Nano modified shrinkage reducing agent as well as preparation method and application thereof

The nano-modified shrinkage reducer avoids shrinkage cracking and adjusts temperature in high-powered volume concrete, which solves the inconsistent effects and environmental protection problems of traditional shrinkage reducer, and improves the durability and overall performance of concrete.

CN118908614APending Publication Date: 2024-11-08WUHAN NAJIN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410815467.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

High-strength large volume concrete is prone to shrinkage and cracking during the curing stage. Traditional shrinkage agents are inconsistent in the effects of them and may contain harmful substances, which is difficult to meet environmental protection requirements.

Method used

Provided is a nanomodification reducing agent, which consists of sodium hydroxide, anionic polyacrylamide, acrylic acid, crosslinking agent, initiator, thermal temperature control agent and sepiolite, and form a loaded nanosepiolite skeleton by preparation method. The mixed solution is soaked in ethanol and dried to make a nanomodified shrinkage agent used in high-powered volume concrete to avoid shrinkage cracking and adjust temperature.

Benefits of technology

Effectively reduce the shrinkage pressure of concrete substrate, reduce crack formation, improve the long-term performance and durability of concrete, have the ability to adjust temperature, avoid cracks and collapses caused by high temperature, and maintain concrete fluidity at low temperatures, which can replace some fine aggregates and improve Overall strength and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a nano modified shrinkage reducing agent as well as a preparation method and application thereof, and belongs to the technical field of building material concrete admixtures. The nano modified shrinkage reducing agent is prepared from the following components in parts by mass: 40 parts of sodium hydroxide, 20 to 60 parts of anionic polyacrylamide, 120 parts of acrylic acid, 0.16 part of a cross-linking agent, 0.8 part of an initiator, 10 to 40 parts of a thermosensitive temperature control agent, 60 to 100 parts of sepiolite and 10 to 40 parts of a thermal buffering agent. The nano modified shrinkage reducing agent is added into the high-strength large-volume concrete, and has the main function of curing the interior of the high-strength large-volume concrete in a curing stage and avoiding shrinkage and cracking of a matrix. Meanwhile, the nano modified shrinkage reducing agent has a certain capability of adjusting temperature. Besides, the nano-modified shrinkage reducing agent also has certain strength, can replace part of fine aggregate, and avoids adverse effects such as strength reduction and the like caused by holes left due to the collapse of the water-absorbent resin when the mass concrete is in the age or after the curing is finished.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of building material concrete admixtures, and in particular to a nano-modified shrinkage reducing agent, a preparation method and an application thereof. Background Art

[0002] In the field of construction engineering, with the increase in people's demand for buildings and the increase in the demand for high-strength concrete in construction engineering, the construction of high-strength bulk concrete has become a common phenomenon. However, high-strength concrete often has large autogenous shrinkage in the early stage, which may cause cracks on the concrete surface and affect the overall performance of the concrete. At the same time, due to the dense structure of high-strength bulk concrete, it is difficult for external maintenance to penetrate into the interior of the concrete, resulting in unsatisfactory early strength development of the concrete, and even uneven strength. In addition, when high-grade concrete is made into large-volume concrete, the problem of hydration temperature rise becomes more prominent. Due to the large volume of large-volume concrete, the heat released by the hydration reaction cannot be effectively dissipated, resulting in the internal temperature of the concrete rising too fast and too high, which is easy to cause cracks and temperature stress, affecting the mechanical properties and durability of the concrete.

[0003] In order to solve the problems that are prone to occur in the pouring and curing stages of high-grade, large-volume concrete, the traditional methods mainly include: (1) Controlling the concrete mix ratio; reducing the water-cement ratio can reduce the shrinkage deformation of concrete and reduce the risk of cracking; (2) Rationally selecting admixtures; selecting suitable admixtures, such as fly ash, silica fume, etc., can improve the performance of concrete and reduce cracking; (3) Strengthening the reinforcement and quantity of steel bars; increasing the density and quantity of steel bars in areas where cracking needs to be prevented to improve the crack resistance of concrete; (4) Controlling temperature and humidity; such as pre-setting cooling pipelines in the early stage of large-volume concrete pouring, repeating manual curing for many times, and reducing the volume of concrete; (5) Using prestressing technology; applying tension in concrete through prestressing technology so that the internal stress of concrete is balanced when it is stressed, reducing the formation of cracks. By adding shrinkage reducers, it is possible to solve the problem of cracking of large-volume concrete while reducing the loss of concrete performance, reducing the difficulty and cost of construction, and having the advantages of convenience, economy and high controllability.

