Low-carbon cementing material prepared from supercritical carbon dioxide and preparation method of low-carbon cementing material

By using supercritical carbon dioxide and activated solutions in construction solid waste, the activity of regenerated micropowder is improved, the problem of low efficiency of conventional carbonization treatment is solved, and the performance improvement of efficient carbon neutrality and cement-based materials is achieved.

CN118908631AActive Publication Date: 2024-11-08SOUTHEAST UNIV +2

Patent Information

Application Number
CN202310507959.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-08
Estimated Expiration
2043-05-08

AI Technical Summary

Technical Problem

The efficiency of conventional carbonization treatment is low and cannot be implemented on a large scale, resulting in the problem of high energy consumption and insufficient carbon neutrality efficiency in the development of low carbon in the cement industry.

Method used

The regenerated micropowder is treated with supercritical carbon dioxide and activated solution. Through the carbonization reaction in the supercritical carbon dioxide environment, a highly active calcium carbonate and silica gel is generated. It is combined with cement as auxiliary gelling materials to prepare low-carbon gelling Material.

Benefits of technology

It significantly improves the activity index of regenerated micropowders, shortens the carbonization time, reduces energy consumption and carbon emissions, and improves the mechanical properties of cement-based materials and carbon capture efficiency throughout the life cycle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004216217690000041
    Figure BDA0004216217690000041
  • Figure BDA0004216217690000071
    Figure BDA0004216217690000071
Patent Text Reader

Abstract

The invention discloses a low-carbon cementing material prepared from supercritical carbon dioxide and a preparation method, and belongs to the technical field of building materials. The low-carbon cementing material is prepared by the following steps: dipping regenerated micro-powder in an activating solution, carbonizing the regenerated micro-powder in a supercritical carbon dioxide environment to obtain an auxiliary cementing material, and compounding the auxiliary cementing material with cement, thereby obtaining the low-carbon cementing material, the activating solution comprises a surfactant and a calcium ion complexing agent; the surfactant is one or more of phosphoric acid, soluble phosphate and soluble aluminum salt; the calcium ion complexing agent is one of ethylene diamine tetraacetic acid, nitrilotriacetic acid trisodium salt and triethanolamine. Waste concrete recycled micro powder is taken as an object, a reinforced product is obtained through supercritical carbon dioxide mineralization, cement clinker in a certain proportion is replaced, carbon dioxide is sealed and stored while efficient resource utilization of building solid waste is achieved, and a novel low-carbon cementing material is provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and in particular relates to a low-carbon gelling material prepared by using supercritical carbon dioxide and a preparation method thereof. Background Art

[0002] Building materials are the material basis for national economic construction and social development and progress. Since the invention of Portland cement, cement and concrete have become the most commonly used and mainstream civil construction materials. In 2021, China produced about 2.378 billion tons of cement. However, the cement industry is a high-emission and high-energy-consuming industry. The cement industry accounts for 8%-9% of the world's total carbon emissions and 2%-3% of total energy consumption.

[0003] Reducing and reducing emissions and energy consumption from all angles of the entire life cycle of cement concrete is the key research direction of the current cement production industry, and there are three main directions. The first is to optimize the cement production process and find alternatives to fossil fuels; the second is to reduce the amount of cement clinker, such as using solid waste to replace part of the cement and developing new cementitious materials; the third is to develop durability improvement technology and prepare long-life concrete. Among them, carbon reduction focuses on the development and utilization of industrial solid waste to achieve the goal of "less cement in concrete, less clinker in cement, and less alite minerals in clinker". In my country's large-scale urbanization construction, about 3 billion tons of construction solid waste are discharged each year. After crushing, the larger particle size can be used as aggregate to replace natural sand and gravel, and the recycled micropowder less than 0.075mm can be used as a mineral admixture to replace part of the cement. The main components of recycled micropowder are sand and gravel fragments, as well as a small amount of hydration products such as CSH gel and calcium hydroxide. They have low chemical activity and basically do not participate in cement hydration. After replacing cement, they mainly rely on the nucleation effect of fine particles to promote cement hydration. However, since it also contains a small amount of hardened cement stone and a small amount of unhydrated cement particles, and a large number of microcracks are introduced during the crushing process, its water demand is greater than that of cement, which affects the working performance of cement-based materials.

