Grinding aid for ultrafine refining of high-grade limestone ore as well as preparation method and application of grinding aid

By using a grinding aid system composed of dispersants and other components in high-grade limestone ore ball mills, the problem of 'sticky ball' phenomenon and poor dispersion is solved, the dispersion and activation of limestone powder are improved, and its in-cement Application properties and mechanical properties in base materials.

CN118908261APending Publication Date: 2024-11-08TIANJIN BUILDING MATERIALS SCI RES INST +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410957642.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

High-grade limestone ore has a 'sticky ball' phenomenon during the ultra-refining process of ball milling, resulting in increased energy consumption of ball milling, reduced efficiency and uneven dispersion. The existing abrasive agents cannot effectively improve the dispersion and activation of limestone powder, and limit the Its application performance in cement-based materials.

Method used

A grinding aid system consisting of dispersants, isolators, chelators, shielding agents, cracking agents and activators is prepared by mechanical stirring and other methods. It is used for high-grade limestone ore ball milling to improve the dispersion and activation of limestone powder. , reduce the bonding amount and agglomeration phenomenon.

Benefits of technology

It effectively reduces the bonding and agglomeration of limestone powder, improves its specific surface area and surface activity, improves its application performance and mechanical properties in cement-based materials, and reduces ball grinding energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004949332530000081
    Figure BDA0004949332530000081
  • Figure BDA0004949332530000082
    Figure BDA0004949332530000082
  • Figure BDA0004949332530000091
    Figure BDA0004949332530000091
Patent Text Reader

Abstract

The invention provides a grinding aid for ultrafine refining of high-grade limestone ore as well as a preparation method and application of the grinding aid. The grinding aid for ultrafine refining of the high-grade limestone ore comprises the following components in percentage by mass: 5%-15% of a dispersing agent, 25%-30% of an isolating agent, 10%-15% of a chelating agent, 15%-20% of a shielding agent, 1%-8% of a cracking agent, 10%-20% of an activating agent and the balance of water, totaling 100%. The grinding aid for ultrafine refining of the high-grade limestone ore solves the problem of ball sticking generated when the specific surface area is larger than 1000 m < 2 > / kg in the ball-milling ultrafine process of the high-grade limestone ore, the dispersity of high-grade ultrafine limestone powder particles is enhanced, agglomeration of micro-nano particles is improved, meanwhile, the activation degree of the high-grade ultrafine limestone powder is improved, and the service life of the high-grade ultrafine limestone powder is prolonged. The high value-added utilization of the high-grade superfine limestone powder in the cement-based material is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of green and low-carbon materials, and in particular relates to a grinding aid for ultrafine processing of high-grade limestone ore, and a preparation method and application thereof. Background Art

[0002] It is a long-term and significant research to rationally allocate limestone resources, prevent the low use of high-quality mines to the greatest extent, develop high-value utilization of high-quality limestone resources, and accelerate the development of the limestone industry towards high quality. According to the gradient change of CaO content in limestone ore, limestone ore with CaO content greater than 54.0% is a high-grade limestone ore. After screening, crushing, ball milling and other treatments, such high-grade limestone ore can be used as an auxiliary cementitious material to replace a certain amount of cement, thereby improving the working performance, mechanical properties and durability of cement-based materials, and contributing to the quality improvement, cost reduction, energy conservation and carbon reduction of the building materials industry.

[0003] Compared with the vertical mill grinding method, the limestone powder obtained by ball milling high-grade limestone ore has better sphericity, which can improve the workability of mortar and concrete mixtures through the "ball effect".

[0004] When the specific surface area of ​​limestone powder is greater than 1000m 2 / kg, it has higher activity and can react with clinker mineral C3A to form semi-carbonate aluminate during cement hydration, thereby increasing the volume of hydration products. In addition, limestone powder that does not participate in the reaction will also fill the pores of hydration products, thereby improving the density of the cement matrix. The above effects can effectively improve the mechanical properties of cement-based materials.

[0005] Limestone powder can hinder the transmission of harmful external ions in cement-based materials through filling effect, and limestone powder reacts with C3A to reduce the content of calcium aluminate in the hydration product, which has a significant effect on improving the sulfate corrosion resistance of mortar and concrete and effectively improves durability.

