High-hydrophilicity composite plastic material and preparation method thereof
By using a combination of hyperbranched supramolecular hydrophilic agents and other additives in composite materials, the problem of poor hydrophilic properties of existing composite materials is solved, and the hydrophilicity, toughness and heat resistance of the materials are improved. It is suitable for high-loving Areas of water requirements.
Patent Information
- Application Number
- CN202411404565.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-10
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The poor hydrophilic properties of existing composite materials limit their application in areas with high hydrophilic requirements, especially in the textile industry, where the electrostatic properties and toughness of the materials are insufficient.
Using a combination of polymer polymers, hyperbranched supramolecular hydrophilic agents, common hydrophilic agents, compatibility agents, toughening agents, antioxidants and antistatic agents, the preparation of the specific reaction and extrusion granulation process is carried out. A highly hydrophilic composite plastic material improves the hydrophilicity, toughness and heat resistance of the material.
It significantly improves the hydrophilic properties of the material, enhances its range of use at low temperatures, and improves the mechanical properties and heat resistance of the material through the addition of antioxidants and compatibilizers, and extends the service life of the material.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite materials, in particular to a composite material for improving the hydrophilicity of resin, and more particularly to a highly hydrophilic composite plastic material and a preparation method thereof. Background Art
[0002] Composite plastic materials are widely used in the fields of automobiles, aviation, ships, construction, electronics and electrical appliances due to their superior mechanical properties, light weight, easy processing and low cost. However, due to the chemical structure, plastic materials have low surface energy, resulting in poor hydrophilicity, which also greatly limits the application of plastic materials in some fields with high hydrophilicity requirements. For example, in the textile industry, if the hydrophilicity of the material is high, it is not easy to generate static electricity, which can improve the physical feel of the material.
[0003] Chinese patent document CN114381066A discloses a super-hydrophilic polypropylene composite material and its preparation method, the super-hydrophilic polypropylene composite material is composed of the following components in the following weight fractions: 24-60% polypropylene, 10-20% thermoplastic polyurethane rubber, 10-15% corn starch, 10-15% aluminum hydroxide, 5-10% maleic anhydride grafted polypropylene, 3-10% hydrophilic agent and 1-3% dispersant. The raw material used in the document is polypropylene material, and the hydrophilic property of polypropylene material is solved. The method of changing the hydrophilicity of the material has poor wide applicability. Chinese patent document CN107174978A discloses a hydrophilic polyvinylidene fluoride composite material, which is modified by blending amphiphilic copolymer and polyvinylidene fluoride in a solvent, but the effect of the hydrophilic modification is poor, and the contact angle of the composite material after hydrophilic modification is still above 45°.
[0004] Therefore, how to provide a composite material with strong applicability and good hydrophilic effect is a problem that those skilled in the art need to solve urgently. Summary of the invention
[0005] In view of the defects of the prior art, the object of the present invention is to provide a highly hydrophilic modified plastic material and a preparation method thereof, so as to solve the problems existing in the above-mentioned background technology.
[0006] The first aspect of the present invention provides a highly hydrophilic composite plastic material, which comprises the following components by weight: 47.5-86.2 parts of a high molecular polymer, 10-30 parts of a hyperbranched supramolecular hydrophilic agent, 0-6 parts of a common hydrophilic agent, 2-8 parts of a compatibilizer, 5-10 parts of a toughening agent, 0.2-1 parts of an antioxidant, 1-3 parts of an antistatic agent, and 0.1-0.5 parts of a lubricant, wherein the hyperbranched supramolecular hydrophilic agent is prepared by reacting glycerol acrylamide, an amino-terminated polymer, and a long-chain fatty amine.
[0007] As a preferred technical solution, the method for preparing the hyperbranched supramolecular hydrophilic agent comprises at least the following steps: Step 1: Weigh glycerol acrylamide and amino-terminated polymer separately in a molar ratio of 1:1; Step 2: adding the glycerol acrylamide and the amino-terminated polymer weighed in step 1 to a polar solvent at 50-80° C., stirring while adding, at a stirring speed of 100-300 r / min, and a stirring time of 20-40 min, to dissolve them, wherein the polar solvent is selected from one or more combinations of methanol, ethanol, and water; Step 3: weigh a monobasic long-chain fatty amine, wherein the molar ratio of the monobasic long-chain fatty amine to propylene glycol acrylamide is 1:2, and the weighed monobasic long-chain fatty amine is added to the mixture in step 2, and reacted at 50-85° C. for 20-30 min, with a stirring speed of 200-500 r / min during the reaction. After the reaction is completed, a hyperbranched supramolecular hydrophilic agent is obtained.
