Ceramic substrate and preparation method and application thereof
By using specific formulas of ceramic powder and sintering aids, including magnesium borate and magnesium hydroxide, the surface uneven problem caused by oxygen impurities during the sintering process of ceramic substrates is solved, high density and flatness are achieved, and processing is simplified Steps and reduce costs.
Patent Information
- Application Number
- CN202410894583.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-08
AI Technical Summary
During the sintering process, the thermal conductivity of existing ceramic substrates is unstable due to oxygen impurities, resulting in deformation and uneven surfaces, requiring additional grinding or grinding processing, which increases costs, and large water grinding is prone to leaving gear marks and is difficult to flatten. .
The formula is 95-97% of ceramic powder and 3-5% of sintering aid, including magnesium borate and magnesium hydroxide. Magnesium borate becomes viscous fluid state at low temperatures. Magnesium hydroxide increases electrostatic repulsion, and makes ceramics synergistically The surface of the substrate is flat, the surface thickness difference does not exceed 0.01 mm, and has a high density.
The surface flatness and high density of the ceramic substrate are achieved, grinding or grinding of subsequent processing is avoided, production costs are reduced, and the mechanical strength and density of the ceramic substrate are improved.
Smart Images

Figure BDA0004928544110000051 
Figure BDA0004928544110000061 
Figure BDA0004928544110000062
Abstract
Description
Technical Field
[0001] The present invention relates to the field of ceramics, and in particular to a ceramic substrate and a preparation method and application thereof. Background Art
[0002] Ceramic substrates are widely used in the fields of integrated circuit packaging, LED lighting, heat dissipation substrates, pressure sensors, etc. in the electronic information industry because of their advantages such as thinness, high temperature resistance, high electrical insulation performance, low dielectric loss, and good chemical stability. The ceramic substrate obtained by sintering will be affected by oxygen impurities in the green body during the sintering process, and the thermal conductivity cannot be stably controlled, resulting in varying degrees of deformation and uneven surface. To obtain a ceramic substrate with a smooth surface, it is necessary to use grinding or grinding to process it, which adds additional costs. In addition, the use of large water mills to grind is likely to leave gear marks on the surface of the ceramic substrate product, and it is difficult to grind it flat with a cast iron grinder in the later stage, resulting in uneven thickness and poor flatness of the product. Summary of the invention
[0003] In order to overcome at least one technical problem existing in the above-mentioned prior art, one of the objectives of the present invention is to provide a ceramic substrate.
[0004] A second object of the present invention is to provide a method for preparing the above-mentioned ceramic substrate.
[0005] A third object of the present invention is to provide application of the above ceramic substrate in electronic products or heat dissipation substrates.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] The first aspect of the present invention provides a ceramic substrate, the raw material of the ceramic substrate includes powder, the powder includes the following components in mass percentage: 95-97% ceramic powder, 3-5% sintering aid; the sintering aid includes magnesium borate and magnesium hydroxide. Magnesium borate has a low melting point and becomes a viscous flow state at low temperature. Under capillary pressure, it can promote the rearrangement of powder particles in the ceramic substrate green body to achieve densification; -OH in magnesium hydroxide increases electrostatic repulsion, making the powder more uniform in dispersion and more compact in stacking; through the synergistic effect of magnesium borate and magnesium hydroxide, the ceramic substrate has a higher surface flatness, the surface thickness difference does not exceed 0.01mm, and has a higher density.
[0008] Preferably, the mass percentage of the ceramic powder is 96-97%.
[0009] Preferably, the mass percentage of the sintering aid is 3-4%.
[0010] Preferably, the ceramic substrate comprises the following raw materials in percentage by mass: 60-72% powder, 10-15% binder, and 18-30% solvent.
[0011] Preferably, the mass percentage of the powder is 68-70%.
[0012] Preferably, the mass percentage of the binder is 10-12%.
[0013] Preferably, the mass percentage of the solvent is 18-26%; further preferably, the mass percentage of the solvent is 20-26%.
[0014] Preferably, the total mass percentage of the magnesium borate and magnesium hydroxide is 37%-52% based on the total mass percentage of the sintering aid being 100%. Magnesium borate and magnesium hydroxide play a major role in the early stage of sintering, so the content of magnesium borate and magnesium hydroxide in the sintering aid should not be too high.
