Static dissipation wood fiber foam with strain response and preparation method thereof

By adding additives such as nanocellulose and carbon fiber to the lime fiber foam, electrostatic dissipative lime fiber foam with strain response is prepared, which solves the problem of insufficient durability and recyclability of existing antistatic foam materials and achieves more efficient Electrostatic dissipation performance and lower production costs, suitable for packaging and transportation of electronic products.

CN118909299AActive Publication Date: 2024-11-08SOUTH CHINA UNIV OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411129764.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-08
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

Existing antistatic foam materials have poor durability, high cost, difficult to recycle and degrade, and may affect the stability of electronic components such as circuit boards in humid environments, and cannot meet strict industry standards and specific application requirements.

Method used

By stirring mechanically treated ligno fibers with nanocellulose, ammonium polyphosphate, carbon fiber and ammonium dodecyl sulfate at high speed in deionized water, electrostatic dissipative ligno fiber foam with strain response is prepared to improve its electrical conductivity and Electrostatic dissipation capability.

Benefits of technology

It achieves excellent electrostatic dissipation strain response effect of wood fiber foam, reduces costs, improves durability and recycling, and maintains good antistatic properties in humid environments, meeting the high precision requirements of electronic product packaging and transportation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909299A_ABST
    Figure CN118909299A_ABST
Patent Text Reader

Abstract

The invention discloses static dissipation wood fiber foam with strain response and a preparation method of the static dissipation wood fiber foam. The preparation method comprises the following steps: (1) fully stirring and mixing wood fibers and CNF in an aqueous solution to obtain mixed slurry; (2) stirring the mixed slurry obtained in the step (1) with ammonium polyphosphate (APP), lauryl sodium sulfate (SDS) and carbon fiber (CF) at a high speed of 3000rpm for 10 minutes; and (3) pouring the mixed solution stirred in the step (2) into a polytetrafluoroethylene circular hollow mold to filter unstable moisture. And (4) drying the wet foam obtained in the step (3) in a drying oven to obtain dry wood fiber foam. The wood fiber foam prepared by the invention has excellent static dissipative property of strain effect, and has wide application prospects in the fields of electronic product packaging, transportation and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of foaming materials, and in particular relates to a strain-responsive electrostatically dissipative wood fiber foam and a preparation method thereof. Background Art

[0002] Petroleum-based plastic foam is the most widely used cushioning material in the packaging and transportation of electronic products. However, due to its non-degradable and difficult to recycle disadvantages, it is piled up and incinerated in large quantities after use, which has placed a heavy burden on the environment. Pulp fiber foam has green properties such as natural, degradable, and recyclable, and is expected to become a substitute for petroleum-based foam. However, the high insulation of wood fiber foam limits its application in electronic products. Therefore, it is necessary to develop a static dissipative wood fiber foam to replace commercial petroleum-based plastic foam, which is very important for social development and environmental health.

[0003] According to ANSI / ESDA standards, the volume resistivity of antistatic dissipative materials is 10 4 -10 11 Ω-cm or surface resistivity is 10 5 -10 12 Therefore, the packaging and transportation of high-precision products in the electronics industry (computers, televisions, communications and medical equipment, etc.) require higher antistatic ability of foam materials (<10 9 Ω-cm). Improving the conductivity of foam is mainly achieved by adding conductive materials (metal particles, carbon, graphene and conductive polymers, etc.) to adjust the resistivity to meet various usage scenarios. Carbon fiber (CF) has a fibrous and soft appearance, is easy to process, and has high temperature resistance and excellent conductivity. It is an excellent conductive additive. In addition, due to the chemical inertness of carbon fiber, physical blending is conducive to the separation of wood cellulose and carbon fiber during the recycling process, which is more natural and environmentally friendly than plastic foam.