[0008] As a preferred technical solution, the preparation method of glycerol acrylamide comprises at least the following steps: S1: Heat glycerol to 200-250°C; S2: slowly adding acrylamide to glycerol, wherein the molar ratio of glycerol to acrylamide is 1:3, and stirring at a stirring speed of 200-500 r / min; S3: After sufficient reaction, glycerol acrylamide is obtained, unreacted glycerol is washed away with water, and the mixture is fully dried in vacuum to obtain purified glycerol acrylamide.
[0009] As a preferred technical solution, the common hydrophilic agent is one or more combinations of polyvinyl alcohol, azodimethyldisilane, and sodium dodecyl sulfate.
[0010] As a preferred technical solution, the high molecular polymer is one or more combinations of polypropylene (PP), polyamide (PA), polybutylene terephthalate (PBT), polyethylene terephthalate (PET), and polyphenylene sulfide (PPS), and the compatibilizer is at least one of maleic anhydride grafted polypropylene or a silane coupling agent.
[0011] As a preferred technical solution, the toughening agent is one or more combinations of ethylene propylene diene monomer rubber (EPDM), ethylene-1-octene or butene copolymer (POE), maleic anhydride (MAH) grafted ethylene-1-octene or butene copolymer (POE~g~MAH), and maleic anhydride grafted ethylene propylene diene monomer rubber (EPDM~g~MAH).
[0012] As a preferred technical solution, the antioxidant is one or more combinations of 2,6-di-tert-butyl-p-cresol, β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, tris(nonylphenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, dioctadecyl pentaerythritol diphosphite, and dilauryl thiodipropionate.
[0013] As a preferred technical solution, the antistatic agent is one or more combinations of glyceryl monostearate, ethoxylated amine, N,N-dihydroxyethyl octadecylamine, polyether hindered block copolymer, and polyether block amide.
[0014] As a preferred technical solution, the lubricant is at least one of erucamide and oleamide.
[0015] The second aspect of the present invention provides a method for preparing the highly hydrophilic composite material, comprising at least the following steps: Step 1: Weighing: Weigh the high molecular polymer, hyperbranched supramolecular compound, common hydrophilic agent, compatibilizer, toughening agent, antioxidant, antistatic agent, and lubricant according to the weight ratio and set aside; Step 2: Mixing: firstly, a high molecular polymer, a hyperbranched supramolecular hydrophilic agent, a common hydrophilic agent, a compatibilizer, a toughening agent, an antioxidant, an antistatic agent, and a lubricant are uniformly mixed to obtain a mixture; then, the mixture is extruded and granulated to obtain a highly hydrophilic composite material, wherein the granulation is performed by a twin-screw extruder, and the temperature of each section of the twin-screw extruder is between 170 and 250° C., and the screw speed is between 180 and 500 rpm / min.
[0016] Beneficial Effects
[0017] (1) The highly hydrophilic composite material of the present invention can significantly reduce the water contact angle of the polymer by using a hyperbranched supramolecular hydrophilic agent, thereby effectively improving the hydrophilicity of the highly hydrophilic composite material and solving the problem of poor hydrophilicity of the polymer in the prior art.
[0018] (2) The toughness of the matrix of the fiber composite material in the present invention is destroyed due to the presence of the hyperbranched supramolecular hydrophilic agent. The inventors have improved the toughness of the material by adding a toughening agent, thereby broadening the application range of the material at low temperatures. The inventors have made the water absorption of the hyperbranched supramolecular hydrophilic agent better by adding an antistatic agent, thereby achieving a superimposed resonance effect of one plus one being greater than two.
[0019] (3) The inventors improved the compatibility of the matrix and the hydrophilic agent by adding a compatibilizer, thereby improving the mechanical properties of the material. The inventors effectively improved the heat resistance of the material by adding an antioxidant, preventing the material from discoloring and degrading, and solving the problem of aging during long-term use of the material.
