Preparation method of reprocessable thermosetting plastic of polyhydric alcohol cross-linked cellulose
By oxidizing cellulose by sodium periodate and crosslinking with polyols to construct acetal/hemiacetal dynamic covalent bonds, reprocessable cellulose thermosetting plastics are generated, which solves the problem of difficult reprocessing of thermosetting materials and waste of resources, and realizes the problem of the difficulty of reprocessing of thermosetting materials and the problem of waste of resources. Environmentally friendly, biodegradable high-performance plastic materials.
Patent Information
- Application Number
- CN202410988513.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-08
AI Technical Summary
Existing thermosetting plastics are difficult to reprocess and use, resulting in waste of resources and environmental pollution. In addition, traditional cellulose esters require the addition of a large amount of plasticizer, which may lead to the exudation of plasticizers and limit their application scope.
Cellulose is converted into bialdehyde cellulose through mild conditions of sodium periodate, and cross-linking of acetal/hemiacetal dynamic covalent bonds is constructed by cross-linking with polyols to generate reprocessable cellulose thermosetting plastics. Weak the hydrogen bond network and improve the mobility and mechanical properties of the cellulose chain.
It realizes the high-temperature reprocessing properties and excellent thermal stability and mechanical properties of cellulose plastics, avoids the risk of plasticizer leakage, solves the problems of difficult recycling and resource waste in traditional thermosetting materials, and provides environmentally friendly and degradable New plastic materials.
Smart Images

Figure CN118909149A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of bio-based thermosetting plastic preparation, and relates to a method for preparing a reprocessable thermosetting plastic of polyol cross-linked cellulose. Background Art
[0002] Plastics have been widely used in every corner of modern society due to their advantages such as low cost, light weight, good formability, high mechanical stability and environmental stability, and good barrier ability to gases and liquids. It is estimated that by 2025, the global plastic production will exceed 500 million tons. According to different structural characteristics, plastics can be simply divided into two categories: thermoplastics and thermosetting plastics. Due to the linear molecular structure, thermoplastics can soften and flow after heating, and can be repeatedly plasticized and formed. At present, the top few in the production scale and market share of plastics are all thermoplastics, including polyethylene (PE), polypropylene (PP), polyvinyl chloride (PVC) and polystyrene (PS). Thermosetting plastics usually refer to linear molecular chains that have been cross-linked to form a cross-linked network structure. Compared with thermoplastic materials, they have better solvent corrosion resistance, thermal stability and mechanical properties, but they cannot be melted or dissolved after heating. Therefore, once cross-linked and cured, it is difficult to reprocess and reuse. Thermosetting resins are mainly phenolic resins, urea-formaldehyde resins, and epoxy resins. Discarded thermosetting plastics can usually only be incinerated or landfilled, which can easily cause huge pollution to the ecological environment and waste resources. In order to reduce plastic pollution, one of the most promising solutions is to develop new processable plastic materials using renewable, degradable and cheap raw materials.
[0003] Cellulose is the most abundant renewable and biodegradable biopolymer and is considered one of the most promising plastic substitutes. However, natural cellulose is difficult to heat-process like traditional plastics due to its abundant and strong hydrogen bonding interactions, which leads to a high crystalline structure and low mobility of the cellulose molecular chain. The processability of cellulose can be improved by chemical modification to replace the hydroxyl groups on the cellulose molecular chain. For example, the synthesis and commercialization of cellulose esters (such as cellulose acetate) have been going on for more than a century. However, these cellulose esters cannot be directly heat-processed and usually require the addition of a large amount (about 30%) of plasticizers. The added plasticizer may gradually seep out over time, which not only affects the reprocessability of cellulose plastics, but also the toxic plasticizer that seeps out may limit its application in food packaging, children's toys and other fields. Therefore, it is urgent to develop new preparation methods for environmentally friendly cellulose plastics. Summary of the invention
[0004] In order to solve the technical problems such as the difficulty in recycling existing waste thermosetting materials, causing serious waste of resources and environmental pollution, the present invention proposes a method for preparing a reprocessable thermosetting plastic of polyol cross-linked cellulose. First, cellulose is converted into dialdehyde cellulose (DAC) under mild conditions using sodium periodate, and then DAC is cross-linked with polyols to construct a heat-processable cellulose thermosetting plastic (ACC). The hydroxyl groups of the polyol react with the aldehyde groups of the DAC to generate a cross-linked network structure with acetal / hemiacetal dynamic covalent bonds as cross-linking sites. The acetal dynamic covalent bonds partially replace the strong hydrogen bond network of the original cellulose, weakening the constraints of hydrogen bonds on the movement of cellulose chains. The formation of the cross-linked network makes the ACC plastic have solvent resistance, thermal stability and excellent mechanical properties close to those of traditional thermosetting materials, and the reversible exchange reaction of acetal dynamic covalent bonds at high temperature gives the cellulose chain excellent mobility, so that it can be reprocessed at 90°C. The present invention solves the problem that traditional thermosetting materials are difficult to recycle and use petroleum-based chemicals as raw materials for environmental pollution; at the same time, it solves the problem of resource waste and ecological pollution caused by the difficulty in degrading waste polymers.