[0004] In the prior art, commercial antistatic foam has obvious limitations, which are as follows: first, the durability of antistatic foam is poor, and aging under long-term use or high temperature conditions has a great impact on the antistatic performance. This aging may also produce tiny particles, affecting the cleanliness of the packaged items and greatly affecting the application of sensitive equipment; second, due to the complex preparation process of the foam, its cost is relatively high; during the transportation of large equipment, it is not as good as other materials such as hard plastics. Excellent protective performance. In addition, some antistatic foam materials may have a certain degree of hygroscopicity, which may affect its antistatic effect in a humid environment, and may cause electronic components such as circuit boards to short-circuit or other failures due to moisture. The main problem of the widely used antistatic foam is that it is not easy to recycle and degrade, which increases environmental pressure and burden. Different types of antistatic foams have significant differences in the static dissipation rate, and some products may not meet strict industry standards or specific application requirements, which may lead to failure to effectively protect equipment at critical moments. In summary, although antistatic foam plays an important role in many fields, its limitations and potential problems also need to be paid attention to. When selecting materials, it is important to consider various factors comprehensively to ensure effective protection and economical solutions. Summary of the invention

[0005] In view of the deficiencies in the prior art, the object of the present invention is to provide a strain-responsive electrostatically dissipative wood fiber foam and a preparation method thereof.

[0006] In order to achieve the above object, the present invention is implemented through the following technical solutions:

[0007] In a first aspect, the present invention provides a method for preparing an electrostatic dissipator having a strain response, comprising the following steps:

[0008] The mechanically treated wood fiber is fully mixed with nanocellulose (CNF). Then, ammonium polyphosphate (APP), carbon fiber (CF), and ammonium dodecyl sulfate (SDS) are added thereto and stirred at high speed in deionized water. The concentration of wood fiber is 2%, the amount of CNF is 6% of the absolute dry pulp mass, the amount of APP is 15% of the absolute dry pulp mass: the amount of SDS is, and the amount of CF is 0%-80% of the absolute dry pulp mass. The high-speed stirring speed is 3000rpm, and the stirring time is 10min.

[0009] A specific method for preparing an electrostatically dissipative wood fiber foam having a strain response comprises the following steps:

[0010] (1) fully stirring and mixing wood fiber and CNF in an aqueous solution to obtain a mixed slurry;

[0011] (2) stirring the mixed slurry of step (1) with ammonium polyphosphate (APP), sodium dodecyl sulfate (SDS) and carbon fiber (CF) at high speed;

[0012] (3) pouring the mixed solution after stirring in step (2) into a polytetrafluoroethylene circular hollow mold to filter out unstable water;

[0013] (4) Drying the wet foam obtained in step (3) in an oven to obtain a dry wood fiber foam, wherein the static dissipative wood fiber foam has an excellent static dissipative strain response effect.

[0014] Further preferably, in step (1), the wood fiber needs to be pretreated in advance by beating the wood fiber with a PFI refiner for 6000-12000r.

[0015] Further preferably, in step (1), the absolute dry mass of the wood fiber is 10-20 g, and the absolute dry mass of the CNF is 0.6-1.2 g.

[0016] Further preferably, in step (1), the CNF is Tempo-oxidized nanocellulose.

[0017] Further preferably, in step (2), the length of the carbon fiber is 4-8 mm.

[0018] Further preferably, in step (2), the high-speed stirring speed is: 20000-30000 rpm; the time is: 10-20 min.

[0019] Further preferably, in step (2), the amount of APP is 15-25%, the amount of SDS is 0.4-0.8%, and the amount of CF is 3-8%, wherein the amount of each additive is relative to the absolute dry weight of the wood fiber.

[0020] Further preferably, in step (4), the drying time is 8-12 hours and the drying temperature is 60-80°C.

[0021] The applicant has found through experiments that the extremely low impedance of CF can effectively improve the electrical conductivity of wood fiber foam. In addition, wood fiber foam will change its electrical conductivity due to the deformation of the foam caused by external pressure, and has a specific strain response. Therefore, the change in electrical conductivity caused by the amount of CF can be used to meet different environmental requirements.

[0022] In some embodiments, the mechanical treatment method is: after the unbleached softwood pulp board is deflagrated, the pulp is mechanically beaten using a PFI refiner, with the beating speed being 9000r and the beating concentration being 10%.

