Maleic anhydride-isobutylene-styrene terpolymer microsphere as well as preparation method and application thereof
By preparing maleic anhydride-isobutylene-styrene terpolymer microspheres as polar modifiers, the problem of improving hydrophilicity of polyolefin materials is solved, and the water contact angle reduction and mechanical properties are achieved is achieved, and traditional modification is avoided. flaws of sexual methods.
Patent Information
- Application Number
- CN202310512797.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-08
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-05-08
AI Technical Summary
In the prior art, the preparation process of styrene-maleic anhydride copolymer is complicated, and does not involve the preparation scheme of maleic anhydride-isobutene-styrene terpolymer, and is used to improve the hydrophilicity of polyolefins. The grafting rate of modifiers is low, the hydrophilicity improvement is limited and the aging resistance is poor.
Maleic anhydride-isobutylene-styrene terpolymer microspheres are used as polar modifiers, and the polymerization reaction is carried out to obtain terpolymer microspheres by dissolving the polymerized monomer and the initiator in an inert atmosphere. , the specific molar ratio and molar content ensure uniform particle size and clean surface of the microspheres, which are used in polyolefins to significantly reduce the water contact angle without affecting the mechanical properties.
The significant hydrophilicity of polyolefin materials is achieved, the water contact angle is reduced, and the material mechanical properties remain stable, avoiding the high cost and safety risks of traditional modification methods.
Smart Images

Figure CN118909185A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of high molecular polymers, and in particular to maleic anhydride-isobutylene-styrene terpolymer microspheres and a preparation method and application thereof. Background Art
[0002] Maleic anhydride copolymers have a wide range of applications due to their good processing properties, excellent reactivity, good hydrophilicity and low price. Sun Dali et al. achieved the purification of high-concentration lead ion wastewater by using styrene-maleic anhydride copolymers in "Application research of styrene-maleic anhydride copolymers for continuous multi-stage treatment of high-concentration lead ion wastewater, New Chemical Materials, 2022, 50(01): 303-307+312".
[0003] Tang Longdong et al. used styrene-maleic anhydride copolymer as a modifier to prepare polyamide 6 / glass fiber / styrene-maleic anhydride copolymer composites in "Study on wear resistance modification of nylon 6 / glass fiber composites by styrene-maleic anhydride copolymer, Plastic Industry. 2017, 45(04): 48-51.", which effectively improved the wear resistance of polyamide 6 / glass fiber composites.
[0004] In the prior art, most copolymers containing maleic anhydride are prepared by solution or traditional precipitation polymerization. Ling Zhicheng et al. prepared star-shaped maleic anhydride-styrene copolymers by precipitation polymerization in "Esterification and Application of Star-shaped Styrene-Maleic Anhydride Copolymers [J]. Coatings and Protection, 2019, 40(11): 20-25.", and reduced the glass transition temperature of the copolymers by esterification modification, thereby improving their dispersion effect on pigments.
[0005] Shi Xuelong et al. prepared styrene-maleic anhydride random copolymers by solution polymerization using green solvent dimethyl carbonate as solvent in "Synthesis and characterization of styrene-maleic anhydride random copolymers in green solvents, Plastics Science and Technology, 2019, 47(02): 24-28."
[0006] Polypropylene is an important general-purpose thermoplastic material, which is widely used due to its good mechanical properties, processing performance, corrosion resistance and electrical insulation. At the same time, polypropylene is also a crystalline polymer with a regular structure and lacks active groups on the surface. Therefore, its water contact angle is large and its surface wettability is poor, which limits its application in water environment, surface coating, surface bonding and composite materials. At present, the methods to improve the hydrophilicity of polypropylene materials mainly include flame treatment, isopropyl alcohol wiping and adding polar modifiers such as grafted polypropylene. Among them, flame treatment and isopropyl alcohol wiping are the most commonly used, but there are problems such as high labor costs and high safety risks.