[0004] In existing reports, there have been many studies on the materials of concrete shrinkage reducers, but traditional concrete shrinkage reducers are affected by factors such as material composition and production process, resulting in inconsistent effects in concrete, affecting the working performance of concrete and making it difficult to achieve reliable shrinkage reduction and temperature control effects. In addition, some traditional shrinkage reducers may contain harmful substances, such as volatile organic compounds (VOCs), which pollute the environment, do not meet modern environmental protection requirements, and may cause harm to construction workers and the use environment. The Chinese patent "CN202110595549.X" discloses a composite anti-cracking agent for super-long and large-volume concrete and a preparation method thereof, including: 60% to 70% expansion component, 10% to 20% hydration heat regulation component, 10% to 20% composite admixture, 5% to 10% water-reducing component, and 0.5% to 1.0% anti-cracking fiber; wherein the expansion group; the calcium expansion component and the magnesium expansion component are in a mass ratio of 0.5 to 1:2; the composite admixture: 30% to 40% calcined diatomaceous earth, 30% to 40% activated zeolite powder, 20% to 30% phosphorus slag powder, and the hydration heat inhibition component is an ester compound and a retarder in a mass ratio of 1 to 5:1. Another Chinese patent "CN116514444A" discloses a micro-expansion anti-cracking agent for concrete and a preparation method, comprising the following components: 20-40 parts of fluorgypsum powder, 30-50 parts of magnesium oxide powder, 5-15 parts of hydrotalcite powder and 0.1-0.5 parts of β-cyclodextrin, which uses fluorgypsum powder, magnesium oxide powder and hydrotalcite powder as expansion sources, and adds a small amount of β-cyclodextrin to stabilize fluorgypsum powder, magnesium oxide powder and hydrotalcite powder. The above technologies do not explain the degree of reducing hydration heat and the mechanical effects on concrete.

[0005] Therefore, there is an urgent need to develop a high-performance, low-cost, environmentally friendly shrinkage reducer to solve the problem of shrinkage cracking caused by excessive internal temperature during the curing of high-strength concrete. Summary of the invention

[0006] In view of this, the purpose of the present application is to provide a nano-modified shrinkage-reducing agent, a preparation method and an application. The nano-modified shrinkage-reducing agent is added to high-strength bulk concrete, and its main function is to perform curing inside the high-grade bulk concrete during the curing stage and avoid shrinkage and cracking of the matrix. At the same time, the nano-modified shrinkage-reducing agent has a certain ability to regulate temperature. In addition, the nano-modified shrinkage-reducing agent also has a certain strength, can replace part of the fine aggregate, and avoids the bulk concrete from leaving holes due to the collapse of the water-absorbing resin during the age or at the end of the curing, causing adverse effects such as reduced strength.

[0007] To achieve the above objectives, this application provides at least the following technical solutions:

[0008] In the first aspect, the present application provides a nano-modified shrinkage reducing agent, which includes the following components, measured by mass: 30 to 50 parts of sodium hydroxide, 20 to 60 parts of anionic polyacrylamide, 80 to 150 parts of acrylic acid, 0.1 to 0.2 parts of a cross-linking agent, 0.5 to 1 parts of an initiator, 10 to 40 parts of a thermosensitive temperature controller, 60 to 100 parts of sepiolite, and 10 to 40 parts of a thermal buffer.

[0009] Furthermore, the relative molecular mass of the anionic acrylamide is 3 million to 12 million.

[0010] Furthermore, the crosslinking agent is at least one of trimethoxyvinyltrimethoxysilane, diisocyanate or polyanhydride.

[0011] Furthermore, the initiator is at least one of ammonium persulfate or sodium persulfate.