[0006] However, in the process of ball milling high-grade limestone, when the specific surface area is greater than 800m 2 / kg, the limestone powder will have serious "sticky ball" phenomenon (such as Figure 1 As shown in the figure, the ball milling energy consumption increases, the ball milling efficiency decreases, and the limestone powder agglomerates and disperses unevenly, which greatly weakens the application performance of the limestone powder.

[0007] So far, the chemical additives used to improve the ball milling efficiency and dispersibility of ultrafine powder mainly include cement raw material grinding aids, cement clinker grinding aids, steel slag grinding aids, etc. However, the existing grinding aid system is not suitable for ball milling of high-grade limestone, often cannot play a good dispersing role in the ultrafineness of limestone powder, and basically has no activation effect on ultrafine limestone powder, which results in poor application performance of limestone powder in cement-based materials.

[0008] CN201410658083.3 provides a large-volume limestone grinding aid, which relates to the technical field of cement admixtures, and includes the following components by weight percentage: 18-25% alkanolamine compound, 1-5% water-retaining cellulose, 5-10% ethyl maltol, 5-10% sodium fatty acid, 10-15% polystyrene, 2-7% sodium pyrophosphate, 0.5-2% polytetrafluoroethylene, 0.1-0.7% sodium gluconate, 3-7% sugars, 1-5% xanthan gum, and water balance. It is mainly added during cement grinding in order to significantly increase the amount of limestone powder added to cement. It does not improve the performance of the limestone itself, and does not significantly improve the performance and application effect of limestone powder as a single component.

[0009] CN202311457300.8 discloses a modified limestone powder and its preparation method and application, belonging to the field of building materials technology. The preparation method includes mixing and grinding limestone raw materials and grinding aids; the grinding aids include sodium pyrophosphate, sodium gluconate, sodium citrate, alcoholamine compounds and water. The preparation method can effectively reduce the particle size of the modified limestone powder obtained, improve its sphericity, and at the same time reduce the content of free calcium ions therein. However, the specific surface area of ​​the limestone powder prepared by this method is only greater than 300m 2 / kg, which does not reach the category of ultrafine powder, does not involve the solution to the "ball sticking" problem in the process of limestone ultrafine ball milling, and has limited effect on the activation of limestone powder.

[0010] CN202410094166.8 discloses a limestone powder modified grinding aid, a preparation method and an application thereof, wherein the limestone powder modified grinding aid comprises, by weight: 1 to 15 parts of polyol, 0.1 to 5 parts of emulsifier, 1 to 15 parts of silicate, 3 to 20 parts of organic salt, 0.1 to 6 parts of sodium alcohol and 1 to 30 parts of alcoholamine compound. The limestone powder modified grinding aid can not only greatly improve the grinding effect of limestone powder, but also improve the hydration activity of limestone powder. However, the target of the modified grinding aid is ordinary limestone ore, and the fineness of limestone powder does not reach the level of ultrafine powder, and its effect on high-grade ultrafine limestone powder is limited. Summary of the invention

[0011] In view of this, in order to solve the above technical problems, the present invention proposes a grinding aid for ultrafine processing of high-grade limestone ore and its preparation method and application. By adding the grinding aid in the ball milling process, the problem of high-grade limestone ore with a specific surface area greater than 1000m 2 / kg, enhance the dispersibility of high-grade ultrafine limestone powder particles, improve the agglomeration of micro-nano-sized particles, and at the same time improve the activation degree of high-grade ultrafine limestone powder, ultimately achieving high added value utilization of high-grade ultrafine limestone powder in cement-based materials.

[0012] To achieve the above object, the technical solution of the present invention is achieved as follows:

[0013] On the one hand, the present invention provides a grinding aid for ultrafine processing of high-grade limestone ore, comprising the following components in percentage by mass: 5% to 15% of dispersant, 25% to 30% of isolating agent, 10% to 15% of chelating agent, 15% to 20% of shielding agent, 1% to 8% of cracking agent, 10% to 20% of activating agent, and the balance being water, totaling 100%.

