Cross-linked polymer doped and modified perfluorosulfonic acid membrane and preparation method thereof

Through the preparation method of crosslinked polymer doping modified perfluorosulfonic acid film, the problem of vanadium ion permeability in vanadium batteries is solved, the Coulomb efficiency and mechanical properties are improved, phase separation is avoided, and the battery stability is achieved. Energy efficiency.

CN118909287AInactive Publication Date: 2024-11-08HANGZHOU DEHAI AIKE ENERGY TECH CO LTD

Patent Information

Application Number
CN202411404346.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-10
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing perfluorosulfonic acid films have serious vanadium ion penetration problems in vanadium batteries, resulting in reduced battery banking efficiency and increased maintenance costs, and inorganic nanomaterial doping modification methods will lead to mechanical performance degradation and phase separation.

Method used

The crosslinked polymer doping modified perfluorosulfonic acid film preparation method is adopted to form a crosslinked polymer suspension by combining crosslinked polyvinylpyrrolidone and crosslinked poly4-vinylpyridine with perfluorosulfonic acid resin. , the film is formed and dried by casting method, so as to reduce the pore size of the water molecule channel in the film and improve the vanadium resistance performance.

Benefits of technology

The Coulomb efficiency and energy efficiency of vanadium batteries are improved, the mechanical properties of the membrane are maintained, the phase separation problem is avoided, and the stability of the membrane is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909287A_ABST
    Figure CN118909287A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of all-vanadium redox flow battery diaphragms, and discloses a cross-linked polymer doped and modified perfluorosulfonic acid membrane and a preparation method thereof.The preparation method at least comprises the following steps that firstly, commercial perfluorosulfonic acid resin is sequentially washed with hydrogen peroxide and deionized water and then dried, and perfluorosulfonic acid resin powder is obtained; adding the powder into a solvent, heating and stirring to dissolve the powder to obtain a perfluorosulfonic acid solution, and centrifuging and filtering to obtain a pure perfluorosulfonic acid solution; and secondly, grinding cross-linked polymer powder, adding the ground cross-linked polymer powder into the pure perfluorosulfonic acid solution, magnetically stirring and defoaming to obtain a perfluorosulfonic acid cross-linked polymer suspension, forming a membrane by a tape casting method, drying and demolding to obtain the cross-linked polymer doped and modified perfluorosulfonic acid membrane. The perfluorosulfonic acid membrane prepared by the method can well meet the requirements of high ion selectivity, high ion conductivity and high stability required by a vanadium battery diaphragm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of all-vanadium liquid flow battery diaphragm, in particular to a cross-linked polymer doped modified perfluorosulfonic acid membrane and a preparation method thereof. Background Art

[0002] All-vanadium liquid flow batteries (abbreviated as vanadium batteries) have the advantages of large energy storage capacity, flexible design, recyclable electrolyte, safety and reliability, economic and long-term effects, etc., and are increasingly attracting widespread attention from the society. As one of the key components of the battery, the ion exchange membrane not only isolates the positive and negative electrolytes in the vanadium battery, but also serves as a medium for transferring protons. The performance of the ion exchange membrane directly affects the performance and service life of the vanadium battery. The ideal ion exchange membrane should have excellent ion conductivity, high ion selectivity, excellent mechanical and chemical stability, and low cost.

[0003] At present, perfluorosulfonic acid membranes (such as Nafion membranes) have become the most widely used ion exchange membranes for vanadium batteries due to their excellent electrochemical properties and chemical stability. However, during the long-term operation of the battery, the ion exchange membrane will experience severe vanadium ion penetration, which will greatly reduce the coulombic efficiency of the battery and gradually decay the discharge capacity of the battery, greatly increasing the maintenance cost of the vanadium battery. Therefore, it is necessary to modify the perfluorosulfonic acid membrane to improve its vanadium resistance. Among many modification methods, doping inorganic nanomaterials in perfluorosulfonic acid resin to prepare inorganic-modified perfluorosulfonic acid membranes is one of the commonly used modification methods. Inorganic particles are filled into the pores of the membrane itself to reduce the pore size of the water molecule channel in the membrane, thereby reducing the migration of vanadium ions. However, this method also has fatal disadvantages, that is, the addition of inorganic substances will cause the mechanical properties of the membrane to deteriorate, and long-term use will cause the membrane to phase separate and the coulombic efficiency to decrease.