[0015] Preferably, the mass ratio of magnesium borate to magnesium hydroxide is (0.5-5.5): 1; further preferably, the mass ratio of magnesium borate to magnesium hydroxide is (1.2-2.3): 1; more preferably, the mass ratio of magnesium borate to magnesium hydroxide is (1.2-1.5): 1. When the mass ratio of magnesium borate to magnesium hydroxide is within the above range, the density of the obtained ceramic substrate is better. On the one hand, the formation of boric acid glass can be avoided, and the strength of the ceramic substrate can be improved. Excessive magnesium borate in the system can easily form boric acid glass. The presence of boric acid glass can cause the ceramic substrate to be brittle and the strength to be reduced. On the other hand, the hydroxyl group in magnesium hydroxide can be avoided from corroding the production equipment, and the service life of the production equipment can be improved. A high content of magnesium hydroxide can make the system alkaline and have a certain corrosive effect on the production equipment. If the content of magnesium hydroxide is too low, the repulsion between the powder particles is small, and the powder is easy to agglomerate. Mechanical weak points are easy to exist in the ceramic substrate, resulting in a decrease in the strength of the ceramic substrate.
[0016] Preferably, the sintering aid also includes at least one compound selected from manganese oxide, chromium oxide, magnesium oxide, and silicon oxide; the sintering aid in the present invention includes magnesium borate, magnesium hydroxide and at least one compound selected from manganese oxide, chromium oxide, magnesium oxide, and silicon oxide; further preferably, the sintering aid includes magnesium borate, magnesium hydroxide and manganese oxide.
[0017] Preferably, the amount of the magnesium borate is less than the amount of the manganese oxide.
[0018] Preferably, the ceramic powder includes at least one of α-alumina, zirconia toughened alumina ceramic powder (ZTA), and zirconia.
[0019] Preferably, the particle size of the ceramic powder is 6-8 μm.
[0020] Preferably, the solvent is selected from at least one of xylene, ethyl acetate, toluene, acetone and isopropanol; further preferably, the solvent is selected from xylene and ethyl acetate; more preferably, the mass ratio of xylene to ethyl acetate is (2-3):1.
[0021] Preferably, the binder is selected from at least one of polyvinyl alcohol, ammonium polyacrylate and polyvinyl butyral.
[0022] Preferably, the density of the ceramic substrate is greater than 3.6 cm 2 / g.
[0023] The second aspect of the present invention provides a method for preparing the ceramic substrate provided by the first aspect of the present invention, comprising the following steps:
[0024] S1: ball milling the ceramic powder for the first time to obtain ceramic powder;
[0025] S2: mixing the ceramic powder with a sintering aid and then performing a second ball milling to obtain a powder;
[0026] S3: mixing the powder, solvent and binder and then ball milling for the third time to obtain a mixed slurry;
[0027] S4: coating the mixed slurry, pressing and molding, and then sintering to obtain the ceramic substrate;
[0028] In the first ball milling step, the particle size of the grinding balls is 10 to 18 μm, the total ball milling time is 18 to 30 hours, the added mass of the grinding balls is 30 to 40% of the added mass of the ceramic powder, and the ball milling speed is 40 to 70 r / min;
[0029] In the second ball milling step, the particle size of the grinding balls is 2 to 4 μm, the total ball milling time is 10 to 20 hours, the mass of the grinding balls added is 30 to 40% of the mass of the powder, and the ball milling speed is 35 to 55 r / min;
[0030] In the third ball milling step, the total ball milling time is 15 to 20 hours, and the ball milling speed is 30 to 40 r / min.
[0031] In the preparation method of the present invention, in the first grinding step, it is necessary to control the amount of grinding balls added. If the amount of grinding balls added is too little, only part of the powder can be ground, the grinding is uneven, and the particle size distribution of the powder after grinding is likely to be uneven. If the amount of grinding balls added is too large, the friction between the grinding balls is large, the loss is large, and impurities are likely to be generated. In addition, the particle size of the grinding balls must be larger than the particle size of the ceramic powder to play a grinding role, but when the particle size of the grinding balls is too large, the gaps between the grinding balls are large, and the grinding efficiency is reduced.
[0032] In the second grinding step, the purpose of controlling the amount of grinding balls added is mainly to make the powders mix evenly. The second ball milling needs to replace the grinding balls with smaller particle sizes in order to further grind the larger particles after the first grinding so that the particle sizes of the powders become uniform.
[0033] Preferably, the grain size of the powder of the mixed slurry is 3-4 μm.
