Polycarbonate resin with high refractive index as well as preparation method and application thereof

By using ester bonded diol monomers in optical resins with fluorene and naphthalene monomers, the problems of insufficient light transmittance in existing optical resins at high refractive index, low birefractive index and low wavelength are solved, and the light transmittance in existing optical resins is achieved. Polycarbonate resin with high refractive index, low ABB number and low b value, suitable for multi-scene optical lens applications.

CN118909238AActive Publication Date: 2024-11-08WANHUA CHEM GRP CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202311609558.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-11-29
Publication Date
2024-11-08
Estimated Expiration
2043-11-29

AI Technical Summary

Technical Problem

Existing optical resins have shortcomings in high refractive index, low birefractive index, low glass transition temperature, etc., which is difficult to meet the growing demand for lens imaging quality. In the low wavelength range, the light transmittance is low, and the color is yellow and high. The problem of b value.

Method used

By copolymerizing diol monomers with ester bonds with fluorene and naphthalene monomers, a high refractive polycarbonate resin has a high refractive index, low Abbe number and low b value, and The light transmittance in the range of 450-1100nm is ≥85%, which improves the problem of yellowing of color.

Benefits of technology

It achieves the improvement of optical performance while high refractive index and low birefractive index, especially in the low wavelength range, which significantly improves the light transmittance and reduces the b value. It is suitable for multi-scene applications, optimizes the appearance of the lens, and is suitable for optical lenses and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004576357480000031
    Figure BDA0004576357480000031
  • Figure BDA0004576357480000041
    Figure BDA0004576357480000041
  • Figure BDA0004576357480000042
    Figure BDA0004576357480000042
Patent Text Reader

Abstract

The invention discloses polycarbonate resin with high refractive index as well as a preparation method and application thereof. The polycarbonate resin is formed by reacting a diol monomer with an ester bond, a fluorene monomer, a naphthalene monomer and a carbonic acid diester compound. According to the present invention, the optimal optical lens with the refractive index of 1.60-1.70 and the Abbe number of less than 25 under the conditions of 23 DEG C and 589 nm can be prepared by using the injection molding optical lens, the optical transmittance of the optical lens within the wavelength range of 450-1100 nm is more than or equal to 85%, the b value of the 1 mm sample plate formed by injection molding of the polycarbonate resin is less than 3, and the industrial prospect is provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polycarbonate, and in particular to a polycarbonate resin with high refractive index, low Abbe number, low b value and high light transmittance under a wide wavelength range, and a preparation method and application thereof. Background Art

[0002] Optical glass or optical resin plays an increasingly important role in people's daily lives. It is widely used in various optical systems such as mobile phone lenses, vehicles, drones, VR (virtual reality), AR (augmented reality), etc. Optical glass has high transparency, excellent heat resistance and refractive index, but its cost is high, molding and processing are difficult, and production efficiency is low. In particular, the processing of aspheric lenses requires extremely high costs and technical barriers, which limits its development in the rapidly growing optical material market.

[0003] Correspondingly, optical resins are increasingly favored by the lens market due to their advantages such as easy molding, higher production efficiency and controllable costs. The annual shipment growth rate of high-refractive-index resin lenses is 10-15%, with a broad market and high versatility.

[0004] Bisphenol A type polycarbonate resin is the most common and commonly used polycarbonate resin. When it was first used for optical lenses, it was limited by its own shortcomings such as low refractive index, high birefringence, and low glass transition temperature. Its application in the market and different scenarios was subject to many restrictions, and it was difficult to continuously meet the growing needs of lens imaging quality. The development of high refractive index and low birefringence polycarbonate resin can greatly improve the imaging quality. A series of polycarbonate resins obtained by homopolymerization or copolymerization of diphenol or diol compounds with polycyclic aromatic ring structures of fluorene have been developed. They have the advantages of high refractive index, low birefringence, and high glass transition temperature, and have occupied a dominant position in the optical material market.

[0005] As mentioned above, patent US5633331A uses 9,9-bis-(4-hydroxyphenyl)fluorene and bisphenol A as comonomers, and the resulting copolycarbonate / polysulfone resin composition is used as a resin for optical lenses. It has a refractive index of 1.627, a large birefringence, and a poor imaging effect. It has gradually lost favor in the market and has been replaced by products with higher refractive index and lower birefringence.

