Graphene preparation process for middle-high voltage power cable
By forming a continuous graphene film on a copper or nickel substrate and transferring it using TFPA-NH2 crosslinked molecules, the problem of electrolysis cannot prepare large-area and high-quality graphene, achieving efficient graphene preparation and low cost Transfer, suitable for medium and high voltage power cables.
Patent Information
- Application Number
- CN202411137378.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-08
AI Technical Summary
The existing graphene preparation process mainly uses electrolysis, and large-area, high-quality graphene cannot be continuously prepared.
Using substrate metal treatment, pre-carbon metal decomposition, graphene nucleation, adhesion and film transfer, continuous graphene films are formed on copper or nickel substrates, and TFPA-NH2 cross-linked molecules and polymerization are used. The substance forms covalent bonds, which improves the adsorption force of graphene, thereby achieving efficient transfer of graphene.
A large area continuous graphene finished product is achieved, which reduces transfer costs and increases the quality and tensile strength of graphene, which is suitable for the preparation of medium and high voltage power cables.
Smart Images

Figure CN118908197A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of graphene cable preparation, and in particular to a graphene preparation process for medium- and high-voltage power cables. Background Art
[0002] Graphene is a carbon atom in the form of sp 2 The hybrid orbitals form a hexagonal honeycomb lattice of two-dimensional carbon nanomaterials. It has excellent optical, electrical and mechanical properties, and has important application prospects in materials science, micro-nano processing, energy, biomedicine and drug delivery. It is considered to be a revolutionary material in the future. In the preparation process of the cable, graphene is usually added to increase its tensile strength. After searching, it is found that the typical graphene preparation process in the prior art is a graphene preparation process with publication number CN104370286B, which includes at least the following steps: S001: placing graphite particles and electrolyte in a stirrer, and the stirrer stirs the graphite particles in a magnetic field environment so that the graphite particles form millimeter-sized graphene under the shear force of the stirrer; S002: the millimeter-sized graphene rotates in the magnetic field environment to generate a potential difference, so that the ions in the electrolyte combine with the graphene to form a graphene conjugate and an electrolyte mixture; S003: the graphene conjugate and the electrolyte mixture are centrifuged to remove the agglomerated graphene precipitation and collect the suspension; S004: the suspension is filtered, washed, dried and calcined to obtain graphene. Its main characteristics are simple preparation process, strong operability, improved graphene purity, improved graphene production efficiency and reduced production costs.
[0003] In summary, most of the existing graphene is prepared by electrolysis, but the electrolysis preparation process cannot continuously prepare large-area, high-quality graphene. In view of the above problems, the existing equipment needs to be improved. Summary of the invention
[0004] The purpose of the present invention is to provide a graphene preparation process for medium and high voltage power cables to solve the problem mentioned in the above background technology that most of the existing graphene is prepared by electrolysis, and the electrolysis preparation process cannot continuously prepare large-area, high-quality graphene.
[0005] To achieve the above object, the present invention provides the following technical solution: a graphene preparation process for medium and high voltage power cables, comprising the following steps:
[0006] S1, substrate metal processing stage: select a substrate metal copper foil of suitable size, clean it, dry it and set it aside;
[0007] S2, pre-carbon metal decomposition stage: put the base metal copper foil into a vacuum furnace, introduce auxiliary gas protection and heat to 900-1000℃, stabilize the temperature and maintain it, then stop introducing the protective gas and introduce the carbon source instead, and the reaction is completed;
[0008] S3, graphene nucleation stage: After the methane molecules are dehydrogenated, the carbon species on the copper surface aggregate with each other to generate new CC bonds and clusters, and begin to nucleate to form graphene islands. Carbon atoms nucleate at metal defect locations, i.e., metal steps.
[0009] S4, attachment and merging stage: As the number of graphene nuclei on the copper surface increases, the carbon atoms or clusters generated thereafter continue to attach to the nucleation sites, causing the graphene nuclei to gradually grow until they are "stitched" or merged with each other, and then removed from the heating device for cooling and finally connected into a continuous graphene film;
[0010] S5, film transfer stage: first, graphene is grown by the cVD method and the polymer is surface treated to improve the adsorption force between the graphene and the polymer; then, the graphene and TFPA-NH: are fully contacted, that is, the graphene / Cu and TFPA-NH are imprinted by a nanoimprinter at a specific temperature and pressure; finally, the graphene is separated from the metal substrate, that is, after the transfer is completed, it is used for the preparation of medium and high voltage power cables.