[0014] In some preferred embodiments of the grinding aid for ultrafine processing of high-grade limestone ore of the present invention, the following components are included in percentage by mass: 10% dispersant, 29% isolating agent, 12.5% ​​chelating agent, 17.5% shielding agent, 6% cracking agent, 16% activator, and the balance is water, totaling 100%.

[0015] In some preferred embodiments of the grinding aid for ultrafine processing of high-grade limestone ore of the present invention, the dispersant is a mixture of comb-like polycarboxylic acid polymers HPEG-Co-AA, TPEG-Co-AA and EPEG-Co-AA.

[0016] HPEG-Co-AA is obtained by copolymerization of methyl allyl polyoxyethylene ether (HPEG, molecular weight 2400) and acrylic acid (AA);

[0017] TPEG-Co-AA is obtained by copolymerization of isopentenyl polyoxyethylene ether (TPEG, molecular weight 2400) and acrylic acid (AA);

[0018] EPEG-Co-AA is obtained by copolymerization of ethylene glycol polyoxyethylene ether (EPEG, molecular weight 3000) and acrylic acid (AA).

[0019] In some more preferred embodiments of the grinding aid for ultrafine processing of high-grade limestone ore of the present invention, the mass ratio of the comb-like polycarboxylic acid polymers HPEG-Co-AA, TPEG-Co-AA, and EPEG-Co-AA is (1-3): (2-4): (3-6).

[0020] In some preferred embodiments of the grinding aid for ultrafine grinding of high-grade limestone ore of the present invention, the isolation agent is a mixture of polyvinyl pyrrolidone (K13-18) with an average molecular weight of 10,000, polyvinyl pyrrolidone (K29-32) with an average molecular weight of 58,000, and polyvinyl pyrrolidone (K88-96) with an average molecular weight of 130,000.

[0021] In some more preferred embodiments of the grinding aid for ultrafine processing of high-grade limestone ore of the present invention, the mass ratio of polyvinyl pyrrolidone with an average molecular weight of 10,000, polyvinyl pyrrolidone with an average molecular weight of 58,000, and polyvinyl pyrrolidone with an average molecular weight of 130,000 is (10-15):(3-9):(1-5).

[0022] In some preferred embodiments of the grinding aid for ultrafine processing of high-grade limestone ore of the present invention, the chelating agent is a mixture of ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate and tetrasodium BAPTA.

[0023] In some more preferred embodiments of the grinding aid for ultrafine processing of high-grade limestone ore of the present invention, the mass ratio of ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate, and tetrasodium BAPTA is (1.5-3.5):(0.5-1.0):(0.5-1.0).

[0024] In some preferred embodiments of the grinding aid for ultrafine processing of high-grade limestone ore of the present invention, the shielding agent is a mixture of glycerol, molasses and sodium gluconate.

[0025] In some more preferred embodiments of the grinding aid for ultrafine processing of high-grade limestone ore of the present invention, the mass ratio of glycerol, molasses and sodium gluconate is (4.9-5.5): (3.0-3.5): (0.8-1.2).

[0026] In some preferred embodiments of the grinding aid for ultrafine processing of high-grade limestone ore of the present invention, the cracking agent is a mixture of formamide, sodium molybdate and sodium tripolyphosphate. Ball milling is a representative mechanochemical method that makes materials have certain defects through mechanical stirring. Formamide, sodium molybdate and sodium tripolyphosphate can reduce the free energy of particles during the ball milling of limestone, and have the effect of adsorbing on the calcareous material to promote the generation of cracks and prevent crack compounding.

[0027] In some more preferred embodiments of the grinding aid for ultrafine processing of high-grade limestone ore of the present invention, the mass ratio of formamide, sodium molybdate and sodium tripolyphosphate is (0.1-0.5):(0.5-1.0):(1.0-2.0).

[0028] In some preferred embodiments of the grinding aid for ultrafine processing of high-grade limestone ore of the present invention, the activator is an ester of alkanolamine and an organic acid.

[0029] In some more preferred embodiments of the grinding aid for ultrafine processing of high-grade limestone ore of the present invention, the activator is an ester of triethanolamine and glacial acetic acid (TG-E), an ester of diethanolamine and fumaric acid (DF-E), or a mixture of an ester of diethanol monoisopropanolamine and maleic anhydride (DM-E).

