Multi-layer reinforced composite thermoplastic elastomer foaming sheet as well as preparation method and application thereof

By adopting a multi-layer reinforced composite structure in the polyolefin thermoplastic elastomer foamed sheet, the combination of polypropylene laminated material and thermoplastic elastomer composition foamed sheet is solved, and the scratch resistance and compatibility problems are achieved. High performance and high recycling polyolefin composite materials.

CN118906602AActive Publication Date: 2024-11-08CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310511959.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-08
Estimated Expiration
2043-05-08

AI Technical Summary

Technical Problem

The existing polyolefin thermoplastic elastomer foamed sheets have low scratch resistance and low bending modulus during use, which leads to scratches and deformations easily in long-term use, and the composite reinforcement sheet and foamed sheet are between There are compatibility problems, it is difficult to achieve ideal physical properties, and it is difficult to recycle and process.

Method used

Multi-layer reinforced composite thermoplastic elastomer foamed sheets are made of polypropylene laminated material and thermoplastic elastomer composition foamed sheets. The high-strength, high-impact polypropylene composite sheets are used as reinforced composite materials to form a sandwich structure , improves apparent density and physical properties, and can be directly crushed, melted and repelled during recycling.

Benefits of technology

It achieves high strength, high impact resistance and high peel strength, while improving the compatibility and recycling rate of materials, reducing density and thermal conductivity, and expanding the application field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004221418990000091
    Figure BDA0004221418990000091
  • Figure BDA0004221418990000231
    Figure BDA0004221418990000231
  • Figure BDA0004221418990000261
    Figure BDA0004221418990000261
Patent Text Reader

Abstract

The invention belongs to the technical field of high polymer materials, and particularly relates to a multi-layer reinforced composite thermoplastic elastomer foaming sheet as well as a preparation method and application thereof. The multi-layer reinforced composite foamed sheet has a laminated structure and comprises at least two layers of reinforced composite sheets and at least one layer of thermoplastic elastomer composition foamed sheet, and the reinforced composite sheets are arranged on the outer layers of the multi-layer reinforced composite foamed sheet; the reinforced composite sheet material comprises at least one layer of polypropylene sheet material and / or at least one layer of polypropylene fabric obtained by weaving the polypropylene sheet material; the polypropylene sheet comprises a layer A and layers B and B'located on the two sides of the layer A, and the structure of the polypropylene sheet is BAB '; the thermoplastic elastomer composition foaming sheet and the reinforced composite sheet are bonded through hot-pressing fusion. The multi-layer reinforced composite thermoplastic elastomer foaming sheet has excellent apparent density, physical properties and thermal insulation properties, also has the advantages of high strength, high impact resistance and high peel strength, and is convenient to recycle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a multi-layer reinforced composite thermoplastic elastomer foam sheet and a preparation method and application thereof. Background Art

[0002] Polyolefin thermoplastic elastomer (POE) is an elastic material composed of two components, rubber and polyolefin. Taking vinyl thermoplastic elastomer as an example, the crystalline region of the polyethylene chain as the resin phase mainly plays the role of physical crosslinking points, and the introduction of a certain amount of α-olefin can weaken the crystalline region of the polyethylene chain, forming the so-called rubber phase (amorphous region of rubber elastomer). The relative molecular mass distribution of POE is very narrow and the side chains are short, so it has excellent physical and mechanical properties (good elasticity, high strength, and high elongation). In addition, its molecular chain is saturated and contains fewer tertiary carbon atoms, which makes POE also have excellent heat aging resistance and UV resistance. The narrow relative molecular mass distribution makes the material less prone to bending during injection and extrusion processing. Because POE has high strength and elongation, and has excellent aging resistance, products with low requirements for heat resistance and permanent deformation can be directly processed into products using POE, which can be recycled while improving production efficiency. In order to reduce the cost of raw materials and improve certain material properties (such as tear strength, hardness, etc.), a certain amount of fillers, reinforcing agents and processing aids need to be added during compounding to improve the overall performance and reduce costs.

[0003] POE foam material has excellent properties such as good impact resistance, shock resistance, heat insulation, sound absorption, and moisture resistance. As a polyolefin thermoplastic elastomer composition foam material, the rebound rate and other properties of POE / EVA composite foam material are better than those of traditional foam materials such as pure EVA (ethylene-vinyl acetate copolymer). The application of foam materials is not limited to foam sole materials. There are two major categories of soles: foam slippers and sports shoe midsoles, which are divided into super elastic and ultra light directions. In the field of sports and leisure, POE composite foam materials also have a large number of extended applications, such as common yoga mats, sun hats, life jackets, kickboards, helmet shock pads, and even home decoration sound insulation wallpaper. When used for lightweight structural materials, due to the low scratch resistance and low bending modulus of POE foam materials, long-term use is prone to scratches and deformation, thus affecting the performance.

[0004] In order to further improve the physical properties of polyolefin thermoplastic elastomer composition foam sheet products, it is currently a new process scheme to compound inorganic or organic reinforcing sheets on the surface of polyolefin thermoplastic elastomer composition foam sheets. In the existing technology, the composite reinforcing sheets have high requirements for mechanical properties, and mainly use composite materials such as glass fiber / carbon fiber reinforced thermoplastic resins. These reinforcing sheets are prone to compatibility problems with polyolefin thermoplastic elastomer composition foam sheets, resulting in not only difficulty in achieving ideal physical properties such as compression and heat insulation. Even if a polyolefin thermoplastic elastomer foam sheet product that meets the product performance is successfully obtained, the presence of the reinforcing sheet brings problems such as high apparent density, long molding time and high energy consumption, and it is difficult to recycle and process after mixing the reinforcing phase materials other than polyolefin thermoplastic elastomers (such as glass fiber, carbon fiber). It is expected that there is a high-strength and high-impact polyolefin composite sheet material that can be used for reinforcement on the surface of a polyolefin thermoplastic elastomer foam sheet material. The polyolefin thermoplastic elastomer foam sheet product does not need to be separated and processed during recycling, and can be directly crushed and melted, and then granulated again for use. However, conventional polyolefin composite sheets either do not meet the requirements in terms of strength, impact resistance, or interlayer peeling strength. There is no polyolefin composite sheet material that has high strength, high impact resistance, and high peeling strength. Therefore, how to provide a polyolefin composite sheet material that has high strength, high impact resistance, and high peeling strength as a reinforced composite thermoplastic elastomer foam sheet material for reinforcing the sheet material is the research purpose of the present invention. Summary of the invention

[0005] In view of the deficiencies of the above-mentioned prior art, the present invention provides a multi-layer reinforced composite thermoplastic elastomer foam sheet and its preparation method and application. The foam sheet is composed of a polypropylene laminate material and a thermoplastic elastomer composition foam sheet. Specifically, the multi-layer reinforced composite thermoplastic elastomer foam sheet uses a high-strength and high-impact polypropylene composite sheet as a reinforced composite sheet of a thermoplastic polyolefin elastomer composite foam material, so that the multi-layer reinforced composite thermoplastic elastomer foam sheet has excellent apparent density, physical properties and thermal insulation performance, and also has the advantages of high strength, high impact resistance and high peel strength. Moreover, compared with other pre-reinforced sheets of non-pure polyolefin materials on the market, the multi-layer reinforced composite thermoplastic elastomer foam sheet has greatly improved compatibility, and does not need to be separated and processed during recycling, and can be directly crushed and melted, and granulated again for application, which has broad market prospects in the field of thermoplastic polyolefin elastomer composition foam sheet technology. The inventor of the present invention found that the thermoplastic elastomer composition foam material and the reinforced composite sheet form a sandwich structure. The thermoplastic elastomer composition foam material has good buffering and energy absorption properties, increases the drop weight impact strength of the multi-layer reinforced composite thermoplastic elastomer foam sheet, reduces the density, and reduces the thermal conductivity while achieving lightweight. The reinforced composite sheet also improves the tensile strength of the thermoplastic elastomer composition foam material, which can effectively expand the application fields of the two materials, such as the thermal insulation field of the thermoplastic elastomer composition foam material with high mechanical requirements, and the application fields of polypropylene reinforced materials with lightweight requirements.

[0006] The first aspect of the present invention is to provide a multi-layer reinforced composite foam sheet (i.e., a multi-layer reinforced composite thermoplastic elastomer foam sheet) having a laminated structure, comprising at least two layers of reinforced composite sheets and at least one layer of thermoplastic elastomer composition foam sheet, and the outer layers of the multi-layer reinforced composite foam sheet are all reinforced composite sheets;

[0007] The reinforced composite sheet comprises at least one layer of polypropylene sheet and / or at least one layer of polypropylene fabric woven from polypropylene sheets; wherein the polypropylene sheet comprises layer A and layers B and B' located on both sides of layer A, and the structure is BAB';

[0008] Wherein layer A contains polypropylene composition A, layer B and layer B' are the same or different, and each layer contains polypropylene composition B and polypropylene composition B', and the melting point of the polypropylene composition A is greater than the melting points of the polypropylene composition B and the polypropylene composition B';

[0009] The polypropylene composition A comprises homopolymer polypropylene a and impact copolymer polypropylene b; the polypropylene composition B and the polypropylene composition B' each comprise random copolymer polypropylene x and thermal bonding enhancer y;

[0010] The thermoplastic elastomer composition foamed sheet and the reinforced composite sheet are bonded by hot pressing fusion.

[0011] According to the present invention, the layers B and B' on both sides of the layer A are the same or different. In a preferred embodiment of the present invention, the layers B and B' on both sides of the layer A are the same.

[0012] According to some preferred embodiments of the present invention, based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 50-99wt% of homopolypropylene a and 1-50wt% of impact copolymer polypropylene b; preferably, the polypropylene composition A comprises 70-90wt% of homopolypropylene a and 10-30wt% of impact copolymer polypropylene b.

[0013] According to some preferred embodiments of the present invention, based on the total weight of the polypropylene composition B and the polypropylene composition B', the polypropylene composition B and the polypropylene composition B' each include 70-99wt% of random copolymer polypropylene x and 1-30wt% of thermal adhesion enhancer y; preferably, the polypropylene composition B and the polypropylene composition B' each include 80-90wt% of random copolymer polypropylene x and 10-20wt% of thermal adhesion enhancer y.

[0014] According to some preferred embodiments of the present invention, based on the total thickness of the polypropylene sheet, the thickness of layer A accounts for 51%-89% of the total thickness, preferably 71%-89%, and more preferably 71%-80%.

[0015] The thicknesses of the layers B, B' on both sides of the layer A may be the same or different, preferably the same.

[0016] The present invention does not limit the thickness of the polypropylene sheet, and can be selected in a wide range according to its practical application field. Preferably, the thickness of the polypropylene sheet can be 10-1000 μm, preferably 30-500 μm, and more preferably 50-300 μm.

[0017] According to the present invention, the thickness of the layers A, B, B' can be controlled by the melt pump of the extruder during processing.

[0018] According to some preferred embodiments of the present invention, the homopolypropylene a has: a melting point of 150-170°C, preferably 160-170°C; and / or a melt flow rate at 230°C and 2.16kg load of 0.5-50g / 10min, preferably 1-20g / 10min, further preferably 2.5-18g / 10min; and / or an isotacticity (mm) of not less than 96%.

[0019] According to some preferred embodiments of the present invention, the impact-resistant copolymerized polypropylene b has: the melting point of the impact-resistant copolymerized polypropylene b is 150-170°C: and / or the monomer of the impact-resistant copolymerized polypropylene b and propylene copolymer is ethylene or butene, preferably butene; and / or the melt flow rate of the impact-resistant copolymerized polypropylene b at 230°C and a load of 2.16 kg is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and further preferably 2.5-18 g / 10 min; and / or the cantilever beam impact strength of the impact-resistant copolymerized polypropylene b is not less than 20 KJ / m 2 (23℃).

[0020] According to the research conducted by the inventors, when the melt mass flow rate and polymer composition ratio of the polypropylene composition A are within the above preferred ranges, the high impact copolymer polypropylene b in the composition can absorb impact energy well, meet the requirements of impact performance, and make the sheet have good impact performance. At the same time, since the macromolecular segments in the homopolymer polypropylene a are relatively regular, crystallization occurs during the sheet preparation process, so the sheet also has good tensile properties.

[0021] According to some preferred embodiments of the present invention, the random copolymer polypropylene x has: a melting point of 110-150°C, preferably 120-140°C; and / or a melt flow rate at 230°C and a load of 2.16 kg of 0.5-50 g / 10 min, preferably 1-20 g / 10 min, further preferably 3-18 g / 10 min; and / or a molecular weight distribution Mw / Mn of 5-12, preferably 7-10; and / or a copolymer of propylene and ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer and / or a propylene-ethylene binary copolymer.

[0022] According to some preferred embodiments of the present invention, the thermal adhesion enhancer y has: a melting point or a viscosity flow temperature of 50-110°C; and / or a melt flow rate at 190°C and a load of 2.16 kg of 0.5-50 g / 10min, preferably 1-20 g / 10min, and further preferably 1-18 g / 10min; and / or, selected from one or more of polyolefin elastomers, EPDM rubber, SEBS (hydrogenated styrene-butadiene block copolymer), SBS (styrene-based thermoplastic elastomer), EVA, and petroleum resins; preferably, a polyolefin elastomer and / or a petroleum resin.

[0023] According to some preferred embodiments of the present invention, the polyolefin elastomer is a copolymer elastomer of ethylene and propylene and / or α-olefin, the α-olefin is preferably a C4-C12 α-olefin, more preferably 1-butene and / or 1-octene; and / or the petroleum resin is a C5 and / or C9 hydrogenated petroleum resin having a softening point of 100-150°C; preferably a cyclopentadiene type resin.

[0024] In the present invention, since the foaming material is a polyolefin thermoplastic elastomer, the thermal adhesion enhancer y is particularly preferably a polyolefin elastomer.