[0011] Preferably, the S1 stage substrate metal includes single metals and alloys, and the single metals include Fe, Ru, Co, Rh, Ir, Ni, Pd, Pt, Cu and Au, while the alloys include Co-Ni, Au-Ni, Ni-Mo and stainless steel.
[0012] Preferably, the substrate metal selection in the S1 stage is based on the melting point of the metal, the amount of carbon dissolved, and the stability of the metal carbide.
[0013] Preferably, the S2 stage precursor includes a carbon source and an auxiliary gas, wherein the carbon source includes solid, liquid and gas, and the solid is a carbon-containing polymer material, the liquid is anhydrous ethanol, etc., and the gas includes methane, acetylene and ethylene.
[0014] Preferably, the auxiliary gas in the S2 stage includes hydrogen, argon and nitrogen, and the heating temperature holding time in the S2 stage is 18-20 minutes, and the carbon source introduction time in the S2 stage is 25-30 minutes. At the same time, the vacuum furnace in the S2 stage needs to be cleaned before processing, and the cleaning operation includes cleaning the gas path and removing impurities inside the vacuum furnace.
[0015] Preferably, the air pressure environment in the S4 stage includes ultra-low pressure, low pressure and normal pressure, and the normal pressure environment is 105Pa, the low pressure environment is 10-3Pa~105Pa, and the ultra-low pressure environment is <10-3Pa.
[0016] Preferably, the cooling temperature of the S4 stage is room temperature, and auxiliary cooling and temperature reduction are performed by cooling equipment in the S4 stage.
[0017] Preferably, the carrier gas types in the S4 stage are inert gas, nitrogen and the reducing gas hydrogen used in large quantities; and the inert gas includes helium and argon, and the growth pressure is set to 3atm, the flow rate of the carbon source gas is 10sccm, the flow rate of hydrogen is 500sccm, and the flow rate of argon is 1000sccm.
[0018] Preferably, the S4 stage graphene is divided into high temperature, medium temperature and low temperature according to different growth temperatures, and the high temperature is >800°C, the medium temperature is 600°C to 800°C and the low temperature is <600°C.
[0019] Preferably, the principle of the S5 stage transfer medium is to first deposit a cross-linked molecule called N-ethylamino-4-diazo-tetrafluorobenzoate, i.e., TFPA-NH2, onto polystyrene surface treated with oxygen plasma. The cross-linked molecule can form a covalent bond a with graphene, and the adsorption force generated by the covalent bond between the polymer and graphene is much greater than the adsorption force between the graphene and the metal substrate, thereby enabling the graphene to be separated from the metal substrate.
[0020] Compared with the prior art, the beneficial effects of the present invention are: the graphene preparation process of the medium and high voltage power cable,
[0021] The present invention can effectively solve the problem that most of the existing graphene is prepared by electrolysis, but the electrolysis preparation process cannot continuously prepare large-area, high-quality graphene. In the S4 stage, as the number of graphene nuclei on the copper surface increases, the carbon atoms or clusters generated thereafter continuously adhere to the nucleation positions, so that the graphene nuclei gradually grow until they are "stitched" or merged with each other, thereby forming a continuous large-area finished product of graphene. In addition, the S5 stage adopts dry transfer, and the metal substrate is not etched during the dry transfer and can be reused, so that the transfer cost is greatly reduced. In addition, the graphene transferred to the polymer is of high quality. At the same time, this method can transfer the graphene grown by CVD to various organic or inorganic substrates, thereby further ensuring its large-area characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a schematic diagram of the preparation process of the present invention;
[0023] Figure 2 This is a comparison chart for evaluating the area continuity of the finished product obtained by the present invention;
[0024] Figure 3 A comparison chart of tensile strength evaluation of the finished product obtained by the present invention;
[0025] Figure 4 This is a comparative chart of the impact of the transfer method on the finished products obtained in Example 1, Example 2 and Example 3 of the present invention. DETAILED DESCRIPTION
[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] See also Figure 1-4 The present invention provides a technical solution: a graphene preparation process for medium and high voltage power cables.