[0030] In some more preferred embodiments of the grinding aid for ultrafine processing of high-grade limestone ore of the present invention, the mass ratio of the ester of triethanolamine and glacial acetic acid, the ester of diethanolamine and fumaric acid, and the ester of diethanol monoisopropanolamine and maleic anhydride is (0.1-0.5):(8.0-9.0):(0.5-1.5).

[0031] The second aspect of the present invention provides a method for preparing a grinding aid for ultrafine processing of high-grade limestone ore, comprising the following steps:

[0032] S1. Prepare a dispersant: stir and mix HPEG-Co-AA, TPEG-Co-AA, and EPEG-Co-AA weighed in a mass ratio of (1-3): (2-4): (3-6) to obtain the dispersant;

[0033] Preparation of a release agent: adding polyvinyl pyrrolidone with an average molecular weight of 10,000, polyvinyl pyrrolidone with an average molecular weight of 58,000, and polyvinyl pyrrolidone with an average molecular weight of 130,000 weighed in a mass ratio of (10-15):(3-9):(1-5) to water in sequence, stirring and dissolving to obtain the release agent;

[0034] Preparation of a chelating agent: adding ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate, and tetrasodium BAPTA weighed in a mass ratio of (1.5-3.5): (0.5-1.0): (0.5-1.0) into water in sequence and dissolving them to obtain the chelating agent;

[0035] Preparation of shielding agent: weighing glycerol, molasses and sodium gluconate in a mass ratio of (4.9-5.5): (3.0-3.5): (0.8-1.2), mixing glycerol and molasses evenly, adding sodium gluconate and dissolving to obtain the shielding agent;

[0036] Preparation of a cracking agent: adding formamide, sodium molybdate and sodium tripolyphosphate weighed in a mass ratio of (0.1-0.5):(0.5-1.0):(1.0-2.0) into water in sequence and dissolving them to obtain the cracking agent;

[0037] Preparation of an activator: uniformly mixing an ester of triethanolamine and glacial acetic acid, an ester of diethanolamine and fumaric acid, and an ester of diethanol monoisopropanolamine and maleic anhydride weighed in a mass ratio of (0.1-0.5):(8.0-9.0):(0.5-1.5) to obtain the activator;

[0038] S2. Weigh each component in proportion, add the weighed dispersant, isolating agent, chelating agent, shielding agent, cracking agent and activator to the weighed water in sequence, stir and mix evenly to obtain the grinding aid.

[0039] The third aspect of the present invention provides the use of a grinding aid for ultrafine processing of high-grade limestone ore, which is used as a grinding aid in preparing high-grade ultrafine limestone powder by ball milling of high-grade limestone ore.

[0040] In some preferred embodiments of the use of the grinding aid for ultrafine processing of high-grade limestone ore of the present invention, during ball milling, the amount of the grinding aid is 0.05% to 0.1% of the mass of the limestone ore.

[0041] Compared with the prior art, the grinding aid for ultrafine processing of high-grade limestone ore and its preparation method and application described in the present invention have the following advantages:

[0042] (1) The grinding aid for ultrafine processing of high-grade limestone ore described in the present invention can effectively reduce the amount of limestone powder adhering to steel balls and slow down the agglomeration of limestone powder during the ultrafine processing of high-grade limestone ore by ball milling, thereby playing a good role in reducing ball milling energy consumption and improving the dispersibility of limestone powder.

[0043] (2) The grinding aid for ultrafine processing of high-grade limestone ore described in the present invention can greatly increase the specific surface area and surface activity of limestone powder when used in the process of ultrafine processing of high-grade limestone ore by ball milling; at the same time, the high-grade limestone powder containing the grinding aid exhibits good adaptability and enhancement effect when used in cement-based materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 When the specific surface area is greater than 800m 2 / kg, limestone powder will have serious "sticky ball" phenomenon diagram;

[0045] Figure 2 This is a characteristic diagram of particle size distribution of high-grade limestone powder added with the grinding aid for ultrafine processing of high-grade limestone prepared in Examples 1 to 5 of the present invention and a blank group. DETAILED DESCRIPTION

[0046] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.