[0012] Furthermore, the thermosensitive temperature control agent includes polyethylene glycol, sodium chloride, and water components, and the mass ratio thereof is 18:2:20.

[0013] Furthermore, the thermal buffer is formed by compounding graphene oxide powder with any one of polyacrylate, polybutyl acrylate or polybutyl methacrylate in a mass ratio of 5:1.

[0014] In a second aspect, the present application provides a method for preparing the aforementioned nano-modified shrinkage-reducing agent, which comprises the following steps:

[0015] (1) adding 40 parts by weight of sodium hydroxide to 480 parts by weight of deionized water to obtain a sodium hydroxide solution, and adding 20 to 60 parts by weight of anionic polyacrylamide to the sodium hydroxide solution until the solution becomes a transparent gel to obtain an anionic acrylamide solution;

[0016] (2) adding 120 parts by weight of acrylic acid, 0.16 parts by weight of a cross-linking agent, 0.8 parts by weight of an initiator, and 10 to 40 parts by weight of a thermosensitive temperature control agent to an anionic allylamine solution to obtain a shrinkage-reducing thermosensitive filler;

[0017] (3) adding 60 to 100 parts by weight of a nano-sepiolite skeleton and 10 to 40 parts by weight of a thermal buffer to a shrinkage-reducing heat-sensitive filler, and performing an internal curing treatment to obtain a mixed solution loaded with a nano-sepiolite skeleton;

[0018] (4) heating the mixed solution in (3) to obtain a nano-modified shrinkage reducing agent raw material;

[0019] (5) soaking the nano-modified shrinkage reducing agent raw material in an ethanol solution;

[0020] (6) taking out the raw material of the nano-modified shrinkage-reducing agent, drying it, crushing it and grinding it to make the nano-modified shrinkage-reducing agent.

[0021] In a third aspect, the present application provides the use of the aforementioned nano-modified shrinkage-reducing agent in the preparation of high-strength volume concrete.

[0022] The present application provides a nano-modified shrinkage-reducing agent, a preparation method and an application, which have at least the following beneficial effects:

[0023] 1. The nano-modified shrinkage-reducing agent provided in the present application is cured internally during the curing stage and avoids shrinkage and cracking of the matrix. By adding the nano-modified shrinkage-reducing agent to high-strength bulk concrete, the shrinkage pressure of the concrete matrix can be effectively reduced, and the shrinkage crack formation of the matrix can be reduced, thereby improving the long-term performance and durability of the concrete. The nano-modified shrinkage-reducing agent can form a uniformly distributed network structure inside the matrix, effectively fill the cracks and holes in the matrix, and improve the stability and reliability of the concrete.

[0024] 2. The nano-modified shrinkage-reducing agent provided in the present application has a certain ability to regulate temperature, and can regulate the temperature inside high-strength bulk concrete to avoid matrix cracks and collapse caused by high temperature. At the same time, the nano-modified shrinkage-reducing agent can maintain the fluidity and volatility of concrete at low temperatures, which is beneficial to the pouring and repair of high-strength bulk concrete.

[0025] 3. The nano-modified shrinkage-reducing agent provided in the present application has certain strength and durability, and can act as part of the fine aggregate in high-strength volume concrete, thereby improving the overall strength and durability of the concrete.

[0026] 4. The nano-modified shrinkage-reducing agent provided in the present application prevents the water-absorbing resin from collapsing and leaving holes. The nano-modified shrinkage-reducing agent can absorb cement particles in the early stage of high-strength bulk concrete formation, effectively fill the holes left by the collapse of the water-absorbing resin, and improve the overall strength and durability of the concrete. At the same time, the nano-modified shrinkage-reducing agent can form a uniformly distributed network structure inside the high-strength bulk concrete, effectively reduce the cracks and holes in the matrix, and improve the stability and reliability of the concrete. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical solution and advantages of the present application more clear, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described here are only used to explain the present application and are not used to limit the present application.