[0028] Embodiment 1
[0029] S1, substrate metal processing stage: select a substrate metal copper foil of suitable size, clean it, dry it and set it aside;
[0030] The S1 stage substrate metal includes single metals and alloys, and the single metals include Fe, Ru, Co, Rh, Ir, Ni, Pd, Pt, Cu and Au, while the alloys include Co-Ni, Au-Ni, Ni-Mo and stainless steel.
[0031] The selection criteria for the substrate metal in the S1 stage include the melting point of the metal, the amount of carbon dissolved, and the stability of the metal carbide.
[0032] S2, pre-carbon metal decomposition stage: put the base metal copper foil into a vacuum furnace, introduce auxiliary gas protection and heat to 900-1000℃, stabilize the temperature and maintain it, then stop introducing the protective gas and introduce the carbon source instead, and the reaction is completed;
[0033] The precursors in the S2 stage include a carbon source and an auxiliary gas, wherein the carbon source includes solids, liquids and gases, and the solids are carbon-containing polymer materials, the liquids are anhydrous ethanol, etc., and the gases include methane, acetylene and ethylene.
[0034] The auxiliary gases in the S2 stage include hydrogen, argon and nitrogen, and the heating temperature holding time in the S2 stage is 18-20 minutes. The carbon source introduction time in the S2 stage is 25-30 minutes. At the same time, the vacuum furnace in the S2 stage needs to be cleaned before processing, and the cleaning operation includes cleaning the gas path and removing impurities inside the vacuum furnace.
[0035] S3, graphene nucleation stage: After the methane molecules are dehydrogenated, the carbon species on the copper surface aggregate with each other to generate new CC bonds and clusters, and begin to nucleate to form graphene islands. Carbon atoms nucleate at metal defect locations, i.e., metal steps.
[0036] S4, attachment and merging stage: As the number of graphene nuclei on the copper surface increases, the carbon atoms or clusters generated thereafter continue to attach to the nucleation sites, causing the graphene nuclei to gradually grow until they are "stitched" or merged with each other, and then removed from the heating device for cooling and finally connected into a continuous graphene film;
[0037] The air pressure environment in stage S4 includes ultra-low pressure, low pressure and normal pressure, and the normal pressure environment is 105Pa, the low pressure environment is 10-3Pa~105Pa, and the ultra-low pressure environment is <10-3Pa.
[0038] The cooling temperature of the S4 stage is room temperature, and the S4 stage is assisted by cooling equipment for cooling.
[0039] The carrier gas types in the S4 stage are inert gas, nitrogen and the reducing gas hydrogen used in large quantities; and the inert gas includes helium and argon. At the same time, the growth pressure is set to 3atm, the flow rate of the carbon source gas is 10sccm, the flow rate of hydrogen is 500sccm, and the flow rate of argon is 1000sccm.
[0040] In the S4 stage, graphene is divided into high temperature, medium temperature and low temperature according to the growth temperature, and the high temperature is >800℃, the medium temperature is 600℃~800℃ and the low temperature is <600℃.
[0041] S5, film transfer stage: first, graphene is grown by the cVD method and the polymer is surface treated to improve the adsorption force between the graphene and the polymer; then, the graphene and TFPA-NH: are fully contacted, that is, the graphene / Cu and TFPA-NH are imprinted by a nanoimprinter at a specific temperature and pressure; finally, the graphene is separated from the metal substrate, that is, after the transfer is completed, it is used for the preparation of medium and high voltage power cables.
[0042] The principle of the S5 stage transfer medium is to first deposit a cross-linked molecule called N-ethylamino-4-diazo-tetrafluorobenzoate, i.e. TFPA-NH2, onto polystyrene that has been surface-treated with oxygen plasma. This cross-linked molecule can form a covalent bond with graphene. The adsorption force generated by the covalent bond between the polymer and graphene is much greater than the adsorption force between graphene and the metal substrate, thereby enabling the graphene to be separated from the metal substrate.
[0043] Embodiment 2
[0044] S1, substrate metal processing stage: select a substrate metal copper foil of suitable size, clean it, dry it and set it aside;
[0045] The S1 stage substrate metal includes single metals and alloys, and the single metals include Fe, Ru, Co, Rh, Ir, Ni, Pd, Pt, Cu and Au, while the alloys include Co-Ni, Au-Ni, Ni-Mo and stainless steel.