[0023] In some embodiments, the CNF is Tempo-oxidized nanocellulose.

[0024] In some embodiments, the solvent is water.

[0025] In some embodiments, the length of the CF is 6 mm.

[0026] In a second aspect, the present invention provides a strain-responsive electrostatically dissipative wood fiber foam material prepared by the preparation method.

[0027] In a third aspect, the present invention provides a strain-responsive electrostatically dissipative wood cellulosic foam material prepared by a one-pot wet process and drying.

[0028] In some embodiments, the mixed solution after stirring is poured into a polytetrafluoroethylene mold with a filter screen, and then placed in an oven for drying at 60° C. for 12 hours until the wet foam is stable to obtain a dry wood fiber foam.

[0029] The beneficial effects achieved by one or more embodiments of the present invention are as follows:

[0030] CF can effectively improve the electrostatic dissipation ability of wood fiber foam. In addition, the electrostatic dissipation of wood fiber foam is very good, so CF-improved wood fiber foam has a wide range of application prospects in the fields of electronic product packaging and transportation. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a graph showing the change in volume resistance of foam during compression. DETAILED DESCRIPTION

[0032] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0033] A method for preparing a strain-responsive electrostatically dissipative wood fiber foam comprises the following steps:

[0034] (1) fully stirring and mixing wood fiber and CNF in an aqueous solution to obtain a mixed slurry;

[0035] (2) stirring the mixed slurry of step (1) with ammonium polyphosphate (APP), sodium dodecyl sulfate (SDS) and carbon fiber (CF) at high speed;

[0036] (3) pouring the mixed solution after stirring in step (2) into a polytetrafluoroethylene circular hollow mold to filter out unstable water;

[0037] (4) Drying the wet foam obtained in step (3) in an oven to obtain dry wood fiber foam.

[0038] In the above method, in step (1), the wood fiber needs to be pretreated in advance by beating the wood fiber with a PFI refiner for 6000-12000r, preferably 9000r.

[0039] In the above method, in step (1), the absolute dry mass of the wood fiber is 10-20 g, preferably 10 g, and the absolute dry mass of the CNF is 0.6-1.2 g, preferably 0.6 g.

[0040] In the above method, in step (1), the CNF is Tempo-oxidized nanocellulose.

[0041] In the above method, in step (2), the length of the carbon fiber is 4-8 mm.

[0042] In the above method, in step (2), the high-speed stirring speed is: 20000-30000rpm; the time is: 10-20min.

[0043] In the above method, in step (2), the amount of APP is 15-25%, the amount of SDS is 0.4-0.8%, and the amount of CF is 3-8%, wherein the amount of each additive is relative to the absolute dry weight of wood fiber.

[0044] In the above method, in step (4), the drying time is 8-12 hours and the drying temperature is 60-80°C.

[0045] The static dissipative wood fiber foam of the present invention has excellent static dissipative strain response effect.

[0046] The present invention will be further described in detail below in conjunction with specific embodiments, but the embodiments of the present invention are not limited thereto. For process parameters not particularly noted, conventional techniques may be used.

[0047] Example 1

[0048] (1) Weigh 10 g of absolute dry pulp (after beating) and thoroughly stir and mix it with 6% CNF in an aqueous solution.

[0049] (2) The mixed solution of step (1) was stirred with 15% APP, 4% SDS, and 0% CF at 3000 rpm for 10 min.

[0050] (3) Pour the mixed solution after stirring in step (2) into a polytetrafluoroethylene circular hollow mold to filter out unstable water.

[0051] (4) Drying the wet foam obtained in step (3) in an oven at 60° C. for 12 h to obtain dry wood fiber foam.

[0052] Example 2

[0053] (1) Weigh 10 g of absolute dry pulp (after beating) and thoroughly stir and mix it with 6% CNF in an aqueous solution.

[0054] (2) The mixed solution of step (1) was stirred with 15% APP, 4% SDS and 30% CF at 3000 rpm for 10 min.