[0034] Preferably, the first ball milling is segmented ball milling, and the specific steps are: first stirring at a rotation speed of 40-50 r / min for 1-3 h; then stirring at a rotation speed of 68-70 r / min for 1-3 h, and then stirring at a rotation speed of 55-60 r / min until the material is discharged.
[0035] Preferably, the second ball milling is segmented ball milling, and the specific steps are: first stirring at a rotation speed of 35-38 r / min for 1-3 h; then stirring at a rotation speed of 50-55 r / min for 1-3 h, and then stirring at a rotation speed of 40-45 r / min until the material is discharged.
[0036] Preferably, the third ball milling is segmented ball milling, and the specific steps are: first stirring at a rotation speed of 30 to 33 r / min for 1 to 3 hours; and then stirring at 38 to 40 r / min until the material is discharged.
[0037] Preferably, the first ball milling and the second ball milling are both carried out in three stages at different rotation speeds. The reason is that the slow stirring is to mix the particles evenly first, the fast stirring is to grind away the large particles, and the medium-speed stirring is to make the particle size uniform.
[0038] Preferably, the third ball milling is carried out in two stages with different rotation speeds. The reason is that the third ball milling is to homogenize the particles of the slurry after the second ball milling, so the grinding speed used is slower than that of the second ball milling; first slowly mix evenly and then increase the speed to make the particle size uniform.
[0039] Preferably, the compression molding step is stamping molding.
[0040] Preferably, the sintering temperature is 1500-1700°C.
[0041] Preferably, the sintering time is 15-20 hours.
[0042] The third aspect of the present invention provides the use of the ceramic substrate provided by the first aspect of the present invention in electronic products or heat dissipation substrates.
[0043] Preferably, the electronic product includes an integrated circuit, an LED, and a pressure sensor.
[0044] The beneficial effects of the present invention are as follows: the surface flatness of the ceramic substrate of the present invention is good, the thickness range does not exceed 0.01 mm, and the ceramic substrate obtained after sintering does not need to be polished or ground, which can simplify the processing steps of the ceramic substrate and reduce the production cost; the ceramic substrate also has high mechanical strength and high density, specifically: Weber strength exceeds 400MPa, impact strength exceeds 420MPa, and density is greater than 3.6cm 2 / g, meeting the use requirements of high-performance, high-density and high-strength ceramic substrates.
[0045] The preparation method of the present invention controls the particle size of the grinding balls, the amount of grinding balls added, the grinding speed, the grinding time and other parameters, so that the powder grains in the obtained mixed slurry are smaller. The powder with smaller grains has a large specific surface area and high activity. After sintering the mixed slurry, a ceramic substrate with small ceramic particle size, dense grain accumulation and high surface flatness is obtained. The ceramic substrate does not need to be subsequently ground by a large water mill, has high production efficiency and low cost, and can be industrially produced in large quantities. DETAILED DESCRIPTION
[0046] The specific implementation of the present invention is further described in detail below in conjunction with examples, but the implementation and protection of the present invention are not limited thereto. It should be noted that if there are processes that are not particularly described in detail below, they can be implemented or understood by those skilled in the art with reference to the prior art. The reagents or instruments used that do not indicate the manufacturer are all conventional products that can be purchased commercially.
[0047] The raw material information used in the examples and comparative examples of the present invention is as follows:
[0048] The ceramic powder is α-alumina, and the particle size of the ceramic powder is 6 μm;
[0049] The solvent is a mixture of xylene and ethyl acetate in a mass ratio of 2:1;
[0050] The binder is polyvinyl alcohol.
[0051] Embodiment 1:
[0052] This example provides a ceramic substrate, and its formula is shown in Table 1 below. The ceramic substrate in this example is made of the following raw materials in mass percentage: 69% powder, 21% solvent, and 10% binder; the formula of the powder is shown in Table 2 below, specifically: the powder is composed of 96.5% ceramic powder and 3.5% sintering aid by mass, the ceramic powder is α-alumina, and the particle size of the ceramic powder is 6μm. The formula of the sintering aid is shown in Table 3 below, which is a mixture of magnesium borate, magnesium hydroxide and manganese oxide, wherein the mass of magnesium borate and magnesium hydroxide accounts for 43% of the total mass of the sintering aid, and the mass ratio of magnesium borate to magnesium hydroxide is 1.25:1; the solvent is a mixture of xylene and ethyl acetate in a mass ratio of 2:1, and the binder is polyvinyl alcohol.