[0046] The selection criteria for the substrate metal in the S1 stage include the melting point of the metal, the amount of carbon dissolved, and the stability of the metal carbide.
[0047] S2, pre-carbon metal decomposition stage: put the base metal copper foil into a vacuum furnace, introduce auxiliary gas protection and heat to 900-1000℃, stabilize the temperature and maintain it, then stop introducing the protective gas and introduce the carbon source instead, and the reaction is completed;
[0048] The precursors in the S2 stage include a carbon source and an auxiliary gas, wherein the carbon source includes solids, liquids and gases, and the solids are carbon-containing polymer materials, the liquids are anhydrous ethanol, etc., and the gases include methane, acetylene and ethylene.
[0049] The auxiliary gases in the S2 stage include hydrogen, argon and nitrogen, and the heating temperature holding time in the S2 stage is 18-20 minutes. The carbon source introduction time in the S2 stage is 25-30 minutes. At the same time, the vacuum furnace in the S2 stage needs to be cleaned before processing, and the cleaning operation includes cleaning the gas path and removing impurities inside the vacuum furnace.
[0050] S3, graphene nucleation stage: After the methane molecules are dehydrogenated, the carbon species on the copper surface aggregate with each other to generate new CC bonds and clusters, and begin to nucleate to form graphene islands. Carbon atoms nucleate at metal defect locations, i.e., metal steps.
[0051] S4, attachment and merging stage: As the number of graphene nuclei on the copper surface increases, the carbon atoms or clusters generated thereafter continue to attach to the nucleation sites, causing the graphene nuclei to gradually grow until they are "stitched" or merged with each other, and then removed from the heating device for cooling and finally connected into a continuous graphene film;
[0052] The air pressure environment in stage S4 includes ultra-low pressure, low pressure and normal pressure, and the normal pressure environment is 105Pa, the low pressure environment is 10-3Pa~105Pa, and the ultra-low pressure environment is <10-3Pa.
[0053] The cooling temperature of the S4 stage is room temperature, and the S4 stage is assisted by cooling equipment for cooling.
[0054] The carrier gas types in the S4 stage are inert gas, nitrogen and the reducing gas hydrogen used in large quantities; and the inert gas includes helium and argon. At the same time, the growth pressure is set to 3atm, the flow rate of the carbon source gas is 10sccm, the flow rate of hydrogen is 500sccm, and the flow rate of argon is 1000sccm.
[0055] In the S4 stage, graphene is divided into high temperature, medium temperature and low temperature according to the growth temperature, and the high temperature is >800℃, the medium temperature is 600℃~800℃ and the low temperature is <600℃.
[0056] S5, thin film transfer stage: the transfer medium spin-coated on the graphene surface is used as a support layer; then it is immersed in an appropriate chemical solution to corrode the metal substrate; it is then scooped out and cleaned with distilled water and transferred to the target substrate, with one side of the graphene attached to the substrate; then the support layer material on the graphene surface is removed, and after the transfer is completed, it is used for the preparation of medium and high voltage power cables.
[0057] Embodiment 3
[0058] S1, substrate metal processing stage: select a substrate metal copper foil of suitable size, clean it, dry it and set it aside;
[0059] The S1 stage substrate metal includes single metals and alloys, and the single metals include Fe, Ru, Co, Rh, Ir, Ni, Pd, Pt, Cu and Au, while the alloys include Co-Ni, Au-Ni, Ni-Mo and stainless steel.
[0060] The selection criteria for the substrate metal in the S1 stage include the melting point of the metal, the amount of carbon dissolved, and the stability of the metal carbide.
[0061] S2, pre-carbon metal decomposition stage: put the base metal nickel foil into a vacuum furnace, introduce auxiliary gas protection and heat to 900-1000℃, stabilize the temperature and maintain it, then stop introducing the protective gas and introduce the carbon source instead, and the reaction is completed;
[0062] The precursors in the S2 stage include a carbon source and an auxiliary gas, wherein the carbon source includes solids, liquids and gases, and the solids are carbon-containing polymer materials, the liquids are anhydrous ethanol, etc., and the gases include methane, acetylene and ethylene.
[0063] The auxiliary gases in the S2 stage include hydrogen, argon and nitrogen, and the heating temperature holding time in the S2 stage is 18-20 minutes. The carbon source introduction time in the S2 stage is 25-30 minutes. At the same time, the vacuum furnace in the S2 stage needs to be cleaned before processing, and the cleaning operation includes cleaning the gas path and removing impurities inside the vacuum furnace.