[0004] In existing research, mechanical grinding and heat treatment are used to improve the activity of regenerated micropowder, but there is a problem of high energy consumption. In recent years, the carbonization treatment has been emerging to achieve carbon neutrality while improving the activity of regenerated micropowder. However, the efficiency of conventional carbonization treatment is too low to achieve large-scale application. For example, CN112125541B discloses a method for wet carbonization of waste concrete regenerated micropowder and the application of regenerated micropowder. By controlling the ratio of regenerated micropowder to water, ventilation rate, carbon dioxide concentration, water temperature, carbonization reaction time and other parameters, carbonation reaction of carbon dioxide and regenerated micropowder is used to generate highly active calcium carbonate and silica gel, which is used as an auxiliary cementitious material. This method uses the convection of carbon dioxide and water, and then improves the rapid carbonization reaction of regenerated micropowder by stirring.

[0005] In summary, in order to meet the urgent needs of low-carbon development of the cement industry, using construction solid waste to prepare low-carbon cementitious materials is an effective treatment method. Therefore, seeking more efficient and low-carbon treatment methods, further improving production efficiency, and reducing new energy consumption generated in the process of solid waste resource utilization are important development directions for realizing the application of solid waste in the field of low-carbon cementitious materials. Summary of the invention

[0006] In order to solve the technical problem that conventional carbonization treatment is inefficient and cannot be applied on a large scale, the present invention provides a low-carbon cementitious material prepared by supercritical carbon dioxide and a preparation method thereof. The waste concrete recycled micropowder is used as the object, and a reinforced product is obtained by supercritical carbon dioxide mineralization, which replaces a certain proportion of cement clinker to obtain a low-carbon cementitious material. While solving the problem of efficient resource utilization of construction solid waste, the carbon dioxide is sealed, providing a new low-carbon cementitious material.

[0007] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0008] A low-carbon cementitious material prepared by supercritical carbon dioxide, wherein the regenerated micropowder is impregnated with an activation solution and then carbonized in a supercritical carbon dioxide environment to obtain an auxiliary cementitious material, and the auxiliary cementitious material is compounded with cement to obtain a low-carbon cementitious material;

[0009] The activation solution includes a surfactant and a calcium ion complexing agent; the surfactant is one or more of phosphoric acid, soluble phosphate and soluble aluminum salt; the calcium ion complexing agent is one of ethylenediaminetetraacetic acid, trisodium nitrilotriacetate and triethanolamine; the concentration of the surfactant in the activation solution is 0.01 mol / L to 1 mol / L , The calcium ion complexing agent accounts for 0.01% to 1% of the mass of the activation solution.

[0010] The mass ratio of the regenerated micropowder to the activation solution is 1:5-20;

[0011] The regenerated micropowder is made from waste concrete, waste mortar or waste cement paste generated during the demolition of waste buildings and the production of commercial concrete mixing stations, and is produced after crushing, grinding, screening and drying. The regenerated micropowder contains cement hydration products CSH, CH, AFt and unhydrated minerals C2S, C3S and C4AF, and has carbonization ability; the particle size of the regenerated micropowder is less than 0.075 mm, and the specific surface area is greater than 350 m 2 / kg.

[0012] The cement is one of cement clinker, Portland cement, ordinary Portland cement, sulphoaluminate cement, high belite cement and belite sulphoaluminate cement; the mass ratio of the auxiliary cementitious material to the cement is 1:1 to 1:9.

[0013] On the other hand, the present invention also provides a method for preparing a low-carbon gelling material using supercritical carbon dioxide, which specifically comprises the following steps:

[0014] (1) placing the regenerated micropowder in a container, adding an activation solution, and mixing uniformly to obtain an impregnation mixture;

[0015] (2) placing the impregnation mixture in a reaction device, and introducing carbon dioxide gas into the reaction device, setting the temperature to 35-60° C. and the pressure to 7.5-10 MPa to obtain supercritical carbon dioxide, and carbonizing the impregnation mixture in a supercritical carbon dioxide environment;

[0016] (3) After the carbonization is completed, the pressure is released, the carbonization product is taken out, and the auxiliary cementitious material is obtained by drying after solid-liquid separation. The auxiliary cementitious material is compounded with cement to obtain a low-carbon cementitious material.