[0053] The ceramic substrate in this example is prepared by the following preparation method, the specific steps are:
[0054] (1) First ball milling: Ceramic powder was added to a ball mill with a grinding ball particle size of 10 μm for ball milling for a total ball milling time of 20 h to obtain powder A. The mass of the grinding balls added was 30% of the mass of the ceramic powder added; the specific ball milling steps were: first, stirring slowly at a speed of 50 r / min for 2 h, then stirring quickly at a speed of 70 r / min for 2 h, and finally stirring at a speed of 55 r / min for 16 h before discharging;
[0055] (2) Second ball milling: Add sintering aid to powder A; ball mill in a ball mill with a grinding ball particle size of 3 μm for a total ball milling time of 20 hours to obtain powder B. The mass of the grinding balls added is 40% of the mass of the powder. The ball milling needs to be segmented. The specific ball milling steps are: first, stir slowly at a speed of 35 r / min for 2 hours, then stir quickly at a speed of 55 r / min for 2 hours, and finally stir at a speed of 40 r / min for 16 hours before discharging;
[0056] (3) The third ball milling: Solvent and binder were added to powder B in sequence, and the ball milling was continued for a total of 20 h to obtain slurry C. The specific ball milling steps were: stirring slowly at a speed of 30 r / min for 2 h, and then stirring at a speed of 38 r / min for 18 h, and then discharging.
[0057] (4) Molding: After the slurry C is coated on a coating machine, it is punched and formed using a manual punching machine to obtain a semi-finished ceramic substrate.
[0058] (5) Sintering: After sintering at a sintering temperature of 1650° C. for 15 h, the finished ceramic substrate in this example was obtained.
[0059] Table 1 Ceramic substrate formulation (mass percentage / %)
[0060]
[0061]
[0062] Table 2 Powder formula (mass percentage / %)
[0063] Powder Type Ceramic powder content Sintering aid content Types of sintering aids F1 96.5 3.5 S3 F2 97 3 S3 F3 96 4 S3 F4 95 5 S3 F5 96.5 3.5 S1 F6 96.5 3.5 S2 F7 96.5 3.5 S4 F8 96.5 3.5 S5 F9 96.5 3.5 S6 F10 96.5 3.5 S7 F11 96.5 3.5 S8 F12 96.5 3.5 S9 F13 96.5 3.5 S10 F14 96.5 3.5 S11 F15 96.5 3.5 S12 F16 96.5 3.5 S13 F17 96.5 3.5 S14 F18 96.5 3.5 S15 F19 96.5 3.5 S16 F20 96.5 3.5 S17 F21 96.5 3.5 S18 F22 96.5 3.5 S19 F23 96.5 3.5 S20 F24 93 7 S3 F25 98 2 S3 F26 96.5 3.5 S21 F27 96.5 3.5 S22
[0064] Table 3 Formulation of sintering aids
[0065]
[0066]
[0067] Embodiments 2 to 26
[0068] The formulations of the ceramic substrates provided in Examples 2 to 26 are shown in Table 1, respectively. The formulations of the powders used in the formulations of the ceramic substrates are shown in Table 2. The formulations of the sintering aids used are shown in Table 3.
[0069] The ceramic substrates provided in Examples 2 to 26 can all be prepared using the preparation method in Example 1.
[0070] Comparative Examples 1 to 6
[0071] The formulas of the ceramic substrates provided in Comparative Examples 1 to 6 are shown in Table 1, respectively. The formulas of the powders used in the ceramic substrate formulas are shown in Table 2. The formulas of the sintering aids used are shown in Table 3.
[0072] The ceramic substrates provided in Comparative Examples 1 to 6 can all be prepared using the preparation method in Example 1.
[0073] Embodiment 27
[0074] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0075] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that the total ball milling time in the first ball milling step in this example is 18 hours, and the specific ball milling steps are: first, slowly stir at a speed of 50 r / min for 2 hours, then quickly stir at a speed of 70 r / min for 2 hours, and finally stir at a speed of 55 r / min for 14 hours to discharge the material.
[0076] Embodiment 28
[0077] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0078] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that the total ball milling time in the first ball milling step in this example is 30 hours, and the specific ball milling steps are: first, slowly stir at a speed of 50 r / min for 2 hours, then quickly stir at a speed of 70 r / min for 2 hours, and finally stir at a speed of 55 r / min for 26 hours before discharging.
[0079] Embodiment 29
[0080] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0081] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that the mass of the grinding balls added in the first ball milling in this example is 40% of the mass of the ceramic powder added.
[0082] Embodiment 30
[0083] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0084] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that the mass of the grinding balls added in the first ball milling in this example is 35% of the mass of the ceramic powder added.