[0047] The present invention will be described in detail below with reference to the embodiments and the accompanying drawings.

[0048] Embodiments 1 to 5

[0049] Preparation of grinding aids for ultrafine processing of high-grade limestone ore

[0050] Step 1, weigh the following components according to the mass percentages shown in Table 1: dispersant, isolating agent, chelating agent, shielding agent, cracking agent, activator, and water;

[0051] Step 2: add dispersant, isolating agent, chelating agent, shielding agent, cracking agent and activating agent to the weighed water in sequence, stir for 1.5 hours until the mixture is uniformly mixed, and obtain a grinding aid for ultrafine processing of high-grade limestone ore.

[0052] Table 1. Ratio of raw material components of grinding aids prepared in Examples 1 to 5

[0053]

[0054] in:

[0055] 1) Preparation of dispersant: HPEG-Co-AA, TPEG-Co-AA and EPEG-Co-AA were weighed and mixed in a mass ratio of 1.8:3.5:4.7, and stirred for 30 min at room temperature to obtain a dispersant.

[0056] HPEG-Co-AA is synthesized by free radical copolymerization of HPEG and AA. The process of preparing 1000 g of HPEG-Co-AA is shown in Table 2:

[0057] Table 2. Preparation of HPEG-Co-AA

[0058]

[0059] Weigh the components required for the base material according to the proportions shown in Table 2, and mix and stir evenly;

[0060] Weigh the components required for material A according to the proportions shown in Table 2, and mix and stir evenly;

[0061] Weigh the components required for material B according to the proportions shown in Table 2, and mix and stir evenly;

[0062] Add material A and material B to the bottom material by double dropping method for reaction;

[0063] After the addition is completed, water is added and the temperature is kept to obtain HPEG-Co-AA.

[0064] TPEG-Co-AA is synthesized by free radical copolymerization of TPEG and AA. The process of preparing 1000 g of TPEG-Co-AA is shown in Table 3:

[0065] Table 3. Preparation of TPEG-Co-AA

[0066]

[0067] Weigh the components required for the base material according to the proportions shown in Table 3, and mix and stir evenly;

[0068] Weigh the components required for material A according to the proportions shown in Table 3, and mix and stir evenly;

[0069] Weigh the components required for material B according to the proportions shown in Table 3, and mix and stir evenly;

[0070] Add material A and material B to the bottom material by double dropping method for reaction;

[0071] After the addition is completed, water is added and the temperature is kept to obtain TPEG-Co-AA.

[0072] EPEG-Co-AA is synthesized by free radical copolymerization of EPEG and AA. The process of preparing 1000 g of EPEG-Co-AA is shown in Table 4:

[0073] Table 4. EPEG-Co-AA preparation

[0074]

[0075]

[0076] Weigh the components required for the base material according to the proportions shown in Table 4, and mix and stir evenly;

[0077] Weigh the components required for material A according to the proportions shown in Table 4, and mix and stir evenly;

[0078] Weigh the components required for material B according to the proportions shown in Table 4, and mix and stir evenly;

[0079] Add material A and material B to the bottom material by double dropping method for reaction;

[0080] After the addition is completed, water is added and the temperature is kept to obtain EPEG-Co-AA.

[0081] 2) Preparation of release agent: Weigh polyvinyl pyrrolidone with an average molecular weight of 10,000, polyvinyl pyrrolidone with an average molecular weight of 58,000, polyvinyl pyrrolidone with an average molecular weight of 130,000 and water in a mass ratio of 15:8:5:72, add polyvinyl pyrrolidone with an average molecular weight of 10,000 to water and stir for 10 minutes, then add polyvinyl pyrrolidone with an average molecular weight of 58,000 and continue stirring for 20 minutes, finally add polyvinyl pyrrolidone with an average molecular weight of 130,000 and stir for 40 minutes to fully dissolve to obtain the release agent.