[0004] Therefore, the search for perfluorosulfonic acid membranes with high stability, high ion selectivity, and high ion conductivity for vanadium batteries and their modification methods has become one of the hot topics in the field of vanadium batteries. Summary of the invention

[0005] In view of the above problems or shortcomings, the present invention provides a cross-linked polymer doped modified perfluorosulfonic acid membrane and a preparation method thereof. The technical solution adopted by the present invention is as follows: A method for preparing a cross-linked polymer doped perfluorosulfonic acid membrane comprises at least the following steps: Step S1, pretreatment of perfluorosulfonic acid resin: ultrasonically clean the commercial perfluorosulfonic acid resin with hydrogen peroxide, and then repeatedly clean it with deionized water and dry it to obtain perfluorosulfonic acid resin powder; Step S2, preparation of casting liquid: weigh 5-20 parts by mass of perfluorosulfonic acid resin powder, add it to 80-95 parts by mass of solvent, heat it to 150° C. and stir it to dissolve it, to obtain a perfluorosulfonic acid solution with a mass fraction of 5%-20%; centrifuge the perfluorosulfonic acid solution, and filter it through a sand core filter device with a pore size of 2 μm polytetrafluoroethylene microporous filter membrane to obtain a pure perfluorosulfonic acid solution; weigh 0.5-4 parts by mass of cross-linked polymer powder, grind it and add it to 96-99.5 parts by mass of pure perfluorosulfonic acid solution, and obtain a perfluorosulfonic acid cross-linked polymer suspension with a mass fraction of 0.5%-4% after magnetic stirring and degassing; Step S3, film formation: 30-60 parts by weight of the perfluorosulfonic acid cross-linked polymer suspension in step S2 is placed in a constant temperature oscillator for oscillation treatment for 1 hour, and then slowly poured onto a flat glass plate by a casting method to form a film, and then dried and removed to obtain a cross-linked polymer doped modified perfluorosulfonic acid film.

[0006] Preferably, the mass percentage of hydrogen peroxide in step S1 is 5% to 10%.

[0007] Preferably, the drying temperature in step S1 is 60-90°C.

[0008] Preferably, the solvent in step S2 is at least one of N,N-dimethylacetamide (DMAc), N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), and N-methylpyrrolidone (NMP).

[0009] Preferably, the cross-linked polymer in step S2 is at least one of cross-linked polyvinyl pyrrolidone and cross-linked poly 4-vinyl pyridine.

[0010] Preferably, the particle size of the cross-linked polymer powder in step S2 is 0.1-5 μm.

[0011] Preferably, in step S3, the temperature of the constant temperature oscillator is set to 30-40° C., and the oscillation frequency is set to 200-300 times / min.

[0012] Preferably, the drying in step S3 is controlled by programmed temperature, i.e., keeping warm at 60-80°C for 1 hour, and then keeping warm at 140-160°C for 2 hours.

[0013] A cross-linked polymer doped and modified perfluorosulfonic acid membrane is prepared by adopting the above-mentioned method for preparing a cross-linked polymer doped and modified perfluorosulfonic acid membrane.

[0014] The beneficial effects of the present invention include at least: 1. Cross-linked polyvinyl pyrrolidone and cross-linked poly 4-vinyl pyridine can be obtained by the repolymerization of polyvinyl pyrrolidone and poly 4-vinyl pyridine, respectively, retaining the positively charged pyrrole ring and pyridine ring structure, having good vanadium barrier properties, and can reduce vanadium shuttling; 2. The cross-linked polymer is insoluble in water. Filling the pores of the perfluorosulfonic acid membrane can reduce the pore size of the water molecule channel in the membrane, thereby reducing the migration of vanadium ions and improving the coulombic efficiency of the battery; 3. Compared with inorganic particles, cross-linked polymers are organic powders and have better compatibility with perfluorosulfonic acid resins, avoiding the problem of phase separation of the membrane. The mechanical properties of the membrane are maintained and the stability is greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 The present invention is a flow chart for preparing a cross-linked polymer doped modified perfluorosulfonic acid membrane; Figure 2 It is a molecular fragment structure diagram of cross-linked polyvinyl pyrrolidone and cross-linked poly 4-vinyl pyridine in the present invention. DETAILED DESCRIPTION

[0016] The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0017] The present invention discloses a cross-linked polymer doped perfluorosulfonic acid membrane, which is Figure 1 The preparation method shown is obtained and is further illustrated by the following examples.