[0028] The present application embodiment provides a nano-modified shrinkage-reducing agent, which includes the following components by mass: 30-50 parts of sodium hydroxide, 20-60 parts of anionic polyacrylamide, 80-150 parts of acrylic acid, 0.1-0.2 parts of a cross-linking agent, 0.5-1 parts of an initiator, 10-40 parts of a thermosensitive temperature control agent, 60-100 parts of sepiolite, and 10-40 parts of a thermal buffer. The present application embodiment provides a nano-modified shrinkage-reducing agent, which greatly improves the working performance of concrete, and can effectively reduce the internal temperature of concrete, and the improvement effect in shrinkage reduction is also very obvious.

[0029] In certain preferred embodiments, a nano-modified shrinkage-reducing agent comprises the following components, measured by mass: 40 parts of sodium hydroxide, 20-60 parts of anionic polyacrylamide, 120 parts of acrylic acid, 0.16 parts of a cross-linking agent, 0.8 parts of an initiator, 10-40 parts of a thermosensitive temperature controller, 60-100 parts of sepiolite, and 10-40 parts of a thermal buffer.

[0030] In some embodiments, the relative molecular mass of the anionic acrylamide is 3 million to 12 million. In some preferred embodiments, the relative molecular mass of the anionic acrylamide is 12 million.

[0031] In certain embodiments, the crosslinking agent is at least one of trimethoxyvinyltrimethoxysilane, diisocyanate, or polyanhydride.

[0032] In certain embodiments, the initiator is at least one of ammonium persulfate or sodium persulfate.

[0033] In certain embodiments, the thermosensitive temperature control agent includes polyethylene glycol, sodium chloride, and water in a mass ratio of 18:2:20.

[0034] In some embodiments, the thermal buffer is formed by compounding graphene oxide powder with any one of polyacrylate, polybutyl acrylate or polybutyl methacrylate in a mass ratio of 5:1.

[0035] Based on this, the present invention provides a method for preparing the aforementioned nano-modified shrinkage-reducing agent, which comprises the following steps:

[0036] (1) Prepare anionic acrylamide solution. First, add 480 parts by weight of deionized water into a beaker, then add 40 parts by weight of sodium hydroxide into the beaker, wait for the solute to dissolve, then add 20 to 60 parts by weight of anionic polyacrylamide and stir until it becomes a transparent gel;

[0037] (2) 120 parts by weight of acrylic acid is slowly added dropwise to the anionic acrylamide solution and stirred to disperse. After uniform mixing, 0.16 parts by weight of a crosslinking agent, 0.8 parts by weight of an initiator and 10 to 40 parts of a thermosensitive temperature control agent are added respectively, and after uniform ultrasonic dispersion, a shrinkage-reducing thermosensitive filler is obtained;

[0038] (3) 60 to 100 parts by weight of sepiolite are placed in a ball mill, zirconium oxide dry grinding balls are added, and mechanical grinding is performed to obtain a nano sepiolite skeleton;

[0039] (4) Add 60-100 parts by weight of nano-sepiolite skeleton and 10-40 parts by weight of thermal buffer to the shrinkage-reducing heat-sensitive filler, and first disperse the nano-sepiolite skeleton and the thermal buffer in the shrinkage-reducing filler. Then, use a negative pressure filter to internally solidify the solution in step (2) and the nano-sepiolite skeleton;

[0040] (5) After the mixed solution is loaded into the nano-sepiolite skeleton, it is heated in a water bath to form a nano-modified shrinkage-reducing agent raw material;

[0041] (6) soaking the formed nano-modified shrinkage-reducing agent raw material in an ethanol solution to remove unreacted monomers, such as anionic polyacrylamide;

[0042] (7) The raw material of the nano-modified shrinkage-reducing agent is placed in a vacuum freeze drying box for drying, and after drying, it is crushed and ground to prepare the nano-modified shrinkage-reducing agent.

[0043] In certain embodiments, the relative molecular mass of the anionic acrylamide in step (1) is 3 million to 12 million.

[0044] In certain embodiments, the anionic polyacrylamide in step (1) is stirred for 60 to 90 minutes until all the particles are dissolved.

[0045] In certain embodiments, the crosslinking agent in step (2) is at least one of trimethoxyvinyltrimethoxysilane, diisocyanate or polyanhydride.

[0046] In certain embodiments, the initiator in step (2) is at least one of ammonium persulfate or sodium persulfate.