[0025] According to the research conducted by the present inventors, when the melt mass flow rate and polymer composition ratio of the polypropylene composition B and the polypropylene composition B' are within the preferred range, the low melting point random copolymer polypropylene x and the thermal adhesion enhancer y in the composition can significantly reduce the hot pressing temperature and broaden the hot pressing temperature window, and the thermal adhesion enhancer y provides the sheet with good adhesion performance and can further improve the interlayer peeling strength.

[0026] According to the research of the present inventors, when the melt mass flow rate, polymer composition ratio and thickness distribution of the polypropylene composition A, the polypropylene combination B and the polypropylene combination B' are within the preferred range, the sheet preparation process can be made smoother, so that the sheet has better uniformity, tensile strength, impact resistance and interlayer peeling strength.

[0027] According to some preferred embodiments of the present invention, the layer A further contains a β-crystal nucleating agent; preferably, the β-crystal nucleating agent is selected from at least one of condensed ring aromatic hydrocarbons, Group IIA two-component complexes, aromatic diamides, rare earth compounds and cyclic dicarboxylates.

[0028] According to some preferred embodiments of the present invention, the content of the β-crystal nucleating agent in layer A is 0.01-0.5 parts by weight relative to 100 parts by weight of the polypropylene composition A. For example, it can be 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5 parts by weight, and any two values ​​or any interval between any two values.

[0029] According to the research of the present inventors, when the melt mass flow rate, polymer composition ratio and thickness distribution of layer A of the polypropylene composition A and the polypropylene combinations B and B' are within the preferred range, the preparation process of the composite material can be made smoother, so that the composite material has better uniformity, tensile strength, impact resistance and interlayer peeling strength.

[0030] The BAB' layer structure of the polypropylene sheet can be prepared by various methods. In a preferred embodiment of the present invention, the BAB' layer structure of the polypropylene sheet is obtained by co-extruding components including the polypropylene composition A and the polypropylene compositions B and B'.

[0031] According to some preferred embodiments of the present invention, the melting point of the homopolymerized polypropylene a in the polypropylene composition A is greater than the melting point of the random copolymerized polypropylene x in the polypropylene compositions B and B', and preferably the temperature difference of the corresponding melting points is greater than or equal to 10 degrees. In this preferred embodiment, the inventors of the present invention surprisingly found that the obtained polypropylene sheet laminated thermoplastic elastomer composition foamed sheet is hot-pressed to obtain a multi-layer reinforced composite thermoplastic elastomer foamed sheet, and the multi-layer reinforced composite thermoplastic elastomer foamed sheet has more excellent mechanical properties and better interlayer peeling strength. Even at a lower hot pressing temperature and a wider hot pressing temperature range, the obtained multi-layer reinforced composite thermoplastic elastomer foamed sheet has a higher interlayer peeling strength.

[0032] The polypropylene fabric in the present invention is obtained by weaving the polypropylene sheet mentioned above; preferably, the polypropylene fabric has a three-dimensional structure of plain, twill and / or satin.

[0033] In order to facilitate weaving, the polypropylene sheet is preferably cut into polypropylene sheets with a width of 2-5 mm, and then woven to obtain the polypropylene fabric.

[0034] In a more preferred embodiment of the present invention, the polypropylene fabric is a plain, twill, satin or three-dimensional polypropylene fabric obtained by weaving three layers of co-extruded polypropylene stretch flat tapes. In a more preferred embodiment of the present invention, the polypropylene fabric is a plain, twill, satin or three-dimensional polypropylene fabric obtained by weaving three layers of co-extruded polypropylene stretch flat tapes, and the three-layer co-extruded polypropylene stretch flat tape comprises at least one layer A formed by a high-melting point polypropylene combination A and at least one layer B formed by a low-melting point polypropylene composition B, wherein the polypropylene composition A comprises homopolymer polypropylene a and impact copolymer polypropylene b; the polypropylene composition B comprises random copolymer polypropylene x and thermal bonding enhancement enhancer y, and the polymer film B layer is located on both sides of the A layer.

[0035] According to some preferred embodiments of the present invention, each layer of the reinforced composite sheet comprises a plurality of sequentially stacked polypropylene sheet unit groups; each polypropylene sheet unit group comprises at least one identical or different polypropylene sheet unit, each polypropylene sheet unit comprises a core layer A i and located in the core layer A i The outer layer B on both sides i , B' i , structure B iA i B' i The structure of the reinforced composite sheet is nth group...ith group...2nd group, 1st group, 2nd group...ith group...nth group from bottom to top, and the total number of stacked groups of polypropylene sheet unit groups is 2n-1; i and n are both integers not less than 2, and i≤n; wherein the core layer A in the polypropylene sheet unit i Containing polypropylene composition A i , outer layer B i With outer layer B' i The same or different, each corresponding to a polypropylene composition B i , polypropylene composition B' i , the polypropylene composition A i The melting point is greater than that of the polypropylene composition B i , the polypropylene composition B' i The average melting point of all outer layers in the i-th group is greater than or equal to the average melting point of all outer layers in the i-1-th group.

[0036] More preferably, the polypropylene composition A i Melting point and polypropylene composition B i The difference in melting points, polypropylene composition A i The melting point of polypropylene composition B' i The difference in melting points is 5°C or more, preferably 10°C or more, and more preferably 20°C or more.

[0037] According to the present invention, preferably, the total number of stacked groups of the polypropylene sheet unit group is 2n-1. The present invention has a wide selection range for the total number of stacked groups of the polypropylene sheet unit group. In a preferred embodiment of the present invention, 2≤n≤100 is selected, more preferably, 2≤n≤50, and further preferably, 2≤n≤30.

[0038] According to the present invention, the selection range of the number of polypropylene sheet units included in each polypropylene sheet unit group is relatively wide. In a preferred embodiment of the present invention, each polypropylene sheet unit group independently includes 1 to 10, preferably 1 to 5, more preferably 1 to 3 identical or different polypropylene sheet units, more preferably 1 polypropylene sheet unit. Preferably, the number of polypropylene sheet units included in each polypropylene sheet unit group is the same.

[0039] Preferably, but not necessarily, the melting point of any outer layer in each group is within ±10°C, within ±5°C, preferably within ±3°C, more preferably within ±1°C of the average melting point of all outer layers in the group.

[0040] In the embodiment where each polypropylene sheet unit group includes only one polypropylene sheet unit, for example, the structure of the polypropylene composite material can be B from bottom to top. n A n B' n ……B i A i B' i ...B2A2B'2, B1A1B'1, B2A2B'2...B i A i B' i ……B n A n B' n , the total number of stacked layers of the polypropylene sheet unit is 2n-1; i and n are both integers not less than 2, and i≤n.

[0041] In the embodiment where each polypropylene ply unit group includes 2 or more polypropylene ply units, for example, the structure of the i-th polypropylene ply unit group is B i1 A i1 B' i1 , B i2 A i2 B' i2 ……B ip A ip B' ip The structure of the polypropylene composite material can be sequentially as follows from bottom to top: n1 A n1 B' n1 , B n2 A n2 B' n2 ……B nq A nq B' nq )……(B i1 A i1 B' i1 , B i2 A i2 B' i2 ……B ip A ip B' ip )……(B 21 A 21 B' 21 , B 22 A 22 B' 22 ……B 2k A 2k B' 2k )(B 11 A 11 B' 11 , B 12 A12 B' 12 ……B 1j A 1j B' 1j )(B 21 A 21 B' 21 , B 22 A 22 B' 22 ……B 2k A 2k B' 2k )……(B i1 A i1 B' i1 , B i2 A i2 B' i2 ……B ip A ip B' ip )……(B n1 A n1 B' n1 , B n2 A n2 B' n2 ……B nq A nq B' nq ), the total number of stacked polypropylene sheet units is j+2k+...2p+...2q; j, k, p, q are each independently an integer not less than 2, preferably an integer from 2 to 10, more preferably from 2 to 5, and more preferably from 2 to 3.

[0042] According to some preferred embodiments of the present invention, the multi-layer reinforced composite foam sheet has a multi-layer sandwich structure, that is, a reinforced composite sheet, a plastic elastomer composition foam sheet, a reinforced composite sheet, a plastic elastomer composition foam sheet, and a reinforced composite sheet. The upper and lower platens may not be heated during hot pressing, and the entire portion to be hot pressed may be placed in an oven, and hot pressing may be achieved as long as the hot melt temperature of the thermoplastic elastomer composition foam material is reached.

[0043] According to some preferred embodiments of the present invention, based on the total thickness of the multi-layer reinforced composite foam sheet, the total thickness of the reinforced composite sheet accounts for 1.3%-15.5% of the total thickness of the multi-layer reinforced composite foam sheet. The inventors of the present invention have found through research that within this preferred range, the multi-layer foam sheet is easier to be hot-pressed together, and the interlayer peeling strength is higher. At the same time, the multi-layer reinforced composite foam sheet has both high resilience (i.e., drop weight impact strength) and tensile strength that can meet application requirements. More preferably, based on the total thickness of the multi-layer reinforced composite foam sheet, the total thickness of the reinforced composite sheet accounts for 4%-15.5% of the total thickness of the multi-layer reinforced composite foam sheet. In this more preferred embodiment, the obtained multi-layer reinforced composite foam sheet has higher tensile strength and higher resilience (i.e., drop weight impact strength), and better overall performance.

[0044] According to some preferred embodiments of the present invention, the thickness of a layer of thermoplastic elastomer composition foamed sheet has a wide selection range. Preferably, the thickness of a layer of thermoplastic elastomer composition foamed sheet is 4.5-60 mm, preferably 5-60 mm. In this preferred embodiment, the multi-layer foamed sheet is easier to be hot-pressed together, and the interlayer peeling strength is higher. At the same time, the multi-layer reinforced composite foamed sheet has both high resilience (i.e., drop weight impact strength) and tensile strength that can better meet application requirements.

[0045] In the examples below, the total thickness of the plastic elastomer composition foam sheet in the multi-layer reinforced composite foam sheet is the thickness of the multi-layer reinforced composite foam sheet in the example minus the thickness of all reinforced composite sheets, wherein the thickness of the reinforced composite sheet, i.e. the laminated sheet, does not deform during hot pressing and is a fixed value. Taking Example 1 as an example, the thickness of the reinforced composite sheet is 0.8 mm.

[0046] According to some preferred embodiments of the present invention, the number of laminated layers of the reinforced composite sheet and the thermoplastic elastomer composition foamed sheet is greater than or equal to 3 layers, preferably 3-100 layers, and more preferably 6-60 layers.

[0047] According to some preferred embodiments of the present invention, the thermoplastic elastomer composition foamed sheets are stacked from top to bottom at 0-90° along their respective machine directions, preferably with more than or equal to 1 layer, more preferably 1-10 layers, and most preferably 2-5 layers.

[0048] According to some preferred embodiments of the present invention, the reinforced composite sheets are stacked from top to bottom in a 0-90° angle along their respective machine directions, and preferably the total number of layers of polypropylene sheets and polypropylene fabrics in each layer of the reinforced composite sheet is greater than or equal to 2 layers, more preferably 2-100 layers, and most preferably 4-40 layers.

[0049] According to some preferred embodiments of the present invention, the density of the thermoplastic elastomer composition foamed sheet is 0.01 to 0.5 g / L, preferably 0.1 to 0.4 g / L.

[0050] According to the present invention, the thermoplastic elastomer composition foamed sheet contains a polyolefin thermoplastic elastomer composition. Preferably, the polyolefin thermoplastic elastomer composition contains POE and EVA and optional auxiliary agents.

[0051] As a preferred embodiment of the polyolefin thermoplastic elastomer composition foamed sheet provided by the present invention, the preparation method of the foamed sheet comprises: adding a foaming agent to the polyolefin thermoplastic elastomer composition to foam the foamed sheet.

[0052] Preferably, in parts by weight, based on the total weight of POE and EVA being 100 parts by weight, the content of POE is 5 to 50 parts by weight, and the total amount of EVA is 50 to 95 parts by weight.

[0053] Preferably, the auxiliary agent is selected from a cross-linking agent, a foaming agent, stearic acid, zinc stearate, zinc oxide, a filler and maleic anhydride copolymer microspheres.

[0054] More preferably, in parts by weight, relative to 100 parts by total weight of POE and EVA, the content of the cross-linking agent is 0.1 to 1 parts by weight, preferably 0.3 to 0.8 parts by weight; the content of the foaming agent is 0.1 to 10 parts by weight, preferably 2 to 7 parts by weight; the content of the stearic acid is 0.1 to 1 parts by weight, preferably 0.2 to 0.5 parts by weight; the content of the zinc stearate is 0.1 to 1 parts by weight, preferably 0.2 to 0.5 parts by weight; the content of the zinc oxide is 0.1 to 10 parts by weight, preferably 0.5 to 2 parts by weight; the content of the filler is 1 to 40 parts by weight, preferably 5 to 30 parts by weight; the content of the maleic anhydride copolymer microspheres is 0.1 to 5 parts by weight, preferably 0.2 to 1 part by weight.

[0055] To further explain the present invention, preferably, the polyolefin thermoplastic elastomer foam sheet composition, based on the total weight of the polyolefin thermoplastic elastomer foam sheet composition as 100 parts by weight, may comprise the following components in parts by weight:

[0056] POE 5-50 parts by weight;

[0057] EVA 50-95 parts by weight;

[0058] Cross-linking agent: 0.1-1 parts by weight, preferably 0.3-0.8 parts by weight;

[0059] Foaming agent: 0.1 to 10 parts by weight, preferably 2 to 7 parts by weight;

[0060] Stearic acid: 0.1-1 parts by weight, preferably 0.2-0.5 parts by weight;

[0061] Zinc stearate: 0.1-1 parts by weight, preferably 0.2-0.5 parts by weight;

[0062] Zinc oxide: 0.1 to 10 parts by weight, preferably 0.5 to 2 parts by weight;

[0063] Filler: 1-40 weight powder, preferably 5-30 weight powder;

[0064] Maleic anhydride copolymer microspheres: 0.1 to 5 parts by weight, preferably 0.2 to 1 part by weight.