[0018] Example 1: The preparation of the present invention film comprises the following steps: Step S1, pretreatment of perfluorosulfonic acid resin: ultrasonically clean the commercial perfluorosulfonic acid resin with 5% by mass hydrogen peroxide, then repeatedly clean it with deionized water and dry it at 60° C. to obtain perfluorosulfonic acid resin powder; Step S2, preparation of casting solution: weigh 5 g of perfluorosulfonic acid resin powder, add it to 95 g of N,N-dimethylacetamide (DMAc), heat it to 150° C. and stir it to dissolve it, to obtain a perfluorosulfonic acid solution with a mass fraction of 5%; centrifuge the perfluorosulfonic acid solution, and filter it through a sand core filter device with a pore size of 2 μm polytetrafluoroethylene microporous filter membrane to obtain a pure perfluorosulfonic acid solution; weigh 0.5 g of cross-linked polyvinyl pyrrolidone powder with a particle size of 0.1 μm, grind it and add it to 99.5 g of pure perfluorosulfonic acid solution, and obtain a perfluorosulfonic acid cross-linked polymer suspension with a mass fraction of 0.5% after magnetic stirring and degassing; Step S3, film formation: 30 g of the perfluorosulfonic acid cross-linked polymer suspension is placed in a constant temperature oscillator, the temperature of the constant temperature oscillator is set to 30° C., the oscillation frequency is 200 times / min, after oscillation treatment for 1 hour, it is slowly poured onto a flat glass plate by a casting method to form a film, and after drying at a programmed temperature of 60° C. for 1 hour and 140° C. for 2 hours, the film is removed to obtain a cross-linked polymer doped and modified perfluorosulfonic acid film.

[0019] Example 2: The preparation of the present invention film comprises the following steps: Step S1, pretreatment of perfluorosulfonic acid resin: ultrasonically clean the commercial perfluorosulfonic acid resin with 6% by mass hydrogen peroxide, then repeatedly clean it with deionized water and dry it at 65° C. to obtain perfluorosulfonic acid resin powder; Step S2, preparation of casting solution: weigh 8g of perfluorosulfonic acid resin powder, add it to 92g of N,N-dimethylformamide (DMF), heat it to 150°C and stir it to dissolve it, to obtain a perfluorosulfonic acid solution with a mass fraction of 8%; centrifuge the perfluorosulfonic acid solution, and filter it through a sand core filter device with a pore size of 2μm polytetrafluoroethylene microporous filter membrane to obtain a pure perfluorosulfonic acid solution; weigh 1g of cross-linked polyvinyl pyrrolidone powder with a particle size of 1μm, grind it and add it to 99g of pure perfluorosulfonic acid solution, and obtain a perfluorosulfonic acid cross-linked polymer suspension with a mass fraction of 1% after magnetic stirring and degassing; Step S3, film formation: 35 g of the perfluorosulfonic acid cross-linked polymer suspension is placed in a constant temperature oscillator, the temperature of the constant temperature oscillator is set to 30° C., the oscillation frequency is 200 times / min, after oscillation treatment for 1 hour, it is slowly poured onto a flat glass plate by a casting method to form a film, and after drying at a programmed temperature of 60° C. for 1 hour and 140° C. for 2 hours, the film is removed to obtain a cross-linked polymer doped modified perfluorosulfonic acid film.

[0020] Example 3: The preparation of the present invention film comprises the following steps: Step S1, pretreatment of perfluorosulfonic acid resin: ultrasonically clean the commercial perfluorosulfonic acid resin with 7% by mass hydrogen peroxide, then repeatedly clean it with deionized water and dry it at 70° C. to obtain perfluorosulfonic acid resin powder; Step S2, preparation of casting solution: weigh 10g of perfluorosulfonic acid resin powder, add it to 90g of dimethyl sulfoxide (DMSO), heat it to 150°C and stir it to dissolve it, and obtain a perfluorosulfonic acid solution with a mass fraction of 10%; centrifuge the perfluorosulfonic acid solution, and filter it through a sand core filter device with a pore size of 2μm polytetrafluoroethylene microporous filter membrane to obtain a pure perfluorosulfonic acid solution; weigh 1.5g of cross-linked poly 4-vinyl pyridine powder with a particle size of 2μm, grind it and add it to 98.5g of pure perfluorosulfonic acid solution, and obtain a perfluorosulfonic acid cross-linked polymer suspension with a mass fraction of 1.5% after magnetic stirring and degassing; Step S3, film formation: 40 g of the perfluorosulfonic acid cross-linked polymer suspension is placed in a constant temperature oscillator, the temperature of the constant temperature oscillator is set to 30° C., the oscillation frequency is 200 times / min, after oscillation treatment for 1 hour, it is slowly poured onto a flat glass plate by a casting method to form a film, and after drying at a programmed temperature of 60° C. for 1 hour and 140° C. for 2 hours, the film is removed to obtain a cross-linked polymer doped and modified perfluorosulfonic acid film.