[0007] However, in the prior art, there is no report that a copolymer comprising maleic anhydride-isobutylene-styrene can be added as a polar modifier to a polymer system such as polypropylene to improve its hydrophilicity. Summary of the invention
[0008] The purpose of the present invention is to overcome the problems that the preparation process of styrene-maleic anhydride copolymer in the prior art is complicated, and no scheme for preparing copolymers containing maleic anhydride-isobutylene-styrene is involved. In addition, the grafting rate of grafted polypropylene polar modifiers currently used to improve the hydrophilicity of polyolefin systems is low, the improvement of hydrophilicity is limited, and the aging resistance is poor. Provided are maleic anhydride-isobutylene-styrene terpolymer microspheres and a preparation method and application thereof. The surface of the maleic anhydride-isobutylene-styrene terpolymer microspheres is clean and pollution-free, and the microsphere particles are uniform. The structural units provided by isobutylene and the structural units provided by styrene have a specific molar ratio, and are matched with a specific molar content of the structural units provided by maleic anhydride. The microspheres are used as polar modifiers in polyolefins, and the water contact angle of the polyolefin material can be reduced without causing a decrease in the mechanical properties of the material.
[0009] In order to achieve the above-mentioned object, the first aspect of the present invention provides a maleic anhydride-isobutylene-styrene terpolymer microsphere, wherein, based on the total molar amount of the terpolymer, the molar content of the structural unit provided by maleic anhydride is 47-52%; the molar ratio of the structural unit provided by isobutylene to the structural unit provided by styrene is 1:0.2-7.5.
[0010] The second aspect of the present invention provides a method for preparing maleic anhydride-isobutylene-styrene terpolymer microspheres, wherein the method comprises the following steps:
[0011] S1. In an inert atmosphere, dissolving the polymerization monomer and the initiator in a reaction medium to form a homogeneous solution;
[0012] S2, after the homogeneous solution is subjected to polymerization reaction to obtain a copolymer emulsion suspension, separation is performed to obtain the terpolymer microspheres;
[0013] Wherein, the polymerization monomers are maleic anhydride, styrene and isobutylene;
[0014] Based on the total mass of the polymerized monomers, the molar content of maleic anhydride is 47-52%;
[0015] The molar ratio of the isobutylene to the styrene is 1:0.2-7.5.
[0016] The third aspect of the present invention provides maleic anhydride-isobutylene-styrene terpolymer microspheres prepared by the preparation method described in the second aspect.
[0017] The fourth aspect of the present invention provides a use of the maleic anhydride-isobutylene-styrene terpolymer microspheres described in the first aspect or the third aspect as a polar modifier in polyolefins.
[0018] Through the above technical scheme, the maleic anhydride-isobutylene-styrene terpolymer microspheres provided by the present invention and the preparation method and application thereof obtain the following beneficial effects: the maleic anhydride-isobutylene-styrene terpolymer microspheres have uniform particle size and clean surface without pollution. The structural units provided by isobutylene and the structural units provided by styrene have a specific molar ratio, and the molar content of the structural units provided by maleic anhydride is matched, so that the terpolymer microspheres have good application as a polar modifier in polyolefins, significantly reducing the water contact angle of polyolefin materials without causing a decrease in the mechanical properties of the materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 is the infrared spectrum of the copolymer microspheres prepared in Example 1;
[0020] Figure 2 is a scanning electron microscope image of the copolymer microspheres prepared in Example 1. DETAILED DESCRIPTION
[0021] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0022] The first aspect of the present invention provides a maleic anhydride-isobutylene-styrene terpolymer microsphere, wherein, based on the total molar amount of the terpolymer, the molar content of the structural unit provided by maleic anhydride is 47-52%; the molar ratio of the structural unit provided by isobutylene to the structural unit provided by styrene is 1:0.2-7.5.
[0023] In the present invention, in the terpolymer microspheres, the structural units provided by isobutylene and the structural units provided by styrene satisfy the above-mentioned molar ratio range, and the molar content of the structural units provided by maleic anhydride is matched, so that when the terpolymer microspheres are used as a polar modifier in polyolefins, the water contact angle of the polyolefin material can be significantly reduced without causing a decrease in the mechanical properties of the material.
[0024] According to the present invention, based on the total molar amount of the terpolymer, the molar content of the structural unit provided by maleic anhydride is 48-51%; the molar ratio of the structural unit provided by isobutylene to the structural unit provided by styrene is 1:1-5.
[0025] According to the present invention, the particle size of the terpolymer microspheres is 500-920 μm.
[0026] In the present invention, the particle size of the terpolymer microspheres meets the above range, and can further increase the water contact angle of the polyolefin when used.
[0027] Furthermore, the particle size of the terpolymer microspheres is 530-800 nm.