[0065] According to the present invention, the POE can be selected from conventional POEs in the art. Preferably, the POE has the following characteristics:

[0066] The comonomer is 1-butene, 1-hexene or 1-octene, and the comonomer content is 10-20 mol%. The catalyst is CGC catalyst (a complex formed by monocyclopentadiene and a transition metal of the group IV in a coordination bond), a metallocene catalyst, or a salicylaldehyde imine titanium catalyst.

[0067] In addition, preferably, the weight average relative molecular mass of the POE is 100,000 to 200,000, preferably 120,000 to 170,000, and the molecular weight distribution width is preferably 1 to 3, preferably 1.5 to 2.5.

[0068] Preferably, the mass melt flow rate of the POE is 0.1 to 2 g / 10 min (2.16 kg, 190° C.), preferably 0.4 to 1.5 g / 10 min (2.16 kg, 190° C.).

[0069] Preferably, the EVA has the following characteristics: the vinyl acetate (VA) content is 5 to 35 mol%, measured by NMR, the NMR experiment is performed on an Agilent 400-MR DD2 nuclear magnetic resonance spectrometer, the solvent is CDCl3, and the test temperature is 40° C. The mass melt flow rate is 1 to 10 g / 10 min (2.16 kg, 190° C.), preferably 2 to 7 g / 10 min (2.16 kg, 190° C.).

[0070] The polyolefin thermoplastic elastomer foamed sheet composition may also contain one or more of the following processing aids commonly used in the polyolefin thermoplastic elastomer foaming process, such as but not limited to:

[0071] Graphite toner: added amount 1%-8%, preferably 2-5%; antioxidant: added amount 0.1-15‰, preferably 0.1-5‰; antistatic agent: added amount 0.1-10%, preferably 0.5-5%; lubricant: added amount 0.1-10%, preferably 0.5-3%; anti-aging agent: added amount 0.01-5%, preferably 0.1-2%. Flame retardant: added amount 0.1-25%, preferably 1-20%. The content of processing aids is well known in the industry and will not be repeated here.

[0072] According to the present invention, the density of the polyolefin thermoplastic elastomer composite foam material can be adjusted according to demand and specific process.

[0073] Preferably, the density of the foaming material is 0.01 to 0.5 g / L, preferably 0.1 to 0.4 g / L;

[0074] Preferably, the tensile strength stress of the foamed material is greater than 2 MPa, preferably greater than 2.2 MPa, for example, it can be 2 to 4 MPa. (GB / T 6344-2008)

[0075] Preferably, the elongation at break of the foamed material should be greater than 250%, preferably greater than 300%, for example, it can be 250-400%. (GB / T 6344-2008)

[0076] Preferably, the resilience of the foam material is greater than 50%, preferably greater than 60%, for example, may be 50-80%.

[0077] Unless otherwise specified, the polyolefin thermoplastic elastomer composition foamed sheets used in the embodiments of the present invention are within the preferred ranges indicated by the density, tensile strength stress, elongation at break, and resilience of the above-mentioned foamed materials.

[0078] The polyolefin thermoplastic elastomer composition foamed sheet of the present invention is preferably foamed by compression molding. Preferably, the compression molding foaming comprises the following steps:

[0079] (1) The temperature of the compression molding machine is raised to 180°C and stabilized for 15 minutes;

[0080] (2) crushing the composition into particles or granulating it and adding it into a foaming machine;

[0081] (3) The foaming temperature was set to 180°C, the molding foaming time was 550s, and the back pressure was 10MPa;

[0082] (4) After the pressure holding time is reached, the pressure is released and the mold is jumped to obtain the foamed material.

[0083] The foaming agent used in the present invention can be selected from a physical foaming agent or a chemical foaming agent, and the physical foaming agent can be an organic physical foaming agent or an inorganic physical foaming agent. Organic physical foaming agents include but are not limited to aliphatic hydrocarbons such as propane, butane, pentane, hexane and heptane, alicyclic hydrocarbons such as cyclobutane and cyclohexane, and halogenated hydrocarbons such as chlorofluoromethane, trifluoromethane, 1,2-difluoroethane, 1,2,2,2-tetrafluoroethane, methyl chloride, ethyl chloride and dichloromethane. The inorganic physical foaming agent includes but is not limited to at least one of air, nitrogen, carbon dioxide, oxygen and water. The added foaming agent decomposes and releases gas at a specific temperature and pressure to form a porous foam structure in expandable materials such as resins. The most commonly used chemical foaming agents are organic chemical foaming agents, including azodicarbonamide (AC), azobisisobutyronitrile (AIBN), barium azodicarboxylate (BaAC) and azodicarboxylic acid esters, dinitrosopentamethylenetetramine (DPT), N,N'-dinitrosopentamethylenetetramine, N,N'-dimethyl-N,N-dinitrosoterephthalamide (NTA) and trinitrosotrimethylenetriamine, 4,4'-oxybisbenzenesulfonylhydrazide (OBSH), toluenesulfonylsemicarbazide (TSSC), triphosphorus triazine (CTHT), 5-phenyltetrazolyl, 2,4-toluene disulfonylhydrazide, p-toluenesulfonylhydrazide, etc.

[0084] The antioxidant may be any antioxidant conventionally used in the art. Preferably, the antioxidant is a hindered phenol antioxidant and a phosphite antioxidant mixed in a mass ratio of 1:3 to 3:1; wherein the hindered phenol antioxidant may be selected from antioxidant 1010 (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate; CAS No.: 6683-19-8), 3114 (1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanuric acid; CAS: 27676-62-6) or 330 (1,3,5-trimethyl-2,4,6-tris( ... The phosphite antioxidant can be selected from at least one of antioxidant 168 (tris[2.4-di-tert-butylphenyl]phosphite; CAS: 31570-04-4), antioxidant 618 (pentaerythritol distearyl diphosphite; CAS: 3806-34-6) or antioxidant 2,2'-ethylenebis(4,6-di-tert-butylbenzene)fluorophosphite; CAS: 118337-09-0).

[0085] The crosslinking agent is mainly selected from organic peroxides, diisopropylbenzene peroxide, peroxyneoheptanoic acid, 1-dimethyl-3-hydroxybutyl ester, peroxyneodecanoic acid, tert-amyl perbenzoate, tert-butyl perbenzoate, tert-amyl peroctanoate, tert-butyl peroctanoate, di-tert-butyl peroxide diisopropylbenzene, and triallyl isocyanurate.

[0086] The filler is preferably selected from inorganic powders such as talc, kaolin, calcium carbonate, borax, zinc borate, aluminum hydroxide and silicon dioxide, and polymers such as polytetrafluoroethylene, polyethylene wax, polycarbonate, polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, polycyclohexanedimethylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, silicone, methyl methacrylate copolymer and cross-linked polystyrene. Inorganic powders are preferred, and talc is particularly preferred.

[0087] According to some more preferred embodiments of the present invention, the polyolefin thermoplastic elastomer foamed sheet composition contains maleic anhydride copolymer microspheres. The inventors of the present invention have found that the maleic anhydride copolymer microspheres can be used as a compatible dispersant to improve the compatibility between the components in the polyolefin thermoplastic elastomer composition.

[0088] In the present invention, the particle size of the maleic anhydride copolymer microspheres is 1000-1600 nm, preferably 1000-1500 nm.

[0089] In the present invention, the average particle size of the copolymer microspheres is measured by a scanning electron microscopy (SEM) method.

[0090] In the present invention, the copolymer in the maleic anhydride copolymer microspheres comprises a structural unit A provided by maleic anhydride and a structural unit B provided by α-methylstyrene. Based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A is 46-53%, and the molar content of the structural unit B is 47-54%.

[0091] In the present invention, the total amount of the structural unit A provided by maleic anhydride and the structural unit B provided by α-methylstyrene is 100%.

[0092] In the present invention, the molar content of each structural unit in the copolymer is tested by 1H NMR, and the test method is to calculate the ratio of the peak area corresponding to the characteristic hydrogen in the corresponding structural unit in 1H NMR.

[0093] In the present invention, when the maleic anhydride copolymer contains the structural unit with the specific molar content, the maleic anhydride copolymer can have microspheres with good uniformity, and the copolymer has a clean surface, good dispersibility in the medium, and no aggregation.

[0094] Furthermore, in order to obtain a maleic anhydride copolymer with better comprehensive performance, based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A is 48%-52%, and the molar content of the structural unit B is 49%-51%.

[0095] In the present invention, the maleic anhydride copolymer microspheres are prepared according to the following steps:

[0096] S1. In an inert atmosphere, dissolving the polymerization monomer and the initiator in a reaction medium to form a homogeneous solution;

[0097] S2, the homogeneous solution is subjected to polymerization reaction to obtain a copolymer emulsion suspension, and then solid-liquid separation is performed to obtain the maleic anhydride copolymer;

[0098] Wherein, the polymerizable monomers are maleic anhydride and α-methylstyrene; based on the total weight of the polymerizable monomers, the amount of maleic anhydride is 29-63wt%, and the amount of α-methylstyrene is 36-72wt%;

[0099] The reaction medium is a mixture of compound I represented by formula (1) and compound II represented by formula (2);

[0100]

[0101] Wherein, R1 and R2 are each independently an alkyl group having 1 to 3 carbon atoms; R3, R4 and R5 are each independently H, methyl or ethyl.

[0102] In the present invention, maleic anhydride and alpha-methylstyrene are copolymerized in a specific ratio in the presence of a specific reaction medium by a copolymerization method, so that the obtained maleic anhydride copolymer is in the form of microspheres with excellent uniformity, and the copolymer has the characteristics of clean surface, good dispersibility in the medium, no aggregation, and no special smell.

[0103] Furthermore, in order to obtain maleic anhydride copolymer microspheres with more uniform particles and better morphology, the inventors studied the dosage of maleic anhydride and α-methylstyrene in the polymerization process. The study showed that when the dosage of maleic anhydride is 40-50wt% and the dosage of α-methylstyrene is 45-55wt% based on the total weight of the polymerized monomers, the obtained maleic anhydride copolymer has more uniform particles and better morphology, and is spherical, and the overall performance of the copolymer is better.

[0104] In the present invention, based on the total weight of the homogeneous solution, the mass concentration of the polymerizable monomer is 5-25wt%, preferably 5-20wt%.

[0105] In the present invention, the initiator is an organic peroxide and / or an azo compound.

[0106] In the present invention, the organic peroxide is at least one selected from dibenzoyl peroxide, diisopropyl peroxide, di-tert-butyl peroxide, dodecyl peroxide, tert-butyl perbenzoate, diisopropyl peroxydicarbonate and dicyclohexyl peroxydicarbonate.

[0107] In the present invention, the azo compound is selected from azobisisobutyronitrile and / or azobisisoheptanenitrile.

[0108] In the present invention, based on the total weight of the homogeneous solution, the mass concentration of the initiator is 0.2-3.1 wt %, preferably 1-2 wt %.

[0109] In the present invention, a mixture of compound I represented by formula (1) and compound II represented by formula (2) is selected as the reaction medium, which can cooperate with the specific amount of maleic anhydride and α-methylstyrene described in the present invention to achieve a self-stabilizing precipitation polymerization reaction of maleic anhydride and α-methylstyrene. The polymerization reaction system does not need to add any stabilizer or co-stabilizer, has a self-stabilizing dispersion effect, and the surface of the obtained polymer microspheres is clean and pollution-free.

[0110] Furthermore, in formula (3), R1 and R2 are each independently a methyl group or an ethyl group.

[0111] Furthermore, in formula (3), R3, R4 and R5 are each independently methyl or ethyl.

[0112] In the present invention, the amount of the compound II is 50-90 vol% based on the total volume of the reaction medium.

[0113] In the present invention, when the amount of compound I and compound II in the reaction medium meets the above range, a maleic anhydride copolymer with a more excellent polymer microsphere morphology can be obtained. Further, when the amount of compound II is 60-90 vol% based on the total volume of the reaction medium, the effect is more excellent.

[0114] In the present invention, the conditions of the polymerization reaction include: the polymerization temperature is 60-90° C., preferably 70-80° C.; the polymerization time is 1-24 h, preferably 3-12 h.

[0115] In the present invention, a water bath and / or an oil bath is used to provide the heat required for the polymerization of the present invention.

[0116] In the present invention, the solid-liquid separation may be a conventional solid-liquid separation method in the art, such as centrifugal separation.

[0117] In the present invention, when centrifugal separation is adopted, the centrifugal speed is 1000-4000 rad / min, and the centrifugal time is 10-40 min.

[0118] The mechanical strength and thermal insulation performance of the composite foam sheet are compared with the composite foam sheet without reinforcement prepared by the same process, the tensile strength is improved, the elongation at break is improved, and the thermal conductivity is improved by no more than 15%, preferably no more than 10%. Compared with composite sheets with other reinforcement methods (glass fiber reinforced sheets), the mechanical strength is improved, the elongation at break is improved, and the thermal conductivity is reduced by 15%, preferably by 30%. Test method: The thermal conductivity is measured according to the method specified in GB / T 10294.

[0119] According to the present invention, preferably, the multi-layer reinforced composite foam sheet is prepared by the following method: comprising laminating the polypropylene sheet and / or the polypropylene fabric with the thermoplastic elastomer composition foam sheet, fusing them by hot pressing, and then cooling and shaping to obtain the multi-layer reinforced composite foam sheet (referred to as method one); or comprising first laminating the polypropylene sheet and / or the polypropylene fabric, fusing them by hot pressing to obtain a reinforced composite sheet; and then laminating the reinforced composite sheet with the thermoplastic elastomer composition foam sheet, fusing them at 60-80°C, to obtain the multi-layer reinforced composite foam sheet (referred to as method two).