[0047] In certain embodiments, the specific synthesis process of the thermosensitive temperature control agent described in step (2) is: 20 parts by mass of water are mixed with 18 parts by mass of polyethylene glycol, and then 2 parts by mass of sodium chloride are added and mixed evenly.

[0048] In certain embodiments, the frequency of the ultrasonic dispersion in step (2) is 10 to 30 kHz, and the dispersion time is 20 to 40 min.

[0049] In certain embodiments, the specific synthesis process of the thermal buffer described in step (3) is as follows: adding natural graphite powder to an acidic solution containing 50% sulfuric acid or nitric acid for oxidation reaction to generate graphene oxide; filtering, washing, and drying to obtain graphene oxide powder; mixing the prepared graphene oxide powder with one of polyacrylate, polybutyl acrylate, or polybutyl methacrylate in a ratio of 5:1, and mechanically grinding at a speed of 400 to 600 r / min; hot pressing under high temperature and high pressure (200 to 300°C, 10 to 100 standard atmospheres) to fully compound and shape the graphene oxide and the polymer to obtain the thermal buffer.

[0050] In certain embodiments, the mechanical grinding speed in step (3) is 400 r / min, and the dry grinding time is 20 min.

[0051] In some embodiments, the dispersion treatment in step (4) is ultrasonic dispersion, the vibration frequency is 400-600 r / min, and the dry grinding time is 20-40 min; the internal curing process is to fix the shrinkage-reducing heat-sensitive filler on the nano-sepiolite skeleton and closely bond it. The curing time is set to 5 min, 10 min, 20 min, 40 min, 60 min, and the load is completed.

[0052] In certain embodiments, the water bath heating temperature in step (5) is 55-75° C., and the water bath time is 10-30 min.

[0053] In certain embodiments, the vacuum drying in step (6) is carried out at a temperature of 70 to 90° C. and for 24 hours.

[0054] Based on this, the embodiments of the present application also provide the use of the aforementioned nano-modified shrinkage-reducing agent in the preparation of high-strength volume concrete.

[0055] In some embodiments, in the high-strength volume concrete, the mass proportion of the nano-modified shrinkage-reducing agent is 1% to 3%. In some preferred embodiments, the mass proportion of the nano-modified shrinkage-reducing agent is 2%.

[0056] The technical solution of the present application and the technical effects achieved are described in detail below through more specific embodiments.

[0057] Example 1

[0058] This embodiment provides a method for preparing a nano-modified shrinkage-reducing agent, which specifically comprises the following steps:

[0059] (1) Preparation of shrinkage-reducing thermosensitive filler: first, add 480 parts by weight of deionized water into a beaker, then add 40 parts by weight of sodium hydroxide into the beaker, wait for the solute to dissolve, add 20 parts by weight of anionic polyacrylamide and stir until it becomes a transparent colloid, to obtain an anionic acrylamide solution; slowly drop 120 parts by weight of acrylic acid into the anionic acrylamide solution, stir and disperse, and after uniform mixing, add 0.16 parts by weight of a cross-linking agent (trimethoxyvinyl trimethoxysilane), 0.8 parts by weight of an initiator (ammonium persulfate), 30 parts by weight of a thermosensitive temperature control agent (prepared by: mixing 20 parts by weight of water with 18 parts by weight of polyethylene glycol, and then adding 2 parts by weight of sodium chloride) and 30 parts by weight of a thermal buffer (synthesized by the aforementioned preparation method), and uniformly disperse by ultrasonication to obtain a shrinkage-reducing thermosensitive filler;

[0060] (2) Preparation of nano-sepiolite skeleton and internal curing treatment: 80 parts of sepiolite are placed in a ball mill, and zirconium oxide dry grinding balls are added for mechanical grinding at a speed of 400 r / min for 20 min to obtain a nano-sepiolite skeleton; the nano-sepiolite skeleton is added to a shrinkage-reducing thermosensitive filler, and the nano-sepiolite skeleton is first dispersed in the shrinkage-reducing thermosensitive filler, and then the shrinkage-reducing thermosensitive filler and the nano-sepiolite skeleton are internally cured by using a negative pressure filter;

[0061] (3) Preparation of nano-modified shrinkage-reducing agent: After loading the nano-sepiolite skeleton, it is heated in a water bath to form a nano-modified shrinkage-reducing agent raw material; the nano-modified shrinkage-reducing agent raw material is placed in a vacuum freeze drying box for drying, and after drying, it is crushed and ground to form a nano-modified shrinkage-reducing agent.