[0028] The second aspect of the present invention provides a method for preparing maleic anhydride-isobutylene-styrene terpolymer microspheres, wherein the method comprises the following steps:
[0029] S1. In an inert atmosphere, dissolving the polymerization monomer and the initiator in a reaction medium to form a homogeneous solution;
[0030] S2, after the homogeneous solution is subjected to polymerization reaction to obtain a copolymer emulsion suspension, separation is performed to obtain the terpolymer microspheres;
[0031] Wherein, the polymerization monomers are maleic anhydride, styrene and isobutylene;
[0032] Based on the total mass of the polymerized monomers, the molar content of maleic anhydride is 47-52%;
[0033] The molar ratio of the isobutylene to the styrene is 1:0.2-7.5.
[0034] In the present invention, maleic anhydride monomer, isobutylene monomer and styrene monomer are polymerized in a specific ratio by copolymerization, so that the prepared maleic anhydride-isobutylene-styrene copolymer presents microspheres with excellent uniformity, and the terpolymer has the characteristics of clean surface and uniform particle size. The terpolymer microspheres obtained are polar, can significantly reduce the water contact angle, and improve its hydrophilicity.
[0035] According to the present invention, based on the total mass of the polymerized monomers, the molar content of the maleic anhydride is 48-51%; the molar ratio of the isobutylene to the styrene is 1:1-5.
[0036] According to the present invention, based on the total weight of the homogeneous solution, the mass concentration of the polymerizable monomer is 4-23 wt %, preferably 6-21 wt %.
[0037] According to the present invention, the initiator is an organic peroxide and / or an azo compound.
[0038] According to the present invention, the organic peroxide is at least one selected from dibenzoyl peroxide, diisopropyl peroxide, di-tert-butyl peroxide, dodecyl peroxide, tert-butyl perbenzoate, diisopropyl peroxydicarbonate and dicyclohexyl peroxydicarbonate.
[0039] According to the present invention, the azo compound is selected from azobisisobutyronitrile and / or azobisisoheptanenitrile.
[0040] According to one embodiment of the present invention, the reaction medium is an organic acid alkyl ester.
[0041] According to one embodiment of the present invention, the reaction medium is a mixed solvent of a ketone compound and an alkane compound.
[0042] According to one embodiment of the present invention, the reaction medium is a mixed solvent of an organic acid alkyl ester, a ketone compound and an alkane compound.
[0043] In the present invention, the compound selected from the above types is used as a reaction medium, which can cooperate with the specific amount of polymerization monomers described in the present invention, and no additional additives such as stabilizers and precipitants are required to be added, so that a self-stabilized precipitation polymerization reaction of maleic anhydride, isobutylene and styrene can be achieved. No stabilizer or co-stabilizer needs to be added to the polymerization reaction system, and the system has a self-stabilizing dispersion effect. The obtained copolymer microspheres have a clean surface and a uniform particle size. The copolymer microspheres thus obtained can be used as a polar modifier in polyolefins to reduce the water contact angle of the polyolefin material.
[0044] Furthermore, when a mixed solvent of a ketone compound and an alkane compound or a mixed solvent of an organic acid alkyl ester, a ketone compound and an alkane compound is used, the problem of the material having a special odor caused by using an ester solvent alone can be improved.
[0045] According to the present invention, the general formula of the organic acid alkyl ester is R1COOR2, wherein R1 is selected from H, C 1-5 Alkyl or C 6-10 Aralkyl, R2 is C 1-10 of alkyl.
[0046] In the present invention, C 1-5 The alkyl group includes a C1-C5 straight-chain alkyl group and a C3-C5 branched-chain alkyl group, and specific examples thereof may include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, and the like.
[0047] In the present invention, the term "aralkyl" can be represented by Ar x-N-, wherein x Ar are the same or different and are independently aryl, N is an alkyl, and x is an integer from 1 to 3. 10 Specific examples of the aralkyl group may include, but are not limited to, phenylmethyl, phenylethyl, phenyl-n-propyl, phenyl-n-butyl, phenyl-t-butyl, phenyl-isopropyl, phenyl-n-butyl and the like.
[0048] Furthermore, R1 is C 1-5 Alkyl or C 6-9 Aralkyl, R2 is C 1-7 of alkyl.