[0005] The technical solution of the present invention:
[0006] A method for preparing a reprocessable thermosetting plastic of polyol cross-linked cellulose, comprising the following steps:
[0007] Step 1: Add the cellulose raw material and sodium periodate into solvent A according to the mass ratio, stir the reaction in a dark environment, and then purify it by centrifugation or dialysis.
[0008] The mass ratio of the cellulose raw material to sodium periodate is in the range of 1:0.3-1:1.4.
[0009] The reaction temperature ranges from 30°C to 50°C.
[0010] The reaction time ranges from 3h to 9h.
[0011] The solvent A is one of water, ethanol, acetone and methanol or a mixture of two or more thereof.
[0012] The cellulose raw material is cellulose powder and one or a mixture of two or more of wood, cotton, cotton linter, wheat straw, rice straw, reed, hemp, mulberry bark, paper mulberry bark and bagasse with a cellulose mass content higher than 60%.
[0013] Step 2: Add dialdehyde cellulose and polyol into solvent B according to a certain molar ratio of aldehyde group to hydroxyl group, pre-crosslink in an oil bath, and then transfer to an oven for post-curing. The solvent is recovered and reused by condensation.
[0014] The molar ratio of aldehyde group to hydroxyl group is 1:1-1:4.
[0015] The pre-crosslinking temperature ranges from 90°C to 120°C.
[0016] The pre-crosslinking time ranges from 1h to 6h.
[0017] The post-curing temperature range is 100℃-150℃.
[0018] The post-curing time ranges from 3h to 10h.
[0019] The solvent B is one or a mixture of two or more of dimethyl sulfoxide, N-N-dimethylacetamide, N-N-dimethylformamide, ionic liquid, low eutectic solvent, alkali-urea system, LiCl / N,N-dimethylacetamide, NMMO, cuprammonia solution, molten salt, and quaternary ammonium salt dissolution system.
[0020] The polyol is an alcohol containing two or more hydroxyl groups, specifically one or a mixture of two or more of pentaerythritol, dipentaerythritol, glycerol, decaglycerol, pentanediol, ethylene glycol, propylene glycol, butylene glycol, hexylene glycol, xylitol, and sorbitol.
[0021] Beneficial effects of the present invention:
[0022] The present invention discloses a method for preparing a reprocessable thermosetting plastic of polyol cross-linked cellulose. By oxidizing cellulose with sodium periodate under mild conditions, 1) active aldehyde groups are introduced, which can be used as cross-linking sites. 2) The hydrogen bonds of cellulose are weakened, and the mobility of cellulose chains under heating conditions is improved. 3) The anhydrous glucose ring structure of the cellulose chain is destroyed by oxidation, and the flexibility of the cellulose chain is improved. A cross-linked network with acetal and hemiacetal bonds as cross-linking sites is generated by cross-linking dialdehyde cellulose with cheap and readily available polyols. The material has excellent solvent resistance, thermal stability and mechanical properties at room temperature. When heated, the chain segments of the material can move freely due to the reversible exchange reaction of the internal acetal dynamic covalent bonds, so the material can be reprocessed like a thermoplastic on a macroscopic scale. The present invention can alleviate the environmental pollution problem caused by the difficulty in recycling traditional thermosetting materials and reduce the dependence on non-renewable fossil resources by utilizing non-food biomass resources.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] 1. The raw material cellulose used in the present invention has good biocompatibility, is widely available, inexpensive, non-toxic and biodegradable. Therefore, it is a thermosetting bio-based polymer material that is sustainable and environmentally friendly.