[0082] 3) Preparation of chelating agent: Ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate, tetrasodium BAPTA and water were weighed in a mass ratio of 6:3:3:88, ethylenediaminetetraacetic acid was added to water and stirred for 20 min, then disodium ethylenediaminetetraacetate was added and stirring was continued for 40 min, and finally tetrasodium BAPTA was added and stirred for 70 min to fully dissolve to obtain the chelating agent.

[0083] 4) Preparation of shielding agent: Glycerol, molasses and sodium gluconate were weighed in a mass ratio of 11:7:2, the glycerol and molasses were mixed and stirred for 20 minutes, and then sodium gluconate was added and stirred for 60 minutes to fully dissolve to obtain the shielding agent.

[0084] 5) Preparation of a cracking agent: Weigh formamide, sodium molybdate, sodium tripolyphosphate and water in a mass ratio of 0.3:1:1:5, add sodium molybdate to water and stir for 10 minutes, then add sodium tripolyphosphate and continue stirring for 20 minutes, finally add formamide and stir for 30 minutes to fully dissolve to obtain a cracking agent.

[0085] 6) Preparation of an activator: The ester of triethanolamine and glacial acetic acid, the ester of diethanolamine and fumaric acid, and the ester of diethanol monoisopropanolamine and maleic anhydride were weighed in a mass ratio of 2:88:10, mixed, and stirred for 30 minutes to obtain an activator.

[0086] The preparation process of the ester of triethanolamine and glacial acetic acid is as follows: by mass percentage, 74.6% of triethanolamine and 25.2% of glacial acetic acid are weighed and added into a four-necked flask, stirred and mixed, 0.2% concentrated sulfuric acid is added dropwise, and the mixture is placed in a heat-collecting constant temperature heating magnetic stirrer and heated to 120° C. and stirred for 4.0 hours, and then cooled to room temperature to obtain TG-E.

[0087] The preparation process of the ester of diethanolamine and fumaric acid is as follows: 16.4% of fumaric acid is weighed into a four-necked flask by mass percentage, 65.8% of water is added, and the mixture is heated to 100°C and stirred for half an hour in a heat-collecting constant temperature heating magnetic stirrer. It is found that part of the fumaric acid is suspended in the water. After 17.8% of diethanolamine is added to the four-necked flask, the suspended particles gradually dissolve, and the mixture is heated to 120°C, stirred for 4.0 hours, and cooled to room temperature to obtain DF-E.

[0088] The preparation process of the ester of diethanol monoisopropanolamine and maleic anhydride is as follows: 20.6% of maleic anhydride is weighed and added into a four-necked flask, 31.1% of water is added, and the mixture is heated to 100°C and stirred for half an hour in a heat-collecting constant temperature heating magnetic stirrer until all the maleic anhydride is dissolved. Then 48.3% of diethanol monoisopropanolamine is added into the four-necked flask, and the mixture is heated to 120°C, stirred for 4.0 hours, and cooled to room temperature to obtain DM-E.

[0089] Performance Test:

[0090] Dosage: The grinding aids for ultrafine processing of high-grade limestone prepared in Examples 1 to 5 were uniformly sprayed on the surface of the high-grade limestone ore at a dosage of 0.05% ωt to carry out ball milling test.

[0091] Test items: Under the same ball milling time, the ball sticking rate, specific surface area, particle size distribution and the reinforcing effect on cement mortar of high-grade limestone powder are tested. The test method is as follows:

[0092] (1) Ball sticking rate: After the high-grade limestone ore is ball-milled for a specified time, the average mass of Φ70 steel balls (9 pieces) with limestone powder is weighed as A / g, the average mass of Φ60 steel balls (22 pieces) is weighed as B / g, the average mass of Φ50 steel balls (33 pieces) is weighed as C / g, the average mass of Φ40 steel balls (40 pieces) is weighed as D / g, and the average mass of steel forgings (234 pieces) is weighed as E / g. The ball sticking rate X is calculated as follows:

[0093]

[0094] (2) Specific surface area and particle size distribution: The specific surface area and particle size distribution of high-grade limestone powder were tested using a laser particle size analyzer.

[0095] (3) Strengthening effect on cement mortar: The proportion of cement mortar is 450g of cement, 225g of water, and 1350g of sand. The replacement amount of high-grade limestone powder for cement is 15%.

