Method for preparing transition metal hydroxide nano thin layer in aqueous solution
By using electrochemical methods in aqueous solution to peel off layered transition metal hydroxides under normal temperature and pressure, the cumbersome problems of organic solvent use and operation steps in traditional methods are solved, and environmentally friendly and convenient nano-level two-dimensional transition metal hydrogen is achieved. Oxide preparation, suitable for a variety of types of transition metal hydroxides.
Patent Information
- Application Number
- CN202410962103.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
Smart Images

Figure CN118908295A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nano material preparation, in particular to a method for preparing a transition metal hydroxide nano thin layer in an aqueous solution with neutral pH. Background Art
[0002] Nanoscale two-dimensional materials are widely used in energy storage, catalysis and other fields. Among them, layered transition metal hydroxides (TMH) with a few nanometer thickness occupy an important position in two-dimensional materials due to their unique electronic properties and crystal structure.
[0003] The crystal structure of traditional TMH is a layered stacking structure similar to brucite or hydrotalcite, such as Figure 6 As shown. The layered structure is composed of alternating main layers and gaps. The main layer is composed of [M(OH)6] octahedra that share edges, where M represents the metal atom at the center of the octahedron, and the hydroxyl groups are the six vertices of the octahedron. Adjacent main layers interact with each other through van der Waals forces and are stacked on each other. The interlayer gaps can exist naturally, or different types of neutral molecules or negatively charged ions can be inserted through a regulatory method called "ion intercalation." Different types of intercalated molecules and ions will result in different main layer spacings. Therefore, the TMH main layer can be peeled off by expanding the interlayer spacing and weakening the interaction between the main layers to obtain nanoscale two-dimensional TMH. This strategy of first obtaining stacked TMH and then obtaining nanoscale two-dimensional thin layer TMH by peeling is also called a "top-down" strategy.
[0004] At present, the "top-down" strategy mainly uses the method of "ion intercalation" + "ion exchange" to expand the interlayer spacing to achieve the purpose of stripping the main layer. For example, in 2022, Chen et al. used an organic solvent chloroform (CHCl3) to dissolve elemental iodine and in situ oxidized the intercalated Co in the brucite structure. 2 / 3 Fe 1 / 3 (OH)2 forms a hydrotalcite-like structure Co with iodine anion intercalation 2 / 3 Fe 1 / 3 The LDH phase can be further subjected to interlayer anion exchange of sodium perchlorate (NaClO4) and ultrasonic oscillation to obtain nano-scale hydroxide flakes [Chem Catalysis, 2022, 2(4): 867-882.].
[0005] However, this strategy often requires the use of strong redox agents or organic solvents, which is not conducive to environmental protection. In addition, it is divided into two steps: "intercalation" and "exchange", which are cumbersome and increase production costs.
[0006] Considering that TMH itself has the characteristics of "ion intercalation", the present invention uses a saline solution with mild chemical composition and neutral pH as the only electrolyte, and adopts a "one-step" electrochemical stripping method to directly obtain nanoscale two-dimensional TMH. Compared with the "multi-step" process using organic solvents, this method is convenient to operate and environmentally friendly. At the same time, this method is applicable to various types of TMH and has a wide range of applications. Summary of the invention
[0007] The purpose of the present invention is to provide a method for preparing a nano-thin layer of transition metal hydroxide in an aqueous solution, which only uses a salt solution of water and does not involve an organic solvent. By an electrochemical method, the layered transition metal hydroxide is directly "one-step" peeled off in a normal temperature and pressure environment, thereby overcoming the problems that the traditional method requires an organic solvent, has cumbersome operating steps, and requires heating.
[0008] To achieve the above object, the present invention provides a method for preparing a transition metal hydroxide nano-thin layer in an aqueous solution, comprising the following steps:
[0009] A. preparing a layered transition metal hydroxide to be stripped and making it into an electrode;
[0010] B. Prepare a salt solution containing chloride ions of a certain concentration;
[0011] C. The layered transition metal hydroxide electrode to be stripped is used as the working electrode, and the prepared saline solution is used as the electrolyte to construct a classic "three-electrode" electrochemical system. The electrode potential or current is controlled by electrochemical methods in the saline solution, so that the solute ions are repeatedly embedded and de-embedded in the interlayer gaps of the layered transition metal hydroxide body to expand the interlayer spacing and strip the layered transition metal hydroxide;
[0012] D. The layered transition metal hydroxide after electrochemical stripping in step C is dispersed in the "stripping electrolyte", and the electrolyte is allowed to stand to obtain nano-scale thin layered transition metal hydroxide in the supernatant. The electrolyte is further ultrasonically treated as needed to increase the yield of nano-scale thin layered transition metal hydroxide.