[0049] According to a particularly preferred embodiment of the present invention, the organic acid alkyl ester is selected from at least one of ethyl formate, propyl formate, isobutyl formate, amyl formate, ethyl acetate, butyl acetate, isobutyl acetate, sec-butyl acetate, amyl acetate, isoamyl acetate, benzyl acetate, methyl propionate, ethyl propionate, butyl propionate, methyl butyrate, ethyl butyrate, butyl butyrate, isoamyl butyrate, ethyl isovalerate, isoamyl isovalerate, methyl benzoate, ethyl benzoate, propyl benzoate, butyl benzoate, isoamyl benzoate, methyl phenylacetate and ethyl phenylacetate.
[0050] According to the present invention, the ketone compound has a structure shown in Formula I:
[0051]
[0052] Wherein, R3 and R4 are alkyl groups having 1 to 6 carbon atoms.
[0053] Furthermore, R3 and R4 are alkyl groups having 1 to 3 carbon atoms.
[0054] According to the present invention, the alkane compound is an alkane having 6-12 carbon atoms, preferably an alkane having 6-10 carbon atoms.
[0055] According to one embodiment of the present invention, the reaction medium is a mixed solvent of a ketone compound and an alkane compound, wherein the amount of the alkane compound is 50-90 vol % of the mixed solvent of the ketone compound and the alkane compound.
[0056] In the present invention, the amount of the alkane compound used satisfies the above range, so that the prepared copolymer microspheres can be applied to polyolefins to further reduce the water contact angle of the polyolefins.
[0057] Furthermore, the amount of the alkane compound used is 50-80 vol% of the mixed solvent of the ketone compound and the alkane compound.
[0058] According to one embodiment of the present invention, the reaction medium is a mixed solvent of an organic acid alkyl ester, a ketone compound and an alkane compound, wherein the amount of the alkane compound is 0-50 vol%, preferably 1-30 vol% of the mixed solvent; the amount of the ketone compound is 1-10 vol%, preferably 1-5 vol% of the mixed solvent of the organic acid alkyl ester, a ketone compound and an alkane compound.
[0059] In the present invention, it should be noted that when the reaction medium is a mixed solvent of an organic acid alkyl ester, a ketone compound and an alkane compound, the amounts of the ketone compound and the alkane compound used are not both 0.
[0060] In the present invention, the polymerization reaction is carried out in a protective atmosphere, and the protective atmosphere can be provided by conventional inert gas or nitrogen in the prior art.
[0061] According to the present invention, the conditions of the polymerization reaction include: polymerization temperature of 40-95°C, preferably 50-80°C; polymerization time of 1-24h, preferably 3-10h.
[0062] In the present invention, in order to achieve self-stabilization of the polymerization system and obtain copolymer microspheres with uniform particle size and clean and pollution-free surface, the inventors studied the conditions of the polymerization reaction. The study shows that when the polymerization temperature is 40-95°C and the polymerization time is 1-24h, the polymerization system forms a stable self-stabilizing system, in which maleic anhydride, isobutylene and styrene are polymerized to form microspheres, and the microspheres do not aggregate and have good dispersibility.
[0063] In the present invention, the separation may be a conventional solid-liquid separation method in the art, such as centrifugal separation.
[0064] In the present invention, when centrifugal separation is adopted, the centrifugal speed is 1500-5000 rad / min, and the centrifugal time is 5-60 min.
[0065] The third aspect of the present invention provides maleic anhydride-isobutylene-styrene terpolymer microspheres prepared by the preparation method described in the second aspect.
[0066] According to the present invention, based on the total molar amount of the terpolymer, the molar content of the structural unit provided by maleic anhydride is 47-52%, preferably 48-51%; the molar ratio of the structural unit provided by isobutylene to the structural unit provided by styrene is 1:0.2-7.5, preferably 1:1-5.
[0067] According to the present invention, the particle size of the terpolymer microspheres is 500-920 nm, preferably 530-800 nm.
[0068] The fourth aspect of the present invention provides a use of the maleic anhydride-isobutylene-styrene terpolymer microspheres described in the first aspect or the third aspect as a polar modifier in polyolefins.
[0069] According to the present invention, the amount of the terpolymer microspheres is 1-10 wt % based on the total weight of the polyolefin.