[0096] Test results: The calculation results of the ball adhesion rate of the high-grade limestone powder obtained by ball milling for 20 minutes for the blank group and the high-grade limestone powder prepared by the high-grade limestone ore ultrafine grinding aids prepared by Examples 1 to 5 with 0.05% ωt and the specific surface area of ​​the high-grade limestone powder are shown in Table 5. The particle size distribution is shown in Table 5. Figure 2 The reinforcement results of cement mortar are shown in Table 6.

[0097] Table 5. Ball sticking rate and specific surface area of ​​high-grade limestone powder

[0098]

[0099] It can be seen from the calculation results of the ball adhesion rate of the high-grade limestone powder in Table 5 that, compared with the blank group, the limestone ore added with 0.05% ωt of the high-grade limestone ore ultrafine grinding aid prepared in Examples 1 to 5 has a significantly reduced ball adhesion rate under the same ball milling time. In addition, the ball encapsulation rate of the high-grade limestone powder added in Example 1 is reduced more significantly, which is of great significance for reducing the energy consumption of ball milling.

[0100] Combined with the specific surface area test results of high-grade limestone powder in Table 5 and Figure 2 From the particle size distribution in the figure, it can be seen that the high-grade limestone powder added with the grinding aid for ultrafine processing of high-grade limestone prepared in Examples 1 to 5 has a larger specific surface area, and the content of small-size particles is relatively high. By comparison, it is found that the above-mentioned performance of the high-grade limestone powder added with Example 1 is more prominent, which has a significant improvement effect on solving the agglomeration phenomenon in the ultrafine processing of high-grade limestone powder, and improves the application performance of high-grade ultrafine limestone powder.

[0101] Table 6. Mechanical strength of cement mortar with 15% high-grade limestone (MPa)

[0102]

[0103] It can be seen from the mortar strength test results in Table 6 that the mortar specimens prepared by replacing 15% of cement with high-grade ultrafine limestone powder mixed with grinding aids for ultrafine high-grade limestone prepared in Examples 1 to 5 have higher flexural and compressive strengths at all ages. Among them, the mortar formed by replacing part of the cement with ultrafine high-grade limestone powder of Example 1 has better mechanical properties, which is mainly because part of the high-grade ultrafine limestone powder reacts with C3A in cement under the action of the grinding aid to form carbon aluminate or semi-carbon aluminate, which has a certain supplement and filling effect on the pores and defects in the cement hydration product, making the structure of the cement hydration product more compact, thereby achieving the effect of increasing the mechanical strength.

[0104] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A grinding aid for ultrafine processing of high-grade limestone ore, characterized in that: The composition comprises the following components by mass percentage: 5% to 15% of dispersant, 25% to 30% of isolating agent, 10% to 15% of chelating agent, 15% to 20% of shielding agent, 1% to 8% of cracking agent, 10% to 20% of activating agent, and the balance is water, which is 100% in total; Preferably, the following components are included by mass percentage: 10% dispersant, 29% isolating agent, 12.5% ​​chelating agent, 17.5% shielding agent, 6% cracking agent, 16% activator, and the balance is water, which is 100% in total.

2. The grinding aid for ultrafine processing of high-grade limestone ore according to claim 1, characterized in that: The dispersant is a mixture of comb-shaped polycarboxylic acid polymers HPEG-Co-AA, TPEG-Co-AA and EPEG-Co-AA; Preferably, the mass ratio of the comb-shaped polycarboxylic acid polymers HPEG-Co-AA, TPEG-Co-AA, and EPEG-Co-AA is (1-3): (2-4): (3-6).

3. The grinding aid for ultrafine processing of high-grade limestone ore according to claim 1, characterized in that: The release agent is a mixture of polyvinyl pyrrolidone with an average molecular weight of 10,000, polyvinyl pyrrolidone with an average molecular weight of 58,000 and polyvinyl pyrrolidone with an average molecular weight of 130,000; Preferably, the mass ratio of polyvinyl pyrrolidone with an average molecular weight of 10,000, polyvinyl pyrrolidone with an average molecular weight of 58,000, and polyvinyl pyrrolidone with an average molecular weight of 130,000 is (10-15):(3-9):(1-5).