[0120] According to the present invention, the number of layers of the thermoplastic elastomer composition foam sheet is preferably greater than or equal to 1 layer, more preferably 1-10 layers, and most preferably 2-5 layers. The preparation method of the multi-layer reinforced composite foam sheet can be flexibly selected according to the number of layers of the thermoplastic elastomer composition foam sheet in the target product. For example, the polypropylene sheet and / or the polypropylene fabric can be laminated with the thermoplastic elastomer composition foam sheet, hot-pressed and fused, and then cooled and shaped to obtain the multi-layer reinforced composite foam sheet, that is, hot-pressed and fused once to obtain the multi-layer reinforced composite foam sheet; the polypropylene sheet and / or the polypropylene fabric can also be first prepared into a reinforced composite sheet by hot-pressing fusion, and then the reinforced composite sheet and the thermoplastic elastomer composition foam sheet are laminated and fused at 60-80°C, and the hot-pressing pressure is 3.5-7MPa. More preferably, the pressure increases with the increase of the number of interlayer sheets to obtain the multi-layer reinforced composite foam sheet.

[0121] Method 2 is suitable for all situations in which the effects of the present invention are achieved, that is, when the thermoplastic elastomer composition foamed sheet preferably has 1 layer or more, more preferably 1-10 layers, and most preferably 2-5 layers, method 2 can be used for preparation.

[0122] Preferably, when the number of layers of the thermoplastic elastomer composition foamed sheet is equal to 1, it can be prepared by method 1, that is, it is prepared by one-time hot pressing fusion.

[0123] The second aspect of the present invention is to provide a method for preparing the multi-layer reinforced composite foam sheet described in the first aspect, comprising laminating the polypropylene sheet and / or the polypropylene fabric with the thermoplastic elastomer composition foam sheet, fusing them by hot pressing, and then cooling and shaping to obtain the multi-layer reinforced composite foam sheet (referred to as method one); or, comprising first laminating the polypropylene sheet and / or the polypropylene fabric, fusing them by hot pressing to obtain a reinforced composite sheet; and then laminating the reinforced composite sheet with the thermoplastic elastomer composition foam sheet, fusing them at 60-80°C to obtain the multi-layer reinforced composite foam sheet (referred to as method two).

[0124] According to the present invention, preferably, the polypropylene sheets and / or the polypropylene fabrics are stacked in the order of forming corresponding layers of reinforced composite sheets.

[0125] The conditions of hot pressing fusion in method 1 and method 2 may be the same or different. In a preferred embodiment of the present invention, the temperature of hot pressing fusion is 115-170°C, preferably 115-159°C, and more preferably 140-159°C.

[0126] In a preferred embodiment of the present invention, the pressure of the hot pressing fusion is 2-10 MPa.

[0127] In a preferred embodiment of the present invention, the preheating time of the hot pressing fusion is 5-600s, and the hot pressing time is 1-600s, preferably 10-500s.

[0128] In a preferred embodiment of the present invention, the cooling and shaping pressure is 2-8 MPa, and the cooling and shaping time is 30s-700s.

[0129] In a preferred embodiment of the present invention, the number of laminated layers of the polypropylene sheet and / or polypropylene fabric and the polyolefin elastomer foam sheet is greater than or equal to 3 layers, preferably 3-100 layers; more preferably 6-60 layers.

[0130] In a preferred embodiment of the present invention, adjacent layers of the polypropylene sheet laminate are placed at 0-90° along respective machine directions, wherein the machine direction is the stretching direction (MD).

[0131] In a preferred embodiment of the present invention, adjacent layers of the polypropylene fabric laminate are placed at an angle of 0-90° along the warp direction.

[0132] According to some preferred embodiments of the present invention, the conditions for the hot pressing fusion include:

[0133] The hot pressing temperature is 115-170°C, preferably 115-159°C, and more preferably 140-159°C; and / or, the hot pressing pressure is 2-10MPa, the preheating time is 5-600s, the hot pressing time is 1-600s, and preferably 10-500s; and / or, the cooling pressure is 2-8MPa, and the cooling time is 30-700s.

[0134] In a more preferred embodiment of the present invention, the method for preparing the multi-layer reinforced composite foam sheet comprises the following steps:

[0135] Step a: co-extrude the polypropylene composition A, the polypropylene composition B, and the polypropylene composition B' according to the BAB' structure and cast or calender to obtain a polypropylene co-extruded sheet; preferably, the extrusion casting or calendering temperature is 200-240° C., and the temperature of the calendering roller is 50-70° C.;

[0136] Step b: stretching the coextruded polypropylene sheet at a certain temperature to obtain a stretched polypropylene sheet; the stretching method is free stretching, and / or solid phase stretching, and / or multi-stage stretching; the stretching temperature is preferably 90-165°C, preferably 90-140°C, and more preferably 90-119°C; the stretching ratio is 1-20 times, preferably 2-15 times.

[0137] Step c: cutting the polypropylene stretched sheet to prepare polypropylene flat strips, and weaving the flat strips to prepare polypropylene fabrics; preferably, the width of the polypropylene flat strips is 2-5 mm, and the polypropylene fabrics include plain weave, twill, satin weave or other three-dimensional polypropylene fabrics;

[0138] Step d: After the components of POE, EVA, crosslinking agent, foaming agent, stearic acid and zinc stearate are measured according to the formula, they are added into a high-speed mixer, and continuously stirred at high speed for 1-10 minutes, preferably 2-5 minutes, at room temperature, and then enter into an internal mixer at a mixing temperature of 100° C.-110° C. After mixing for 9-11 minutes, for example, 10 minutes, they are forcibly added into a twin-screw extruder, extruded at 150-180° C., and granulated to obtain polyolefin thermoplastic elastomer composition particles.

[0139] Step e: Preparation of polyolefin elastomer foaming material: the mold installed between the molding presses is heated to a foaming temperature of 130°C-200°C, preferably 170°C-190°C, and stabilized for 10-20 minutes, for example, 15 minutes; the polyolefin thermoplastic elastomer composition particles of step d are placed therein, the molding presses are closed, and the mold is sealed. The gas generated by the foaming agent is diffused into the polyolefin thermoplastic elastomer composition resin particles, the foaming temperature is set to 170-185°C, for example, 180°C, the molding foaming time is 500-600s, for example, 550s, and the back pressure is 9-12MPa, for example, 10MPa; after the holding time is reached, the pressure is released and the mold is jumped to obtain the foaming material. Then the polyolefin thermoplastic elastomer composition foaming sheet of the required thickness is obtained by cutting.

[0140] Step f: laminating and hot-pressing the polypropylene fabric and the foam sheet prepared in step e in sequence, and then cooling and shaping to form a multi-layer reinforced composite foam sheet; preferably, in step f, the hot pressing conditions are: hot pressing temperature 115-170°C, preferably 115-159°C, and more preferably 140-159°C; hot pressing pressure 2-10MPa, preheating time 5-600s, hot pressing time 1-600s, preferably 10-500s, cooling pressure 2-8MPa, cooling time 30s-700s; preferably, adjacent polypropylene fabrics in the multi-layer reinforced composite foam sheet can be placed at 0-90° between the warp and the warp. A thermal bonding enhancer is used between each layer of hot pressing material, wherein the thermal bonding enhancer preferably used between the polyolefin thermoplastic elastomer foam material and the polypropylene laminate material is polyolefin elastomer (POE).

[0141] According to some embodiments of the present invention, in step c, a high-speed slitting machine with multiple blades can be used for cutting to obtain an oriented polypropylene flat ribbon with a width of 2-5 mm; a commercial weaving machine is used to weave the oriented flat ribbon according to the designed fabric structure to obtain plain, twill, satin or other three-dimensional polypropylene fabrics.

[0142] According to the present invention, in a preferred specific embodiment, the pressure is preferably maintained continuously during the hot pressing and cooling process without being reduced. The hot pressing process is carried out continuously, and preferably a continuous hot pressing composite material molding equipment consisting of a preheating machine, a crawler-type continuous flat hot press, a crawler-type continuous flat cooling press, a sheet cutting machine and a sheet stacking machine arranged in sequence is used; preferably, the crawler-type continuous flat hot press has a preheating unit, an independent heating and pressurizing unit, an air cooling unit and a lifting mechanism.

[0143] During the preparation, the polypropylene sheet and / or the polypropylene fabric and the polyolefin thermoplastic elastomer composition foamed sheet are sequentially stacked and preheated by a preheater. The preheated samples are sequentially hot-pressed and fused by a crawler-type flat hot press, and then cooled and shaped by a crawler-type continuous flat cooling press to form a polyolefin thermoplastic elastomer composition foamed sheet / polypropylene composite sheet (i.e., a multi-layer reinforced composite foamed sheet), i.e., a stacked hot-pressed product (multi-layer sandwich structure). Afterwards, the sheet is sliced ​​by a sheet cutter as needed, and the hot-pressed products are stacked and arranged by a sheet stacker. The hot-pressing temperature is controlled by a preheating unit, an independent heating and pressing unit, and an air-cooling unit in the crawler-type flat hot press, and the hot-pressing pressure is controlled by a lifting mechanism. According to the research of the inventors, when the preparation process parameters are within the preferred range, the polyolefin thermoplastic elastomer composition foamed sheet / polypropylene composite sheet prepared by the preparation equipment preferably has better tensile strength, impact performance, and interlayer peeling strength.

[0144] According to the present invention, the number of layers of the thermoplastic elastomer composition foam sheet is preferably greater than or equal to 1 layer, more preferably 1-10 layers, and most preferably 2-5 layers. The preparation method of the multi-layer reinforced composite foam sheet can be flexibly selected according to the number of layers of the thermoplastic elastomer composition foam sheet in the target product. For example, the polypropylene sheet and / or the polypropylene fabric can be stacked with the thermoplastic elastomer composition foam sheet, hot-pressed and fused, and then cooled and shaped to obtain the multi-layer reinforced composite foam sheet, that is, hot-pressed and fused once to obtain the multi-layer reinforced composite foam sheet; the polypropylene sheet and / or the polypropylene fabric can also be first prepared into a reinforced composite sheet by hot-pressing fusion, and then the reinforced composite sheet and the thermoplastic elastomer composition foam sheet are stacked and fused at 60-80°C to obtain the multi-layer reinforced composite foam sheet.

[0145] Method 2 is suitable for all situations in which the effects of the present invention are achieved, that is, when the thermoplastic elastomer composition foamed sheet preferably has 1 layer or more, more preferably 1-10 layers, and most preferably 2-5 layers, method 2 can be used for preparation.

[0146] Preferably, when the number of layers of the thermoplastic elastomer composition foamed sheet is equal to 1, it can be prepared by method 1, that is, it is prepared by one-time hot pressing fusion.

[0147] According to the present invention, in method 2, the temperature at which the reinforced composite sheet and the thermoplastic elastomer composition foamed sheet are fused is 60-80° C., which is close to the softening temperature of the POE elastomer surface.

[0148] Preferably, the process of fusing the reinforced composite sheet with the thermoplastic elastomer composition foamed sheet in method 2 is carried out in an oven containing a pressing plate, the volume of which is larger than the multi-layer reinforced composite foamed sheet, the pressing plate is placed above the topmost reinforced composite sheet, the hot pressing temperature is close to the softening temperature of the POE elastomer surface, the POE elastomer surface is softened, and then kept warm, so that the reinforced composite sheet and the thermoplastic elastomer composition foamed sheet can be fused.

[0149] The time for fusing the reinforced composite sheet with the thermoplastic elastomer composition foam sheet can be selected within a wide range, as long as the thermoplastic elastomer composition foam sheet is softened to achieve the thermoplastic elastomer composition foam sheet bonding the reinforced composite sheet together. Taking the embodiment of the present invention as an example, after the reinforced composite sheet and the polyolefin elastomer composition reach 70°C, the temperature is kept constant for 5 minutes to achieve the softening of the thermoplastic elastomer composition foam sheet, and hot pressing is performed for 30 seconds to complete the molding. Preferably, the temperature is kept at 60-80°C for 2-10 minutes, and then hot pressing is performed for 20-100 seconds.

[0150] The present invention has a wide range of optional pressures when the reinforced composite sheet and the thermoplastic elastomer composition foamed sheet are fused. Preferably, the pressure when the reinforced composite sheet and the thermoplastic elastomer composition foamed sheet are fused is 3.5-7 MPa.

[0151] The third aspect of the present invention is to provide an application of the multi-layer reinforced composite foam sheet described in the first aspect or the multi-layer reinforced composite foam sheet prepared by the preparation method described in the second aspect in the fields of automobiles, communications, aircraft, logistics, insulation, precision machinery and electronic turnover, and packaging.

[0152] Compared with the prior art, the present invention has the following beneficial effects:

[0153] (1) The composite foam sheet provided by the present invention is a composite of a high-strength and high-impact polypropylene sheet and a polyolefin thermoplastic elastomer composition foam sheet. It has good tensile strength, impact resistance and interlayer peeling strength. The multi-layer reinforced composite foam sheet has the following characteristics:

[0154] The longitudinal (MD) tensile strength is ≥4MPa, preferably ≥10MPa; the interlayer peel strength is ≥0.85N / mm, preferably ≥0.9N / mm; when the multi-layer reinforced composite foam sheet is only composed of 10 layers of polypropylene fabric and 1 layer of polyolefin thermoplastic elastomer composition foam sheet, and the thickness is about 5.5mm, the drop hammer impact strength is ≥69J, preferably ≥78J. Compared with the composite foam sheet without reinforcement prepared by the same process, the mechanical strength and thermal insulation performance of the composite foam sheet are improved in tensile strength, and the thermal conductivity is increased by no more than 15%, preferably no more than 10%. Compared with composite sheets with other reinforcement methods (glass fiber reinforced sheets), the mechanical strength is improved, the elongation at break is improved, and the thermal conductivity is reduced by 15%, preferably by 30%. Test method: The thermal conductivity is measured according to the method specified in GB / T 10294.