[0020] (4) The inventors increased the density of hydrophilic groups by using a hydrophilic agent with a hyperbranched supramolecular structure, thereby greatly improving the hydrophilicity of the material, and being able to achieve a high hydrophilicity with a limited addition amount. The hyperbranched supramolecular is a polymer prepared by the reaction of propylene glycol acrylate, terminal amino polymer, and monovalent long-chain fatty amine. It has a hyperbranched supramolecular structure and contains a large number of hydrophilic groups. It can establish an ultra-high density hydrophilic network structure, greatly improving the hydrophilicity of the plastic material. DETAILED DESCRIPTION
[0021] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] Example 1
[0023] The highly hydrophilic composite plastic material in this embodiment includes the following components in parts by weight: 86.2 parts of high molecular polymer copolymer PP, 4 parts of compatibilizer maleic anhydride grafted polypropylene, 7 parts of toughening agent POE (polyolefin elastomer), 0.5 parts of antioxidant 2,6-di-tert-butyl-p-cresol, 2 parts of antistatic agent polyether hindered block copolymer, and 0.3 parts of lubricant erucamide. Copolymer PP was purchased from China SABIC (Tianjin) Petrochemical Co., Ltd. with a brand name of 87MK40T, maleic anhydride grafted polypropylene was purchased from Nantong Rizhisheng New Molecular Material Technology Co., Ltd. with a brand name of CMG 9801, toughening agent POE was purchased from Dow Chemical with a brand name of 8150, antistatic agent was purchased from Akema with a brand name of Pebax® MV2080, and the lubricant used was purchased from Huanqi Chemical with a brand name of FINAWAX SE.
[0024] The preparation process of highly hydrophilic composite plastic materials is as follows: First, copolymerized PP, maleic anhydride grafted polypropylene, POE, 2,6-di-tert-butyl-p-cresol, polyether hindered block copolymer, erucic acid amide were added into a high-speed mixer according to the above proportions and mixed at 40°C for 3 minutes, and then the mixed materials were extruded and granulated through a twin-screw extruder. The temperature setting temperature of each section of the extruder was: 170°C, 180°C, 200°C, 220°C, 220°C, 220°C, 210°C, 210°C, 200°C, and the screw speed was set to 210 rpm / min.
[0025] Example 2
[0026] The highly hydrophilic composite plastic material in this embodiment includes the following components in weight: 84.2 parts by weight of high molecular weight polymer copolymer PP, 2 parts of common hydrophilic agent sodium dodecyl sulfonate, 4 parts of compatibilizer maleic anhydride grafted polypropylene, 7 parts of toughening agent POE, 0.5 parts of antioxidant 2,6-di-tert-butyl-p-cresol, 2 parts of antistatic agent polyether hindered block copolymer, and 0.3 parts of lubricant erucamide. Copolymer PP was purchased from China SABIC (Tianjin) Petrochemical Co., Ltd. with a brand name of 87MK40T, maleic anhydride grafted polypropylene was purchased from Nantong Rizhisheng Molecular New Materials Technology Co., Ltd. with a brand name of CMG 9801, toughening agent POE was purchased from Dow Chemical with a brand name of 8150, antistatic agent was purchased from Akema with a brand name of Pebax® MV2080, and the lubricant used was purchased from Huanqi Chemical with a brand name of FINAWAX SE.
[0027] The preparation process of highly hydrophilic composite plastic materials is as follows: First, copolymerized PP, sodium dodecyl sulfate, maleic anhydride grafted polypropylene, POE, 2,6-di-tert-butyl-p-cresol, polyether hindered block copolymer, erucic acid amide were added to a high-speed mixer according to the above proportions and mixed at 40°C for 3 minutes, and then the mixed materials were extruded and granulated through a twin-screw extruder. The temperature setting temperatures of each section of the extruder were: 170°C, 180°C, 200°C, 220°C, 220°C, 220°C, 210°C, 210°C, 200°C, and the screw speed was set to 210 rpm / min.
[0028] Example 3
[0029] The highly hydrophilic composite plastic material in this embodiment includes the following components in weight: 82.2 parts by weight of high molecular polymer copolymer PP, 4 parts of common hydrophilic agent sodium dodecyl sulfonate, 4 parts of compatibilizer maleic anhydride grafted polypropylene, 7 parts of toughening agent POE, 0.5 parts of antioxidant 2,6-di-tert-butyl-p-cresol, 2 parts of antistatic agent polyether hindered block copolymer, and 0.3 parts of lubricant erucic acid amide. Copolymer PP was purchased from China SABIC (Tianjin) Petrochemical Co., Ltd. with a brand name of 87MK40T, maleic anhydride grafted polypropylene was purchased from Nantong Rizhisheng Molecular New Materials Technology Co., Ltd. with a brand name of CMG 9801, toughening agent POE was purchased from Dow Chemical with a brand name of 8150, antistatic agent was purchased from Akema with a brand name of Pebax® MV2080, and the lubricant used was purchased from Huanqi Chemical with a brand name of FINAWAX SE.