[0062] Example 2

[0063] This embodiment provides a method for preparing a nano-modified shrinkage-reducing agent, which is different from Embodiment 1 only in that the anionic polyacrylamide is adjusted to 40 parts by mass; the remaining steps and parameters are the same.

[0064] Example 3

[0065] This embodiment provides a method for preparing a nano-modified shrinkage-reducing agent, which is different from Embodiment 1 only in that the anionic polyacrylamide is adjusted to 60 parts by mass; the remaining steps and parameters are the same.

[0066] Example 4

[0067] This embodiment provides a method for preparing a nano-modified shrinkage-reducing agent, which is different from Embodiment 1 only in that: the anionic polyacrylamide is adjusted to 40 parts by mass, and the thermosensitive temperature control agent is adjusted to 10 parts by mass; the remaining steps and parameters are the same.

[0068] Example 5

[0069] This embodiment provides a method for preparing a nano-modified shrinkage-reducing agent, which is different from Embodiment 1 only in that: the anionic polyacrylamide is adjusted to 40 parts by mass, and the thermosensitive temperature control agent is adjusted to 20 parts by mass; the remaining steps and parameters are the same.

[0070] Example 6

[0071] This embodiment provides a method for preparing a nano-modified shrinkage-reducing agent, which is different from Embodiment 1 only in that: the anionic polyacrylamide is adjusted to 40 parts by mass, and the thermosensitive temperature control agent is adjusted to 40 parts by mass; the remaining steps and parameters are the same.

[0072] Example 7

[0073] This embodiment provides a method for preparing a nano-modified shrinkage-reducing agent, which is different from Embodiment 1 only in that: the anionic polyacrylamide is adjusted to 40 parts by mass, the thermosensitive temperature control agent is adjusted to 30 parts by mass, and the thermal buffer is adjusted to 10 parts by mass; the remaining steps and parameters are the same.

[0074] Example 8

[0075] This embodiment provides a method for preparing a nano-modified shrinkage-reducing agent, which is different from Embodiment 1 only in that: the anionic polyacrylamide is adjusted to 40 parts by mass, the thermosensitive temperature control agent is adjusted to 30 parts by mass, and the thermal buffer is adjusted to 20 parts by mass; the remaining steps and parameters are the same.

[0076] Example 9

[0077] This embodiment provides a method for preparing a nano-modified shrinkage-reducing agent, which is different from Embodiment 1 only in that: the anionic polyacrylamide is adjusted to 40 parts by mass, the thermosensitive temperature control agent is adjusted to 30 parts by mass, and the thermal buffer is adjusted to 40 parts by mass; the remaining steps and parameters are the same.

[0078] Example 10

[0079] This embodiment provides a method for preparing a nano-modified shrinkage-reducing agent, which is different from Example 1 only in that: the anionic polyacrylamide is adjusted to 40 parts by mass, the thermosensitive temperature control agent is adjusted to 30 parts by mass, the thermal buffer is adjusted to 30 parts by mass, and the sepiolite skeleton is adjusted to 60 parts by mass; the remaining steps and parameters are the same.

[0080] Embodiment 11

[0081] This embodiment provides a method for preparing a nano-modified shrinkage-reducing agent, which is different from Example 1 only in that: the anionic polyacrylamide is adjusted to 40 parts by mass, the thermosensitive temperature control agent is adjusted to 30 parts by mass, the thermal buffer is adjusted to 30 parts by mass, and the sepiolite skeleton is adjusted to 100 parts by mass; the remaining steps and parameters are the same.

[0082] Comparative Example 1

[0083] This comparative example provides a method for preparing a nano-modified shrinkage-reducing agent, which is different from Example 1 only in that the anionic polyacrylamide is not added; the remaining steps and parameters are the same.