[0155] (2) Compared with the glass fiber nylon (polypropylene) composite pre-set sheet or metal sheet reinforced molded body used in the currently common composite reinforced polyolefin thermoplastic elastomer composition composite foam sheet, the compatibility between the pre-set sheet and the matrix resin is greatly improved, which can effectively reduce the apparent density and thermal conductivity of the product.

[0156] (3) The polyolefin thermoplastic elastomer composition foamed sheet of the present invention can be prepared by applying the existing compression foaming molding process, which is simple and has low production cost.

[0157] (4) The polypropylene composite foam sheet of the present invention is a polymer homogeneous component, and does not need to be separated and processed during recycling, and can be directly used in other processing and application fields after crushing, melting and granulating. In particular, since the recycled material contains a polyolefin thermoplastic elastomer composition, the mechanical properties of the recycled material can be maintained to the greatest extent, and it has a prospect of secondary processing and molding.

[0158] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION

[0159] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0160] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0161] In the following examples and comparative examples:

[0162] The extrusion calender and solid phase drawing equipment were purchased from Tianjin Hengrui Company, and the model was HRPC-800 three-layer co-extrusion plastic stretching sheet production line.

[0163] The properties of the polypropylene, polyolefin thermoplastic elastomer composition foamed material and composite sheet are tested according to the following method:

[0164] The test results of composite sheets are shown in Table 1:

[0165] (1) Melt flow rate (MFR): measured according to the method specified in GB / T 3682, where the test temperature is 230°C and the load is 2.16 kg;

[0166] (2) Density: measured according to the methods specified in GB / T 1033.1 and GB / T 6343;

[0167] (3) Melting point: measured according to the method specified in GB / T 28724;

[0168] (4) Tensile strength: measured according to the method specified in GB / T1040.1;

[0169] (5) Drop weight impact strength: measured according to the method specified in GB / T14153;

[0170] (6) Interlayer peel strength: Prepare samples and measure them according to the method specified in GB / T 3903.39-2019.

[0171] (7) Test method for thermal insulation capability of the composite foam sheet: The thermal conductivity is measured in accordance with the method specified in GB / T 10294.

[0172] In the following examples, the β-crystal nucleating agent with the brand name VP101B is sourced from the Beijing Institute of Chemical Technology; the sources of some raw materials are described in the examples, and the remaining raw materials are commercially available unless otherwise specified.

[0173] raw material:

[0174] Polypropylene: Sinopec Beijing Research Institute of Chemical Industry (BRICI);

[0175] Polyolefin thermoplastic elastomer (POE): 1-butene as comonomer, POE-B, comonomer content 13.6 mol%, weight average molecular weight; 1-hexene as comonomer, POE-H, comonomer content 13.1 mol%; 1-octene as comonomer, POE-O, comonomer content 13.8 mol%; Sinopec Beijing Research Institute of Chemical Industry (Beijing Institute of Chemical Industry);

[0176] EVA: 5110 and 6100, BASF-YPC; 2806, Sinochem Refining and Chemical.

[0177] Chemical blowing agent: 4,4'-oxybisbenzenesulfonylhydrazide, Inokite Technology;

[0178] Peroxide: di-tert-butyl peroxide diisopropylbenzene, Inotech Technology. Maleic anhydride copolymer microspheres, Sinopec Beijing Research Institute of Chemical Industry (Beijing Institute of Chemical Industry); Preparation Example A is used to illustrate the preparation of the compatible dispersant maleic anhydride copolymer microspheres of the present invention.

[0179] Preparation Example A1

[0180] 4.9g maleic anhydride, 0.9g azobisisobutyronitrile, 6g α-methylstyrene, 40ml acetone and 60ml toluene were added to a 500mL three-necked flask. After the materials were evenly mixed, nitrogen was passed through for 20 minutes. The three-necked flask was moved into an 80°C water bath and reacted for 24 hours. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 8.3g of polymer solid, corresponding to a polymer yield of 76%. The size of the polymer microspheres was 1200 nanometers. Among them, based on the total weight of the homogeneous solution, the concentration of the polymerization monomer was 6.3wt%, and the concentration of the initiator was 1.1wt%. The microspheres were named MW101.

[0181] The polymer microspheres MW101 were 1 H NMR measurement showed that, based on the total molar amount of each structural unit in the polymer, the molar content of the structural unit A provided by maleic anhydride was 53%, and the molar content of the structural unit B provided by α-methylstyrene was 47%.

[0182] Preparation Example A2

[0183] 4.9g maleic anhydride, 2g azobisisobutyronitrile, 6g α-methylstyrene, 10ml acetone and 90ml toluene were added to a 500mL three-necked flask. After the materials were evenly mixed, a homogeneous solution was obtained. Nitrogen was passed through the three-necked flask for 20 minutes. The three-necked flask was moved into a 70°C water bath and reacted for 5 hours. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 8g of polymer solid, corresponding to a polymer yield of 73%. The size of the polymer microspheres was 1100 nanometers. Among them, based on the total weight of the homogeneous solution, the concentration of the polymerization monomer was 11.1wt%, and the concentration of the initiator was 3.1wt%. The microspheres were named MW102.

[0184] The polymer microspheres MW102 were 1H NMR measurement showed that, based on the total molar amount of each structural unit in the polymer, the molar content of the structural unit A provided by maleic anhydride was 50%, and the molar content of the structural unit B provided by α-methylstyrene was 50%.

[0185] Preparation Example A3

[0186] 4.9g maleic anhydride, 0.9g azobisisobutyronitrile, 6g α-methylstyrene, 50ml acetone and 50ml toluene were added to a 500mL three-necked flask. After the materials were evenly mixed, nitrogen was passed through for 20 minutes. The three-necked flask was moved into a 70°C water bath and reacted for 5 hours. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 7.5g of polymer solid, corresponding to a polymer yield of 69%. The size of the polymer microspheres was 1000 nanometers. Among them, based on the total weight of the homogeneous solution, the concentration of the polymerized monomer was 11.5wt%, and the concentration of the initiator was 1wt%. The microspheres were named MW103.

[0187] The polymer microspheres MW103 were 1 H NMR measurement showed that, based on the total molar amount of each structural unit in the polymer, the molar content of the structural unit A provided by maleic anhydride was 51%, and the molar content of the structural unit B provided by α-methylstyrene was 49%.

[0188] Example 1

[0189] This embodiment is used to illustrate the preparation method of the multi-layer reinforced composite foam sheet provided by the present invention, which comprises the following steps:

[0190] (1) Preparation of polypropylene composition A:

[0191] Component a is a homopolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 160°C, a melt flow rate (melt mass flow rate) of 3.2g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer produced by Sinopec Beijing Research Institute of Chemical Industry, with an ethylene content of 11wt%, a melting point of 155°C, and an Izod impact strength of 23KJ / m 2 (23°C), the melt flow rate is 2.0 g / 10 min. The components prepared above are weighed and mixed according to the proportions, wherein the mass fraction Wa of component a is 80 parts by weight, and the mass fraction Wb of component b is 20 parts by weight.

[0192] 0.05 parts by weight of a β-crystal nucleating agent of grade VP101B was added. The mixture was then added to a high-speed stirrer for uniform mixing, and then the mixed material was added to the feeder of a twin-screw extruder manufactured by W&P Company, and the material entered the twin screw through the feeder. During the processing, the temperature of the screw was maintained between 200-230° C. The screw was melt-mixed uniformly, extruded, granulated and dried to obtain a polypropylene composition pellet A. The melting point of the polypropylene composition pellet A was found to be 157° C.

[0193] (2) Polypropylene composition B i Preparation:

[0194] Component x1 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution of Mw / Mn of 8.9, a melt flow rate of 8.1 g / 10 min and a melting point of 130°C; component x2 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution of Mw / Mn of 7.6, a melt flow rate of 7.2 g / 10 min and a melting point of 135°C; component x3 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution of Mw / Mn of 7.3, a melt flow rate of 6.6 g / 10 min and a melting point of 140°C; component y is a polyolefin elastomer with a brand number of 6102, purchased from Exxon, and is an ethylene-propylene copolymer.

[0195] The components prepared above are weighed and mixed according to the ratio, wherein component x i The mass fraction Wx i The mass fraction Wy of component y is 85 parts by weight, the mass fraction Wy of component y is 15 parts by weight, and the other steps are the same as step (1), and finally a polypropylene composition B is obtained. i Granules (i.e. x i +y=B i , i=1, 2, 3), after testing, the melting point of B1 is 127°C, the melting point of B2 is 132°C, and the melting point of B3 is 138°C.

[0196] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0197] The polypropylene composition A and the polypropylene composition B obtained in the above steps (1) and (2) are i The pellets are dried, and then the polypropylene composition A is added to the core layer extruder of the multi-layer extrusion calendering, and the polypropylene composition B is added to the core layer extruder of the multi-layer extrusion calendering. iAdd to the upper and lower surface extruders of the multi-layer extrusion casting machine. After the pellets are co-extruded and compounded through the extruder die, they pass through the calendering roller and the traction roller in sequence, and then undergo solid phase stretching, trimming and winding to obtain sheets B1AB1, B2AB2, and B3AB3 respectively. Among them, the temperature of the extrusion casting is 230°C, and the temperature of the calendering roller is 58°C. The temperature during the solid phase stretching process is 140°C, the stretching rate is 2m / min, and the stretching ratio is 7 times.

[0198] The composite film (polypropylene sheet) made by stretching and rolling is composed of the upper surface layer (the outer layer of the film B i ), core layer (film A) and lower surface layer (outer film B i The thickness of the composite film is 80 μm, wherein the thickness of the film layer A accounts for 80% of the total thickness of the sheet.

[0199] (4) Preparation of polypropylene fabric:

[0200] The three-layer co-extruded polypropylene sheet obtained in the above step (3) is cut by a high-speed slitting machine with multiple blades to obtain an oriented polypropylene flat ribbon with a width of 3 mm; the oriented flat ribbon is woven by a commercial weaving machine according to the designed fabric structure to obtain plain polypropylene fabrics B1AB1, B2AB2, B3AB3.

[0201] (5) Preparation of polyolefin thermoplastic elastomer composition for foam sheet:

[0202] 50 g of POE-B, 50 g of EVA (6110), 4.2 g of 4,4'-oxybisbenzenesulfonyl hydrazide, 0.1 g of di-tert-butyl peroxide diisopropylbenzene, 0.1 g of stearic acid, 0.1 g of zinc stearate, 0.2 g of zinc oxide, 20 g of talc, and 1 g of MW101 were mixed and kneaded at a kneading temperature of 100° C. for 10 min. A single-screw extruder was used in combination with underwater pelletizing to prepare composite particles, and the composite was dried at 60° C. to obtain the composite.

[0203] (6) Preparation of polyolefin thermoplastic elastomer foamed sheet

[0204] The temperature of the compression foaming machine was raised to 170°C and stabilized for 15 minutes; the granulated particles of the composition were added to the foaming machine; the foaming temperature was set to 175°C, the compression foaming time was 500 seconds, and the back pressure was 10MPa; after the pressure holding time was 40 seconds, the pressure was released and the mold was jumped to obtain the polyolefin thermoplastic elastomer composition foaming material, and the foamed sheet of the required size was obtained by laser line cutting. The density of the foamed sheet is 0.18g / cm 3 , the thickness after cutting is 5mm.

[0205] (7) Preparation of multi-layer reinforced composite foam sheet:

[0206] The polypropylene fabric obtained in the above step (4) is stacked in sequence, and the polypropylene fabric obtained in the above step (4) is stacked in sequence, from bottom to top, B3AB3, B2AB2, B1A1B1, B2AB2, B3AB3, and the total number of stacked layers is 5. A piece of polyolefin thermoplastic elastomer composition foamed sheet obtained in the above step (6) is placed in the middle of the two sets of 5-layer fabrics (80μm*5(5 layers)*2(2 sets)=0.8mm), that is, the structure is a PP fabric with a total number of stacked layers of B3AB3, B2AB2, B1A1B1, B2AB2, B3AB3 on the top and bottom, and the polyolefin thermoplastic elastomer composition foamed sheet is in the middle. The laminated polypropylene fabric and the polyolefin elastomer composition foamed sheet are simultaneously hot-pressed and fused, and then cooled and shaped to form a multi-layer reinforced composite foamed sheet. The polypropylene fabric is placed in a direction of 90° between the warp and the warp. The hot pressing conditions used were: temperature 135°C, hot pressing pressure 4MPa, preheating time 160s, cooling time 520s. The thickness of the prepared multi-layer reinforced composite foam sheet was 5.62mm.

[0207] Example 2

[0208] This embodiment is used to illustrate the preparation method of the multi-layer reinforced composite foam sheet provided by the present invention, which comprises the following steps:

[0209] (1) Preparation of polypropylene composition A:

[0210] Component a is homopolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 165°C, a melt flow rate of 8.1g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer produced by Sinopec Beijing Research Institute of Chemical Industry, with an ethylene content of 8wt%, a melting point of 155°C, a melt flow rate of 3.2g / 10min, and an cantilever beam impact strength of 25KJ / m 2 (23°C). The above-prepared components are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 70 parts by weight, and the mass fraction Wb of component b is 30 parts by weight. 0.05 parts by weight of β-crystal nucleating agent with the grade VP101B is added. Then the mixture is added to a high-speed stirrer and mixed evenly, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P. The material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 200-230°C. After the screw is melt-mixed evenly, extruded, granulated and dried, a polypropylene composition pellet A is obtained. After testing, the melting point of the polypropylene composition pellet A is 161°C.

[0211] (2) Polypropylene composition B i Preparation:

[0212] Component x1 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution Mw / Mn of 8.4, a melting point of 128°C, and a melt flow rate of 7.8 g / 10 min; Component x2 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution Mw / Mn of 7.6, a melting point of 134°C, and a melt flow rate of 6.9 g / 10 min; Component x3 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution Mw / Mn of 7.1, a melting point of 142°C, and a melt flow rate of 5.2g / 10min; component y is a polyolefin elastomer produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene copolymer with an ethylene content of 15%wt, a melting point of 105°C, and a melt flow rate of 9g / 10min under a load of 2.16kg.