[0006] Patent CN201310062561.X uses 9,9-bis-(4-(2-hydroxyethoxy)phenyl)fluorene as a comonomer and provides a polycarbonate resin that can be used for optical lenses and a method for manufacturing the same. The polycarbonate resin has a refractive index of 1.64 and is widely used in the low-end market of optical materials, but its refractive index still has significant limitations in high-end products.

[0007] Patent CN201380057423.0 discloses a polycarbonate resin, which is mainly copolymerized with 2,2-bis-(2-hydroxyethoxy)-1,1-binaphthyl and fluorene monomers. The polycarbonate obtained in the embodiment has a maximum refractive index of 1.665 and is used in the mid-to-high-end market. Its optical properties are relatively excellent. However, although the polycarbonate resin obtained by copolymerizing such monomers has a high transmittance under the conventional wavelength of 589nm, its transmittance is relatively low in the low wavelength range (450nm~550nm), often less than 85%, which limits its application in multiple scenarios. In addition, such materials generally have a yellowish color and a high b value.

[0008] Patent KR101743352B1 discloses a polycarbonate resin, which has a structure of a bisphenol A derivative and a structure containing a para-aromatic diester, and contains an ester bond. It has excellent weather resistance, processability, and impact resistance. Its monomer composition is relatively simple and is still limited to ordinary bisphenol A polycarbonate. It has limited applications and poor optical properties. It is not in the same category as high-refractive polycarbonate, and the patent discusses the failure to improve its optical properties such as transmittance at different wavelengths. Summary of the invention

[0009] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a high-refractive polycarbonate resin that can be used for optical components and a preparation method thereof. The present invention uses a diol monomer with an ester bond to copolymerize with a fluorene-based and naphthalene-based monomer to synthesize a high-refractive polycarbonate. The polycarbonate resin not only has high refractive index, low Abbe number, and other properties, but also has a low b value. At the same time, the light transmittance of its injection-molded lens in the wavelength range of 450-1100nm is ≥85%. Compared with other high-refractive polycarbonates, the optical lens using this material has a higher transmittance in a wider range of wavelengths, which increases its application scenarios and application effects, and the lens has a better appearance and improves its common problem of yellowing color. The polycarbonate resin manufacturing method is simple and has industrial prospects.

[0010] To solve the above problems, the present invention provides a polycarbonate resin comprising a structural unit represented by general formula (A),

[0011]

[0012] In the general formula (A), Z represents a C1-C6 straight chain or branched alkylene, a C6-C20 aromatic ring, a C3-C20 alicyclic ring, a heterocyclic ring such as furan, thiophene, pyrrole, thiazole, imidazole, pyridine, pyrazine, pyrimidine, pyridazine, indole, etc., preferably a methyl group, an ethyl group, a phenyl group, a cyclopropyl group, a cyclohexyl group, and a furan group, and more preferably a methyl group, an ethyl group, and a phenyl group; X each independently represents a C1-C10 alkylene group, preferably a C1-C6 alkylene group, more preferably a methylene group, an ethylene group, and a propylene group, and further preferably an ethylene group.

[0013] In the present invention, as a preferred embodiment, the polycarbonate resin further comprises a structural unit represented by general formula (B),

[0014]

[0015] In the general formula (B), Z1 each independently represents a C6-C24 aryl group, preferably a phenyl group, a naphthyl group, a biphenyl group, an anthracenyl group, or a phenanthryl group; R1 to R4 each independently represent a hydrogen atom, a halogen atom, a cyano group, a C1-C20 alkyl group, a C1-C20 alkoxy group, a C5-C20 cycloalkyl group, a C5-C20 cycloalkyloxy group, a C6-C20 aryl group, or a C6-C20 aryloxy group, preferably a methyl group, an ethyl group, a phenyl group, a naphthyl group, or a biphenyl group; Y each independently represents a C1-C10 alkylene group, preferably a C1-C6 alkylene group, more preferably a methylene group, an ethylene group, or a propylene group; the value of m each independently ranges from 0 to 10, preferably from 0 to 2; the value of n each independently ranges from 0 to 4, preferably from 0 to 2.