[0030] The preparation process of highly hydrophilic composite plastic materials is as follows: First, copolymerized PP, sodium dodecyl sulfate, maleic anhydride grafted polypropylene, POE, 2,6-di-tert-butyl-p-cresol, polyether hindered block copolymer, erucic acid amide were added to a high-speed mixer according to the above proportions and mixed at 40°C for 3 minutes, and then the mixed materials were extruded and granulated through a twin-screw extruder. The temperature setting temperatures of each section of the extruder were: 170°C, 180°C, 200°C, 220°C, 220°C, 220°C, 210°C, 210°C, 200°C, and the screw speed was set to 210 rpm / min.
[0031] Example 4
[0032] The highly hydrophilic composite plastic material in this embodiment includes the following components in weight: 80.2 parts by weight of high molecular weight polymer copolymer PP, 6 parts of common hydrophilic agent sodium dodecyl sulfonate, 4 parts of compatibilizer maleic anhydride grafted polypropylene, 7 parts of toughening agent POE, 0.5 parts of antioxidant 2,6-di-tert-butyl-p-cresol, 2 parts of antistatic agent polyether hindered block copolymer, and 0.3 parts of lubricant erucamide. Copolymer PP was purchased from China SABIC (Tianjin) Petrochemical Co., Ltd. with a brand name of 87MK40T, maleic anhydride grafted polypropylene was purchased from Nantong Rizhisheng Molecular New Materials Technology Co., Ltd. with a brand name of CMG 9801, toughening agent POE was purchased from Dow Chemical with a brand name of 8150, antistatic agent was purchased from Akema with a brand name of Pebax® MV2080, and the lubricant used was purchased from Huanqi Chemical with a brand name of FINAWAX SE.
[0033] The preparation process of highly hydrophilic composite plastic materials is as follows: First, copolymerized PP, sodium dodecyl sulfate, maleic anhydride grafted polypropylene, POE, 2,6-di-tert-butyl-p-cresol, polyether hindered block copolymer, erucic acid amide were added to a high-speed mixer according to the above proportions and mixed at 40°C for 3 minutes, and then the mixed materials were extruded and granulated through a twin-screw extruder. The temperature setting temperatures of each section of the extruder were: 170°C, 180°C, 200°C, 220°C, 220°C, 220°C, 210°C, 210°C, 200°C, and the screw speed was set to 210 rpm.
[0034] Example 5
[0035] The highly hydrophilic composite plastic material in this embodiment includes the following components in parts by weight: 81.7 parts by weight of high molecular weight polymer copolymer PP, 10 parts by weight of hyperbranched supramolecular hydrophilic agent, 2 parts by weight of compatibilizer, 5 parts by weight of toughening agent, 0.2 parts by weight of antioxidant, 1 part by weight of antistatic agent, and 0.1 parts by weight of lubricant.
[0036] The preparation method of the hyperbranched supramolecular hydrophilic agent in this embodiment comprises the following steps: S1: Heat glycerol to 225±25℃; S2: slowly add acrylamide white crystalline powder, wherein the molar ratio of glycerol to acrylamide is 1:3, and stir thoroughly at a stirring speed of 350±50 r / min; S3: After sufficient reaction, glycerol acrylamide is obtained, unreacted glycerol is washed away with water, and then fully dried in vacuum; S4: Methanol and ethanol are mixed in a weight ratio of 1:2, and then half the volume of distilled water (based on the total volume of methanol and ethanol, the volume of distilled water is 1 / 2 of the total volume of methanol and ethanol) is added, and the temperature is raised to 65±5°C; S5: Take glycerol acrylamide and amino-terminated polymer (manufacturer: Jinan Jinyu Chemical Co., Ltd., brand: fl1000), weigh them separately according to a molar ratio of 1:1, add them to the methanol-ethanol aqueous solution respectively, and stir them in a stirrer at a stirring temperature of 65±5°C, a stirring speed of 200±30r / min, and a stirring time of 15±5min to dissolve them, wherein the mass ratio of the methanol-ethanol aqueous solution to glycerol acrylamide is 1:1; S6: Finally, add (the molar ratio between monovalent long-chain fatty amine and propylene glycol acrylamide is 1:2) monovalent long-chain fatty amine (manufacturer is Jinan Jinyu Chemical Co., Ltd., brand is hexadecylamine superior grade), react at 65±5°C for 30±5min, reaction speed is 350±50r / min, and after sufficient reaction, a hyperbranched supramolecular hydrophilic agent is obtained; S7: Wash and remove the methanol and ethanol solutions, dehydrate in a centrifuge, and remove excess solution and water.