[0021] Example 4: The preparation of the present invention film comprises the following steps: Step S1, pretreatment of perfluorosulfonic acid resin: ultrasonically clean the commercial perfluorosulfonic acid resin with 8% by mass hydrogen peroxide, then repeatedly clean it with deionized water and dry it at 70° C. to obtain perfluorosulfonic acid resin powder; Step S2, preparation of casting solution: weigh 12g of perfluorosulfonic acid resin powder, add it to 88g of N,N-dimethylacetamide (DMAc), heat it to 150°C and stir it to dissolve it, and obtain a perfluorosulfonic acid solution with a mass fraction of 12%; centrifuge the perfluorosulfonic acid solution, and filter it through a sand core filter device with a pore size of 2μm polytetrafluoroethylene microporous filter membrane to obtain a pure perfluorosulfonic acid solution; weigh 2g of cross-linked polyvinyl pyrrolidone powder with a particle size of 3μm, grind it and add it to 98g of pure perfluorosulfonic acid solution, and obtain a perfluorosulfonic acid cross-linked polymer suspension with a mass fraction of 2% after magnetic stirring and degassing; Step S3, film formation: 45 g of the perfluorosulfonic acid cross-linked polymer suspension is placed in a constant temperature oscillator, the temperature of the constant temperature oscillator is set to 30° C., the oscillation frequency is 200 times / min, after oscillation treatment for 1 hour, it is slowly poured onto a flat glass plate by a casting method to form a film, and after drying at a programmed temperature of 60° C. for 1 hour and 140° C. for 2 hours, the film is removed to obtain a cross-linked polymer doped modified perfluorosulfonic acid film.

[0022] Example 5: The preparation of the present invention film comprises the following steps: Step S1, pretreatment of perfluorosulfonic acid resin: ultrasonically clean the commercial perfluorosulfonic acid resin with 8% by mass hydrogen peroxide, then repeatedly clean it with deionized water and dry it at 75° C. to obtain perfluorosulfonic acid resin powder; Step S2, preparation of casting solution: weigh 15g of perfluorosulfonic acid resin powder, add it to 85g of N-methylpyrrolidone (NMP), heat it to 150°C and stir it to dissolve it, to obtain a perfluorosulfonic acid solution with a mass fraction of 15%; centrifuge the perfluorosulfonic acid solution, and filter it through a sand core filter device with a pore size of 2μm polytetrafluoroethylene microporous filter membrane to obtain a pure perfluorosulfonic acid solution; weigh 2.5g of cross-linked poly 4-vinylpyridine powder with a particle size of 3μm, grind it and add it to 97.5g of pure perfluorosulfonic acid solution, and obtain a perfluorosulfonic acid cross-linked polymer suspension with a mass fraction of 2.5% after magnetic stirring and degassing; Step S3, film formation: 50 g of the perfluorosulfonic acid cross-linked polymer suspension is placed in a constant temperature oscillator, the temperature of the constant temperature oscillator is set to 30° C., the oscillation frequency is 200 times / min, after oscillation treatment for 1 hour, it is slowly poured onto a flat glass plate by a casting method to form a film, and after drying at a programmed temperature of 60° C. for 1 hour and 140° C. for 2 hours, the film is removed to obtain a cross-linked polymer doped and modified perfluorosulfonic acid film.