[0016] Preferably, the polycarbonate resin described in the present invention comprises a structural unit represented by the general formula (A) and a structural unit represented by the general formula (B), wherein the molar ratio (A / B) of the structural unit represented by the general formula (A) to the structural unit represented by the general formula (B) is 0.1 / 99.9 to 50 / 50, preferably 1 / 99 to 30 / 70.

[0017] As a preferred embodiment, the polycarbonate resin further comprises a structural unit represented by general formula (C):

[0018]

[0019] In the general formula (C), W represents a C1-C10 alkylene group, preferably a C1-C3 alkylene group; R5 to R8 each independently represent a hydrogen atom, a C1-C20 alkyl group, a C1-C20 alkoxy group, a C5-C20 cycloalkyl group, a C5-C20 cycloalkyloxy group, a C6-C20 aryl group or a C6-C20 aryloxy group, preferably a hydrogen atom, a methyl group, an ethyl group, a phenyl group, a naphthyl group or a biphenyl group.

[0020] As a preferred embodiment, the polycarbonate resin of the present invention comprises structural units represented by general formula (A), general formula (B), and general formula (C), wherein:

[0021] The ratio of the structural unit represented by the general formula (A) is 0.1 to 50 mol%, preferably 1 to 30 mol%.

[0022] The ratio of the structural unit represented by the general formula (B) is 0.1 to 99.8 mol%, preferably 20 to 60 mol%.

[0023] The proportion of the structural unit represented by the general formula (C) is 0.1 to 99.8 mol%, preferably 30 to 70 mol%, based on the total amount of the structural units represented by the general formulas (A), (B) and (C) being 100 mol%.

[0024] To the extent that the effects of the invention are not impaired, the structural units of the polycarbonate resin of the present invention may contain other structural units in addition to the structural units represented by the general formula (A), the general formula (B), and the general formula (C), preferably including less than 15 mol%, more preferably less than 10 mol%, and further preferably less than 5 mol% of other structural units.

[0025] There is no particular limitation on the form in which the structural units represented by the general formula (A), general formula (B) and general formula (C) described in the present invention are contained in the resin. For example, in the present invention, the polycarbonate resin may contain a copolymer containing the structural units represented by the general formula (A), general formula (B) and general formula (C), or may be a binary or ternary resin composition containing a homopolymer composed of each structural unit; or may be a blend obtained by blending homopolymers containing the structural units represented by the general formula (A), (B) and (C). The polycarbonate resin described in the present invention may contain any structure of random, block and alternating copolymer structures.

[0026] The weight average molecular weight (Mw) of the polycarbonate resin of the present invention is 10,000 to 300,000, preferably 30,000 to 150,000. When Mw is less than 10,000, the molded body becomes brittle and is not preferred. When Mw is greater than 300,000, the melt viscosity increases, resulting in poor fluidity, making it difficult to perform injection molding in a molten state, which is also not preferred.

[0027] The present invention uses a diol monomer with an ester bond to copolymerize with other fluorene-based naphthalene-based monomers, thereby ensuring that the obtained polycarbonate resin has excellent optical properties and improving the low-wavelength (450nm-550nm) transmittance, so that the transmittance in the wavelength range of 450-1100nm is ≥85%, and the b value can be lowered to improve the color. The b value of a 1mm sample of the polycarbonate resin injection molding is less than 3, and the preferred value can be less than 1. The optical lens obtained by injection molding has a refractive index of 1.60-1.70 at 23°C and a wavelength of 589nm, and an Abbe value of less than 25.

[0028] The polycarbonate resin of the present invention may be added with auxiliary agents such as antioxidants, mold release agents, ultraviolet absorbers, plasticizers, crystal nucleating agents, reinforcing agents, dyes, antistatic agents or antibacterial agents.

[0029] The present invention also provides a method for preparing the polycarbonate resin, which can be prepared by reacting a dihydroxy compound having a structure represented by formula (1), and optionally a dihydroxy compound having a structure represented by formula (2) or formula (3) with a carbonate diester.