[0017] Furthermore, the carbon dioxide gas in step 2 is industrial tail gas or commercial gas with a concentration of not less than 90%, and the industrial tail gas comes from the steel industry, cement industry, electric power industry, chemical industry and other industries or any combination of tail gas.

[0018] Furthermore, in step (2), the flow rate of carbon dioxide gas is 20-50 L / min.

[0019] Furthermore, the carbonization reaction time in step (2) is 1-3h.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) The present invention utilizes supercritical carbon dioxide to cure the regenerated micropowder. Supercritical carbon dioxide has both gas and liquid properties in terms of physical properties. Its density is several hundred times that of gas, close to that of liquid. This also gives supercritical carbon dioxide a strong solvation ability and a relatively high diffusion coefficient of gas. These properties can improve the mass transfer efficiency of supercritical carbon dioxide entering the microporous structure of the regenerated micropowder and effectively accelerate the carbonization of the substance. After supercritical carbon dioxide curing, the time required for conventional carbon dioxide curing can be greatly shortened, the reaction temperature and energy consumption during the treatment process can be reduced. At the same time, since supercritical carbon dioxide has a strong transmission performance, it can be fully carbonized on the surface of the regenerated micropowder and can fully enter the internal pores of the regenerated micropowder, making the carbonization more complete. This solves the problem that during conventional carbon dioxide curing, dense hydration products are quickly generated on the surface of the regenerated micropowder, which hinders the gas from further entering the internal pores of the regenerated micropowder and makes it difficult to achieve complete carbonization. The porosity of the regenerated micropowder after full carbonization decreases, which weakens the impact of the decline in the working performance of the cement-based material caused by its incorporation, and at the same time improves the mechanical properties of the cement-based material.

[0022] (2) The present invention uses a surfactant and a calcium ion complexing agent solution to mix with the regenerated micropowder. The surfactant can improve the dispersibility of the regenerated micropowder in water, and the calcium ion complexing agent can promote the dissolution of calcium ions in the regenerated micropowder components, thereby improving the subsequent carbonization efficiency.

[0023] (3) The technical solution provided by the present invention utilizes supercritical carbon dioxide curing to effectively improve the performance of construction solid waste recycling products, provides a new low-carbon cementitious material and CCUS technology, and at the same time reduces carbon emissions throughout the life cycle of cement-based materials, which has important social and environmental significance. DETAILED DESCRIPTION

[0024] In order to better understand the present invention, the content of the present invention is further described below in conjunction with embodiments, but the content of the present invention is not limited to the scope of the embodiments. On the contrary, these embodiments are provided to explain the principles of the present invention and its practical application, so that other technical personnel in the field can understand the various embodiments of the present invention and various modifications suitable for specific intended applications.

[0025] The regenerated micro powder in the embodiments and comparative examples is a cement slurry with a water-cement ratio of 0.40 prepared in the laboratory, which is crushed and ball-milled for 20 minutes, and then further sieved to obtain a powder with a particle size of less than 0.075 mm, and a specific surface area of ​​more than 350 m 2 / kg.

[0026] The activation solution and carbon dioxide in the embodiments and comparative examples are selected as shown in Table 1 below:

[0027] Table 1 Selection of activation solution and carbon dioxide in Examples and Comparative Examples

[0028]

[0029]

[0030] Example 1

[0031] (1) placing the regenerated micropowder in a container, adding an activation solution, and mixing uniformly to obtain an impregnation mixture;

[0032] (2) placing the impregnation mixture in a reaction device, and introducing carbon dioxide gas into the reaction device, setting the temperature to 35° C. and the pressure to 7.5 MPa to obtain supercritical carbon dioxide, the carbon dioxide gas flow rate is 25 L / min, and the impregnation mixture is carbonized in a supercritical carbon dioxide environment for 1 hour;

[0033] (3) After the carbonization is completed, the pressure is released, the carbonization product is taken out, and the auxiliary cementitious material is obtained after solid-liquid separation and drying. The auxiliary cementitious material and cement are compounded in a mass ratio of 3:7 to obtain a low-carbon cementitious material.

