annealing or annealing at a temperature equal to or lower than 250° C., the amount of delamination is substantially worse.
[0199] Can be Fig.15 The blush performance of the samples of group 1500 can be seen in and / or quantified as follows on a scale of 1 to 10, with 10 being the best. Sample 1502, sample 1504, sample 1506, sample 1508, sample 1510 can have blush values of 4, 4, 5, 1, and 1, respectively. Sample 1512, sample 1514, sample 1516, sample 1518, sample 1520 can have blush values of 9, 9, 8, 1, and 1, respectively. Sample 1522, sample 1524, sample 1526, sample 1528, sample 130 can have blush values of 4, 4, 6, 1, and 1, respectively. Notably, the blushing performance can be characterized by comparing approximately the lower two-thirds of each sample to a sample or portion of aluminum metal that has not been exposed to any acid test or similar conditions, or has been exposed to a neutral bath (e.g., a deionized water bath) under similar conditions (e.g., time and temperature) as the acid tested sample. For example, although the color difference between the upper third and the lower two-thirds of sample 1530 may be only slight, the blushing performance of sample 1530 can be characterized as 1 compared to the untreated aluminum metal piece.
[0200] The foregoing description of the embodiments, including the illustrated embodiments, is presented for purposes of illustration and description only and is not intended to be exhaustive or to limit the precise form disclosed. Many modifications, adaptations, and uses thereof will be apparent to those skilled in the art. Although described with reference to moving metal strips in a continuous production line, aspects of the present disclosure are applicable on stationary metal billets.
[0201] As used below, any reference to a series of instances should be understood as a separate reference to each of those instances (eg, "Instance 1 through Instance 4" should be understood as "Instance 1, Instance 2, Instance 3, or Instance 4").
[0202] Example 1 is a method for preparing a can cover material, the method comprising: preheating a metal strip to a first temperature below 250°C; laminating a polymer film to a first side of the metal strip to produce a laminated metal strip, wherein a main component of the polymer film has a melting temperature higher than the first temperature; and annealing the laminated metal strip at an annealing temperature, wherein the annealing temperature is higher than the melting temperature of the polymer film.
[0203] Example 2 is the method of Example 1, wherein the metal strip is an aluminum strip.
[0204] Example 3 is the method of example 1 or example 2, wherein the metal strip is AA5182 aluminum alloy.
[0205] Example 4 is the method of example 1 to example 3, further comprising applying a conversion coating to the metal strip, wherein laminating the polymer film to the first side of the metal strip comprises laminating the polymer film to the conversion coating.
[0206] Example 5 is the method of example 1 to example 4, wherein laminating the polymer film comprises laminating a polyethylene terephthalate film to the metal strip.
[0207] Example 6 is the method of Examples 1 to 5, further comprising applying a paint layer or another polymer film to the second side of the metal strip, wherein the first side of the metal strip corresponds to the inner side of the can lid formed by the metal strip, and wherein the second side of the metal strip corresponds to the outer side of the can lid formed by the metal strip.
[0208] Example 7 is the method of examples 1 to 6, wherein annealing the laminated metal strips comprises raising the temperature of the polymer film for a duration sufficient to melt the polymer film into the surface texture of the metal strips.
[0209] Example 8 is the method of examples 1 to 7, wherein annealing the laminated metal strips comprises raising the temperature of the polymer film to at least 250°C.
[0210] Example 9 is the method of examples 1 to 8, wherein annealing the laminated metal strips comprises raising the temperature of the polymer film to at least 265°C.
[0211] Example 10 is the method of examples 1 to 9, wherein annealing the laminated metal strips comprises raising the temperature of the polymer film to at least 280°C.
[0212] Example 11 is the method of Example 1 to Example 10, further comprising cooling the laminated metal strips after annealing the laminated metal strips to ensure that the polymer film remains amorphous.
[0213] Example 12 is the method of Example 1 to Example 11, further comprising applying a lubricant to the laminated metal strip after annealing the laminated metal strip.
[0214] Example 13 is the method of Example 1 to Example 12, the method further comprising: selecting a conversion layer parameter from a plurality of conversion layer parameter candidates based on the tested performance and applying a conversion layer to the metal strip according to the conversion layer parameter before laminating the polymer film to the first side of the metal strip.
[0215] Example 14 is the method of Example 13, wherein the property tested is blush performance.
[0216] Example 15 is a method for determining conversion layer parameters, the method comprising: determining a plurality of conversion layer parameter candidates; preparing a can cover material sample for each of the plurality of conversion layer parameter candidates according to the methods of Examples 1 to 14; evaluating the whitening performance of each of the can cover material samples; and selecting conversion layer parameters from the plurality of conversion layer parameter candidates based on the evaluated whitening performance.
[0217] Example 16 is the method of Example 1 to Example 15, further comprising adjusting the surface roughness of the metal strip before laminating the polymer film to the first side of the metal strip.