[0030] Preferably, the polycarbonate resin is prepared by reacting a dihydroxy compound represented by formula (1), and optionally formula (2) or formula (3) with a carbonic acid diester in the presence of a basic compound catalyst, an ester exchange catalyst or a mixed catalyst consisting of both, or in the absence of a catalyst, by a melt transesterification polycondensation method.

[0031] In the preparation method of the invention, the dihydroxy compound structure represented by formula (1) to (3) is as follows:

[0032]

[0033] In formula (1), Z represents a C1-C6 straight chain or branched alkylene group, a C6-C20 aromatic ring, a C3-C20 alicyclic ring, a heterocyclic ring such as furan, thiophene, pyrrole, thiazole, imidazole, pyridine, pyrazine, pyrimidine, pyridazine, indole, etc., preferably a methyl group, an ethyl group, a phenyl group, a cyclopropyl group, a cyclohexyl group, or a furan group, and more preferably a methyl group, an ethyl group, or a phenyl group; X each independently represents a C1-C10 alkylene group, preferably a C1-C6 alkylene group, more preferably a methylene group, an ethylene group, or a propylene group, and further preferably an ethylene group.

[0034]

[0035] In formula (2), Z1 each independently represents a C6-C24 aryl group, preferably a phenyl group, a naphthyl group, a biphenyl group, an anthracenyl group, or a phenanthryl group; R1 to R4 each independently represent a hydrogen atom, a halogen atom, a cyano group, a C1-C20 alkyl group, a C1-C20 alkoxy group, a C5-C20 cycloalkyl group, a C5-C20 cycloalkyloxy group, a C6-C20 aryl group, or a C6-C20 aryloxy group, preferably a methyl group, an ethyl group, a phenyl group, a naphthyl group, or a biphenyl group; Y each independently represents a C1-C10 alkylene group, preferably a C1-C6 alkylene group, more preferably a methylene group, an ethylene group, or a propylene group; the value of m each independently ranges from 0 to 10, preferably from 0 to 2; the value of n each independently ranges from 0 to 4, preferably from 0 to 2.

[0036]

[0037] In formula (3), W represents a C1-C10 alkylene group, preferably a C1-C3 alkylene group; R5 to R8 each independently represent a hydrogen atom, a C1-C20 alkyl group, a C1-C20 alkoxy group, a C5-C20 cycloalkyl group, a C5-C20 cycloalkyloxy group, a C6-C20 aryl group or a C6-C20 aryloxy group, preferably a hydrogen atom, a C1-C3 alkyl group or a C6-C12 aryl group; more preferably a hydrogen atom, a methyl group, an ethyl group, a propyl group, a phenyl group, a naphthyl group or a biphenyl group.

[0038] Preferably, the dihydroxy compound represented by formula (1) is the following dihydroxy compound derivative structure:

[0039]

[0040] Preferably, the dihydroxy compound represented by formula (2) is the following dihydroxy compound derivative structure:

[0041]

[0042] Preferably, the dihydroxy compound represented by formula (3) is the following dihydroxy compound derivative structure:

[0043]

[0044] In the preparation method of the present invention, the carbonic acid diester is one or more of diphenyl carbonate, ditolyl carbonate, dimethyl carbonate, diethyl carbonate, dibutyl carbonate, dicyclohexyl carbonate, etc., preferably diphenyl carbonate.

[0045] In the preparation method of the present invention, the molar ratio of the carbonic acid diester to the sum of the dihydroxy compounds represented by formula (1), (2) and (3) is 0.95 to 1.14:1, preferably 0.98 to 1.12:1.

[0046] In the preparation method of the present invention, the alkaline compound catalyst is sodium hydroxide, magnesium hydroxide, calcium hydroxide, strontium hydroxide, barium hydroxide, lithium bicarbonate, sodium bicarbonate, potassium bicarbonate, magnesium bicarbonate, calcium bicarbonate, strontium bicarbonate, barium bicarbonate, sodium carbonate, magnesium carbonate, calcium carbonate, strontium carbonate, barium carbonate, cesium carbonate, calcium chloride, potassium chloride, cesium chloride, strontium chloride, barium chloride, lanthanum acetylacetonate, cerium acetylacetonate, magnesium acetate, calcium acetate, strontium acetate, acetic acid One or more of barium, magnesium stearate, calcium stearate, calcium benzoate, phenyl magnesium phosphate, tetrabutyl titanate, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, trimethylbenzylammonium hydroxide, triethylamine, dimethylbenzylamine, triphenylamine, diethylamine, tetramethylammonium borohydride, tetrabutylammonium borohydride, tetrabutylammonium tetraphenylborate, tetraphenylammonium tetraphenylborate, preferably one or more of sodium hydroxide, sodium bicarbonate, and cesium carbonate.