[0084] Comparative Example 2

[0085] This comparative example provides a method for preparing a nano-modified shrinkage-reducing agent, which differs from Example 1 only in that the thermosensitive temperature-controlling agent is not added; the remaining steps and parameters are the same.

[0086] Comparative Example 3

[0087] This comparative example provides a method for preparing a nano-modified shrinkage-reducing agent, which differs from Example 1 only in that the thermal buffer is not added; the remaining steps and parameters are the same.

[0088] Comparative Example 4

[0089] This comparative example provides a method for preparing a nano-modified shrinkage-reducing agent, which is different from Example 1 only in that the sepiolite skeleton is not added; the remaining steps and parameters are the same.

[0090] The nano-modified shrinkage-reducing agents prepared in Examples 1 to 11 and Comparative Examples 1 to 4 were used as additives to prepare concrete samples. The specific preparation process is as follows:

[0091] The raw materials were weighed according to the content of cement 350kg, nano-modified shrinkage reducer 7kg, sand 560kg, aggregate 945kg, water 157L, and water reducer 500g per cubic meter of concrete. The nano-modified shrinkage reducer was first added to the cement for pre-mixing, and then added into the mixer with water, water reducer, sand and aggregate, and mixed evenly. The concrete sample was obtained by mixing for 5 minutes.

[0092] The concrete samples obtained above were numbered respectively, and the performance tests were performed on the concrete samples according to the standards listed in Table 1 below:

[0093] Table 1 Test items and reference standards

[0094] Test items Reference Standards Expansion, slump GB50164-2011 "Concrete Quality Control Standard" Compressive strength, flexural strength GB / T 50081-2019 "Standard for test methods of physical and mechanical properties of concrete" Crack resistance GB / T50152-2012 Standard for Test Methods of Concrete Structures Shrinkage performance evaluation JC / T 2361-2016 Mortar and concrete shrinkage reducer Internal temperature measurement GB / T51028-2015 Technical Specification for Temperature Measurement and Control of Mass Concrete

[0095] The test results are shown in Tables 2 to 5:

[0096] Table 2 Concrete working performance test

[0097]

[0098]

[0099] Table 3 Evaluation of concrete crack resistance

[0100]

[0101] Table 4 Concrete shrinkage performance evaluation

[0102]

[0103]

[0104] Table 5 Concrete internal temperature measurement

[0105]

[0106] Table 2 shows the test results of concrete sample expansion, slump, compressive strength, flexural strength and other working properties; Table 3 shows the test results of concrete sample crack resistance, including cracking time, maximum crack width, average crack area of ​​a single crack, number of cracks, number of cracks per unit area, and total crack area per unit area; Table 4 shows the test results of concrete sample shrinkage performance from 1 to 60 days; Table 5 shows the test results of concrete sample internal temperature. The following conclusions can be drawn from the test results in Tables 2 to 4:

[0107] The nano-modified shrinkage-reducing agent prepared in the embodiment is superior to the comparative example in performance tests, indicating that the nano-modified shrinkage-reducing agent provided by the present application improves the compressive and flexural strengths of concrete, reduces the degree of cracking of concrete during the curing process, and can effectively reduce the internal temperature of concrete. At the same time, the improvement effect in shrinkage reduction is also very obvious.

[0108] Compared with Comparative Example 1, the anionic acrylamide in the embodiment can significantly reduce the cracking of concrete during curing, and can improve the compressive strength and flexural strength of concrete, and play an anti-cracking role; compared with Comparative Example 2, it can be seen that the thermosensitive temperature controller can effectively improve the internal environment of concrete and reduce the internal temperature of concrete during curing; compared with Comparative Example 3, it can be seen that the thermal buffer can effectively reduce the maximum temperature of concrete and play a role of heat buffer; at the same time, the thermosensitive temperature controller and the thermal buffer both have the effect of reducing the shrinkage of concrete; compared with Comparative Example 4, it can be seen that the sepiolite without the addition of nano-modified sepiolite has a greater impact on the later concrete strength, and the shrinkage reducer containing nano-modified sepiolite can effectively prevent the reduction of concrete strength and the occurrence of cracks. From the test results of Examples 1 to 11 and Comparative Examples 1, 2, 3 and 4, it can be concluded that the nano-modified shrinkage-reducing agent synthesized from 40 parts by mass of sodium hydroxide, 120 parts by mass of acrylic acid, 0.16 parts by mass of a cross-linking agent, 0.8 parts by mass of an initiator, 40 parts by mass of anionic polyacrylamide, 80 parts by mass of sepiolite, 30 parts by mass of a thermosensitive temperature controller and 30 parts by mass of a thermal buffer has the best effect.