[0023] Example 6: The preparation of the present invention film comprises the following steps: Step S1, pretreatment of perfluorosulfonic acid resin: ultrasonically clean the commercial perfluorosulfonic acid resin with 9% by mass hydrogen peroxide, then repeatedly clean it with deionized water and dry it at 80° C. to obtain perfluorosulfonic acid resin powder; Step S2, preparation of casting solution: weigh 18g of perfluorosulfonic acid resin powder, add it to 82g of N,N-dimethylformamide (DMF), heat it to 150°C and stir it to dissolve it, and obtain a perfluorosulfonic acid solution with a mass fraction of 18%; centrifuge the perfluorosulfonic acid solution, and filter it through a sand core filter device with a pore size of 2μm polytetrafluoroethylene microporous filter membrane to obtain a pure perfluorosulfonic acid solution; weigh 3g of cross-linked polyvinyl pyrrolidone powder with a particle size of 4μm, grind it and add it to 97g of pure perfluorosulfonic acid solution, and obtain a perfluorosulfonic acid cross-linked polymer suspension with a mass fraction of 3% after magnetic stirring and degassing; Step S3, film formation: 55 g of the perfluorosulfonic acid cross-linked polymer suspension is placed in a constant temperature oscillator, the temperature of the constant temperature oscillator is set to 38° C., the oscillation frequency is 280 times / min, after oscillation treatment for 1 hour, it is slowly poured onto a flat glass plate by a casting method to form a film, and after drying at a programmed temperature of 70° C. for 1 hour and 160° C. for 2 hours, the film is removed to obtain a cross-linked polymer doped and modified perfluorosulfonic acid film.

[0024] Example 7: The preparation of the present invention film comprises the following steps: Step S1, pretreatment of perfluorosulfonic acid resin: ultrasonically clean the commercial perfluorosulfonic acid resin with 10% by mass hydrogen peroxide, then repeatedly clean it with deionized water and dry it at 90° C. to obtain perfluorosulfonic acid resin powder; Step S2, preparation of casting solution: weigh 20g of perfluorosulfonic acid resin powder and add it to 80g of N,N-dimethylacetamide (DMSIc), heat to 150°C and stir to dissolve it, to obtain a perfluorosulfonic acid solution with a mass fraction of 20%; centrifuge the perfluorosulfonic acid solution, and filter it through a sand core filter device with a pore size of 2μm polytetrafluoroethylene microporous filter membrane to obtain a pure perfluorosulfonic acid solution; weigh 4g of cross-linked polyvinyl pyrrolidone powder with a particle size of 5μm, grind it and add it to 96g of pure perfluorosulfonic acid solution, and obtain a perfluorosulfonic acid cross-linked polymer suspension with a mass fraction of 4% after magnetic stirring and degassing; Step S3, film formation: 60 g of the perfluorosulfonic acid cross-linked polymer suspension is placed in a constant temperature oscillator, the temperature of the constant temperature oscillator is set to 40° C., the oscillation frequency is 300 times / min, after oscillation treatment for 1 hour, it is slowly poured onto a flat glass plate by a casting method to form a film, and after drying at a programmed temperature of 80° C. for 1 hour and 160° C. for 2 hours, the film is removed to obtain a cross-linked polymer doped and modified perfluorosulfonic acid film.

[0025] Comparative Example 1: The preparation process is the same as that of Example 4, except that no cross-linking polymer is added to the perfluorosulfonic acid solution, and the film is formed directly from the perfluorosulfonic acid solution.

[0026] Comparative Example 2: The preparation process is the same as that of Example 4, except that in step S2, 2 g of inorganic SiO2 with a particle size of 3 μm is used instead of the cross-linked polymer powder.

[0027] The films obtained in Examples 1 to 7 and Comparative Examples 1 to 2 were subjected to mechanical property (tensile strength) tests and stacking tests. The coulombic efficiency, voltage efficiency, and energy efficiency at the 10th and 1000th cycles were tested and recorded under the same test conditions. The test results are shown in Table 1: Table 1 Summary of test results of membrane mechanical properties and stack performance

[0028] As shown in Table 1, compared with Comparative Example 1, Examples 1 to 7 have little difference in tensile strength and voltage efficiency of the stack, while the stack has higher coulombic efficiency and energy efficiency in the initial test and after 1000 cycles. This is because cross-linked polyvinyl pyrrolidone and cross-linked poly 4-vinyl pyridine can be obtained by repolymerization of polyvinyl pyrrolidone and poly 4-vinyl pyridine, respectively. Figure 2As shown, the positively charged pyrrole ring and pyridine ring structure are retained, thereby having better vanadium resistance performance. At the same time, the cross-linked polymer is insoluble in water. Filling it into the pores of the perfluorosulfonic acid membrane itself can reduce the pore size of the water molecule channel in the membrane, thereby reducing the migration of vanadium ions. The result of the combined effect is the improvement of coulomb efficiency and energy efficiency. Compared with Comparative Example 2, Examples 1 to 7 have little difference in the voltage efficiency of the battery stack, but have higher coulomb efficiency and energy efficiency in tensile strength, initial test performance of the battery stack and after 1000 cycles. This is because the cross-linked polymer has better vanadium resistance performance than inorganic particles, and has better compatibility with perfluorosulfonic acid resin, which avoids the problem of phase separation of the membrane, maintains the mechanical properties of the membrane, and greatly improves the stability.