[0025] 2. The present invention is the first to use cheap and readily available polyols as crosslinking agents for dialdehyde-modified cellulose to prepare cellulose thermosetting plastics that can be reprocessed based on acetal dynamic covalent bonds. The preparation method of the present invention is simple and efficient, with mild conditions, limited chemical pollution, and no impact on the environment.
[0026] 3. The cellulose plastic prepared by the present invention replaces the cellulose hydrogen bond network with acetal dynamic covalent bonds, without the need to add additional plasticizers, thus avoiding the risk of plasticizer leakage. In addition, the dynamic covalent bond cross-linking strategy enables the material to have excellent thermal and mechanical properties at room temperature while taking into account the reprocessability under high temperature conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is the preparation principle diagram of cellulose plastic (ACC)
[0028] Figure 2 is the infrared spectrum of dialdehyde cellulose (DAC) in Example 1;
[0029] Figure 3 is the XRD spectrum of dialdehyde cellulose (DAC) in Example 1;
[0030] Figure 4 is the infrared spectrum of the cellulosic plastic (ACC) in Example 1;
[0031] Figure 5 is the XRD spectrum of the cellulose plastic (ACC) in Example 1;
[0032] Figure 6 is the DMA curve of the cellulosic plastic (ACC) in Example 1;
[0033] Figure 7 is the TGA curve of the cellulosic plastic (ACC) in Example 1 in a nitrogen atmosphere;
[0034] Figure 8 It is a schematic diagram of the tensile strength of the cellulose plastic (ACC) in Example 1 after being reshaped ten times. DETAILED DESCRIPTION
[0035] The specific implementation of the present invention is further described below in conjunction with the accompanying drawings and technical solutions.
[0036] Embodiment 1:
[0037] 5g of cellulose and 7g of sodium periodate (mass ratio of 1:1.4) were placed in 250mL of deionized water and stirred at 30℃ for 9h. The entire oxidation process was kept in the dark to avoid the decomposition of sodium periodate. After the oxidation was completed, it was centrifuged three times with deionized water and then dialyzed until the remaining iodide was removed. The product was freeze-dried to obtain dialdehyde cellulose (DAC). The aldehyde content of DAC was titrated using the hydroxylamine hydrochloride method, and the aldehyde content of DAC was 6.6mmol / g.
[0038] 2 g DAC and 1.12 g dipentaerythritol crosslinker (the molar ratio of aldehyde to hydroxyl is 1:2) were added to 100 °C DMSO and dissolved completely, then heated to 110 °C for pre-crosslinking for 2 h, then transferred to a 110 °C oven for post-curing for 10 h, and finally hot-pressed at 150 °C for 20 min to completely cure the sample to obtain cellulose plastic (ACC).
[0039] Combined with the attached drawings: Figure 1 The schematic diagram of the preparation of cellulose plastics is that dialdehyde cellulose is prepared by periodic acid oxidation, and then the dialdehyde cellulose is cross-linked with polyol to obtain a cellulose thermosetting plastic based on acetal dynamic covalent bonds as cross-linking sites. At room temperature, the cellulose plastic of the present invention has a stability close to that of traditional thermosetting plastics, and after heating, the reversible bond exchange of acetal bonds is stimulated, which gives the cellulose plastic reprocessability. Figure 2 This is the infrared spectrum of cellulose and dialdehyde cellulose (DAC). The infrared spectrum of DAC is 1730cm -1 A relatively obvious characteristic peak belonging to the aldehyde group appeared at the cellulose surface, indicating that aldehyde groups were introduced by oxidation of cellulose with periodic acid. Figure 3 Figure 2 is the XRD spectrum of cellulose and DAC. The XRD diffraction peak intensity of DAC is weaker than that of the original cellulose, indicating that the oxidation process destroys the regular structure of cellulose, weakens the hydrogen bonds of cellulose, and destroys some of the crystalline areas of cellulose. Figure 4 This is the infrared spectrum of the cellulose plastic ACC. Aldehyde groups (1730 cm -1 ) indicates that the aldehyde groups of dialdehyde cellulose have been consumed during the curing process due to the reaction with the hydroxyl groups of the cross-linking agent, and the sample has been completely cured. Figure 5 This is the XRD spectrum of ACC. The XRD diffraction peak intensity of ACC is further reduced compared with that of DAC. This is because the introduction of the cross-linking agent leads to further destruction of the hydrogen bond network.