[0070] In the present invention, the amount of the terpolymer microspheres used meets the above range, which can reduce the water contact angle of the polyolefin material without reducing the mechanical properties of the polyolefin material.
[0071] Furthermore, based on the total weight of the polyolefin, the amount of the terpolymer microspheres is 2-6 wt %.
[0072] According to the present invention, the polyolefin is polypropylene.
[0073] According to the present invention, the polypropylene has a melt index of 3-12 g / 10 min at 190° C. and a load of 2.16 kg.
[0074] In the present invention, the melt index of the polypropylene meets the above range and can be better blended with the microsphere material.
[0075] Furthermore, the polypropylene has a melt index of 4-10 g / 10 min at 190° C. and a load of 2.16 kg.
[0076] The present invention will be described in detail below by way of examples. In the following examples,
[0077] The polymerization yield (C p ) to calculate
[0078] Cp=Mp×100% / Mm
[0079] Wherein, Mp is the mass of the obtained polymer; Mm is the total mass of the added monomers;
[0080] The morphology and particle size of copolymer microspheres were observed and measured using scanning electron microscopy (SEM).
[0081] The infrared spectra of copolymers were tested by FI-IR;
[0082] The content of each structural unit in the copolymer is 1 H NMR was tested by 1 The content of each structural unit is calculated from the ratio of the peak area corresponding to the characteristic hydrogen in the corresponding structural unit in HNMR;
[0083] The water contact angle test of the modified polypropylene material was carried out in accordance with GB-T-30693-2014, using a sample size of 20mm*20mm*2mm and a dynamic contact angle meter.
[0084] The room temperature Izod notched impact strength of the modified polypropylene material was tested in accordance with GB-T-1843-2008.
[0085] Other raw materials used in the examples and comparative examples are all commercially available.
[0086] Example 1
[0087] 49g maleic anhydride, 1g azobisisobutyronitrile, 8.4g isobutylene, 36.4g styrene, 500mL isoamyl acetate (R1 is a C1 alkyl group, R2 is a C5 alkyl group) were added to a 2L reactor, the materials were mixed evenly, the temperature was raised to 70°C, and the reaction was performed for 4h. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 85.43g of maleic anhydride-isobutylene-styrene terpolymer microspheres, and the yield of the corresponding copolymer was 90.12%. The particle size of maleic anhydride-isobutylene-styrene terpolymer microsphere A1 was 650nm. Among them, the molar content of maleic anhydride was 50%; the molar ratio of isobutylene to styrene was 1:2.3.
[0088] like Figure 1 The FI-IR spectrum of copolymer microspheres A1 is shown at 1785 cm -1 、1850cm -1 It is the characteristic absorption peak of anhydride group.
[0089] like Figure 2 The SEM image of the copolymer microsphere A1 is shown. It can be seen from the image that the particles of the copolymer microsphere are uniform and the surface of the particles is clean and not contaminated.
[0090] Example 2
[0091] 49g maleic anhydride, 1g azobisisobutyronitrile, 4.66g isobutylene, 43.43g styrene, 500mL isoamyl acetate (R1 is a C1 alkyl group, R2 is a C5 alkyl group) were added to a 2L reactor, the materials were mixed evenly, the temperature was raised to 70°C, and the reaction was performed for 6h. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 88.08g of maleic anhydride-isobutylene-styrene terpolymer microspheres, and the yield of the corresponding copolymer was 89.79%. The particle size of maleic anhydride-isobutylene-styrene terpolymer microsphere A2 was 750nm. Among them, the molar content of maleic anhydride was 50%; the molar ratio of isobutylene to styrene was 1:5.
[0092] Example 3
[0093] 51g maleic anhydride, 1g azobisisobutyronitrile, 14g isobutylene, 26g styrene, 500mL butyl acetate (R1 is a C1 alkyl group, R2 is a C4 alkyl group) were added to a 2L reactor, the materials were mixed evenly, the temperature was raised to 65°C, and the reaction was performed for 6h. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 78.38g of maleic anhydride-isobutylene-styrene terpolymer microspheres, and the yield of the corresponding copolymer was 85.2%. The particle size of maleic anhydride-isobutylene-styrene terpolymer microsphere A3 was 590nm. Among them, the molar content of maleic anhydride was 51%; the molar ratio of isobutylene to styrene was 1:1.