[0013] Preferably, in step A, the method for preparing the layered transition metal hydroxide to be stripped is one of electrodeposition, co-deposition and hydrothermal method.
[0014] Preferably, in step B, the solute in the saline solution is a chloride salt, preferably NaCl or KCl, the solvent is water, and the pH of the solution is neutral.
[0015] Preferably, in step C, the electrochemical method is a controlled potential method or a controlled current method, preferably a cyclic voltammetry method or a chronopotentiometry method.
[0016] The advantages and positive effects of the method for preparing a transition metal hydroxide nano-thin layer in an aqueous solution of the present invention are:
[0017] 1. The present invention only uses aqueous solution and common chloride salts, does not require organic solvents, the production process is environmentally friendly, and the generated waste liquid is convenient for wastewater treatment.
[0018] 2. The peeling process of the present invention does not involve operations such as heating, and the preparation process is safe and has relatively low energy consumption.
[0019] 3. The stripping method of the present invention is effective for most layered transition metal hydroxides, has no special requirements for the chloride salt used, and has a wide range of applicability.
[0020] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 A flow chart of a method for preparing a transition metal hydroxide nano-thin layer in an aqueous solution according to the present invention;
[0022] Figure 2 Schematic diagram of a nano-thin layer of TMH prepared in an embodiment of the present invention suspended in a salt aqueous solution, wherein A is the nano-thin layer of TMH prepared in Example 1, and B is the nano-thin layer of TMH prepared in Example 3;
[0023] Figure 3 The performance test diagram of the nano-thin layer TMH prepared in Example 1 of the present invention, wherein (a) is the AFM scanning diagram of the nano-thin layer TMH and the selected direction of height measurement (red dotted line); (b) is the height value in the selected direction;
[0024] Figure 4 The performance test diagram of the nano-thin layer TMH prepared in Example 2 of the present invention, wherein (a) is the AFM scanning diagram of the nano-thin layer TMH and the selected direction of height measurement (red dotted line); (b) is the height value in the selected direction;
[0025] Figure 5 The performance test diagram of the nano-thin layer TMH prepared in Example 3 of the present invention, wherein (a) is the AFM scanning diagram of the nano-thin layer TMH and the height measurement selected direction (red dotted line); (b) is the height value in the selected direction;
[0026] Figure 6 Schematic diagram of the layered stacking crystal structure of traditional TMH. DETAILED DESCRIPTION
[0027] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.
[0028] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one having ordinary skills in the field to which the present invention belongs.
[0029] A method for preparing a transition metal hydroxide nano-thin layer in an aqueous solution comprises the following steps:
[0030] A. Prepare a layered transition metal hydroxide to be stripped and make it into an electrode; the method for preparing the layered transition metal hydroxide to be stripped is one of electrodeposition, co-deposition and hydrothermal method.
[0031] B. Prepare a salt water solution containing chloride ions of a certain concentration; the solute in the salt water solution is chloride salt, the solvent is water, and the pH of the solution is neutral.
[0032] C. The layered transition metal hydroxide electrode to be stripped is used as the working electrode and the prepared saline solution is used as the electrolyte to construct a classic "three-electrode" electrochemical system. The electrode potential or current is controlled by an electrochemical method in the saline solution so that the solute ions are repeatedly deintercalated in the interlayer gaps of the layered transition metal hydroxide body to expand the interlayer spacing and strip the layered transition metal hydroxide. The electrochemical method can be a controlled potential method, such as cyclic voltammetry, or a controlled current method, such as chronopotentiometry.
[0033] D. The layered transition metal hydroxide after electrochemical stripping in step C is dispersed in the "stripping electrolyte", and the electrolyte is allowed to stand to obtain nano-scale thin layered transition metal hydroxide in the supernatant. The electrolyte is further ultrasonically treated as needed to increase the yield of nano-scale thin layered transition metal hydroxide.
[0034] Example 1
[0035] (1) TMH electrode preparation: The three-electrode method was used, with conductive carbon fiber paper as the working electrode, metal platinum mesh as the counter electrode, and silver\silver chloride (Ag\AgCl) electrode as the reference electrode. -1 In a (mM) Co(NO3)2 aqueous solution, an intensity of 1 mA cm was applied to the working electrode. -2 The Co(OH)2 electrode can be obtained by reducing the current for 3600 seconds.