[0040] The rich hydrogen bond network of original cellulose makes it difficult to dissolve in conventional solvents, while DAC can be dissolved in many extremely organic solvents such as DMSO due to the destruction of some hydrogen bonds. After DAC is cross-linked with polyols, the formation of a cross-linked network makes it difficult for cellulose plastic molecules to disperse in solvents, so it is insoluble in organic solvents such as DMSO. Cellulose plastic has excellent resistance to solvent erosion. Figure 6 This is the dynamic thermomechanical analysis curve of ACC. The glass transition temperature of cellulose plastic is 78℃. Figure 7 is the TGA curve of ACC, the initial degradation temperature of cellulose plastic (T d5% ) is 263°C, and has relatively good thermal stability. Once a traditional thermosetting plastic forms a cross-linked network, it is difficult to heat, melt and dissolve, and thus loses its reprocessing performance. The cellulose plastic prepared by the present invention contains acetal-type dynamic covalent bonds in the cross-linked network, which can undergo a reversible exchange reaction and achieve the rearrangement of the cross-linked network. Therefore, ACC can be repeatedly reprocessed like thermoplastics. ACC powder can be restored to a dense film after hot pressing at 90°C for 15 minutes, showing excellent reprocessing performance. The reprocessing conditions of the cellulose plastic prepared by the present invention are lower than the current reprocessing temperature of cellulose esters (>150°C), which can save energy losses caused by the reprocessing process and reduce production costs. Figure 8 It shows that ACC still has excellent mechanical properties after 10 reshaping processes, with a tensile strength of 7.1MPa.
[0041] Embodiment 2:
[0042] 5g cotton and 1.5g sodium periodate (mass ratio of 1:0.3) were placed in a 250mL ethanol-acetone (mass ratio of 1:1) mixed solution, stirred at 50℃ for 3h, and the entire oxidation process was kept in the dark to avoid the decomposition of sodium periodate. After the oxidation was completed, it was centrifuged three times with deionized water and then dialyzed until the remaining iodide was removed. The product was freeze-dried to obtain dialdehyde cellulose (DAC). The aldehyde content of DAC was titrated using the hydroxylamine hydrochloride method, and the aldehyde content of DAC was 4.8mmol / g.
[0043] 2 g DAC and 0.3 g sorbitol crosslinker (the molar ratio of aldehyde to hydroxyl is 1:1) were added to a mixed solution of NN dimethylacetamide and NN dimethylformamide (mass ratio 1:1) at 100 °C and dissolved completely. The mixture was heated to 90 °C for pre-crosslinking for 6 h, then transferred to a 100 °C oven for post-curing for 3 h, and finally hot-pressed at 150 °C for 20 min on a flat-plate hot press to completely cure the sample, thereby obtaining cellulose plastic (ACC).
[0044] The initial degradation temperature of cellulose plastics (T d5%) is 259℃, and the tensile strength is 20.8MPa. ACC powder can be restored to a dense film after hot pressing at 90℃ for 15min, showing excellent reprocessing performance. ACC still has relatively excellent mechanical properties after 10 reshaping processes, with a tensile strength of 19.4MPa.
[0045] Embodiment 3:
[0046] A mixture of 5g of straw and reed (mass ratio 1:1) and 4g of sodium periodate (mass ratio 1:0.8) were placed in 250mL of methanol solution and stirred at 40℃ for 5h. The entire oxidation process was kept in the dark to avoid the decomposition of sodium periodate. After the oxidation was completed, it was centrifuged three times with deionized water and then dialyzed until the remaining iodide was removed. The product was freeze-dried to obtain dialdehyde cellulose (DAC). The aldehyde content of DAC was titrated using the hydroxylamine hydrochloride method, and the aldehyde content of DAC was 5.1mmol / g.
[0047] 2 g DAC and 2.1 g 1,5-pentanediol crosslinker (the molar ratio of aldehyde to hydroxyl is 1:4) were added to NMMO and dissolved completely. The temperature was raised to 120 °C for pre-crosslinking for 1 h, and then transferred to a 150 °C oven for post-curing for 5 h. Finally, the sample was hot-pressed at 150 °C for 20 min to completely cure the sample, thereby obtaining cellulose plastic (ACC).