[0034] Example 2

[0035] (1) placing the regenerated micropowder in a container, adding an activation solution, and mixing uniformly to obtain an impregnation mixture;

[0036] (2) placing the impregnation mixture in a reaction device, and introducing carbon dioxide gas into the reaction device, setting the temperature to 35° C. and the pressure to 9 MPa to obtain supercritical carbon dioxide, the carbon dioxide gas flow rate to 45 L / min, and carbonizing the impregnation mixture in a supercritical carbon dioxide environment for 2 h;

[0037] (3) After the carbonization is completed, the pressure is released, the carbonization product is taken out, and the auxiliary cementitious material is obtained after solid-liquid separation and drying. The auxiliary cementitious material is compounded with cement in a mass ratio of 1:8 to obtain a low-carbon cementitious material.

[0038] Example 3

[0039] (1) placing the regenerated micropowder in a container, adding an activation solution, and mixing uniformly to obtain an impregnation mixture;

[0040] (2) placing the impregnation mixture in a reaction device, and introducing carbon dioxide gas into the reaction device, setting the temperature to 45° C. and the pressure to 7.5 MPa to obtain supercritical carbon dioxide, the carbon dioxide gas flow rate is 35 L / min, and the impregnation mixture is carbonized in a supercritical carbon dioxide environment for 3 h;

[0041] (3) After the carbonization is completed, the pressure is released, the carbonization product is taken out, and the auxiliary cementitious material is obtained after solid-liquid separation and drying. The auxiliary cementitious material is compounded with cement in a mass ratio of 1:5 to obtain a low-carbon cementitious material.

[0042] Example 4

[0043] (1) placing the regenerated micropowder in a container, adding an activation solution, and mixing uniformly to obtain an impregnation mixture;

[0044] (2) placing the impregnation mixture in a reaction device, and introducing carbon dioxide gas into the reaction device, setting the temperature to 60° C. and the pressure to 7.5 MPa to obtain supercritical carbon dioxide, the carbon dioxide gas flow rate is 25 L / min, and the impregnation mixture is carbonized in a supercritical carbon dioxide environment for 1 hour;

[0045] (3) After the carbonization is completed, the pressure is released, the carbonization product is taken out, and the auxiliary cementitious material is obtained after solid-liquid separation and drying. The auxiliary cementitious material and cement are compounded in a mass ratio of 3:7 to obtain a low-carbon cementitious material.

[0046] Example 5

[0047] (1) placing the regenerated micropowder in a container, adding an activation solution, and mixing uniformly to obtain an impregnation mixture;

[0048] (2) placing the impregnation mixture in a reaction device, and introducing carbon dioxide gas into the reaction device, setting the temperature to 35° C. and the pressure to 10 MPa to obtain supercritical carbon dioxide, the carbon dioxide gas flow rate is 25 L / min, and the impregnation mixture is carbonized in a supercritical carbon dioxide environment for 1 hour;

[0049] (3) After the carbonization is completed, the pressure is released, the carbonization product is taken out, and the auxiliary cementitious material is obtained after solid-liquid separation and drying. The auxiliary cementitious material and cement are compounded in a mass ratio of 3:7 to obtain a low-carbon cementitious material.

[0050] Example 6

[0051] (1) placing the regenerated micropowder in a container, adding an activation solution, and mixing uniformly to obtain an impregnation mixture;

[0052] (2) placing the impregnation mixture in a reaction device, and introducing carbon dioxide gas into the reaction device, setting the temperature to 35° C. and the pressure to 7.5 MPa to obtain supercritical carbon dioxide, the carbon dioxide gas flow rate is 25 L / min, and the impregnation mixture is carbonized in a supercritical carbon dioxide environment for 3 hours;

[0053] (3) After the carbonization is completed, the pressure is released, the carbonization product is taken out, and the auxiliary cementitious material is obtained after solid-liquid separation and drying. The auxiliary cementitious material and cement are compounded in a mass ratio of 3:7 to obtain a low-carbon cementitious material.

[0054] Comparative Example 1

[0055] The cementitious material is compounded with recycled micro powder and P·Ⅱ52.5 silicate cement, and the mass ratio of recycled micro powder to cement is 3:7.

[0056] Comparative Example 2

[0057] This comparative example is set based on Example 1, the difference being that the regenerated micropowder is subjected to conventional carbon dioxide curing.