[0094] Example 4
[0095] 47.08g maleic anhydride, 1g azobisisobutyronitrile, 3.51g isobutylene, 45.57g styrene, 500mL butyl acetate (R1 is a C1 alkyl group, R2 is a C4 alkyl group) were added to a 2L reactor, the materials were mixed evenly, the temperature was raised to 65°C, and the reaction was performed for 8h. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 91.18g of maleic anhydride-isobutylene-styrene terpolymer microspheres, and the yield of the corresponding copolymer was 93.85%. The particle size of maleic anhydride-isobutylene-styrene terpolymer microsphere A4 was 770nm. Among them, the molar content of maleic anhydride was 49%; the molar ratio of isobutylene to styrene was 1:7.3.
[0096] Example 5
[0097] 51g maleic anhydride, 1g azobisisobutyronitrile, 19.64g isobutylene, 15.62g styrene, 500mL isoamyl acetate (R1 is a C1 alkyl group, R2 is a C5 alkyl group) were added to a 2L reactor, the materials were mixed evenly, the temperature was raised to 70°C, and the reaction was performed for 4h. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 74.92g of maleic anhydride-isobutylene-styrene terpolymer microspheres, and the yield of the corresponding copolymer was 85.86%. The particle size of maleic anhydride-isobutylene-styrene terpolymer microsphere A5 was 548nm. Among them, the molar content of maleic anhydride was 51%; the molar ratio of isobutylene to styrene was 1:0.4.
[0098] Example 6
[0099] 49g maleic anhydride, 1g azobisisobutyronitrile, 22.44g isobutylene, 10.42g styrene, 500mL ethyl acetate (R1 is a C1 alkyl group, R2 is a C2 alkyl group) were added to a 2L reactor, the materials were mixed evenly, the temperature was raised to 70°C, and the reaction was performed for 4h. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 56.86g of maleic anhydride-isobutylene-styrene terpolymer microspheres, and the yield of the corresponding copolymer was 86.11%. The particle size of maleic anhydride-isobutylene-styrene terpolymer microsphere A6 was 532nm. Among them, the molar content of maleic anhydride was 50%; the molar ratio of isobutylene to styrene was 1:0.25.
[0100] Example 7
[0101] 49g maleic anhydride, 1g azobisisobutylene nitrile, 8.4g isobutylene, 36.4g styrene, 250mL acetone (50vol%), 250mL (50vol%) hexane were added to a 2L reactor, the materials were mixed evenly, the temperature was raised to 50°C, and the reaction was performed for 6h. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 84.92g of maleic anhydride-isobutylene-styrene terpolymer microspheres, and the yield of the corresponding copolymer was 89.58%. The particle size of maleic anhydride-isobutylene-styrene terpolymer microsphere A7 was 676nm. Among them, the molar content of maleic anhydride was 51%; the molar ratio of isobutylene to styrene was 1:2.3.
[0102] Example 8
[0103] The method of Example 1 was followed, except that the polymerization reaction temperature was 85°C and the reaction time was 6 hours. 74.21 g of maleic anhydride-isobutylene-styrene terpolymer microspheres were obtained, and the yield of the corresponding copolymer was 78.28%. The particle size of maleic anhydride-isobutylene-styrene terpolymer microspheres A8 was 643 nm. The molar content of maleic anhydride was 50%; and the molar ratio of isobutylene to styrene was 1:2.3.
[0104] Example 9
[0105] The method of Example 7 was followed, except that 50 mL (10 vol%) of acetone and 450 mL (90 vol%) of hexane were used to prepare 65.73 g of maleic anhydride-isobutylene-styrene terpolymer microspheres, with a yield of 69.34% of the corresponding copolymer. The particle size of maleic anhydride-isobutylene-styrene terpolymer microsphere A9 was 918 nm. The molar content of maleic anhydride was 50%; the molar ratio of isobutylene to styrene was 1:2.3.
[0106] Example 10
[0107] 49g maleic anhydride, 1g azobisisobutyronitrile, 8.4g isobutylene, 36.4g styrene, 300mL (60vol%) of ethyl acetate, 20mL (4vol%) of acetone, 180mL (36vol%) of hexane, 80.16g of maleic anhydride-isobutylene-styrene terpolymer microspheres were prepared, and the yield of the corresponding copolymer was 84.56%. The particle size of maleic anhydride-isobutylene-styrene terpolymer microsphere A10 was 665nm. Among them, the molar content of maleic anhydride was 50%; the molar ratio of isobutylene to styrene was 1:2.3.