[0036] (2) TMH stripping preparation: Using the three-electrode method, Co(OH)2 electrode was used as the working electrode, metal platinum mesh was used as the counter electrode, and silver\silver chloride (Ag\AgCl) electrode was used as the reference electrode. 20 ml of 1 mol L -1 The KCl salt solution (M) was used as the “stripping electrolyte” and the working electrode was subjected to cyclic voltammetry scanning at a scanning rate of 10 mV s -1, the potential window is -0.2-1.2 V (vs. Ag / AgCl), and electrochemical stripping is performed after 720 cycles.
[0037] (3) Obtaining a nano-thin layer of TMH: The TMH after electrochemical stripping in step (2) will be dispersed in the "stripping electrolyte". After the electrolyte is left to stand, a nano-thin layer of TMH (such as Figure 2 As shown in A). Or the electrolyte is further ultrasonically treated as needed to increase the yield of nano-thin layer TMH. Figure 3 As shown, Figure 3 (a) is an atomic force microscope (AFM) scan of the nano-thin layer TMH obtained in Example 1. Figure 3 (b) shows the change in height in the selected direction.
[0038] Example 2
[0039] (1) TMH electrode preparation: Using the three-electrode method, conductive carbon fiber paper was used as the working electrode, metal platinum mesh was used as the counter electrode, and silver / silver chloride (Ag / AgCl) electrode was used as the reference electrode. In a 20 mM Co(NO3)2 aqueous solution, an intensity of 1 mA cm was applied to the working electrode. -2 The Co(OH)2 electrode can be obtained by reducing the current for 3600s.
[0040] (2) TMH stripping preparation: Using the three-electrode method, Co(OH)2 electrode was used as the working electrode, metal platinum mesh was used as the counter electrode, silver / silver chloride (Ag / AgCl) electrode was used as the reference electrode, and 20 ml of 1 M NaCl saline solution was used as the "stripping electrolyte". Cyclic voltammetry was performed on the working electrode at a scan rate of 10 mV s -1 , the potential window is -0.2-1.2 V (vs. Ag / AgCl), and electrochemical stripping is performed after 720 cycles.
[0041] (3) Obtaining nano-thin layer TMH: After electrochemical stripping in step (2), the TMH will be dispersed in the "stripping electrolyte". The electrolyte is allowed to stand, and a nano-thin layer of TMH can be obtained in the supernatant. Alternatively, the electrolyte can be further ultrasonically treated as needed to increase the yield of nano-thin layer TMH. The relevant test results are as follows: Figure 4 shown. Figure 4 (a) is an atomic force microscope (AFM) scan of the nano-thin layer TMH obtained in Example 2. Figure 4 (b) shows the change in height in the selected direction.
[0042] Example 3
[0043] (1) Preparation of TMH electrode: Using the three-electrode method, conductive carbon fiber paper was used as the working electrode, metal platinum mesh was used as the counter electrode, and silver\silver chloride (Ag\AgCl) electrode was used as the reference electrode. In a 20 mM FeCl2+KNO3 aqueous solution, a strength of 1 mA cm was applied to the working electrode. -2 The Fe(OH)2 electrode can be obtained by reducing the current for 3600s.
[0044] (2) TMH stripping preparation: Using the three-electrode method, Fe(OH)2 electrode was used as the working electrode, metal platinum mesh was used as the counter electrode, silver / silver chloride (Ag / AgCl) electrode was used as the reference electrode, and 20 ml of 1 M NaCl saline solution was used as the "stripping electrolyte". Cyclic voltammetry was performed on the working electrode at a scan rate of 10 mV s -1 , the potential window is -0.2-1.2 V (vs. Ag / AgCl), and electrochemical stripping is performed after 720 cycles.
[0045] (3) Obtaining a nano-thin layer of TMH: The TMH after electrochemical stripping in step (2) will be dispersed in the "stripping electrolyte". After the electrolyte is left to stand, a nano-thin layer of TMH (such as Figure 2 As shown in B). Alternatively, the electrolyte may be further subjected to ultrasonic treatment as required to increase the yield of nano-thin layer TMH.
[0046] Verification Example
[0047] The performance of the nano-thin layer TMH prepared in Examples 1-3 was tested.
[0048] The test instrument is the American Bruker Dimenson ICON atomic force microscope (AFM). Drop a drop of the supernatant of the TMH dispersion solution obtained in step (3) on a smooth and flat mica sheet and blow it with N2. Place the prepared sample in a watch glass, half cover it, and let it air dry naturally in a fume hood to obtain the sample to be tested. Select the AFM as the surface scanning mode, install the probe, adjust the laser, photodetector, needle tip, focus on the sample surface, and image the 1.5×1.5μm area. The AFM scan of the nano-thin layer of TMH can be obtained. The relevant test results are as follows: Figure 3-5 shown.