[0055] (3) Pour the mixed solution after stirring in step (2) into a polytetrafluoroethylene circular hollow mold to filter out unstable water.

[0056] (4) Dry the wet foam obtained in step (3) in an oven at 60°C for 12 hours to obtain dry wood fiber foam.

[0057] Example 3

[0058] (1) Weigh 10 g of absolute dry pulp (after beating) and thoroughly stir and mix it with 6% CNF in an aqueous solution.

[0059] (2) The mixed solution of step (1) was stirred with 15% APP, 4% SDS and 40% CF at 3000 rpm for 10 min.

[0060] (3) Pour the mixed solution after stirring in step (2) into a polytetrafluoroethylene circular hollow mold to filter out unstable water.

[0061] (4) Drying the wet foam obtained in step (3) in an oven at 60° C. for 12 h to obtain dry wood fiber foam.

[0062] Example 4

[0063] (1) Weigh 10 g of absolute dry pulp (after beating) and thoroughly stir and mix it with 6% CNF in an aqueous solution.

[0064] (2) The mixed solution of step (1) was stirred with 15% APP, 4% SDS and 50% CF at 3000 rpm for 10 min.

[0065] (3) Pour the mixed solution after stirring in step (2) into a polytetrafluoroethylene circular hollow mold to filter out unstable water.

[0066] (4) Drying the wet foam obtained in step (3) in an oven at 60° C. for 12 h to obtain dry wood fiber foam.

[0067] Example 5

[0068] (1) Weigh 10 g of absolute dry pulp (after beating) and thoroughly stir and mix it with 6% CNF in an aqueous solution.

[0069] (2) The mixed solution of step (1) was stirred with 15% APP, 4% SDS and 60% CF at 3000 rpm for 10 min.

[0070] (3) Pour the mixed solution after stirring in step (2) into a polytetrafluoroethylene circular hollow mold to filter out unstable water.

[0071] (4) Drying the wet foam obtained in step (3) in an oven at 60° C. for 12 h to obtain dry wood fiber foam.

[0072] Example 6

[0073] (1) Weigh 10 g of absolute dry pulp (after beating) and thoroughly stir and mix it with 6% CNF in an aqueous solution.

[0074] (2) The mixed solution of step (1) was stirred with 15% APP, 4% SDS and 70% CF at 3000 rpm for 10 min.

[0075] (3) Pour the mixed solution after stirring in step (2) into a polytetrafluoroethylene circular hollow mold to filter out unstable water.

[0076] (4) Drying the wet foam obtained in step (3) in an oven at 60° C. for 12 h to obtain dry wood fiber foam.

[0077] Example 7

[0078] (1) Weigh 10 g of absolute dry pulp (after beating) and thoroughly stir and mix it with 6% CNF in an aqueous solution.

[0079] (2) The mixed solution of step (1) was stirred with 15% APP, 4% SDS and 80% CF at 3000 rpm for 10 min.

[0080] (3) Pour the mixed solution after stirring in step (2) into a polytetrafluoroethylene circular hollow mold to filter out unstable water.

[0081] (4) Drying the wet foam obtained in step (3) in an oven at 60° C. for 12 h to obtain dry wood fiber foam.

[0082] Example 8

[0083] The electrical conductivity of the foam materials prepared in Examples 1-7 was tested according to Figure 1 It can be seen that the uncompressed volume resistivity of the wood fiber foam prepared in Examples 1-7 of the present application is 7.75*10 9Ω~4.42*10 8 The resistance of pulp foam varies greatly with the increase of carbon fiber content. With only 8% carbon fiber added, its volume resistance increases from 10 9 Ω down to 10 4 Ω. The volume of the foam in Example 6 is divided into two processes during the compression process. First, the resistance value is increased from 3.99*10 6 Ω (strain is 0.00%) changes rapidly to 5.64*10 5 Ω (strain 9.21%), and the strain is about 10%, showing an inflection point between the antistatic and conductive levels (10 6 Ω). In the second stage, the volume resistivity of wood fiber foam changes slowly, with a value of 10 4 -10 5 Ω. The wood fiber foam is at an antistatic level under pressure-free conditions, thereby reducing the influence of external static charges. However, a 10% deformation of the pulp foam can be easily achieved by the pressure generated by product transportation. When the deformation of the pulp foam exceeds 10%, the change in its conductivity is small, indicating that the wood fiber foam prepared by this method has an excellent electrostatic dissipation strain response effect.