[0029] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a cross-linked polymer doped perfluorosulfonic acid membrane, comprising at least the following steps: Step S1: pretreatment of perfluorosulfonic acid resin: ultrasonically clean the commercial perfluorosulfonic acid resin with hydrogen peroxide, then clean it with deionized water and dry it to obtain perfluorosulfonic acid resin powder; Step S2: Preparation of casting solution: Weigh 5-20 parts by weight of perfluorosulfonic acid resin powder, add it to 80-95 parts by weight of solvent, heat it to 150° C. and stir it to dissolve it, to obtain a perfluorosulfonic acid solution with a mass fraction of 5%-20%; centrifuge the perfluorosulfonic acid solution, and filter it through a sand core filter device with a pore size of 2 μm polytetrafluoroethylene microporous filter membrane to obtain a pure perfluorosulfonic acid solution; weigh 0.5-4 parts by weight of cross-linked polymer powder, grind it and add it to 96-99.5 parts by weight of pure perfluorosulfonic acid solution, and obtain a perfluorosulfonic acid cross-linked polymer suspension with a mass fraction of 0.5%-4% after magnetic stirring and degassing; Step S3: Film formation: 30-60 parts by weight of the perfluorosulfonic acid cross-linked polymer suspension in step S2 is placed in a constant temperature oscillator for oscillation for 1 hour, and then slowly poured onto a flat glass plate by a casting method to form a film, and then dried and removed to obtain a cross-linked polymer doped and modified perfluorosulfonic acid film.

2. The method for preparing a cross-linked polymer-doped perfluorosulfonic acid membrane as claimed in claim 1, characterized in that: The mass percentage of hydrogen peroxide in step S1 is 5% to 10%.

3. The method for preparing a cross-linked polymer-doped perfluorosulfonic acid membrane as claimed in claim 1, characterized in that: The organic solvent in step S2 is any one of N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, and N-methylpyrrolidone.

4. The method for preparing a cross-linked polymer-doped perfluorosulfonic acid membrane as claimed in claim 1, characterized in that: The cross-linked polymer in step S2 is any one of cross-linked polyvinyl pyrrolidone and cross-linked poly 4-vinyl pyridine.

5. The method for preparing a cross-linked polymer-doped perfluorosulfonic acid membrane as claimed in claim 1, characterized in that: The particle size of the cross-linked polymer powder in step S2 is 0.1-5 μm.

6. The method for preparing a cross-linked polymer-doped perfluorosulfonic acid membrane according to claim 1, characterized in that: In step S3, the temperature of the constant temperature oscillator is set to 30-40° C., and the oscillation frequency is set to 200-300 times / min.

7. The method for preparing a cross-linked polymer-doped perfluorosulfonic acid membrane as claimed in claim 1, characterized in that: In step S3, the drying is carried out by program temperature control, that is, keeping the temperature at 60-80° C. for 1 hour, and then keeping the temperature at 140-160° C. for 2 hours.

8. A cross-linked polymer doped perfluorosulfonic acid membrane, characterized in that: The cross-linked polymer doped and modified perfluorosulfonic acid membrane is prepared by the method for preparing a cross-linked polymer doped and modified perfluorosulfonic acid membrane according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Doped physical bonding cross-linking multilayer perfluorinated ion exchange membrane

    CN101733013A

  • Preparation method of enhanced composite proton exchange membrane

    CN106159300A

  • Cross-linked composite membrane for flow battery as well as preparation and application thereof

    CN112940321A

  • Hydrogen fuel cell, water electrolysis hydrogen production proton exchange membrane and preparation method of proton exchange membrane

    CN116111155A

  • High-ion-selectivity ionic membrane for vanadium redox flow battery and preparation method of high-ion-selectivity ionic membrane

    CN117199465A

Cited By

  • High-ion-selectivity perfluorosulfonic acid ionic membrane for vanadium battery as well as preparation method and application of high-ion-selectivity perfluorosulfonic acid ionic membrane

    CN122025692A