[0037] The high molecular polymer in this embodiment is copolymer PP, the compatibilizer is maleic anhydride grafted polypropylene, the toughening agent is POE, the antioxidant is 2,6-di-tert-butyl-p-cresol, the antistatic agent is a polyether hindered block copolymer, and the lubricant is erucamide.
[0038] Copolymer PP was purchased from Sinopec (Tianjin) Petrochemical Co., Ltd. with the brand name 87MK40T, maleic anhydride grafted polypropylene was purchased from Nantong Rizhisheng Molecular New Materials Technology Co., Ltd. with the brand name CMG 9801, toughening agent POE was purchased from Dow Chemical with the brand name 8150, antistatic agent was purchased from Akema with the brand name Pebax® MV2080, and the lubricant used was purchased from Huanqi Chemical with the brand name FINAWAX SE.
[0039] The method for preparing the highly hydrophilic composite material in this embodiment comprises the following steps: Step 1: Weighing: Weigh the high molecular polymer, hyperbranched supramolecular hydrophilic agent, compatibilizer, toughening agent, antioxidant, antistatic agent, and lubricant according to the weight ratio and set aside; Step 2: Mixing: firstly, the high molecular polymer, the hyperbranched supramolecular hydrophilic agent, the compatibilizer, the toughening agent, the antioxidant, the antistatic agent and the lubricant are uniformly mixed to obtain a mixture; then, the mixture is extruded and granulated to obtain a highly hydrophilic composite material.
[0040] The granulation in this embodiment is carried out by a twin-screw extruder. The temperature settings of each section of the extruder are: 170°C, 180°C, 200°C, 220°C, 220°C, 220°C, 210°C, 210°C, 200°C, and the screw speed is set to 210 rpm.
[0041] Example 6
[0042] The highly hydrophilic composite plastic material in this embodiment includes the following components in parts by weight: The weight parts of high molecular polymer copolymer PP are 47.5 parts, hyperbranched supramolecular hydrophilic agent is 30 parts, compatibilizer is 8 parts, toughening agent is 10 parts, antioxidant is 1 part, antistatic agent is 3 parts, and lubricant is 0.5 parts.
[0043] The preparation method of the hyperbranched supramolecular hydrophilic agent in this embodiment comprises the following steps: S1: Heat glycerol to 225±25℃; S2: slowly add acrylamide white crystalline powder, wherein the molar ratio of glycerol to acrylamide is 1:3, and stir thoroughly at a stirring speed of 350±50 r / min; S3: After sufficient reaction, glycerol acrylamide is obtained, unreacted glycerol is washed away with water, and then fully dried in vacuum; S4: Methanol and ethanol are mixed in a weight ratio of 1:2, and then half the volume of distilled water (based on the total volume of methanol and ethanol, the volume of distilled water is 1 / 2 of the total volume of methanol and ethanol) is added, and the temperature is raised to 65±5°C; S5: glycerol acrylamide and amino-terminated polymer (manufacturer: Jinan Jinyu Chemical Co., Ltd., brand: fl1000) were weighed in a molar ratio of 1:1, added into a methanol-ethanol aqueous solution, stirred in a stirrer at a temperature of 65±5°C, a stirring speed of 200±30r / min, and a stirring time of 15±5min to dissolve them, wherein the mass ratio of methanol-ethanol aqueous solution to glycerol acrylamide was 1:1; S6: Finally, add (the molar ratio between monovalent long-chain fatty amine and propylene glycol acrylamide is 1:2) monovalent long-chain fatty amine (manufacturer is Jinan Jinyu Chemical Co., Ltd., brand is hexadecylamine superior grade), react at 65±5°C for 30±5min, reaction speed is 350±50r / min, and after sufficient reaction, a hyperbranched supramolecular hydrophilic agent is obtained; S7: Wash and remove the methanol and ethanol solutions, dehydrate in a centrifuge, and remove excess solution and water.