[0085] Embodiment 31
[0086] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0087] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that: in the first ball milling step in this example, the specific ball milling steps are: first slowly stirring at a speed of 40 r / min for 2 hours, then rapidly stirring at 70 r / min for 2 hours, and finally continuing to stir at 55 r / min for 16 hours before discharging.
[0088] Embodiment 32
[0089] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0090] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that: in the first ball milling step in this example, the specific ball milling steps are: first slowly stirring at a speed of 45 r / min for 2 hours, then rapidly stirring at 70 r / min for 2 hours, and finally continuing to stir at 55 r / min for 16 hours before discharging.
[0091] Embodiment 33
[0092] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0093] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that: in the first ball milling step in this example, the specific ball milling steps are: first slowly stirring at a speed of 50 r / min for 2 hours, then rapidly stirring at 68 r / min for 2 hours, and finally continuing to stir at 55 r / min for 16 hours before discharging.
[0094] Embodiment 34
[0095] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0096] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that: in the first ball milling step in this example, the specific ball milling steps are: first slowly stirring at a speed of 50 r / min for 2 hours, then rapidly stirring at 70 r / min for 2 hours, and finally continuing to stir at 60 r / min for 16 hours before discharging.
[0097] Embodiment 35
[0098] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0099] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that: in the first ball milling step in this example, the specific ball milling steps are: first slowly stirring at a speed of 50 r / min for 2 hours, then rapidly stirring at 70 r / min for 2 hours, and finally continuing to stir at 58 r / min for 16 hours before discharging.
[0100] Embodiment 36
[0101] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0102] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that the particle size of the grinding balls in the second ball milling step in this example is 4 μm.
[0103] Embodiment 37
[0104] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0105] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that the particle size of the grinding balls in the second ball milling step in this example is 2 μm.
[0106] Embodiment 38
[0107] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0108] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that the mass of the grinding balls added in the second ball milling step in this example is 30% of the mass of the powder.
[0109] Embodiment 39
[0110] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0111] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that in the second ball milling step in this example, the specific ball milling steps are: first slowly stirring at a speed of 38 r / min for 2 hours, then rapidly stirring at 55 r / min for 2 hours, and finally continuing to stir at 40 r / min for 16 hours before discharging.
[0112] Embodiment 40
[0113] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0114] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that in the second ball milling step in this example, the specific ball milling steps are: first slowly stirring at a speed of 35 r / min for 2 hours, then rapidly stirring at 50 r / min for 2 hours, and finally continuing to stir at 40 r / min for 16 hours before discharging.
[0115] Embodiment 41
[0116] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0117] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that: in the second ball milling step in this example, the specific ball milling steps are: first slowly stirring at a speed of 35 r / min for 2 hours, then rapidly stirring at 55 r / min for 2 hours, and finally continuing to stir at 45 r / min for 16 hours before discharging.
[0118] Embodiment 42
[0119] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0120] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that in the second ball milling step in this example, the specific ball milling steps are: first slowly stirring at a speed of 35 r / min for 2 hours, then rapidly stirring at 55 r / min for 2 hours, and finally continuing to stir at 43 r / min for 16 hours before discharging.
[0121] Embodiment 43
[0122] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0123] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that in the third ball milling step in this example, the specific ball milling steps are: slowly stirring at a rotation speed of 33 r / min for 2 hours, then continuing to stir at 38 r / min for 18 hours, and discharging.
[0124] Embodiment 44
[0125] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0126] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that in the third ball milling step in this example, the specific ball milling steps are: slowly stirring at a rotation speed of 30 r / min for 2 hours, then continuing to stir at 40 r / min for 18 hours, and discharging.
[0127] Embodiment 45
[0128] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0129] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that the total grinding time in the third ball milling step in this example is 15 hours, and the specific ball milling steps are: slow stirring at a speed of 30 r / min for 2 hours, and then continuing to stir at a speed of 38 r / min for 13 hours, and discharging.
[0130] Embodiment 46
[0131] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0132] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that the total grinding time in the third ball milling step in this example is 18 hours, and the specific ball milling steps are: slow stirring at a speed of 30 r / min for 2 hours, and then continuing to stir at a speed of 38 r / min for 16 hours, and discharging.
[0133] Comparative Example 7
[0134] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0135] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that the total grinding time in the first ball milling step in this example is 15 hours, and the specific ball milling steps are: first slowly stirring at a speed of 50 r / min for 2 hours, then quickly stirring at a speed of 70 r / min for 2 hours, and finally stirring at a speed of 55 r / min for 11 hours to discharge the material.