[0109] The present application is described in detail above. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the present application and its core ideas. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present application, several improvements and modifications can be made to the present application, and these improvements and modifications also fall within the scope of protection of the claims of the present application.

Claims

1. A nano-modified shrinkage reducing agent, characterized in that: The nano-modified shrinkage-reducing agent comprises the following components in parts by mass: 30-50 parts of sodium hydroxide, 20-60 parts of anionic polyacrylamide, 80-150 parts of acrylic acid, 0.1-0.2 parts of a cross-linking agent, 0.5-1 parts of an initiator, 10-40 parts of a thermosensitive temperature control agent, 60-100 parts of sepiolite, and 10-40 parts of a thermal buffer.

2. The nano-modified shrinkage reducing agent according to claim 1, characterized in that: The sodium hydroxide is 40 parts by mass, the acrylic acid is 120 parts by mass, the cross-linking agent is 0.16 parts by mass, and the initiator is 0.8 parts by mass.

3. The nano-modified shrinkage reducing agent according to claim 1, characterized in that: The crosslinking agent is at least one of trimethoxyvinyltrimethoxysilane, diisocyanate or polyanhydride.

4. The nano-modified shrinkage reducing agent according to claim 1, characterized in that: The initiator is at least one of ammonium persulfate or sodium persulfate.

5. The nano-modified shrinkage-reducing agent according to claim 1, characterized in that: The thermosensitive temperature control agent includes polyethylene glycol, sodium chloride and water, and the mass ratio thereof is 18:2:

20.

6. The nano-modified shrinkage-reducing agent according to claim 1, characterized in that: The thermal buffer is prepared by compounding graphene oxide powder with any one of polyacrylate, polybutyl acrylate or polybutyl methacrylate in a mass ratio of 5:

1.

7. The nano-modified shrinkage-reducing agent according to claim 1, characterized in that: The relative molecular mass of the anionic acrylamide is 3 million to 12 million.

8. The method for preparing the nano-modified shrinkage-reducing agent according to claim 1, characterized in that: The following steps are involved: (1) adding 40 parts by weight of sodium hydroxide to 480 parts by weight of deionized water to obtain a sodium hydroxide solution, and adding 20 to 60 parts by weight of anionic polyacrylamide to the sodium hydroxide solution until the solution becomes a transparent gel to obtain an anionic acrylamide solution; (2) adding 120 parts by weight of acrylic acid, 0.16 parts by weight of a cross-linking agent, 0.8 parts by weight of an initiator, and 10 to 40 parts by weight of a thermosensitive temperature control agent to an anionic allylamine solution to obtain a shrinkage-reducing thermosensitive filler; (3) adding 60 to 100 parts by weight of a nano-sepiolite skeleton and 10 to 40 parts by weight of a thermal buffer to a shrinkage-reducing heat-sensitive filler, and performing an internal curing treatment to obtain a mixed solution loaded with a nano-sepiolite skeleton; (4) heating the mixed solution in (3) to obtain a nano-modified shrinkage reducing agent raw material; (5) soaking the nano-modified shrinkage reducing agent raw material in an ethanol solution; (6) taking out the raw material of the nano-modified shrinkage-reducing agent, drying it, crushing it and grinding it to make the nano-modified shrinkage-reducing agent.

9. Use of the nano-modified shrinkage-reducing agent according to any one of claims 1 to 7 in the preparation of high-strength volume concrete.

10. The use according to claim 9, characterized in that: The mass proportion of the nano-modified shrinkage-reducing agent in the high-strength volume concrete is 1% to 3%.