[0047] In the preparation method of the present invention, the transesterification catalyst is one or more of tin chloride, tin acetate, cerium acetylacetonate, zirconium acetylacetonate, zirconium oxyacetate, tetrabutoxy zirconium, zinc acetate, zinc benzoate, zinc 2-ethylhexanoate, tin chloride, tin acetate, cerium acetylacetonate, zirconium acetylacetonate, zirconium oxyacetate, tetrabutoxy zirconium, etc., preferably one or more of tin chloride, cerium acetylacetonate, and zinc acetate.

[0048] In the preparation method of the present invention, the molar ratio of the sum of the added alkaline compound catalyst and / or the ester exchange catalyst to the sum of the dihydroxy compounds represented by formula (1), formula (2) and formula (3) is 1×10 -7 ~1×10 -2 : 1, preferably 1×10 -6 ~1×10 -3 :1.

[0049] In some preferred embodiments of the present invention, the preparation method of the polycarbonate comprises: adding the dihydroxy compound represented by formula (1), and optionally formula (2) and formula (3), carbonic acid diester, catalyst, and optional auxiliary agent into a reactor, fully replacing the air in the reactor with nitrogen for 3 to 5 times, and then heating the reactor to melt the materials, the melting temperature is 160 to 210°C, preferably 180 to 200°C, the residence time of this stage is 30 to 90 minutes, preferably 40 to 60 minutes, and the pressure under nitrogen atmosphere is 50 kPa to 200 kPa, preferably 90 to 110 kPa. After the materials are melted, stirring is started, and the temperature is raised to the transesterification reaction temperature, the transesterification reaction temperature is 190 to 260°C, preferably 200 to 240°C, the pressure is controlled to be 0.5 to 50 kPa, preferably 1 to 30 kPa, and the residence time of this stage is 60 to 320 minutes, preferably 120 to 240 minutes. Then, the pressure is further reduced and the temperature is increased to start the polycondensation reaction. The system pressure at this stage is 10-500 Pa, preferably 50-100 Pa, the reaction temperature at this stage is 240-320° C., preferably 260-300° C., and the residence time at this stage is 10-120 min, preferably 20-60 min. During the reaction, the generated small molecule compounds are immediately removed by distillation, and the polycarbonate resin is finally obtained in the reactor.

[0050] The application of the polycarbonate resin of the present invention in the field of optical devices is particularly suitable for preparing optical lenses, such as mobile phone lenses, security lenses, vehicle-mounted lenses and the like.

[0051] The polycarbonate resin of the present invention has high refractive index, low Abbe number, good light transmittance and low b value, and is suitable for mobile phone lenses, vehicle lenses, outdoor security lenses and other fields. The optical lens using the polycarbonate resin of the present invention has low b value, good appearance, clear imaging and broad application prospects. DETAILED DESCRIPTION

[0052] The present invention is now described as follows in conjunction with specific embodiments. It should be noted that the embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Any non-substantial improvements and adjustments made to the embodiments according to the content of the present invention are protected by the present invention.

[0053] Main raw material sources:

[0054] A-1 Aladdin Biotechnology Co., Ltd.

[0055] B-1, C-1: Sino Lixing Fine Chemical Co., Ltd.;

[0056] DPC: diphenyl carbonate, Sichuan Zhonglan Guosu Material Technology Co., Ltd.;

[0057] Unless otherwise specified, all other raw materials are commercially available.

[0058] Performance testing method:

[0059] 1) Weight average molecular weight (Mw): Gel permeation chromatography (GPC) was used with dichloromethane as the developing solvent and a calibration curve was prepared using standard polystyrenes of known molecular weight (molecular weight distribution = 1). Based on this calibration curve, Mw was calculated from the retention time of GPC.