[0213] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wxi of component xi is 80 parts by weight, the mass fraction Wy of component y is 20 parts by weight, and the other steps are the same as step (1), and finally a polypropylene composition B is obtained. i Granules (i.e. xi+y=B i , i=1, 2, 3), after testing, the melting point of B1 is 126°C, the melting point of B2 is 133°C, and the melting point of B3 is 140°C.

[0214] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0215] The preparation process is the same as step (3) of Example 1.

[0216] (4) Preparation of polypropylene fabric:

[0217] The preparation process is the same as step (4) of Example 1.

[0218] (5) Preparation of polyolefin thermoplastic elastomer composition for foam sheet:

[0219] 50 g of POE-H, 50 g of EVA (2806), 5.3 g of 2,4-toluene disulfonyl hydrazide, 0.15 g of di-tert-butyl peroxide diisopropylbenzene, 0.11 g of stearic acid, 0.12 g of zinc stearate, 0.21 g of zinc oxide, 25 g of silicon dioxide and 0.5 g of MW102 were mixed and kneaded at a kneading temperature of 105 ° C and a mixing time of 9.5 min. A single-screw extruder was used with air-cooled pelletizing to prepare the composite particles without drying.

[0220] (6) Preparation of polyolefin thermoplastic elastomer composition foamed sheet

[0221] The temperature of the compression foaming machine was raised to 175°C and stabilized for 16 minutes; the granulated particles of the composition were added to the foaming machine; the foaming temperature was set to 180°C, the compression foaming time was 510 seconds, and the back pressure was 12MPa; after the pressure holding time was 50 seconds, the pressure was released and the mold was jumped to obtain the polyolefin thermoplastic elastomer composition foaming material, and the foamed sheet of the required size was obtained by laser line cutting. The density of the foamed sheet is 0.15g / cm 3 , the thickness after cutting is 5mm.

[0222] (7) Preparation of multi-layer reinforced composite foam sheet:

[0223] The preparation process is the same as step (7) of Example 1. The thickness of the prepared multi-layer reinforced composite foam sheet is 5.57 mm.

[0224] Example 3

[0225] This embodiment is used to illustrate the preparation method of the multi-layer reinforced composite foam sheet provided by the present invention, which comprises the following steps:

[0226] (1) Preparation of polypropylene composition A:

[0227] Same as Example 1, wherein the mass fraction Wa of component a is 90 parts by weight, and the mass fraction Wb of component b is 10 parts by weight. 0.05 parts by weight of a β-crystal nucleating agent with a grade of VP101B is added. A pellet of polypropylene composition A is obtained. After testing, the melting point of the pellet of polypropylene composition A is 158°C.

[0228] (2) Polypropylene composition B i Preparation:

[0229] Same as Example 1, wherein the corresponding component x i The mass fraction Wx i The mass fraction Wy of component y is 10 parts by weight, and the polypropylene composition B is finally obtained. i Granules, (i.e. x i +y=B i , i=1, 2, 3), after testing, the melting point of B1 is 128°C, the melting point of B2 is 134°C, and the melting point of B3 is 139°C.

[0230] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0231] The preparation process is the same as step (3) of Example 1.

[0232] (4) Preparation of polypropylene fabric:

[0233] The preparation process is the same as step (4) of Example 1.

[0234] (5) Preparation of polyolefin thermoplastic elastomer composition for foam sheet:

[0235] 40g of POE-O, 60g of EVA (5110), 4.6g of triphosphorus triazine, 0.15g of di-tert-butyl peroxide diisopropylbenzene, 0.13g of stearic acid, 0.15g of zinc stearate, 0.23g of zinc oxide, 32g of kaolin and 1g of MW103 were mixed by internal kneading at a kneading temperature of 105°C and a mixing time of 9.5min. A single-screw extruder was then used with air-cooled pelletizing to prepare the composite particles without drying.

[0236] (6) Preparation of polyolefin thermoplastic elastomer composition foamed sheet:

[0237] The temperature of the compression foaming machine was raised to 168°C and stabilized for 20 minutes; the granulated particles of the composition were added to the foaming machine; the foaming temperature was set to 173°C, the compression foaming time was 580 seconds, and the back pressure was 9MPa; after the pressure holding time was 70 seconds, the pressure was released and the mold was jumped to obtain the polyolefin thermoplastic elastomer composition foaming material, and the foamed sheet of the required size was obtained by laser line cutting. The density of the foamed sheet is 0.21g / cm 3 , the thickness after cutting is 5mm.

[0238] (7) Preparation of multi-layer reinforced composite foam sheet:

[0239] The preparation process is the same as step (7) of Example 1. That is, the structure of the multi-layer reinforced composite foam sheet is 5 (5 layers of fabric) + 1 (foamed sheet) + 5 (5 layers of fabric); the thickness of the prepared multi-layer reinforced composite foam sheet is 5.65 mm.

[0240] Example 4

[0241] This embodiment is used to illustrate the preparation method of the multi-layer reinforced composite foam sheet provided by the present invention, which comprises the following steps:

[0242] (1) Preparation of polypropylene composition A:

[0243] The preparation process is the same as step (1) of Example 1.

[0244] (2) Polypropylene composition B i Preparation:

[0245] The preparation process is the same as step (2) of Example 1.

[0246] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0247] The main steps are the same as those in Example 1. The thickness of the polypropylene sheet is 80 μm, wherein the thickness of the film layer A accounts for 90% of the total thickness of the sheet.

[0248] (4) Preparation of polypropylene fabric:

[0249] The preparation process is the same as step (4) of Example 1.

[0250] (5) Preparation of polyolefin thermoplastic elastomer composition for foam sheet:

[0251] 40g of POE-O, 60g of EVA (5110), 4.6g of triphosphorus triazine, 0.15g of di-tert-butyl peroxide diisopropylbenzene, 0.13g of stearic acid, 0.15g of zinc stearate, 0.23g of zinc oxide, 32g of kaolin and 1g of MW103 were mixed by internal kneading at a kneading temperature of 105°C and a mixing time of 9.5min. A single-screw extruder was then used with air-cooled pelletizing to prepare the composite particles without drying.

[0252] (6) Preparation of polyolefin thermoplastic elastomer composition foamed sheet:

[0253] The temperature of the compression foaming machine was raised to 168°C and stabilized for 20 minutes; the granulated particles of the composition were added to the foaming machine; the foaming temperature was set to 173°C, the compression foaming time was 580 seconds, and the back pressure was 9MPa; after the pressure holding time was 70 seconds, the pressure was released and the mold was jumped to obtain the polyolefin thermoplastic elastomer composition foaming material, and the foamed sheet of the required size was obtained by laser line cutting. The density of the foamed sheet is 0.21g / cm 3 , the thickness after cutting is 5mm.

[0254] (7) Preparation of multi-layer reinforced composite foam sheet:

[0255] The preparation process is the same as step (7) of Example 1. The thickness of the prepared multi-layer reinforced composite foam sheet polypropylene composite material is 5.65 mm.

[0256] Example 5

[0257] This embodiment is used to illustrate the preparation method of the multi-layer reinforced composite foam sheet provided by the present invention, which comprises the following steps:

[0258] (1) Preparation of polypropylene composition A:

[0259] The preparation process is the same as step (1) of Example 1.

[0260] (2) Polypropylene composition B i Preparation:

[0261] The preparation process is the same as step (2) of Example 1.

[0262] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0263] The main preparation process is the same as step (3) of Example 1, wherein the sheet stretching ratio is 10 times.

[0264] (4) Preparation of polypropylene fabric:

[0265] The preparation process is the same as step (4) of Example 1.

[0266] (5) Preparation of polyolefin thermoplastic elastomer composition for foam sheet:

[0267] 20g of POE-B, 20g of POE-O, 60g of EVA (5110), 5.7g of dinitrosopentamethylenetetramine, 0.15g of 1-dimethyl-3-hydroxybutyl ester, 0.10g of stearic acid, 0.12g of zinc stearate, 0.21g of zinc oxide, 27g of zinc borate, and 1.5g of MW101 were mixed and kneaded at a kneading temperature of 95°C and a mixing time of 11.5min. A single-screw extruder was then used with air-cooled pelletizing to prepare the composite particles without drying.

[0268] (6) Preparation of polyolefin thermoplastic elastomer composition foamed sheet:

[0269] The temperature of the compression foaming machine was raised to 173°C and stabilized for 30 minutes; the granulated particles of the composition were added to the foaming machine; the foaming temperature was set to 178°C, the compression foaming time was 600 seconds, and the back pressure was 7MPa; after the pressure holding time was 40 seconds, the pressure was released and the mold was jumped to obtain the polyolefin thermoplastic elastomer composition foaming material, and the foamed sheet of the required size was obtained by laser line cutting. The density of the foamed sheet is 0.25g / cm 3 , the thickness after cutting is 5mm.

[0270] (7) Preparation of multi-layer reinforced composite foam sheet:

[0271] The preparation method is the same as step (7) of Example 1, and the thickness of the prepared multi-layer reinforced composite foam sheet is 5.70 mm.

[0272] Example 6

[0273] This embodiment is used to illustrate the preparation method of the multi-layer reinforced composite foam sheet provided by the present invention, which comprises the following steps:

[0274] (1) Preparation of polypropylene composition A:

[0275] The preparation process is the same as step (1) of Example 1.

[0276] (2) Polypropylene composition B i Preparation:

[0277] The preparation process is the same as step (2) of Example 1.

[0278] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0279] The preparation process is the same as step (3) of Example 1.

[0280] (4) Preparation of polypropylene fabric:

[0281] The preparation process is the same as step (4) of Example 1.

[0282] (5) Preparation of polyolefin thermoplastic elastomer composition for foam sheet:

[0283] The preparation process is the same as step (5) of Example 2.

[0284] (6) Preparation of polyolefin thermoplastic elastomer composition foamed sheet:

[0285] The preparation process is the same as step (6) of Example 2.

[0286] (7) Preparation of multi-layer reinforced composite foam sheet:

[0287] The preparation process is the same as step (7) of Example 1. The polypropylene fabric is placed at 45° between the warp and the warp. The thickness of the prepared multi-layer reinforced composite foam sheet is 5.62 mm.

[0288] Example 7

[0289] This embodiment is used to illustrate the preparation method of the multi-layer reinforced composite foam sheet provided by the present invention, which comprises the following steps:

[0290] (1) Preparation of polypropylene composition A:

[0291] The preparation process is the same as step (1) of Example 1.

[0292] (2) Polypropylene composition B i Preparation:

[0293] The preparation process is the same as step (2) of Example 1.

[0294] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0295] The preparation process is the same as step (3) of Example 1.

[0296] (4) Preparation of polypropylene fabric:

[0297] The preparation process is the same as step (4) of Example 1.

[0298] (5) Preparation of polyolefin thermoplastic elastomer composition for foam sheet:

[0299] The preparation process is the same as step (5) of Example 1.

[0300] (6) Preparation of polyolefin thermoplastic elastomer foamed sheet

[0301] The preparation process is the same as step (6) of Example 1.

[0302] (7) Preparation of multi-layer reinforced composite foam sheet:

[0303] The preparation process is the same as step (7) of Example 1. Instead of preparing the polypropylene fabric, the five-layer co-extruded polypropylene sheet prepared in step (3) replaces the polypropylene fabric obtained in step (4) of Example 1, i.e., the sheets are B3AB3, B2AB2, B1AB1, B2AB2, B3AB3 from bottom to top, with a total of 5 layers, and the stacking and hot pressing are carried out in sequence according to step (5) of Example 1. The middle of the two groups of 5-layer sheets is a polyolefin composition foam sheet, and the thickness of the prepared multi-layer reinforced composite foam sheet is 5.23 mm.

[0304] Example 8

[0305] This embodiment is used to illustrate the preparation method of the multi-layer reinforced composite foam sheet provided by the present invention, which comprises the following steps:

[0306] (1) Preparation of polypropylene composition A:

[0307] The preparation process is the same as step (1) of Example 1.

[0308] (2) Polypropylene composition B i Preparation:

[0309] The preparation process is the same as step (2) of Example 1.

[0310] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0311] The preparation process is the same as step (3) of Example 1.

[0312] (4) Preparation of polypropylene fabric:

[0313] The preparation process is the same as step (4) of Example 1.

[0314] (5) Preparation of polyolefin thermoplastic elastomer composition for foam sheet:

[0315] The preparation process is the same as step (5) of Example 1.

[0316] (6) Preparation of polyolefin thermoplastic elastomer composition foamed sheet:

[0317] The preparation process is the same as step (6) of Example 1, but the thickness after cutting is 10 mm.

[0318] (7) Preparation of multi-layer reinforced composite foam sheet:

[0319] The preparation process is the same as step (7) of Example 1. The difference is that a foam sheet prepared in step (6) is placed between two groups of 5 layers of polypropylene fabric (from bottom to top, B3AB3, B2AB2, B1AB1, B2AB2, B3AB3, and the total number of layers is 5). The thickness of the prepared multi-layer reinforced composite foam sheet is 10.45 mm.

[0320] Example 9

[0321] This embodiment is used to illustrate the preparation method of the multi-layer reinforced composite foam sheet provided by the present invention, which comprises the following steps:

[0322] (1) Preparation of polypropylene composition A:

[0323] The preparation process is the same as step (1) of Example 1.

[0324] (2) Polypropylene composition B i Preparation:

[0325] The preparation process is the same as step (2) of Example 1.

[0326] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0327] The preparation process is the same as step (3) of Example 1.

[0328] (4) Preparation of polypropylene fabric:

[0329] The preparation process is the same as step (4) of Example 1.

[0330] (5) Polyolefin thermoplastic elastomer composition foamed sheet:

[0331] The preparation process is the same as step (5) of Example 1.