[0049] Figure 3 (a) is an atomic force microscope (AFM) scan of the nano-thin layer TMH obtained in Example 1. Figure 3 (b) shows the change in height in the selected direction. Figure 3The dark orange-yellow area in (a) is the substrate, and the light yellow flake area in the middle is the image of the TMH nanosheet. Due to the AFM measurement characteristics, AFM can characterize both the outline of the nanosheet and the height of the nanosheet relative to the substrate (i.e., the thickness of the nanosheet), and express it through different colors: the lighter the color, the higher (thicker) the material height. The relationship between color and height is marked in Figure 3 On the height scale on the left side of (a). Figure 3 As can be seen in (a), the overall color distribution of the TMH nano-thin layer is relatively uniform, indicating that the thickness of the exfoliated TMH thin layer is uniform. The white area may be the crystallization of salt particles. Figure 3 The red dashed line in (a) is the cross section. The value of the height at the cross section changes with the selected direction. The result is Figure 3 As shown in (b). The results show that the thickness of the TMH nanosheet is between 5-6nm and the height varies evenly. Considering that the interlayer spacing of a single-layer TMH nanosheet is between 4-9nm, the TMH nanosheet selected for the image is most likely a single-layer TMH.
[0050] like Figure 4 As shown, Figure 4 This is an atomic force microscope (AFM) scan of the nano-thin layer TMH obtained in Example 2. The overall color distribution of the TMH nano-thin layer is relatively uniform, indicating that the thickness of the exfoliated TMH thin layer is uniform. Figure 4 The red dashed line in (a) is the cross section. The value of the height at the cross section changes with the selected direction. The result is Figure 4 As shown in (b), the thickness of the TMH nanosheet is between 5-6nm, and the height varies evenly. Considering that the interlayer spacing of a single-layer TMH nanosheet is between 4-9nm, the TMH nanosheet selected for the image is most likely a single-layer TMH.
[0051] like Figure 5 As shown, Figure 5 This is an atomic force microscope (AFM) scan of the nano-thin layer TMH obtained in Example 3. Figure 5 The overall color distribution of the TMH nano-thin layer shown in (a) is relatively uniform, indicating that the thickness of the exfoliated TMH thin layer is uniform. Figure 5 The red dotted line in (a) is the cross section. The value of the height at the cross section changes with the selected direction. The result is Figure 5 As shown in (b), the thickness of the TMH nanosheet is between 5-6nm, and the height varies evenly. Considering that the interlayer spacing of a single-layer TMH nanosheet is between 4-9nm, the TMH nanosheet selected for the image is most likely a single-layer TMH.
[0052] Therefore, the present invention adopts the above-mentioned method for preparing a transition metal hydroxide nano-thin layer in an aqueous solution, using only a salt solution of water without involving an organic solvent, and directly "one-step" peeling off the layered transition metal hydroxide in a normal temperature and pressure environment through an electrochemical method, thereby overcoming the problems that the traditional method requires an organic solvent, has cumbersome operating steps, and requires heating.
[0053] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for preparing a transition metal hydroxide nano-thin layer in an aqueous solution, characterized in that: The steps include: A. preparing a layered transition metal hydroxide to be stripped and making it into an electrode; B. Prepare a salt solution containing chloride ions of a certain concentration; C. The layered transition metal hydroxide electrode to be stripped is used as the working electrode, and the prepared saline solution is used as the electrolyte to construct a classic "three-electrode" electrochemical system. The electrode potential or current is controlled by electrochemical methods in the saline solution, so that the solute ions are repeatedly embedded and de-embedded in the interlayer gaps of the layered transition metal hydroxide body to expand the interlayer spacing and strip the layered transition metal hydroxide; D. The layered transition metal hydroxide after electrochemical stripping in step C is dispersed in the "stripping electrolyte", and the electrolyte is allowed to stand to obtain nano-scale thin layered transition metal hydroxide in the supernatant. The electrolyte is further ultrasonically treated as needed to increase the yield of nano-scale thin layered transition metal hydroxide.
2. The method for preparing a transition metal hydroxide nano-thin layer in an aqueous solution according to claim 1, characterized in that: In step A, the method for preparing the layered transition metal hydroxide to be stripped is one of electrodeposition, co-deposition and hydrothermal method.
3. The method for preparing a transition metal hydroxide nano-thin layer in an aqueous solution according to claim 1, characterized in that: In step B, the solute in the brine solution is chloride salt, the solvent is water, and the pH of the solution is neutral.
4. The method for preparing a transition metal hydroxide nano-thin layer in an aqueous solution according to claim 1, characterized in that: In step C, the electrochemical method is a controlled potential method or a controlled current method.