[0048] The initial degradation temperature of cellulose plastics (T d5% ) is 247℃, and the tensile strength is 16.8MPa. ACC powder can be restored to a dense film after hot pressing at 90℃ for 15min, showing excellent reprocessing performance. ACC still has relatively excellent mechanical properties after 10 reshaping processes, with a tensile strength of 12.9MPa.
[0049] It can be seen from the above examples that the method of the present invention can be used to prepare cellulose thermosetting plastics with excellent thermal stability and reprocessing performance, providing a new strategy for solving the problem of white pollution.
Claims
1. A method for preparing a reprocessable thermosetting plastic of polyol cross-linked cellulose, characterized in that: Here are the steps: Step 1: Add cellulose raw material and sodium periodate into solvent A according to the mass ratio, stir the reaction in a dark environment, and then purify by centrifugation or dialysis; The mass ratio of cellulose raw material to sodium periodate ranges from 1:0.3 to 1:1.4; The solvent A is one or a mixture of two or more of water, ethanol, acetone and methanol; Step 2: Add dialdehyde cellulose and polyol into solvent B according to a certain molar ratio of aldehyde group to hydroxyl group, pre-crosslink in an oil bath, and then transfer to an oven for post-curing, and the solvent is recovered and reused by condensation; The molar ratio of aldehyde group to hydroxyl group is 1:1-1:4; The solvent B is one or a mixture of two or more of dimethyl sulfoxide, N-N-dimethylacetamide, N-N-dimethylformamide, ionic liquid, deep eutectic solvent, alkali-urea system, LiCl / N,N-dimethylacetamide, NMMO, cuprammonia solution, molten salt, and quaternary ammonium salt dissolution system; The polyols are alcohols containing two or more hydroxyl groups.
2. The method for preparing a reprocessable thermosetting plastic of polyol cross-linked cellulose according to claim 1, characterized in that: In step 1, the reaction temperature ranges from 30°C to 50°C; the reaction time ranges from 3h to 9h.
3. The method for preparing a reprocessable thermosetting plastic of polyol cross-linked cellulose according to claim 1 or 2, characterized in that: In step 2, the pre-crosslinking temperature ranges from 90°C to 120°C; the pre-crosslinking time ranges from 1h to 6h; the post-curing temperature ranges from 100°C to 150°C; and the post-curing time ranges from 3h to 10h.
4. The method for preparing a reprocessable thermosetting plastic of polyol cross-linked cellulose according to claim 1 or 2, characterized in that: The cellulose raw material is cellulose powder and one or a mixture of two or more of wood, cotton, cotton linter, wheat straw, rice straw, reed, hemp, mulberry bark, paper mulberry bark and bagasse with a cellulose mass content higher than 60%.
5. The method for preparing a reprocessable thermosetting plastic of polyol cross-linked cellulose according to claim 3, characterized in that: The cellulose raw material is cellulose powder and one or a mixture of two or more of wood, cotton, cotton linter, wheat straw, rice straw, reed, hemp, mulberry bark, paper mulberry bark and bagasse with a cellulose mass content higher than 60%.
6. The method for preparing a reprocessable thermosetting plastic of polyol cross-linked cellulose according to claim 1, 2 or 5, characterized in that: The polyol is one or a mixture of two or more of pentaerythritol, dipentaerythritol, glycerol, decaglycerol, pentanediol, ethylene glycol, propylene glycol, butylene glycol, hexylene glycol, xylitol and sorbitol.
7. The method for preparing a reprocessable thermosetting plastic of polyol cross-linked cellulose according to claim 3, characterized in that: The polyol is one or a mixture of two or more of pentaerythritol, dipentaerythritol, glycerol, decaglycerol, pentanediol, ethylene glycol, propylene glycol, butylene glycol, hexylene glycol, xylitol and sorbitol.
8. The method for preparing a reprocessable thermosetting plastic of polyol cross-linked cellulose according to claim 4, characterized in that: The polyol is one or a mixture of two or more of pentaerythritol, dipentaerythritol, glycerol, decaglycerol, pentanediol, ethylene glycol, propylene glycol, butylene glycol, hexylene glycol, xylitol and sorbitol.
Citation Information
Cited By
Artificial wood capable of being switched from thermoplastic to thermosetting and preparation method of artificial wood
CN121673850A