[0218] Example 17 is the method of Example 16, wherein adjusting the surface roughness comprises reducing a height of the surface roughness to a value below a thickness of the contact layer of the polymer film.
[0219] Example 18 is the method of Examples 1 to 17, wherein laminating the polymer film to the first side of the metal strip comprises: pressing the polymer film against the first side of the metal strip using a coating roller having a compressible layer surrounding a hollow metal core; and passing a fluid through the hollow metal core to control the temperature of the compressible layer.
[0220] Example 19 is the method of Example 18, further comprising preheating the compressible layer before laminating the polymer film to the first side of the metal strip.
[0221] Example 20 is the method of example 18 or example 19, wherein passing the fluid through the hollow metal core includes cooling the fluid to extract heat from the inner surface of the compressible layer to induce a thermal gradient between the inner surface of the compressible layer and the outer surface of the compressible layer.
[0222] Example 21 is the method of Example 20, wherein cooling the fluid comprises reducing the temperature of the fluid sufficiently to maintain an internal temperature at the inner surface of the compressible layer below a maximum set point and maintain an external temperature at the outer surface of the compressible layer above a minimum set point.
[0223] Example 22 is the method of example 18 to example 21, the method further comprising: determining a temperature of the compressible layer; and adjusting a temperature or a volumetric flow rate of the fluid based on the temperature of the compressible layer.
[0224] Example 23 is a can cover material product prepared according to the methods described in Examples 1 to 22.
[0225] Example 24 is a beverage can comprising a body and a cap, wherein the cap is formed from the can end stock prepared according to the method described in Examples 1 to 22.
[0226] Example 25 is a system comprising: a preheating furnace, which is used to receive a metal strip and preheat the metal strip to a preheating temperature; a laminating system, which is located downstream of the preheating furnace, and is used to receive the metal strip at the preheating temperature and apply a polymer film to the first side of the metal strip, wherein the preheating temperature is lower than the melting temperature of the main component of the polymer film; and an annealing furnace, which is located downstream of the laminating system, and is used to receive the laminated metal strip and heat the laminated metal strip to an annealing temperature, wherein the annealing temperature is higher than the melting temperature of the main component of the polymer film.
[0227] Example 26 is the system of Example 25, wherein the metal strip is an aluminum strip.
[0228] Example 27 is the system of example 25 or example 26, wherein the metal strip is AA5182 aluminum alloy.
[0229] Example 28 is the system of example 25 to example 27, the system further comprising a conversion coating application system for applying the conversion coating to the metal strip, wherein the lamination system is configured to apply the polymer film to the conversion coating.
[0230] Example 29 is the system of example 25-example 28, wherein the lamination system is coupled to a supply of polyethylene terephthalate film.
[0231] Example 30 is the system of examples 25 to 29, further comprising a paint coating system for applying a layer of paint to the second side of the metal strip.
[0232] Example 31 is the system of Examples 25 to 30, wherein the lamination system is configured to apply an additional polymer film to a second side of the metal strip opposite the first side.
[0233] Example 32 is the system of Example 25 to Example 31, wherein the annealing furnace has a length sufficient to elevate the temperature of the polymer film for a duration sufficient to melt the polymer film into the surface texture of the metal strip.
[0234] Example 33 is the system of Example 25 to Example 32, wherein the annealing furnace is configured to provide heat sufficient to raise the temperature of the polymer film to at least 250°C.
[0235] Example 34 is the system of Examples 25 to 33, wherein the annealing furnace is configured to provide heat sufficient to raise the temperature of the polymer film to at least 265°C.
[0236] Example 35 is the system of Examples 25 to 34, wherein the annealing furnace is configured to provide heat sufficient to raise the temperature of the polymer film to at least 280°C.
[0237] Example 36 is the system of Example 25 to Example 35, further comprising a conversion layer applicator for applying a conversion layer to the metal strip according to conversion layer parameters selected from a plurality of conversion layer parameter candidates based on tested performance.
[0238] Example 37 is the system of Example 25 to Example 36, further comprising a surface roughness adjuster for adjusting the surface roughness of the metal strip, wherein the surface roughness adjuster is located upstream of the lamination system.
[0239] Example 38 is the system of Example 37, wherein the surface roughness adjuster is configured to reduce the height of the surface roughness to a value below the thickness of the contact layer of the polymer film.
[0240] Example 39 is the system of Examples 25 to 38, wherein the lamination system includes: a coating roller comprising a compressible layer surrounding a hollow metal core; and a coolant source for providing a coolant to the channels of the hollow metal core to control the temperature of the compressible layer.
[0241] Example 40 is the system of example 39, further comprising an external heater positioned proximate to the compressible layer to preheat the compressible layer.