[0044] The high molecular polymer in this embodiment is copolymer PP, the compatibilizer is maleic anhydride grafted polypropylene, the toughening agent is POE, the antioxidant is 2,6-di-tert-butyl-p-cresol, the antistatic agent is a polyether hindered block copolymer, and the lubricant is erucamide.
[0045] Copolymer PP was purchased from Sinopec (Tianjin) Petrochemical Co., Ltd. with the brand name 87MK40T, maleic anhydride grafted polypropylene was purchased from Nantong Rizhisheng Molecular New Materials Technology Co., Ltd. with the brand name CMG 9801, toughening agent POE was purchased from Dow Chemical with the brand name 8150, antistatic agent was purchased from Akema with the brand name Pebax® MV2080, and the lubricant used was purchased from Huanqi Chemical with the brand name FINAWAX SE.
[0046] The method for preparing the highly hydrophilic composite material in this embodiment comprises the following steps: Step 1: Weighing: Weigh the high molecular polymer, hyperbranched supramolecular hydrophilic agent, compatibilizer, toughening agent, antioxidant, antistatic agent, and lubricant according to the weight ratio and set aside; Step 2: Mixing: firstly, the high molecular polymer, the hyperbranched supramolecular hydrophilic agent, the compatibilizer, the toughening agent, the antioxidant, the antistatic agent and the lubricant are uniformly mixed to obtain a mixture; then, the mixture is extruded and granulated to obtain a highly hydrophilic composite material.
[0047] The granulation in this embodiment is carried out by a twin-screw extruder. The temperature settings of each section of the extruder are: 170°C, 180°C, 200°C, 220°C, 220°C, 220°C, 210°C, 210°C, 200°C, and the screw speed is set to 210 rpm.
[0048] Performance Testing
[0049] The highly hydrophilic composite plastic materials prepared in Examples 1 to 4 were tested according to ISO 15989 standard, and the results are shown in Table 1; Table 1 Test results Example 1 Example 2 Example 3 Example 4 Contact Angle 98 88 75 74 Compared with Examples 1 and 2, the addition of sodium dodecyl sulfate can effectively reduce the contact angle of the composite plastic material; compared with Examples 2, 3, and 4, when the mass content of sodium dodecyl sulfate is lower than 4%, the contact angle decreases significantly with the increase of the mass content of sodium dodecyl sulfate; when the mass content of sodium dodecyl sulfate is greater than 4%, the contact angle remains basically unchanged when the mass content of sodium dodecyl sulfate is further increased.
[0050] Comparative Example 1: It is basically the same as Example 3, except that no common hydrophilic agent is added.
[0051] Comparative Example 2: It is basically the same as Example 5, except that the proportion of the hyperbranched supramolecular hydrophilic agent is different. In Comparative Example 2, the proportion of the hyperbranched polymer hydrophilic agent is 6 parts.
[0052] The highly hydrophilic composite plastic materials prepared in Examples 5-6 and Comparative Examples 1-2 were tested according to ISO 15989 standard, and the results are shown in Table 2; Table 2 Test results Example 5 Example 6 Comparative Example 1 Comparative Example 2 Contact Angle 25 10 80 35 It can be seen from Examples 5-6 and Comparative Examples 1-2 that after the product is optimized, the contact angle of the product decreases, and the hyperbranched supramolecular hydrophilic agent has a greater influence on the contact angle.
[0053] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0054] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A highly hydrophilic composite plastic material, characterized in that: The invention comprises the following components by weight: 47.5-86.2 parts of high molecular polymer, 10-30 parts of hyperbranched supramolecular hydrophilic agent, 0-6 parts of common hydrophilic agent, 2-8 parts of compatibilizer, 5-10 parts of toughening agent, 0.2-1 parts of antioxidant, 1-3 parts of antistatic agent and 0.1-0.5 parts of lubricant. The hyperbranched supramolecular hydrophilic agent is prepared by reacting glycerol acrylamide, amino-terminated polymer and long-chain fatty amine.