[0058] (1) placing the regenerated micropowder in a container, adding an activation solution, and mixing uniformly to obtain an impregnation mixture;

[0059] (2) placing the impregnation mixture in a reaction device, and introducing carbon dioxide gas into the reaction device, setting the temperature to 80° C., the pressure to 0.2 MPa, and the carbon dioxide concentration to 25%, and carbonizing the impregnation mixture in a carbon dioxide environment for 12 hours;

[0060] (3) After the carbonization is completed, the carbonization product is taken out, and after solid-liquid separation, it is dried to obtain an auxiliary cementitious material. The auxiliary cementitious material is compounded with cement in a mass ratio of 3:7 to obtain a low-carbon cementitious material.

[0061] Comparative Example 3

[0062] This comparative example is based on Example 1, except that no activation solution is added.

[0063] (1) placing the regenerated micropowder in a reaction device, and introducing carbon dioxide gas into the reaction device, setting the temperature to 35° C. and the pressure to 7.5 MPa to obtain supercritical carbon dioxide, the carbon dioxide gas flow rate to 25 L / min, and carbonizing the impregnated mixture in a supercritical carbon dioxide environment for 1 hour;

[0064] (2) After the carbonization is completed, the pressure is released, the carbonization product is taken out, and it is dried to obtain an auxiliary cementitious material. The auxiliary cementitious material is compounded with cement in a mass ratio of 3:7 to obtain a low-carbon cementitious material.

[0065] Performance Test:

[0066] In order to evaluate the improvement effect of the present invention on low-carbon cementitious materials, cement mortar was prepared with low-carbon cementitious materials, the activity index of the regenerated micropowder before and after supercritical carbonization treatment was evaluated, and the compressive strength of the specimens was tested at 3d, 7d, and 28d, respectively, in accordance with "Test Method for Strength of Cement Mortar (ISO Method)" GB / T 17671.

[0067] The mass mix ratio of cement mortar is: low carbon cementitious material: sand: water = 1: 3.0: 0.5, cement is P·Ⅱ52.5 cement, sand is standard sand, and water is tap water. Cement mortar is prepared according to standard curing conditions, the curing conditions are (20±2)℃, and the relative humidity is not less than 95%.

[0068] Table 2 shows the compressive strength test results of cement mortar prepared in various embodiments and comparative examples at 3d, 7d and 28d.

[0069] Table 2 Performance test results of cement mortar

[0070]

[0071] Combined with the results in Table 2, the regenerated micropowder in the cementitious material of Comparative Example 1 has not been carbonized, and its activity index is relatively low. Compared with the data of Example 1, it can be seen that the fluidity and 28d compressive strength of the cement mortar in Comparative Example 1 are much lower than those in Example 1. This is because the regenerated micropowder that has not been carbonized has a low activity index, while the regenerated micropowder that has been carbonized with supercritical carbon dioxide can convert calcium hydroxide and calcium silicate hydrate in the regenerated micropowder into calcium carbonate and silica gel, which has a higher hydration activity and can also play a better nucleation role. In addition, calcium carbonate has a denser structure, which can improve the working performance of cement-based materials and enhance the compressive strength after hardening.

[0072] Comparative Example 2 is a regenerated micropowder treated by a conventional wet carbonization process. Compared with Example 1, the fluidity and 28d compressive strength of the cement mortar in Comparative Example 2 are not as good as those in Example 1. This is because the supercritical carbon dioxide treatment method used in Example 1 can more fully carbonize the regenerated micropowder than the conventional carbonization process, and the porosity of the regenerated micropowder decreases, which weakens the effect of the decrease in the working performance of the cement-based material caused by its incorporation, and at the same time improves the mechanical properties of the cement-based material. In addition, the supercritical carbon dioxide treatment method reduces the reaction time and temperature required, shortens the cycle, increases the reaction rate, reduces the energy consumption and carbon emissions generated by high-temperature treatment, and is more conducive to improving the efficiency of carbon capture.

[0073] Both Example 1 and Comparative Example 3 use supercritical carbon dioxide for carbonization. The difference between Example 1 and Comparative Example 3 is that an activation solution is added. The activation solution can promote the dissolution of calcium ions in the regenerated micropowder, further improve the carbonization efficiency, and the working performance and mechanical strength of the prepared cement mortar are improved.