[0084] In summary, the wood fiber foam prepared in the present application has excellent electrostatic dissipation of strain effect and has broad application prospects in the fields of electronic product packaging and transportation.

[0085] It should be understood that the above detailed description of the technical solution of the present invention with the help of optimized embodiments is illustrative rather than restrictive, and it cannot be determined that the specific implementation methods of the present invention are limited to this. For ordinary technicians in the technical field to which the present invention belongs, without departing from the concept of the present invention, modifications to the technical solutions recorded in the embodiments, or equivalent replacement of some of the technical features therein, should be deemed to fall within the scope of patent protection determined by the claims submitted for the present invention.

[0086] The above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A method for preparing a strain-responsive electrostatically dissipative wood fiber foam, characterized in that: The steps include: (1) fully stirring and mixing wood fiber and CNF in an aqueous solution to obtain a mixed slurry; (2) stirring the mixed slurry of step (1) with ammonium polyphosphate (APP), sodium dodecyl sulfate (SDS) and carbon fiber (CF) at high speed; (3) pouring the mixed solution after stirring in step (2) into a polytetrafluoroethylene circular hollow mold to filter out unstable water; (4) Drying the wet foam obtained in step (3) in an oven to obtain dry wood fiber foam.

2. The method for preparing a strain-responsive electrostatic dissipative wood fiber foam according to claim 1, characterized in that: In step (1), the wood fiber needs to be pretreated in advance by beating the wood fiber with a PFI refiner for 6000-12000r.

3. The method for preparing a strain-responsive electrostatic dissipative wood fiber foam according to claim 1, characterized in that: In step (1), the absolute dry mass of the wood fiber is 10-20 g, and the absolute dry mass of the CNF is 0.6-1.2 g.

4. The method for preparing a strain-responsive electrostatically dissipative wood fiber foam according to claim 1, characterized in that: In step (1), the CNF is Tempo-oxidized nanocellulose.

5. The method for preparing a strain-responsive electrostatically dissipative wood fiber foam according to claim 1, characterized in that: In step (2), the length of the carbon fiber is 4-8 mm.

6. The method for preparing a strain-responsive electrostatically dissipative wood fiber foam according to claim 1, characterized in that: In step (2), the high-speed stirring speed is 20000-30000 rpm and the time is 10-20 min.

7. The method for preparing a strain-responsive electrostatically dissipative wood fiber foam according to claim 1, characterized in that: In step (2), the amount of APP is 15-25%, the amount of SDS is 0.4-0.8%, and the amount of CF is 3-8%, wherein the amount of each additive is relative to the absolute dry weight of the wood fiber.

8. The method for preparing a strain-responsive electrostatically dissipative wood fiber foam according to claim 1, characterized in that: In step (4), the drying time is 8-12 hours and the drying temperature is 60-80°C.

9. The electrostatically dissipative wood fiber foam with strain response prepared by the preparation method according to any one of claims 1 to 6.

10. The static dissipative wood fiber foam according to claim 9, characterized in that The static dissipative wood fiber foam has excellent static dissipative strain response effect.

Citation Information

Patent Citations

  • Carbon fiber static dissipation packing material and method for producing the same

    CN101220204A

  • Nano-cellulose-reinforced paper pulp foam material and preparation method thereof

    CN106835808A

  • Method for preparing ultra-light high-elasticity fire-resistant water-resistant paper pulp foam by adopting wood fiber raw material

    CN109867815A

  • Static dissipative laminate containing an interior special core layer containing carbon fibers