[0060] 2) Light transmittance: The light transmittance was measured by the method of JIS-K-7361-1 using a turbidity meter for a film having a thickness of 0.1 mm made of the polycarbonate resin produced in the examples.

[0061] 3) Refractive index (nD): For a 1 mm thick film composed of the polycarbonate resin prepared in the example, the refractive index (nD) of the polycarbonate resin of the present invention at 23°C and a wavelength of 589 nm was measured using an Abbe refractometer according to the method of JIS-K-7142.

[0062] 4) Abbe number: The refractive index of a 0.1 mm thick film made of the polycarbonate resin produced in the example at wavelengths of 486 nm, 589 nm and 656 nm at 23° C. was measured using an Abbe refractometer, and the Abbe number ν was calculated using the following formula: ν=(nD-1) / (nF-nC).

[0063] 5) b value: After the obtained polycarbonate resin was vacuum dried at 120°C for 4 hours, it was injection molded using an injection molding machine at a barrel temperature of 270°C and a mold temperature of Tg-10°C to obtain a disc-shaped test sheet with a diameter of 50 mm and a thickness of 1 mm. The b value was measured using this sheet in accordance with JIS K7105.

[0064] Example 1

[0065] 2.54 g (0.01 mol) of A-1, 53.1 g (0.09 mol) of B-1, 23.56 g (0.11 mol) of diphenyl carbonate, 0.52 mg (2×10 -6 mol) tin chloride, 0.25 mg (3 × 10 -6 mol) sodium bicarbonate was placed in a 250ml four-necked flask with a stirrer and a distillation device, replaced with nitrogen 4 times, heated to 200°C under a nitrogen atmosphere of 101kPa, and maintained at this temperature for 60min. After confirming that the raw materials were completely dissolved, stirring was turned on, the pressure was adjusted to 20kPa(A), and the temperature was raised to 240°C at a rate of 10°C / hr. At this time, it was confirmed that phenol generated as a by-product began to distill out, and the reaction was maintained at 240°C for 180min, and then the temperature was raised to 280°C at a rate of 20°C / hr. After the temperature reached 280°C, the pressure was gradually reduced to 100Pa(A) within 120min, and the reaction was stirred under this condition for 60min to terminate the reaction. After the reaction was completed, nitrogen was filled into the four-necked flask to restore it to normal pressure, and the generated polycarbonate resin was taken out for performance evaluation. The physical properties of the obtained polycarbonate are shown in Table 1.

[0066] Example 2

[0067] 2.54 g (0.01 mol) of A-1, 33.66 g (0.09 mol) of C-1, 23.56 g (0.11 mol) of diphenyl carbonate, 0.52 mg (2×10 -6 mol) tin chloride, 0.25 mg (3 × 10 -6 mol) of sodium bicarbonate was placed in a 250 ml four-necked flask with a stirrer and a distillation apparatus. Otherwise, the same operations as in Example 1 were performed. The physical properties of the obtained polycarbonate are shown in Table 1.

[0068] Example 3

[0069] 0.25 g (0.001 mol) of A-1, 28.91 g (0.049 mol) of B-1, 18.7 g (0.05 mol) of C-1, 23.56 g (0.11 mol) of diphenyl carbonate, 0.52 mg (2 × 10 -6 mol) tin chloride, 0.25 mg (3 × 10 -6 mol) of sodium bicarbonate was placed in a 250 ml four-necked flask with a stirrer and a distillation apparatus. Otherwise, the same operations as in Example 1 were performed. The physical properties of the obtained polycarbonate are shown in Table 1.

[0070] Example 4

[0071] 7.62 g (0.03 mol) of A-1, 23.6 g (0.04 mol) of B-1, 11.2 g (0.03 mol) of C-1, 23.56 g (0.11 mol) of diphenyl carbonate, 0.52 mg (2 × 10 -6 mol) tin chloride, 0.25 mg (3 × 10 -6 mol) of sodium bicarbonate was placed in a 250 ml four-necked flask with a stirrer and a distillation apparatus. Otherwise, the same operations as in Example 1 were performed. The physical properties of the obtained polycarbonate are shown in Table 1.