[0136] Comparative Example 8
[0137] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0138] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that the total grinding time in the first ball milling step in this example is 40 hours, and the specific ball milling steps are: first, slowly stir at a speed of 50 r / min for 2 hours, then quickly stir at a speed of 70 r / min for 2 hours, and finally stir at a speed of 55 r / min for 36 hours before discharging.
[0139] Comparative Example 9
[0140] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0141] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that the mass of the grinding balls added in the first ball milling in this example is 20% of the mass of the ceramic powder added.
[0142] Comparative Example 10
[0143] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0144] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that the mass of the grinding balls added in the first ball milling in this example is 50% of the mass of the ceramic powder added.
[0145] Comparative Example 11
[0146] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0147] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that: in the first ball milling step in this example, the specific ball milling steps are: first slowly stirring at a speed of 30 r / min for 2 hours, then rapidly stirring at 70 r / min for 2 hours, and finally continuing to stir at 55 r / min for 16 hours before discharging.
[0148] Comparative Example 12
[0149] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0150] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that: in the first ball milling step in this example, the specific ball milling steps are: first slowly stirring at a speed of 60 r / min for 2 hours, then rapidly stirring at 70 r / min for 2 hours, and finally continuing to stir at 55 r / min for 16 hours before discharging.
[0151] Comparative Example 13
[0152] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0153] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that: in the first ball milling step in this example, the specific ball milling steps are: first slowly stirring at a speed of 50 r / min for 2 hours, then rapidly stirring at 65 r / min for 2 hours, and finally continuing to stir at 55 r / min for 16 hours before discharging.
[0154] Comparative Example 14
[0155] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0156] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that: in the first ball milling step in this example, the specific ball milling steps are: first slowly stirring at a speed of 50 r / min for 2 hours, then rapidly stirring at 75 r / min for 2 hours, and finally continuing to stir at 55 r / min for 16 hours before discharging.
[0157] Comparative Example 15
[0158] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0159] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that: in the first ball milling step in this example, the specific ball milling steps are: first slowly stirring at a speed of 50 r / min for 2 hours, then rapidly stirring at 70 r / min for 2 hours, and finally continuing to stir at 50 r / min for 16 hours before discharging.
[0160] Comparative Example 16
[0161] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0162] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that: in the first ball milling step in this example, the specific ball milling steps are: first slowly stirring at a speed of 50 r / min for 2 hours, then rapidly stirring at 70 r / min for 2 hours, and finally continuing to stir at 65 r / min for 16 hours before discharging.
[0163] Comparative Example 17
[0164] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0165] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that the particle size of the grinding balls in the second ball milling step in this example is 5 μm.
[0166] Comparative Example 18
[0167] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0168] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that the particle size of the grinding balls in the second ball milling step in this example is 1 μm.
[0169] Comparative Example 19
[0170] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0171] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that the mass of the grinding balls added in the second ball milling step in this example is 20% of the mass of the powder.
[0172] Comparative Example 20
[0173] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0174] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that the mass of the grinding balls added in the second ball milling step in this example is 50% of the mass of the powder.
[0175] Comparative Example 21
[0176] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0177] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that in the second ball milling step in this example, the specific ball milling steps are: first slowly stirring at a speed of 30 r / min for 2 hours, then rapidly stirring at 55 r / min for 2 hours, and finally continuing to stir at 40 r / min for 16 hours before discharging.
[0178] Comparative Example 22
[0179] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0180] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that: in the second ball milling step in this example, the specific ball milling steps are: first slowly stirring at a speed of 45 r / min for 2 hours, then rapidly stirring at 55 r / min for 2 hours, and finally continuing to stir at 40 r / min for 16 hours before discharging.
[0181] Comparative Example 23
[0182] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0183] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that in the second ball milling step in this example, the specific ball milling steps are: first slowly stirring at a speed of 35 r / min for 2 hours, then rapidly stirring at 45 r / min for 2 hours, and finally continuing to stir at 40 r / min for 16 hours before discharging.
[0184] Comparative Example 24
[0185] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0186] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that in the second ball milling step in this example, the specific ball milling steps are: first slowly stirring at a speed of 35 r / min for 2 hours, then rapidly stirring at 60 r / min for 2 hours, and finally continuing to stir at 40 r / min for 16 hours before discharging.