[0108] Comparative Example 1
[0109] The method of Example 1 was followed, except that 49 g of maleic anhydride, 1 g of azobisisobutyronitrile, 25.2 g of isobutylene, and 5.2 g of styrene were used to obtain 70.52 g of maleic anhydride-isobutylene-styrene terpolymer microspheres, with a corresponding copolymer yield of 88.71%. The particle size of the maleic anhydride-isobutylene-styrene terpolymer microsphere D1 was 492 nm. The molar content of maleic anhydride was 50%; and the molar ratio of isobutylene to styrene was 1:0.11.
[0110] Comparative Example 2
[0111] The method of Example 1 was followed, except that 49 g of maleic anhydride, 1 g of azobisisobutyronitrile, 52 g of styrene, and no isobutylene were used to obtain 96.67 g of maleic anhydride-styrene binary copolymer microspheres, with a yield of 94.77% for the corresponding copolymer. The particle size of the maleic anhydride-styrene binary copolymer microsphere D2 was 947 nm. The molar content of maleic anhydride was 50%, and the molar content of styrene was 50%.
[0112] Test Case
[0113] Extrusion granulation: The copolymer microspheres prepared in the examples and comparative examples were added to polypropylene in the amounts shown in Table 1, and extrusion granulation was performed to obtain polypropylene materials. The experimental conditions for granulation were: feeding section 180°C; plasticizing section 190°C; homogenizing section 195°C; die head 180°C, and the rotation speed was 150rad / min.
[0114] The existing isopropyl alcohol wiping treatment to improve the hydrophilicity of polypropylene materials was used as a control example. The specific treatment method is as follows:
[0115] (1) Clean the surface of a polypropylene sample (20 mm*20 mm*2 mm) with deionized water and blow it clean with nitrogen;
[0116] (2) Soak the wiping cloth with the isoalcohol reagent, wring it out and wipe the surface of the polypropylene sample evenly, and let it dry naturally;
[0117] (3) Repeat step (2) three times to obtain the modified polypropylene material.
[0118] The performance results of the material obtained by adding copolymer microspheres to polypropylene and the polypropylene material improved by wiping with isopropyl alcohol are shown in Table 1.
[0119] Table 1
[0120]
[0121]
[0122] It can be seen from the results in Table 1 that when the terpolymer microspheres prepared by Examples 1-9 of the present invention are applied to polypropylene, the water contact angle of polypropylene can be effectively reduced, and the water contact angle is no more than 70°, while the mechanical properties are not reduced.
[0123] Among them, the preferred embodiments 1-3 and 10 can further reduce the water contact angle to achieve an effect of the water contact angle being no greater than 63°.
[0124] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A maleic anhydride-isobutylene-styrene terpolymer microsphere, in, Based on the total molar amount of the terpolymer, the molar content of the structural unit provided by maleic anhydride is 47-52%; the molar ratio of the structural unit provided by isobutylene to the structural unit provided by styrene is 1:0.2-7.
5.
2. The terpolymer microspheres according to claim 1, in, Based on the total molar amount of the terpolymer, the molar content of the structural unit provided by maleic anhydride is 48-51%; the molar ratio of the structural unit provided by isobutylene to the structural unit provided by styrene is 1:1-5; Preferably, the particle size of the terpolymer microspheres is 500-920 nm, preferably 530-800 nm.
3. A method for preparing maleic anhydride-isobutylene-styrene terpolymer microspheres, in, The method comprises the following steps: S1. In an inert atmosphere, dissolving the polymerization monomer and the initiator in a reaction medium to form a homogeneous solution; S2, after the homogeneous solution is subjected to polymerization reaction to obtain a copolymer emulsion suspension, separation is performed to obtain the terpolymer microspheres; Wherein, the polymerization monomers are maleic anhydride, styrene and isobutylene; Based on the total mass of the polymerized monomers, the molar content of maleic anhydride is 47-52%; The molar ratio of the isobutylene to the styrene is 1:0.2-7.
5.
4. The preparation method according to claim 3, in, Based on the total mass of the polymerized monomers, the molar content of the maleic anhydride is 48-51%; the molar ratio of the isobutylene to the styrene is 1:1-5; Preferably, based on the total weight of the homogeneous solution, the mass concentration of the polymerizable monomer is 4-23 wt %, preferably 6-21 wt %.