[0072] Example 5

[0073] 2.54 g (0.01 mol) of A-1, 23.6 g (0.04 mol) of B-1, 18.7 g (0.05 mol) of C-1, 23.56 g (0.11 mol) of diphenyl carbonate, 0.52 mg (2×10 -6 mol) tin chloride, 0.25 mg (3 × 10 -6 mol) of sodium bicarbonate was placed in a 250 ml four-necked flask with a stirrer and a distillation apparatus. Otherwise, the same operations as in Example 1 were performed. The physical properties of the obtained polycarbonate are shown in Table 1.

[0074] Comparative Example 1

[0075] 29.5 g (0.05 mol) of B-1, 18.7 g (0.05 mol) of C-1, 23.56 g (0.11 mol) of diphenyl carbonate, 0.52 mg (2 × 10 -6 mol) tin chloride, 0.25 mg (3 × 10 -6 mol) of sodium bicarbonate was placed in a 250 ml four-necked flask with a stirrer and a distillation apparatus. Otherwise, the same operations as in Example 1 were performed. The physical properties of the obtained polycarbonate are shown in Table 1.

[0076] Comparative Example 2

[0077] 40.65 (0.1 mol) BPEF, 23.56 g (0.11 mol) diphenyl carbonate, 0.88 mg (2 × 10 -6 mol) cerium acetylacetonate, 0.06 mg (1.5 × 10 -6 mol) of sodium hydroxide was placed in a 250 ml four-necked flask with a stirrer and a distillation apparatus. Otherwise, the same operations as in Example 1 were performed. The physical properties of the obtained polycarbonate are shown in Table 1.

[0078]

[0079] Table 1

[0080]

[0081] Note: The minimum transmittance of this type of polycarbonate resin in the wavelength range of 450nm-1100nm is at a wavelength of 450nm. Therefore, it can be considered that the transmittance in the above wavelength range is greater than or equal to the transmittance value at 450nm.

Claims

1. A high refractive index polycarbonate resin comprising structural units represented by general formula (A), general formula (B) and general formula (C), In the general formula (A), Z represents a C1-C6 straight chain or branched alkylene group, a C6-C20 aromatic ring, a C3-C20 alicyclic ring, or a heterocyclic ring, preferably a methyl group, an ethyl group, a phenyl group, a cyclopropyl group, a cyclohexyl group, or a furan group; X each independently represents a C1-C10 alkylene group, preferably a C1-C6 alkylene group, and more preferably a methylene group, an ethylene group, or a propylene group; In the general formula (B), Z1 each independently represents a C6-C24 aryl group, preferably a phenyl group, a naphthyl group, a biphenyl group, an anthryl group, or a phenanthryl group; R1 to R4 each independently represent a hydrogen atom, a halogen atom, a cyano group, a C1-C20 alkyl group, a C1-C20 alkoxy group, a C5-C20 cycloalkyl group, a C5-C20 cycloalkyloxy group, a C6-C20 aryl group, or a C6-C20 aryloxy group, preferably a methyl group, an ethyl group, a phenyl group, a naphthyl group, or a biphenyl group; Y each independently represents a C1-C10 alkylene group, preferably a C1-C6 alkylene group, more preferably a methylene group, an ethylene group, or a propylene group; the value of m each independently represents a value of 0 to 10, preferably 0 to 2; the value of n each independently represents a value of 0 to 4, preferably 0 to 2; In the general formula (C), W represents a C1-C10 alkylene group, preferably a C1-C3 alkylene group; R5 to R8 each independently represent a hydrogen atom, a C1-C20 alkyl group, a C1-C20 alkoxy group, a C5-C20 cycloalkyl group, a C5-C20 cycloalkyloxy group, a C6-C20 aryl group or a C6-C20 aryloxy group, preferably a hydrogen atom, a methyl group, an ethyl group, a phenyl group, a naphthyl group or a biphenyl group.