[0187] Comparative Example 25
[0188] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0189] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that in the second ball milling step in this example, the specific ball milling steps are: first slowly stirring at a speed of 35 r / min for 2 hours, then rapidly stirring at 55 r / min for 2 hours, and finally continuing to stir at 30 r / min for 16 hours before discharging.
[0190] Comparative Example 26
[0191] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0192] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that: in the second ball milling step in this example, the specific ball milling steps are: first slowly stirring at a speed of 35 r / min for 2 hours, then rapidly stirring at 55 r / min for 2 hours, and finally continuing to stir at 55 r / min for 16 hours before discharging.
[0193] Comparative Example 27
[0194] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0195] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that in the third ball milling step in this example, the specific ball milling steps are: slowly stirring at a rotation speed of 20 r / min for 2 hours, then continuing to stir at 38 r / min for 18 hours, and discharging.
[0196] Comparative Example 28
[0197] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0198] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that in the third ball milling step in this example, the specific ball milling steps are: slowly stirring at a rotation speed of 40 r / min for 2 hours, then continuing to stir at 38 r / min for 18 hours, and discharging.
[0199] Comparative Example 29
[0200] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0201] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that in the third ball milling step in this example, the specific ball milling steps are: slowly stirring at a rotation speed of 30 r / min for 2 hours, then continuing to stir at 35 r / min for 18 hours, and discharging.
[0202] Comparative Example 30
[0203] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0204] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that in the third ball milling step in this example, the specific ball milling steps are: slowly stirring at a rotation speed of 30 r / min for 2 hours, then continuing to stir at 50 r / min for 18 hours, and discharging.
[0205] Comparative Example 31
[0206] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0207] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that the total grinding time in the third ball milling step in this example is 10 hours, first slowly stirring at a speed of 30 r / min for 2 hours, and then continuing to stir at a speed of 38 r / min for 8 hours until the material is discharged.
[0208] Comparative Example 32
[0209] The formula of the ceramic substrate in this example is the same as that in Example 1.
[0210] The preparation method of the ceramic substrate in this example is different from that in Example 1 only in that the total grinding time in the third ball milling step in this example is 30 hours, first slowly stirring at a speed of 30 r / min for 2 hours, and then continuing to stir at a speed of 38 r / min for 28 hours until the material is discharged.
[0211] Performance Testing
[0212] The following properties of the semi-finished ceramic substrates and finished ceramic substrates in Examples 1 to 46 and Comparative Examples 1 to 32 were tested respectively according to the following test methods. The specific test results are recorded in Table 4.
[0213] (1) Flatness of finished product: Based on the nine-point thickness measurement of the surface of the ceramic substrate, the thickness difference within a single piece is required to be ≤0.01mm;
[0214] (2) Density: Use a gas densitometer to test the density of semi-finished and finished ceramic substrates. The requirement is that the density of the finished product is greater than 3.6 cm 2 / g; the density of semi-finished products is greater than 2cm 2 / g 2 ;
[0215] (3) Impact strength of finished product: The impact strength is tested using a flexure tester, and the impact strength is required to be greater than 350 MPa;
[0216] (4) Weber strength of finished product: Weber strength refers to the strength value under the Weber function. The mechanical strength of the finished product is tested using a universal material testing machine, and then the Weber strength is analyzed using the Weber function. The Weber strength is required to be greater than 350 MPa.
[0217] (5) Grain size test method: Use a laser particle size analyzer to test the grains. Add 0.01 g of the test powder (i.e., the powder in slurry C obtained after the third ball milling) to 50 mL of analytical pure alcohol and perform ultrasonic treatment for 5 minutes. Then, add the test powder to the laser particle size analyzer for testing. The grain size is required to be 3-4 μm to be qualified. If the grain size is smaller than 3 μm, the particles are prone to agglomeration and the strength is reduced.
[0218] Table 4 Performance test results of semi-finished ceramic substrates and finished ceramic substrates
[0219]
[0220]
[0221]
[0222] As shown in Table 4, compared with Example 1, Examples 1 to 6 change the type of powder and the type of sintering aid in the powder, and Examples 7 to 32 change the parameters in the first ball milling, the second ball milling, or the third ball milling step. At least one of the flatness of the obtained ceramic substrate, the density of the semi-finished product, the density of the finished product, the Weber strength, the impact strength, and the grain size cannot meet the use requirements of the ceramic substrate. Compared with Examples 1 to 32, Examples 1 to 46 optimize the type of powder, the type of sintering aid in the powder, the parameters in the first ball milling, the second ball milling, or the third ball milling step, so that the grain size of the ceramic slurry obtained after the three ball milling steps is small, between 3 and 4 μm, and not easy to agglomerate. The various properties of the ceramic substrate obtained using the ceramic slurry are all excellent, specifically: the flatness is less than 0.01 mm, with excellent flatness; the density of the semi-finished product is 2 to 2.87 cm 2 / g 2 The density of the finished product is 3.6~3.81cm 2 / g, with high density; Weber strength is 400-495MPa, impact strength is >420MPa, and it has excellent mechanical properties.