[0064] S3, graphene nucleation stage: After the methane molecules are dehydrogenated, the carbon species on the nickel surface aggregate with each other to generate new CC bonds and clusters, and begin to nucleate to form graphene islands. Carbon atoms nucleate at metal defect locations, i.e., metal steps.
[0065] S4, attachment and merging stage: As the number of graphene nuclei on the nickel surface increases, the carbon atoms or clusters generated thereafter continue to attach to the nucleation sites, causing the graphene nuclei to gradually grow until they are "stitched" or merged with each other, and then removed from the heating device for cooling and finally connected into a continuous graphene film;
[0066] The air pressure environment in stage S4 includes ultra-low pressure, low pressure and normal pressure, and the normal pressure environment is 105Pa, the low pressure environment is 10-3Pa~105Pa, and the ultra-low pressure environment is <10-3Pa.
[0067] The cooling temperature of the S4 stage is room temperature, and the S4 stage is assisted by cooling equipment for cooling.
[0068] The carrier gas types in the S4 stage are inert gas, nitrogen and the reducing gas hydrogen used in large quantities; and the inert gas includes helium and argon. At the same time, the growth pressure is set to 3atm, the flow rate of the carbon source gas is 10sccm, the flow rate of hydrogen is 500sccm, and the flow rate of argon is 1000sccm.
[0069] In the S4 stage, graphene is divided into high temperature, medium temperature and low temperature according to the growth temperature, and the high temperature is >800℃, the medium temperature is 600℃~800℃ and the low temperature is <600℃.
[0070] S5, film transfer stage: first, graphene is grown by the cVD method and the polymer is surface treated to improve the adsorption force between the graphene and the polymer; then, the graphene and TFPA-NH: are fully contacted, that is, the graphene / Cu and TFPA-NH are imprinted by a nanoimprinter at a specific temperature and pressure; finally, the graphene is separated from the metal substrate, that is, after the transfer is completed, it is used for the preparation of medium and high voltage power cables.
[0071] The principle of the S5 stage transfer medium is to first deposit a cross-linked molecule called N-ethylamino-4-diazo-tetrafluorobenzoate, i.e. TFPA-NH2, onto polystyrene that has been surface-treated with oxygen plasma. This cross-linked molecule can form a covalent bond with graphene. The adsorption force generated by the covalent bond between the polymer and graphene is much greater than the adsorption force between graphene and the metal substrate, thereby enabling the graphene to be separated from the metal substrate.
[0072] In summary, the graphene films obtained according to this process are Example 1 and Example 3 (the difference is that Example 1 uses copper as the substrate metal, and Example 3 uses nickel as the substrate metal). At the same time, Example 2 is a graphene film obtained by using a wet chemical etching substrate method instead of the dry transfer method in the S5 stage of the present invention. Example 4 is a graphene obtained by a graphene preparation method in Chinese patent CN108190864A. The comparison of the area continuity of the obtained finished products is shown in the attached figure. Figure 2 As shown, the comparison of the tensile strength of the finished product is shown in the attached Figure 3 As shown in the figure, the effect of the transfer method on the finished product obtained in Example 1, Example 2 and Example 3 is compared as shown in the attached figure. Figure 4 As shown, it can be seen from the above that the graphene produced by this process has a large area and is continuous, the transfer cost, i.e. the production cost, is low, and the tensile strength is good. It is used in medium and high voltage power cables to facilitate improving the tensile strength and performance of the cables.