[0074] Compared with Example 1, Example 4, Example 5 and Example 6 respectively adopt the scheme of increasing temperature, pressure and extending reaction time to further accelerate the carbonization rate of supercritical carbon dioxide on regenerated micropowder, which is conducive to accelerating carbonization. The amount of regenerated micropowder has a significant impact on the performance of cement-based materials. Therefore, in practical applications, the specific process parameters of supercritical carbon dioxide curing can be adjusted according to the performance required to be achieved by the regenerated micropowder cement-based material, the replacement rate requirement of the regenerated micropowder and the energy consumption requirement.

Claims

1. A low-carbon gelling material prepared by supercritical carbon dioxide, characterized in that: The regenerated micro powder is impregnated with an activation solution and then placed in a supercritical carbon dioxide environment for carbonization to obtain an auxiliary cementitious material. The auxiliary cementitious material is compounded with cement to obtain a low-carbon cementitious material. The activation solution comprises a surfactant and a calcium ion complexing agent; the surfactant is one or more of phosphoric acid, soluble phosphate and soluble aluminum salt; the calcium ion complexing agent is one of ethylenediaminetetraacetic acid, trisodium nitrilotriacetate and triethanolamine.

2. The low-carbon gelling material prepared by supercritical carbon dioxide according to claim 1, characterized in that: The concentration of the surfactant in the activation solution is 0.01 mol / L to 1 mol / L , The calcium ion complexing agent accounts for 0.01% to 1% of the mass of the activation solution.

3. The low-carbon gelling material prepared by supercritical carbon dioxide according to claim 1, characterized in that: The mass ratio of the regenerated micro powder to the activation solution is 1:5-20.

4. The low-carbon gelling material prepared by supercritical carbon dioxide according to claim 1, characterized in that: The particle size of the regenerated micro powder is less than 0.075 mm and the specific surface area is greater than 350 m 2 / kg.

5. The low-carbon gelling material prepared by supercritical carbon dioxide according to claim 1, characterized in that: The cement is one of cement clinker, Portland cement, ordinary Portland cement, sulphoaluminate cement, high belite cement and belite sulphoaluminate cement.

6. The low-carbon gelling material prepared by supercritical carbon dioxide according to claim 1, characterized in that: The mass ratio of the auxiliary cementitious material to cement is 1:1 to 1:

9.

7. The method for preparing a low-carbon gelling material using supercritical carbon dioxide according to any one of claims 1 to 6, characterized in that: The specific steps include: (1) placing the regenerated micropowder in a container, adding an activation solution, and mixing uniformly to obtain an impregnation mixture; (2) placing the impregnation mixture in a reaction device, and introducing carbon dioxide gas into the reaction device, setting the temperature to 35-60° C. and the pressure to 7.5-10 MPa to obtain supercritical carbon dioxide, and carbonizing the impregnation mixture in a supercritical carbon dioxide environment; (3) After the carbonization is completed, the pressure is released, the carbonization product is taken out, and the auxiliary cementitious material is obtained by drying after solid-liquid separation. The auxiliary cementitious material is compounded with cement to obtain a low-carbon cementitious material.

8. The preparation method according to claim 7, characterized in that: The carbon dioxide gas in step 2 is industrial tail gas or commercial gas with a concentration of not less than 90%.

9. The preparation method according to claim 7, characterized in that: The carbon dioxide gas flow rate in step (2) is 20-50 L / min.

10. The preparation method according to claim 7, characterized in that: The carbonization reaction time in step (2) is 1-3 hours.

Citation Information

Patent Citations

  • Supercritical carbonizing circulating device for modifying cement-based building materials

    CN103172403A

  • Method for carbonizing and activating waste concrete recycled micro powder by wet process and application of regenerated micro-powder

    CN112125541A

  • Cement-based material carbonization recycling method and calcium carbonate whisker material

    CN113213498A

  • Environment-friendly artificial stone prepared from full-granularity mineralized waste cement concrete and preparation method of environment-friendly artificial stone

    CN115286307A

  • Supercritical carbonization system for granular cement-based material

    CN217068783U

Cited By

  • Cementing material in-situ reinforcing agent and early-strength all-solid waste cementing material

    CN120903865A