[0223] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
Claims
1. A ceramic substrate, characterized in that: The raw material of the ceramic substrate includes powder, and the powder includes the following components in mass percentage: 95-97% of ceramic powder and 3-5% of sintering aid; the sintering aid includes magnesium borate and magnesium hydroxide.
2. The ceramic substrate according to claim 1, characterized in that: The ceramic substrate comprises the following raw materials in percentage by mass: 60-72% of powder, 10-15% of binder and 18-30% of solvent.
3. The ceramic substrate according to claim 2, characterized in that: Taking the total mass percentage of the sintering aid as 100%, the total mass percentage of the magnesium borate and magnesium hydroxide is 37%-52%.
4. The ceramic substrate according to claim 2 or 3, characterized in that: The mass ratio of the magnesium borate to the magnesium hydroxide is (0.5-5.5):
1.
5. The ceramic substrate according to claim 4, characterized in that: The mass ratio of the magnesium borate to the magnesium hydroxide is (1.2-2.3):
1.
6. The ceramic substrate according to claim 2, characterized in that: The sintering aid also includes at least one compound selected from manganese oxide, chromium oxide, magnesium oxide, and silicon oxide.
7. The ceramic substrate according to claim 2, characterized in that: The ceramic powder includes at least one of α-alumina, zirconia toughened alumina ceramic powder, and zirconia; And / or, the particle size of the ceramic powder is 6-8 μm.
8. The method for preparing a ceramic substrate according to any one of claims 2 to 7, characterized in that: The following steps are involved: S1: ball milling the ceramic powder for the first time to obtain ceramic powder; S2: mixing the ceramic powder with a sintering aid and then performing a second ball milling to obtain a powder; S3: mixing the powder, solvent and binder and then ball milling for the third time to obtain a mixed slurry; S4: coating the mixed slurry, pressing and molding, and then sintering to obtain the ceramic substrate; In the first ball milling step, the particle size of the grinding balls is 10 to 18 μm, the total ball milling time is 18 to 30 hours, the added mass of the grinding balls is 30 to 40% of the added mass of the ceramic powder, and the ball milling speed is 40 to 70 r / min; In the second ball milling step, the particle size of the grinding balls is 2 to 4 μm, the total ball milling time is 10 to 20 hours, the mass of the grinding balls added is 30 to 40% of the mass of the powder, and the ball milling speed is 35 to 55 r / min; In the third ball milling step, the total ball milling time is 15 to 20 hours, and the ball milling speed is 30 to 40 r / min.
9. The method for preparing a ceramic substrate according to claim 8, characterized in that: The first ball milling is a segmented ball milling, and the specific steps are: first stirring at a speed of 40 to 50 r / min for 1 to 3 hours; then stirring at a speed of 68 to 70 r / min for 1 to 3 hours, and then stirring at a speed of 55 to 60 r / min until the material is discharged; and / or, The second ball milling is a segmented ball milling, and the specific steps are: first stirring at a speed of 35 to 38 r / min for 1 to 3 hours; then stirring at a speed of 50 to 55 r / min for 1 to 3 hours, and then stirring at a speed of 40 to 45 r / min until the material is discharged; and / or, The third ball milling is segmented ball milling, and the specific steps are: first stirring at a rotation speed of 30 to 33 r / min for 1 to 3 hours; and then stirring at 38 to 40 r / min until the material is discharged.
10. Use of the ceramic substrate according to any one of claims 1 to 7 in electronic products or heat dissipation substrates.
Citation Information
Patent Citations
High-purity ultrathin high-strength aluminum oxide ceramic substrate as well as preparation method and application thereof
CN114538900A
Cited By
Preparation method of pressureless sintered silicon carbide granulation powder and silicon carbide bulletproof ceramic
CN120864888A
A pressureless sintering silicon carbide granulated powder and a preparation method of silicon carbide bulletproof ceramic
CN120864888B