[0073] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A graphene preparation process for medium and high voltage power cables, characterized in that , including the following steps: S1, substrate metal processing stage: select a substrate metal copper foil of suitable size, clean it, dry it and set it aside; S2, pre-carbon metal decomposition stage: put the base metal copper foil into a vacuum furnace, introduce auxiliary gas protection and heat to 900-1000℃, stabilize the temperature and maintain it, then stop introducing the protective gas and introduce the carbon source instead, and the reaction is completed; S3, graphene nucleation stage: After the methane molecules are dehydrogenated, the carbon species on the copper surface aggregate with each other to generate new CC bonds and clusters, and begin to nucleate to form graphene islands. Carbon atoms nucleate at metal defect locations, i.e., metal steps. S4, attachment and merging stage: As the number of graphene nuclei on the copper surface increases, the carbon atoms or clusters generated thereafter continue to attach to the nucleation sites, causing the graphene nuclei to gradually grow until they are "stitched" or merged with each other, and then removed from the heating device for cooling and finally connected into a continuous graphene film; S5, film transfer stage: first, graphene is grown by the cVD method and the polymer is surface treated to improve the adsorption force between the graphene and the polymer; then, the graphene and TFPA-NH: are fully contacted, that is, the graphene / Cu and TFPA-NH are imprinted by a nanoimprinter at a specific temperature and pressure; finally, the graphene is separated from the metal substrate, that is, after the transfer is completed, it is used for the preparation of medium and high voltage power cables.
2. The graphene preparation process for medium and high voltage power cables according to claim 1, characterized in that: The S1 stage substrate metal includes single metals and alloys, and the single metals include Fe, Ru, Co, Rh, Ir, Ni, Pd, Pt, Cu and Au, while the alloys include Co-Ni, Au-Ni, Ni-Mo and stainless steel.
3. The graphene preparation process for medium and high voltage power cables according to claim 1, characterized in that: The selection criteria for the substrate metal in the S1 stage include the melting point of the metal, the amount of carbon dissolved, and the stability of the metal carbide.
4. The graphene preparation process for medium and high voltage power cables according to claim 1, characterized in that: The S2 stage precursor includes a carbon source and an auxiliary gas, wherein the carbon source includes solid, liquid and gas, and the solid is a carbon-containing polymer material, the liquid is anhydrous ethanol, etc., and the gas includes methane, acetylene and ethylene.
5. The graphene preparation process for medium and high voltage power cables according to claim 1, characterized in that: The auxiliary gas in the S2 stage includes hydrogen, argon and nitrogen, and the heating temperature holding time in the S2 stage is 18-20 minutes. The carbon source introduction time in the S2 stage is 25-30 minutes. At the same time, the vacuum furnace in the S2 stage needs to be cleaned before processing, and the cleaning operation includes cleaning the gas path and removing impurities inside the vacuum furnace.
6. The graphene preparation process for medium and high voltage power cables according to claim 1, characterized in that: The air pressure environment in the S4 stage includes ultra-low pressure, low pressure and normal pressure, and the normal pressure environment is 105Pa, the low pressure environment is 10-3Pa~105Pa, and the ultra-low pressure environment is <10-3Pa.
7. The graphene preparation process for medium and high voltage power cables according to claim 1, characterized in that: The cooling temperature of the S4 stage is room temperature, and auxiliary cooling and temperature reduction are performed by cooling equipment in the S4 stage.
8. The graphene preparation process for medium and high voltage power cables according to claim 1, characterized in that: The carrier gas types in the S4 stage are inert gas, nitrogen and the reducing gas hydrogen used in large quantities; and the inert gas includes helium and argon. At the same time, the growth pressure is set to 3atm, the flow rate of the carbon source gas is 10sccm, the flow rate of hydrogen is 500sccm, and the flow rate of argon is 1000sccm.
9. The graphene preparation process for medium and high voltage power cables according to claim 1, characterized in that: The S4 stage graphene is divided into high temperature, medium temperature and low temperature according to different growth temperatures, and the high temperature is greater than 800°C, the medium temperature is 600°C to 800°C and the low temperature is less than 600°C.
10. The graphene preparation process for medium and high voltage power cables according to claim 1, characterized in that: The principle of the S5 stage transfer medium is to first deposit a cross-linked molecule called N-ethylamino-4-diazo-tetrafluorobenzoate, i.e., TFPA-NH2, onto polystyrene surface treated with oxygen plasma. The cross-linked molecule forms a covalent bond a with graphene. The adsorption force generated by the covalent bond between the polymer and graphene is greater than the adsorption force between the graphene and the metal substrate, so that the graphene is separated from the metal substrate.
Citation Information
Patent Citations
A kind of graphene preparation technology
CN104370286B
Graphene preparation method
CN108190864A
Transfer method of CVD method prepared graphene
CN106115672A
Preparation method of three-dimensional graphene film and three-dimensional graphene-copper composite cable
CN109264705A
And extruding graphene composite internal and external shielding medium-voltage aluminum alloy cable
CN209691472U