2. The highly hydrophilic composite plastic material according to claim 1, characterized in that: The preparation method of the hyperbranched supramolecular hydrophilic agent comprises at least the following steps: Step 1: Weigh glycerol acrylamide and amino-terminated polymer separately in a molar ratio of 1:1; Step 2: adding the glycerol acrylamide and the amino-terminated polymer weighed in step 1 to a polar solvent at 50-80° C., stirring while adding, at a stirring speed of 100-300 r / min, and a stirring time of 20-40 min, to dissolve them, wherein the polar solvent is selected from one or more combinations of methanol, ethanol, and water; Step 3: weigh a monobasic long-chain fatty amine, wherein the molar ratio of the monobasic long-chain fatty amine to propylene glycol acrylamide is 1:2, and the weighed monobasic long-chain fatty amine is added to the mixture in step 2, and reacted at 50-85° C. for 20-30 min, with a stirring speed of 200-500 r / min during the reaction. After the reaction is completed, a hyperbranched supramolecular hydrophilic agent is obtained.
3. The highly hydrophilic composite plastic material according to claim 2, characterized in that: The preparation method of glycerol acrylamide at least comprises the following steps: S1: Heat glycerol to 200-250°C; S2: slowly adding acrylamide to glycerol, wherein the molar ratio of glycerol to acrylamide is 1:3, and stirring at a stirring speed of 200-500 r / min; S3: After sufficient reaction, glycerol acrylamide is obtained, unreacted glycerol is washed away with water, and the mixture is fully dried in vacuum to obtain purified glycerol acrylamide.
4. The highly hydrophilic composite plastic material according to claim 1, characterized in that: The common hydrophilic agent is one or more combinations of polyvinyl alcohol, azodimethyldisilane, and sodium dodecyl sulfate.
5. The highly hydrophilic composite plastic material according to claim 1, characterized in that: The high molecular polymer is one or more combinations of polypropylene, polyamide, polybutylene terephthalate, polyethylene terephthalate, and polyphenylene sulfide, and the compatibilizer is at least one of maleic anhydride grafted polypropylene or a silane coupling agent.
6. The highly hydrophilic composite plastic material according to claim 1, characterized in that: The toughening agent is one or more combinations of EPDM rubber, ethylene-1-octene or butene copolymer, maleic anhydride grafted ethylene-1-octene or butene copolymer, and maleic anhydride grafted EPDM rubber.
7. The highly hydrophilic composite plastic material according to claim 1, characterized in that: The antioxidant is one or more combinations of 2,6-di-tert-butyl-p-cresol, β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, tris(nonylphenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, dioctadecyl pentaerythritol diphosphite, and dilauryl thiodipropionate.
8. The highly hydrophilic composite plastic material according to claim 1, characterized in that: The antistatic agent is one or more combinations of glyceryl monostearate, ethoxylated amine, N,N-dihydroxyethyl octadecylamine, polyether hindered block copolymer, and polyether block amide.
9. The highly hydrophilic composite plastic material according to claim 1, characterized in that: The lubricant is at least one of erucamide and oleamide.
10. A method for preparing a highly hydrophilic composite plastic material according to any one of claims 1 to 9, characterized in that: At least the following steps are included: Step 1: Weighing: Weigh the high molecular polymer, hyperbranched supramolecular compound, common hydrophilic agent, compatibilizer, toughening agent, antioxidant, antistatic agent, and lubricant according to the weight ratio and set aside; Step 2: Mixing: firstly, a high molecular polymer, a hyperbranched supramolecular hydrophilic agent, a common hydrophilic agent, a compatibilizer, a toughening agent, an antioxidant, an antistatic agent, and a lubricant are uniformly mixed to obtain a mixture; then, the mixture is extruded and granulated to obtain a highly hydrophilic composite material, wherein the granulation is performed by a twin-screw extruder, and the temperature of each section of the twin-screw extruder is between 170 and 250° C., and the screw speed is between 180 and 500 rpm / min.
Citation Information
Patent Citations
Hydrophilic polypropylene mixture and preparing method and application thereof
CN102675730A
Graphene composite antistatic polypropylene plastic and preparation method thereof
CN110172208A
Poly(N-isopropylacrylamide) molecular brush polysebacic acid glyceride fiber membrane, preparation method thereof and application of fiber membrane
CN110359276A
Hyperbranched hydrophilic agent, hydrophilic modified resin and preparation method thereof
CN115181261A
Cited By
Hydrophilic syndiotactic polypropylene composite material with high crystallization temperature and preparation method thereof