4. The grinding aid for ultrafine processing of high-grade limestone ore according to claim 1, characterized in that: The chelating agent is a mixture of ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate and tetrasodium BAPTA; Preferably, the mass ratio of ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate, and tetrasodium BAPTA is (1.5-3.5):(0.5-1.0):(0.5-1.0).

5. The grinding aid for ultrafine processing of high-grade limestone ore according to claim 1, characterized in that: The shielding agent is a mixture of glycerol, molasses and sodium gluconate; Preferably, the mass ratio of glycerol, molasses and sodium gluconate is (4.9-5.5):(3.0-3.5):(0.8-1.2).

6. The grinding aid for ultrafine processing of high-grade limestone ore according to claim 1, characterized in that: The cracking agent is a mixture of formamide, sodium molybdate and sodium tripolyphosphate; Preferably, the mass ratio of formamide, sodium molybdate and sodium tripolyphosphate is (0.1-0.5):(0.5-1.0):(1.0-2.0).

7. The grinding aid for ultrafine processing of high-grade limestone ore according to claim 1, characterized in that: The activator is an ester of alkanolamine and organic acid; Preferably, the activator is a mixture of an ester of triethanolamine and glacial acetic acid, an ester of diethanolamine and fumaric acid, and an ester of diethanol monoisopropanolamine and maleic anhydride; Preferably, the mass ratio of the ester of triethanolamine and glacial acetic acid, the ester of diethanolamine and fumaric acid, and the ester of diethanol monoisopropanolamine and maleic anhydride is (0.1-0.5):(8.0-9.0):(0.5-1.5).

8. The method for preparing the grinding aid for ultrafine processing of high-grade limestone ore according to any one of claims 1 to 7, characterized in that: The steps include: S1. Prepare a dispersant: stir and mix HPEG-Co-AA, TPEG-Co-AA, and EPEG-Co-AA weighed in a mass ratio of (1-3): (2-4): (3-6) to obtain the dispersant; Preparation of a release agent: adding polyvinyl pyrrolidone with an average molecular weight of 10,000, polyvinyl pyrrolidone with an average molecular weight of 58,000, and polyvinyl pyrrolidone with an average molecular weight of 130,000 weighed in a mass ratio of (10-15):(3-9):(1-5) to water in sequence, stirring and dissolving to obtain the release agent; Preparation of a chelating agent: adding ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate, and tetrasodium BAPTA weighed in a mass ratio of (1.5-3.5): (0.5-1.0): (0.5-1.0) into water in sequence and dissolving them to obtain the chelating agent; Preparation of shielding agent: weighing glycerol, molasses and sodium gluconate in a mass ratio of (4.9-5.5): (3.0-3.5): (0.8-1.2), mixing glycerol and molasses evenly, adding sodium gluconate and dissolving to obtain the shielding agent; Preparation of a cracking agent: adding formamide, sodium molybdate and sodium tripolyphosphate weighed in a mass ratio of (0.1-0.5):(0.5-1.0):(1.0-2.0) into water in sequence and dissolving them to obtain the cracking agent; Preparation of an activator: uniformly mixing an ester of triethanolamine and glacial acetic acid, an ester of diethanolamine and fumaric acid, and an ester of diethanol monoisopropanolamine and maleic anhydride weighed in a mass ratio of (0.1-0.5):(8.0-9.0):(0.5-1.5) to obtain the activator; S2. Weigh each component in proportion, add the weighed dispersant, isolating agent, chelating agent, shielding agent, cracking agent, and activating agent to the weighed water in sequence, stir and mix evenly, and obtain the grinding aid.

9. The use of the grinding aid for ultrafine processing of high-grade limestone ore according to any one of claims 1 to 7, characterized in that: It is used as a grinding aid in the preparation of high-grade ultrafine limestone powder by ball milling of high-grade limestone ore.

10. The use of the grinding aid for ultrafine processing of high-grade limestone ore according to claim 9, characterized in that: During ball milling, the amount of the grinding aid is 0.05% to 0.1% of the mass of the limestone ore.