[0332] (6) Preparation of polyolefin thermoplastic elastomer composition foamed sheet

[0333] The preparation process is the same as step (6) of Example 1, but the thickness after cutting is 20 mm.

[0334] (7) Preparation of multi-layer reinforced composite foam sheet:

[0335] The preparation process is the same as step (7) of Example 1. The difference is that a foam sheet prepared in step (6) is placed in the middle of the sheet. The thickness of the prepared polypropylene composite foam sheet is 19.95 mm.

[0336] Example 10

[0337] This embodiment is used to illustrate the preparation method of the multi-layer reinforced composite foam sheet provided by the present invention, which comprises the following steps:

[0338] (1) Preparation of polypropylene composition A:

[0339] The preparation process is the same as step (1) of Example 1.

[0340] (2) Polypropylene composition B i Preparation:

[0341] The preparation process is the same as step (2) of Example 1.

[0342] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0343] The preparation process is the same as step (3) of Example 1.

[0344] (4) Preparation of polypropylene fabric and reinforced composite sheet:

[0345] The preparation process is the same as step (4) of Example 1, and polypropylene fabrics B1AB1, B2AB2, and B3AB3 are obtained respectively. The obtained polypropylene fabrics are stacked in sequence, from bottom to top, B3A3B3, B2A2B2, B1A1B1, B2A2B2, and B3A3B3, and the total number of stacked layers is 5. The stacked polypropylene fabrics are hot-pressed and fused, and then cooled and shaped to form a reinforced composite sheet. The polypropylene fabric is placed in a direction of 90° between the warp and the warp. The hot pressing conditions used are: temperature 145°C, hot pressing pressure 5MPa, preheating time 90s, hot pressing time 90s, and cooling time 300s.

[0346] (5) Preparation of polyolefin thermoplastic elastomer composition for foam sheet:

[0347] The preparation process is the same as step (5) of Example 1.

[0348] (6) Preparation of polyolefin thermoplastic elastomer composition foamed sheet:

[0349] The preparation process is the same as step (6) of Example 1. The cutting thickness is still 5 mm.

[0350] (7) Preparation of multi-layer reinforced composite foam sheet:

[0351] The main steps are the same as step (7) of Example 1. The difference is that the laminated polypropylene sheet includes 3 groups of 5 layers of polypropylene fabrics to prepare reinforced composite sheets and 2 layers of polyolefin elastomer composition foamed sheets. The hot pressing equipment is also different. The reinforced composite sheet and the polyolefin elastomer composition foamed sheet are placed in a set of ovens containing a pressing plate, and the pressing plate is placed on the uppermost reinforced composite sheet. The hot pressing temperature is close to the softening temperature of the surface of polyolefin thermoplastic elastomer, which is 70°C. After the laminated polypropylene sheet and the polyolefin elastomer composition reach 70°C, the temperature is kept constant for 5 minutes, and the hot pressing is completed for 30 seconds. The hot pressing pressure is 3.5MPa, and the thickness of the prepared multi-layer reinforced composite foamed sheet is 10.77mm.

[0352] The structure is shown below:

[0353]

[0354] Embodiment 11

[0355] This embodiment is used to illustrate the preparation method of the multi-layer reinforced composite foam sheet provided by the present invention, which comprises the following steps:

[0356] (1) Preparation of polypropylene composition A:

[0357] The preparation process is the same as step (1) of Example 1.

[0358] (2) Preparation of polypropylene composition B:

[0359] The preparation process is the same as step (2) of Example 1.

[0360] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0361] The preparation process is the same as step (3) of Example 1.

[0362] (4) Preparation of polypropylene fabric:

[0363] The preparation process is the same as step (4) of Example 1.

[0364] (5) Polyolefin thermoplastic elastomer composition foamed sheet:

[0365] The preparation process is the same as step (5) of Example 1.

[0366] (6) Preparation of polyolefin thermoplastic elastomer composition foamed sheet:

[0367] The preparation process is the same as step (6) of Example 1, but the thickness after cutting is 60 mm.

[0368] (7) Preparation of multi-layer reinforced composite foam sheet:

[0369] The preparation process is the same as step (7) of Example 1. The difference is that a foam sheet prepared in step (6) of this example is placed between the two groups of laminated sheets. The thickness of the prepared polypropylene composite foam sheet is 58.13 mm.

[0370] Comparative Example 1

[0371] A three-layer co-extruded polypropylene sheet was prepared according to the method of Example 1, except that only the polypropylene composition A was used for extrusion casting into a single-layer film with a thickness of 80 μm. A polypropylene fabric was prepared according to the method of Example 1.

[0372] The preparation process of the polyolefin thermoplastic elastomer composition for foam sheet is the same as step (5) of Example 1, the preparation process of the polyolefin thermoplastic elastomer composition foam sheet is the same as step (6) of Example 1, and the preparation process of the multi-layer reinforced composite foam sheet is the same as step (7) of Example 1, to obtain a multi-layer reinforced composite foam sheet with a thickness close to that of Example 1, which is 5.61 mm.

[0373] Comparative Example 2

[0374] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 1 except that only polypropylene composition B was used. i The extrusion casting was a single-layer film with a thickness of 80 μm. A polypropylene fabric was prepared according to the method of Example 1.

[0375] The preparation process of the polyolefin thermoplastic elastomer composition for foam sheet is the same as step (5) of Example 1, the preparation process of the polyolefin thermoplastic elastomer composition foam sheet is the same as step (6) of Example 1, and the preparation process of the multi-layer reinforced composite foam sheet is the same as step (7) of Example 1, to obtain a multi-layer reinforced composite foam sheet with a thickness close to that of Example 1, which is 5.63 mm.

[0376] Comparative Example 3

[0377] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 1, except that the polypropylene composition A contained only component b. A polypropylene fabric was prepared according to the method of Example 1.

[0378] The preparation process of the polyolefin thermoplastic elastomer composition for foam sheet is the same as step (5) of Example 1, the preparation process of the polyolefin thermoplastic elastomer composition foam sheet is the same as step (6) of Example 1, and the preparation process of the multi-layer reinforced composite foam sheet is the same as step (7) of Example 1, to obtain a multi-layer reinforced composite foam sheet with a thickness close to that of Example 1, which is 5.62 mm.

[0379] Comparative Example 4

[0380] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 1. iThe polypropylene fabric was prepared according to the method of Example 1.

[0381] The preparation process of the polyolefin thermoplastic elastomer composition for foam sheet is the same as step (5) of Example 1, the preparation process of the polyolefin thermoplastic elastomer composition foam sheet is the same as step (6) of Example 1, and the preparation process of the multi-layer reinforced composite foam sheet is the same as step (7) of Example 1, to obtain a multi-layer reinforced composite foam sheet with a thickness close to that of Example 1, which is 5.63 mm.

[0382] Comparative Example 5

[0383] A coextruded polypropylene sheet was prepared according to the method of Example 6, except that component B i The materials are selected in the following manner: component x1 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 140°C; component x2 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 135°C; component x3 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 130°C; the melt flow rates of components x1-x3 are all 2-10g / 10min.

[0384] Finally, the polypropylene composition B is obtained. i Granules (i.e. x i +y=B i , i=1, 2, 3), after testing, the melting point of B1 is 138° C., the melting point of B2 is 132° C., and the melting point of B3 is 127° C. According to the method of Example 1, a polypropylene fabric is prepared.

[0385] The preparation process of the polyolefin thermoplastic elastomer composition for foam sheet is the same as step (5) of Example 1, the preparation process of the polyolefin thermoplastic elastomer composition foam sheet is the same as step (6) of Example 1, and the preparation process of the multi-layer reinforced composite foam sheet is the same as step (7) of Example 1, to obtain a multi-layer reinforced composite foam sheet with a thickness close to that of Example 1, which is 5.62 mm.

[0386] Comparative Example 6

[0387] The preparation process of the polyolefin thermoplastic elastomer composition for foam sheet is the same as steps (1-5) of Example 1, and the preparation process of the polyolefin thermoplastic elastomer composition foam sheet is the same as step (6) of Example 1. In the hot pressing process, only five layers of fabric (5 layers of fabric, from bottom to top are B3A3B3, B2A2B2, B1A1B1, B2A2B2, B3A3B3, and the total number of stacked layers is 5 layers) prepared in step (6) are hot-pressed and compounded in the middle of the upper and lower polyolefin thermoplastic elastomer foam sheets, that is, the structure is a piece of polyolefin thermoplastic elastomer foam sheet + a group of five layers of fabric + a piece of polyolefin thermoplastic elastomer foam sheet, with a thickness of 10.02 mm.

[0388] Comparative Example 7

[0389] According to the method of Example 1, a three-layer co-extruded polypropylene sheet and a polypropylene fabric were prepared.

[0390] The preparation process of the polyolefin thermoplastic elastomer composition for foam sheet is the same as step (5) of Example 1, the preparation process of the polyolefin thermoplastic elastomer composition foam sheet is the same as step (6) of Example 1, and the preparation process of the multi-layer reinforced composite foam sheet is the same as step (7) of Example 1, except that two square glass fiber / nylon composite sheets with a thickness of 1.7 mm are compounded above and below the two polyolefin thermoplastic elastomer composition foam sheets prepared in step (6), that is, the square glass fiber / nylon composite sheets are used to replace the five layers of fabric in Example 1, to obtain a multi-layer reinforced composite foam sheet with a thickness of 8.24 mm.

[0391] Comparative Example 8

[0392] According to the method of Example 1, a three-layer co-extruded polypropylene sheet and a polypropylene fabric were prepared.

[0393] The preparation process of the polyolefin thermoplastic elastomer composition for the foam sheet is the same as step (5) of Example 1, the preparation process of the polyolefin thermoplastic elastomer composition foam sheet is the same as step (6) of Example 1, and the preparation process of the multi-layer reinforced composite foam sheet is the same as step (7) of Example 1. The hot pressing pressure is 20 MPa, and the multi-layer reinforced composite foam sheet is obtained, and the thickness is 3.55 mm. It can be seen that the thickness of the obtained multi-layer reinforced composite foam sheet is thin, and the excessive pressure causes the microscopic cell structure of the polyolefin elastomer composition foam sheet to break, and it becomes seriously thinner after hot pressing.

[0394] Comparative Example 9

[0395] The preparation method of the multi-layer reinforced composite foam sheet comprises the following steps:

[0396] (1) Preparation of polypropylene composition A:

[0397] The preparation process is the same as step (1) of Example 1.

[0398] (2) Polypropylene composition B i Preparation:

[0399] The preparation process is the same as step (2) of Example 1.

[0400] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0401] The preparation process is the same as step (3) of Example 1.

[0402] (4) Preparation of polypropylene fabric:

[0403] The preparation process is the same as step (4) of Example 1.

[0404] (5) Preparation of polyolefin thermoplastic elastomer composition for foam sheet:

[0405] The preparation process is the same as step (5) of Example 1.

[0406] (6) Preparation of polyolefin thermoplastic elastomer composition

[0407] The preparation process is the same as step (6) of Example 1.

[0408] (7) Preparation of multi-layer reinforced composite foam sheet:

[0409] The main steps are the same as step (7) of Example 1. The difference is that the laminated polypropylene sheet includes 10 layers of polypropylene fabrics all on one side of the foam sheet prepared in step (6), and the thickness of the obtained multi-layer reinforced composite foam sheet is 5.65 mm.

[0410] Comparative Example 10

[0411] The preparation method of the multilayer reinforced composite sheet is the same as that of Example 1, but without step (6), that is, without the polyolefin thermoplastic elastomer composition foamed sheet. The upper and lower groups of polypropylene fabrics in Example 1 are hot pressed to obtain a composite sheet with a thickness of 0.8 mm.

[0412] Comparative Example 11

[0413] The same as step (5) + step (6) of Example 1, without reinforcing sheet and without hot pressing process, the thickness of the obtained polyolefin thermoplastic elastomer foam sheet is 5 mm.

[0414] Comparative Example 12

[0415] The same as Example 11, but the polyolefin elastomer composition foamed sheet does not contain maleic anhydride microspheres, to obtain a multi-layer reinforced composite foamed sheet with a thickness of 58.15 mm.

[0416] Experimental example

[0417] The polypropylene composite foam sheets obtained in the above examples and comparative examples were tested according to the following method. The test results are shown in Table 1.

[0418] (1) Tensile strength: Samples were prepared and measured according to the method specified in GB / T1040.1-2018. The tensile strength in the table is the tensile strength of the foamed composite molding. When testing the tensile strength, it needs to be divided by the cross-sectional area. The foamed sheet part contributes less thickness and strength.

[0419] (2) Interlayer peel strength: Prepare samples and measure them according to the method specified in GB / T 3903.39-2019.

[0420] (3) Drop weight impact strength: measured according to the method specified in GB / T14153-1993.

[0421] (4) The apparent density of the composite foam sheet shall be prepared and measured according to the method specified in GB / T6343.

[0422] (5) The thermal conductivity of the composite foam sheet shall be prepared and measured according to the method specified in GB / T 10294.

[0423] Table 1

[0424]

[0425]

[0426] From the results of the embodiment in Table 1, it can be seen that compared with the common foam sheet without composite reinforcement in Comparative Example 11, the polyolefin thermoplastic elastomer composite foam sheet prepared according to the present invention has both good tensile properties and impact resistance, and has good interlayer peeling strength at a lower hot pressing temperature. And it does not significantly increase the thermal conductivity and reduce its thermal insulation capacity.

[0427] It can be seen from Comparative Examples 1-5 that only using a single-layer sheet structure, a single polymer component or using an interlayer ratio outside the scope of the embodiment will lead to a decrease in the performance of the laminated polypropylene sheet or fabric, thereby causing a decrease in various properties of the final composite foam sheet.

[0428] It can be seen from Example 11 and Comparative Example 8 that increasing the thickness ratio of the polyolefin elastomer composition foam sheet is beneficial to reducing the thermal conductivity of the composite foam material. Excessive hot pressing pressure causes the microscopic cell structure of the polyolefin elastomer composition foam sheet in Comparative Example 8 to rupture, thereby significantly reducing the drop hammer impact and lightweight performance.