[0242] Example 41 is the system of Example 39 or Example 40, wherein the lamination system further includes a controller coupled to the coolant source for adjusting the volume flow rate or temperature of the coolant provided by the coolant source to maintain a temperature gradient across the inner surface of the compressible layer and the outer surface of the compressible layer.
[0243] Example 42 is the system of example 41, wherein the lamination system further includes a temperature sensor coupled to the controller for providing a temperature signal associated with a temperature of the compressible layer.
[0244] Example 43 is the system of example 41 or example 42, wherein the lamination system further includes a data storage containing the model, and wherein the controller is coupled to the data storage to control the coolant source based on the model.
[0245] Example 44 is the system of Example 39 or Example 43, wherein the lamination system further includes a controller coupled to the coolant source for adjusting the volume flow rate or temperature of the coolant provided by the coolant source to maintain the internal temperature of the inner surface of the compressible layer below a maximum set point and maintain the external temperature of the outer surface of the compressible layer above a minimum set point.
[0246] Example 45 is a method for laminating metal, the method comprising: pressing a polymer film against a first side of a preheated metal strip using a coating roller having a compressible layer surrounding a hollow metal core; and passing a fluid through the hollow metal core to control the temperature of the compressible layer.
[0247] Example 46 is the method of Example 45, further comprising preheating the compressible layer before laminating the polymer film to the first side of the metal strip.
[0248] Example 47 is the method of Example 46, wherein preheating the compressible layer comprises passing a heated fluid through the hollow metal core.
[0249] Example 48 is the method of Example 46 or Example 47, wherein preheating the compressible layer comprises externally heating the compressible layer.
[0250] Example 49 is the method of examples 45 to 48, wherein passing the fluid through the hollow metal core includes cooling the fluid to extract heat from the inner surface of the compressible layer to induce a thermal gradient between the inner surface of the compressible layer and the outer surface of the compressible layer.
[0251] Example 50 is the method of Examples 45 to 49, wherein cooling the fluid comprises sufficiently reducing the temperature of the fluid to maintain an internal temperature at an inner surface of the compressible layer below a maximum set point and to maintain an external temperature at an outer surface of the compressible layer above a minimum set point.
[0252] Example 51 is the method of examples 45 to 50, the method further comprising: determining a temperature of the compressible layer; and adjusting a temperature or a volumetric flow rate of the fluid based on the temperature of the compressible layer.
[0253] Example 52 is the method of Example 51, wherein determining the temperature of the compressible layer includes receiving a temperature measurement of the compressible layer from a temperature sensor.
[0254] Example 53 is the method of Example 51 or Example 52, wherein determining the temperature of the compressible layer includes receiving a temperature measurement of an element proximate to the compressible layer from a temperature sensor.
[0255] Example 54 is the method of Example 51 to Example 53, wherein determining the temperature of the compressible layer includes accessing a model.
[0256] Example 55 is the method of examples 45 to 54, further comprising: sensing a change in a linear velocity of the preheated metal strip; and adjusting a temperature or a volumetric flow rate of the fluid based on the change in the linear velocity.
Claims
1. A method for preparing a can cover material, comprising: preheating the metal strip to a first temperature below 250°C; laminating a polymer film to the first side of the metal strip to produce a laminated metal strip, wherein a major component of the polymer film has a melting temperature higher than the first temperature; and The laminated metal strips are annealed at an annealing temperature, wherein the annealing temperature is higher than the melting temperature of the polymer film. The method according to claim 1 , wherein the metal strip is an aluminum strip.
3. The method of claim 1, wherein the metal strip is AA5182 aluminum alloy. 4 . The method of claim 1 , further comprising applying a conversion coating to the metal strip, wherein laminating the polymer film to the first side of the metal strip comprises laminating the polymer film to the conversion coating.
5. The method of claim 1, wherein laminating the polymer film comprises laminating a polyethylene terephthalate film to the metal strip.
6. The method according to claim 1 further includes applying a paint layer or another polymer film to the second side of the metal strip, wherein the first side of the metal strip corresponds to the inner side of the can cover formed by the metal strip, and wherein the second side of the metal strip corresponds to the outer side of the can cover formed by the metal strip.
7. The method of claim 1, wherein annealing the laminated metal strip comprises raising the temperature of the polymer film for a duration sufficient to melt the polymer film into the surface texture of the metal strip.
8. The method of claim 1, wherein annealing the laminated metal strips comprises raising the temperature of the polymer film to at least 250°C.
9. The method of claim 1, wherein annealing the laminated metal strips comprises raising the temperature of the polymer film to at least 265°C.
10. The method of claim 1, wherein annealing the laminated metal strips comprises raising the temperature of the polymer film to at least 280°C.
Citation Information
Patent Citations
Can end formed from laminated metal sheet
US5582319A
Laminated metal sheet
CN1032765A
Laminating polyester onto metal substrate
US7942991B1