5. The preparation method according to claim 3 or 4, in, The initiator is an organic peroxide and / or an azo compound; Preferably, the organic peroxide is at least one selected from dibenzoyl peroxide, diisopropyl peroxide, di-tert-butyl peroxide, dodecyl peroxide, tert-butyl perbenzoate, diisopropyl peroxydicarbonate and dicyclohexyl peroxydicarbonate; Preferably, the azo compound is selected from azobisisobutyronitrile and / or azobisisoheptanenitrile; Preferably, the reaction medium is an organic acid alkyl ester, or a mixed solvent of a ketone compound and an alkane compound, or a mixed solvent of an organic acid alkyl ester, a ketone compound and an alkane compound; Preferably, the general formula of the organic acid alkyl ester is R 1 COOR 2 , where R 1 Selected from H, C 1-5 Alkyl or C 6-10 The aralkyl group, R 2 C 1-10 The alkyl group; Preferably, R 1 C 1-5 Alkyl or C 6-9 The aralkyl group, R 2 C 1-7 The alkyl group; More preferably, the organic acid alkyl ester is selected from at least one of ethyl formate, propyl formate, isobutyl formate, pentyl formate, ethyl acetate, butyl acetate, isobutyl acetate, sec-butyl acetate, pentyl acetate, isoamyl acetate, benzyl acetate, methyl propionate, ethyl propionate, butyl propionate, methyl butyrate, ethyl butyrate, butyl butyrate, isoamyl butyrate, ethyl isovalerate, isoamyl isovalerate, methyl benzoate, ethyl benzoate, propyl benzoate, butyl benzoate, isoamyl benzoate, methyl phenylacetate and ethyl phenylacetate.
6. The preparation method according to claim 5, in, The ketone compound has a structure shown in Formula I: Among them, R 3 and R 4 Each independently is C 1-6 The alkyl group is preferably C 1-3 The alkyl group; Preferably, the alkane compound is C 6-12 Alkanes, preferably C 6-10 of alkanes; Preferably, the amount of the alkane compound in the mixed solvent of the ketone compound and the alkane compound is 50-90 vol%, preferably 50-80 vol% of the mixed solvent; Preferably, the amount of the alkane compound in the mixed solvent of the organic acid alkyl ester, ketone compound and alkane compound is 0-50 vol%, preferably 1-30 vol% of the mixed solvent; the amount of the ketone compound is 0-10 vol%, preferably 1-5 vol% of the mixed solvent.
7. The preparation method according to any one of claims 3 to 6, in, The polymerization reaction conditions include: polymerization temperature of 40-95° C., preferably 50-80° C.; polymerization time of 1-24 h, preferably 3-10 h.
8. Maleic anhydride-isobutylene-styrene terpolymer microspheres prepared by the preparation method described in any one of claims 3 to 7.
9. The maleic anhydride-isobutylene-styrene terpolymer microspheres according to claim 8, in, Based on the total molar amount of the terpolymer, the molar content of the structural unit provided by maleic anhydride is 47-52%, preferably 48-51%; the molar ratio of the structural unit provided by isobutylene to the structural unit provided by styrene is 1:0.2-7.5, preferably 1:1-5; Preferably, the particle size of the terpolymer microspheres is 500-920 nm, preferably 530-800 nm.
10. Use of the maleic anhydride-isobutylene-styrene terpolymer microspheres according to any one of claims 1-2 and 8-9 as a polar modifier in polyolefins.
11. The use according to claim 10, in, Based on the total weight of the polyolefin, the amount of the terpolymer microspheres is 1-10wt%, preferably 2-6wt%; Preferably, the polyolefin is polypropylene; Preferably, the polypropylene has a melt index of 3-12 g / 10 min, preferably 4-10 g / 10 min, at 190° C. and a load of 2.16 kg.
Citation Information
Patent Citations
Maleic anhydride-styrene copolymer microsphere as well as preparation method and application thereof
CN114426617A
Alpha-olefin-maleic anhydride copolymer as well as preparation method and application thereof
CN114426639A
Method for copolymerizing isobutene and maleic anhydride
CN116023570A
Manufacture of maleic anhydride copolymer particle
JP1989204911A