[0429] It can be seen from Examples 9 and 12 that the amount of polypropylene fabric and the amount of foamed sheet have a significant impact on the final product. As the number of fabric layers and the thickness of the foamed sheet increase, some physical properties (drop weight performance) are improved.

[0430] It can be seen from Example 11 and Comparative Example 12 that when the thickness of the added foam sheet is relatively large (60 mm), thanks to the good interface bonding ability of the maleic anhydride microspheres, the polyolefin thermoplastic elastomer composite foam sheet can be hot-pressed with the polypropylene laminate material in multiple layers, while the multi-layer polyolefin elastomer composition foam sheet without maleic anhydride microspheres is difficult to be hot-pressed with the polypropylene fabric to obtain a foamed product with sufficient peel strength. That is, it can be seen from Comparative Example 12 that although the polyolefin elastomer composition foam sheet without maleic anhydride microspheres can be hot-pressed to obtain a multi-layer reinforced composite foam sheet, the interlayer tear strength is reduced to 70% of the original Example 11.

[0431] It can be seen from Comparative Example 7 that although the use of glass fiber / nylon composite sheets and other commonly used sheet composite reinforcement methods in the industry can also improve the physical properties of the composite foam sheet to be close to the level of the embodiments, the glass fiber / nylon composite sheet has poor compatibility with the polyolefin thermoplastic elastomer composition foam sheet. At the same time, the thermal conductivity of glass fiber reinforced nylon (that is, glass fiber / nylon composite sheet) is high, so the peel strength and thermal insulation performance of the composite foam sheet are also greatly reduced. In addition, the density of the glass fiber / nylon composite sheet is high, so the apparent density of the composite foam sheet is also significantly improved.

[0432] It can be seen from Example 5 that the lower the foaming ratio of the polyolefin elastomer composition foam material, the higher the density, the smaller the deformation during hot pressing, and the greater the thickness.

[0433] As can be seen from Example 7, when the polypropylene sheet is used directly instead of the woven polypropylene fabric, the thermoplastic elastomer composition foam material is compressed more significantly during the hot pressing process, resulting in a multi-layer reinforced composite foam sheet with a high density and a low thermal conductivity. It is preferred to use polypropylene fabric.

[0434] It can be seen from Comparative Example 9 that the present invention can be realized only when the outer layers of the multi-layer reinforced composite foamed sheet are all reinforced composite sheets, that is, the structure is a sandwich structure.

[0435] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

[0436] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

Claims

1. A multi-layer reinforced composite foam sheet having a laminated structure, comprising at least two layers of reinforced composite sheets and at least one layer of thermoplastic elastomer composition foam sheet, and the outer layers of the multi-layer reinforced composite foam sheet are all reinforced composite sheets; The reinforced composite sheet comprises at least one layer of polypropylene sheet and / or at least one layer of polypropylene fabric woven from polypropylene sheets; wherein, The polypropylene sheet comprises a layer A and layers B and B' located on both sides of the layer A, and has a structure of BAB'; Wherein layer A contains polypropylene composition A, layer B and layer B' are the same or different, and each layer contains polypropylene composition B and polypropylene composition B', and the melting point of the polypropylene composition A is greater than the melting points of the polypropylene composition B and the polypropylene composition B'; The polypropylene composition A comprises homopolymer polypropylene a and impact copolymer polypropylene b; the polypropylene composition B and the polypropylene composition B' each comprise random copolymer polypropylene x and thermal bonding enhancer y; The thermoplastic elastomer composition foamed sheet and the reinforced composite sheet are bonded by hot pressing fusion.

2. The multi-layer reinforced composite foam sheet according to claim 1, characterized in that: Based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 50-99wt% of homopolypropylene a and 1-50wt% of impact copolymer polypropylene b; preferably, the polypropylene composition A comprises 70-90wt% of homopolypropylene a and 10-30wt% of impact copolymer polypropylene b; and / or, Based on the total weight of the polypropylene composition B and the polypropylene composition B', the polypropylene composition B and the polypropylene composition B' each include 70-99wt% of random copolymer polypropylene x and 1-30wt% of thermal adhesion enhancer y; preferably, the polypropylene composition B and the polypropylene composition B' each include 80-90wt% of random copolymer polypropylene x and 10-20wt% of thermal adhesion enhancer y.

3. The multi-layer reinforced composite foam sheet according to claim 1, characterized in that: Based on the total thickness of the polypropylene sheet, the thickness of layer A accounts for 51%-89% of the total thickness, preferably 71%-89%, and more preferably 71%-80%.

4. The multi-layer reinforced composite foam sheet according to claim 1, characterized in that: The homopolymer polypropylene a has: The melting point is 150-170°C, preferably 160-170°C; and / or, The melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or, The isotacticity (mm) is not less than 96%.

5. The multi-layer reinforced composite foam sheet according to claim 1, characterized in that: The melting point of the impact-resistant copolymer polypropylene b is 150-170° C.: and / or, The monomer of the impact copolymer polypropylene b and propylene copolymer is ethylene or butene, preferably butene; and / or, The impact copolymer polypropylene b has a melt flow rate of 0.5-50 g / 10 min at 230° C. and a load of 2.16 kg, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or, The cantilever beam impact strength of the impact-resistant copolymer polypropylene b is not less than 20KJ / m 2 .

6. The multi-layer reinforced composite foam sheet according to claim 1, characterized in that: The random copolymer polypropylene x has: The melting point is 110-150°C, preferably 120-140°C; and / or, The melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 3-18 g / 10 min; and / or, The molecular weight distribution Mw / Mn is 5-12, preferably 7-10; and / or, It is a copolymer of propylene and ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer and / or a propylene-ethylene binary copolymer.

7. The multi-layer reinforced composite foam sheet according to claim 1, characterized in that: The thermal bonding enhancer y has: The melting point or viscosity flow temperature is 50-110°C; and / or, The melt flow rate at 190°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 1-18 g / 10 min; and / or, One or more selected from polyolefin elastomer, EPDM rubber, SEBS, SBS, EVA, and petroleum resin; preferably, polyolefin elastomer and / or petroleum resin.

8. The multi-layer reinforced composite foam sheet according to claim 7, characterized in that: The polyolefin elastomer is a copolymer elastomer of ethylene and propylene and / or alpha olefin, wherein the alpha olefin is preferably a C4-C12 alpha olefin, more preferably 1-butene and / or 1-octene; and / or, The petroleum resin is a C5 and / or C9 hydrogenated petroleum resin with a softening point of 100-150° C. and is preferably a cyclopentadiene type resin.

9. The multi-layer reinforced composite foam sheet according to claim 1, characterized in that: The layer A also contains a β-crystalline nucleating agent; preferably, The β-crystal nucleating agent is at least one selected from the group consisting of condensed aromatic hydrocarbons, group IIA two-component complexes, aromatic diamides, rare earth compounds and cyclic dicarboxylates; and / or, Relative to 100 parts by weight of the polypropylene composition A, the content of the β-crystal nucleating agent in layer A is 0.01-0.5 parts by weight.

10. The multi-layer reinforced composite foam sheet according to any one of claims 1 to 9, characterized in that: The melting point of the homopolymer polypropylene a in the polypropylene composition A is greater than the melting point of the random copolymer polypropylene x in the polypropylene compositions B and B', and the temperature difference of the corresponding melting points is preferably greater than or equal to 10 degrees; and / or, The BAB' sheet structure of the polypropylene sheet is obtained by co-extruding components including the polypropylene composition A and the polypropylene compositions B and B'.

11. The multi-layer reinforced composite foam sheet according to any one of claims 1 to 9, characterized in that: Each layer of the reinforced composite sheet comprises a plurality of sequentially stacked polypropylene sheet unit groups; each polypropylene sheet unit group comprises at least one identical or different polypropylene sheet unit, each polypropylene sheet unit comprises a core layer A i and located in the core layer A i The outer layer B on both sides i , B' i , structure B i A i B' i The structure of the reinforced composite sheet is nth group...ith group...2nd group, 1st group, 2nd group...ith group...nth group from bottom to top, and the total number of stacked groups of polypropylene sheet unit groups is 2n-1; i and n are both integers not less than 2, and i≤n; Among them, the core layer A in the polypropylene sheet unit i Containing polypropylene composition A i , outer layer B i With outer layer B' i The same or different, each corresponding to a polypropylene composition B i , polypropylene composition B' i , The polypropylene composition A i The melting point is greater than that of the polypropylene composition B i , the polypropylene composition B' i The average melting point of all outer layers in the i-th group is greater than or equal to the average melting point of all outer layers in the i-1th group; preferably, Polypropylene composition A i Melting point and polypropylene composition B i The difference in melting points, polypropylene composition A i The melting point of polypropylene composition B' i The difference in melting points of each is greater than or equal to 5°C, preferably greater than or equal to 10°C, more preferably greater than or equal to 20°C; and / or, The difference between the average melting point of all outer layers in the i-th group and the average melting point of all outer layers in the i-1th group is the same or different, and is 1-40°C, preferably 1-10°C, more preferably 1-5°C; and / or, 2≤n≤100, preferably, 2≤n≤50; and / or, Each group of polypropylene ply units, independently of one another, comprises 1 to 10, preferably 1 to 5, identical or different polypropylene ply units.

12. The multi-layer reinforced composite foam sheet according to any one of claims 1 to 9, characterized in that: The multi-layer reinforced composite foam sheet has a multi-layer sandwich structure; and / or, Based on the total thickness of the multi-layer reinforced composite foam sheet, the total thickness of the reinforced composite sheet accounts for 1.3%-15.5% of the total thickness of the multi-layer reinforced composite foam sheet, preferably 4%-15.5%; and / or, the number of laminated layers of the reinforced composite sheet and the thermoplastic elastomer composition foam sheet is greater than or equal to 3 layers, preferably 3-100 layers, more preferably 6-60 layers; and / or, The thermoplastic elastomer composition foamed sheets are stacked in order from top to bottom along their respective machine directions at an angle of 0-90°, preferably with a number of layers greater than or equal to 1, more preferably 1-10, and most preferably 2-5; and / or, The reinforced composite sheets are stacked from top to bottom in the direction of 0-90° along their respective machine directions. Preferably, the total number of polypropylene sheets and polypropylene fabrics in each layer of the reinforced composite sheet is greater than or equal to 2 layers, more preferably 2-100 layers, and most preferably 4-40 layers.

13. The multi-layer reinforced composite foam sheet according to any one of claims 1 to 9, characterized in that: The density of the thermoplastic elastomer composition foamed sheet is 0.01 to 0.5 g / L, preferably 0.1 to 0.4 g / L; and / or, The thermoplastic elastomer composition foamed sheet contains a polyolefin thermoplastic elastomer composition, and the polyolefin thermoplastic elastomer composition contains POE and EVA and optional additives; preferably, In parts by weight, the total weight of POE and EVA is 100 parts by weight, the content of POE is 5 to 50 parts by weight, and the total amount of EVA is 50 to 95 parts by weight; and / or, the auxiliary agent is selected from a crosslinking agent, a foaming agent, stearic acid, zinc stearate, zinc oxide, a filler and maleic anhydride copolymer microspheres; more preferably, In parts by weight, relative to the total weight of 100 parts of POE and EVA, the content of the cross-linking agent is 0.1 to 1 part by weight, preferably 0.3 to 0.8 parts by weight; the content of the foaming agent is 0.1 to 10 parts by weight, preferably 2 to 7 parts by weight; the content of the stearic acid is 0.1 to 1 part by weight, preferably 0.2 to 0.5 parts by weight; the content of the zinc stearate is 0.1 to 1 part by weight, preferably 0.2 to 0.5 parts by weight; the content of the zinc oxide is 0.1 to 10 parts by weight, preferably 0.5 to 2 parts by weight; the content of the filler is 1 to 40 parts by weight, preferably 5 to 30 parts by weight; the content of the maleic anhydride copolymer microspheres is 0.1 to 5 parts by weight, preferably 0.2 to 1 part by weight.

14. A method for preparing the multi-layer reinforced composite foam sheet according to any one of claims 1 to 13, comprising laminating the polypropylene sheet and / or the polypropylene fabric with the thermoplastic elastomer composition foam sheet, fusing them by hot pressing, and cooling to shape, to obtain the multi-layer reinforced composite foam sheet; or comprising first laminating the polypropylene sheet and / or the polypropylene fabric, fusing them by hot pressing to obtain a reinforced composite sheet; and then laminating the reinforced composite sheet with the thermoplastic elastomer composition foam sheet, fusing them at 60-80° C. to obtain the multi-layer reinforced composite foam sheet; preferably, The polypropylene sheets and / or the polypropylene fabrics are stacked in order to form corresponding layers of reinforced composite sheets.

15. The preparation method according to claim 14, characterized in that: The conditions of the hot pressing fusion include: The hot pressing temperature is 115-170°C, preferably 115-159°C, and more preferably 140-159°C; and / or, the hot pressing pressure is 2-10MPa, the preheating time is 5-600s, the hot pressing time is 1-600s, and preferably 10-500s; and / or, the cooling pressure is 2-8MPa, and the cooling time is 30s-700s.

16. Application of the multi-layer reinforced composite foam sheet according to any one of claims 1 to 13 or the multi-layer reinforced composite foam sheet prepared by the preparation method according to any one of claims 14 to 15 in the fields of automobiles, communications, aircraft, logistics, thermal insulation, precision machinery and electronic turnover, and packaging.

Citation Information

Patent Citations

  • Polyolefin composite foamed bead and preparation method thereof

    CN112759843A

  • Low-density toughened polypropylene foam material composition, low-density toughened polypropylene foam material and preparation method of low-density toughened polypropylene foam material

    CN115850783A

  • High-adhesiveness and high-impact polypropylene composite film as well as preparation method and application thereof

    CN115991033A

  • Layered product

    US20020136914A1