2. The polycarbonate resin according to claim 1, characterized in that In the polycarbonate resin, The proportion of the structural unit represented by the general formula (A) is 0.1 to 50 mol%, preferably 1 to 30 mol%; The proportion of the structural unit represented by the general formula (B) is 0.1 to 99.8 mol%, preferably 20 to 60 mol%; The proportion of the structural unit represented by the general formula (C) is 0.1 to 99.8 mol%, preferably 30 to 70 mol%, based on the total amount of the structural units represented by the general formula (A), the general formula (B) and the general formula (C) being 100 mol%.

3. The polycarbonate resin according to any one of claims 1 to 2, characterized in that The refractive index at 23°C and a wavelength of 589nm is 1.60-1.70, the Abbe number is less than 25, and the b value of a 1mm sample is less than 3; and the light transmittance of the injection-molded lens within the wavelength range of 450-1100nm is ≥85%.

4. A method for preparing the polycarbonate resin according to any one of claims 1 to 3, which can be prepared by reacting a dihydroxy compound having a structure represented by formula (1), a dihydroxy compound having a structure represented by formula (2), and a dihydroxy compound having a structure represented by formula (3) with a carbonic acid diester, wherein the dihydroxy compounds represented by formulas (1) to (3) have the following structures: In formula (1), Z represents a C1-C6 straight chain or branched alkylene group, a C6-C20 aromatic ring, a C3-C20 alicyclic ring, or a heterocyclic ring, preferably a methyl group, an ethyl group, a phenyl group, a cyclopropane group, a cyclohexane group, or a furan group; X each independently represents a C1-C10 alkylene group, preferably a C1-C6 alkylene group, and more preferably a methylene group, an ethylene group, or a propylene group; In formula (2), Z1 each independently represents a C6-C24 aryl group, preferably a phenyl group, a naphthyl group, a biphenyl group, an anthryl group, or a phenanthryl group; R1 to R4 each independently represent a hydrogen atom, a halogen atom, a cyano group, a C1-C20 alkyl group, a C1-C20 alkoxy group, a C5-C20 cycloalkyl group, a C5-C20 cycloalkyloxy group, a C6-C20 aryl group, or a C6-C20 aryloxy group, preferably a methyl group, an ethyl group, a phenyl group, a naphthyl group, or a biphenyl group; Y each independently represents a C1-C10 alkylene group, preferably a C1-C6 alkylene group, more preferably a methylene group, an ethylene group, or a propylene group; the value of m each independently represents a value of 0 to 10, preferably 0 to 2; the value of n each independently represents a value of 0 to 4, preferably 0 to 2; In formula (3), W represents a C1-C10 alkylene group, preferably a C1-C3 alkylene group; R5 to R8 each independently represent a hydrogen atom, a C1-C20 alkyl group, a C1-C20 alkoxy group, a C5-C20 cycloalkyl group, a C5-C20 cycloalkyloxy group, a C6-C20 aryl group or a C6-C20 aryloxy group, preferably a hydrogen atom, a C1-C3 alkyl group or a C6-C12 aryl group; more preferably a hydrogen atom, a methyl group, an ethyl group, a propyl group, a phenyl group, a naphthyl group or a biphenyl group.

5. The method according to claim 4, characterized in that The structural formula of formula (1) is: The structural formula of formula (2) is: The structural formula of formula (3) is:

6. The method according to claim 4, characterized in that The carbonic acid diester is one or more of diphenyl carbonate, ditolyl carbonate, dimethyl carbonate, diethyl carbonate, dibutyl carbonate and dicyclohexyl carbonate.

7. The method according to claim 4, characterized in that The molar ratio of the carbonic acid diester to the sum of the dihydroxy compounds represented by formula (1), (2) and (3) is 0.95 to 1.14:1, preferably 0.98 to 1.12:

1.

8. Use of the polycarbonate resin according to any one of claims 1 to 3 or the polycarbonate resin prepared by the method according to any one of claims 4 to 7 in the field of optical devices, preferably in the preparation of optical lenses and optical films.

Citation Information

Patent Citations

  • Resin composition and molded object thereof

    CN101018824A

  • Resin produced by polycondensation, and resin composition

    CN109593196A

  • Thermoplastic resin and optical member

    CN110741030A

  • Polycarbonate resin composition, production method therefor, and optical lens

    CN111630109A

  • Diol compound, polycarbonate, and preparation method thereof

    CN113412257A