Heat-conducting silica gel gasket and preparation method thereof

Through the combination of alumina filler with different particle sizes and multi-viscosity silicone oil, combined with platinum catalyst treatment, the formulation of thermally conductive silicone sheet is optimized, and the shortcomings of thermal and mechanical properties are solved, and the silicone gasket with high thermal conductivity, low cost and long life are achieved .

CN118909449APending Publication Date: 2024-11-08GANSU XUCARBON NEW MATERIAL CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411094255.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing thermal conductivity of silicone films has low thermal conductivity and poor mechanical properties, high cost, complex process, and excessive powder filling, resulting in reduced reliability and short service life.

Method used

By combining alumina thermal fillers of different particle sizes, combining vinyl silicone oil and vinyl green glue with different viscosity, platinum catalyst and coupling agent are used for curing and vulcanization, the thermal filler formulation is optimized and the thermal conductivity and mechanical properties are improved.

Benefits of technology

It achieves high thermal conductivity (10~15W/m·k) and excellent mechanical properties, improves the reliability and service life of silicone gaskets, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909449A_ABST
    Figure CN118909449A_ABST
Patent Text Reader

Abstract

The invention relates to a heat-conducting silica gel gasket and a preparation method thereof. The heat-conducting silica gel gasket comprises the following components: 5-30 parts of vinyl silicone oil with first viscosity, 1-20 parts of vinyl silicone oil with second viscosity, 1-10 parts of vinyl silicone oil with third viscosity, 50-150 parts of a heat-conducting filler, 2-10 parts of vinyl raw rubber, 0.1-0.5 part of a platinum catalyst and 3-8 parts of a coupling agent. The heat-conducting filler comprises aluminum oxide with the particle size of 100-120 microns, aluminum oxide with the particle size of 40-70 microns and aluminum oxide with the particle size of 3-10 microns. By compounding the heat-conducting fillers with different particle sizes, the formula of the heat-conducting filler is optimized, and the heat-conducting property of the heat-conducting silica gel gasket can be effectively improved; by using vinyl silicone oil and vinyl raw rubber with different viscosities, the flexibility of the heat-conducting silica gel gasket can be ensured, so that the heat-conducting silica gel gasket can meet various special requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of heat-conducting materials, and in particular to a heat-conducting silicone gasket and a preparation method thereof. Background Art

[0002] "Thermal conductive silicone" is a thermal conductive medium material synthesized through a special process with silicone as the base material and various auxiliary materials such as metal oxides added. In the industry, it is also called thermal conductive silicone pad, thermal conductive silicone sheet, soft thermal conductive pad, thermal conductive silicone gasket, etc. It is specially produced for the design of transferring heat through gaps. It can fill the gaps, open up the heat channel between the heating part and the heat dissipation part, and effectively improve the heat transfer efficiency. At the same time, it also plays the role of insulation, shock absorption, sealing, etc. It can meet the design requirements of miniaturization and ultra-thinness of equipment. It is an excellent thermal conductive filling material.

[0003] The existing thermally conductive silicone sheet technology is mature, but the thermal conductivity is mostly below 4W / m·k. Although there are products in the market for thermally conductive silicone sheets of 5W / m·k and above, the cost is high and the process is complicated. It is usually necessary to add expensive powders such as boron nitride, carbon fiber, carbon nanotubes, aluminum nitride and diamond powder. At the same time, a series of processes are required to stabilize the system to achieve high thermal conductivity and maintain the mechanical properties of the silicone sheet. This may also result in a decrease in mechanical properties and powder loss due to excessive powder filling, resulting in a decrease in the reliability of the silicone sheet and a shortened service life.

[0004] Therefore, how to prepare thermally conductive silicone gaskets with high thermal conductivity and excellent mechanical properties has become the focus of research. Summary of the invention

[0005] The purpose of the present invention is to provide a thermally conductive silicone gasket and a preparation method thereof, wherein the thermally conductive silicone gasket has high thermal conductivity and excellent mechanical properties.

[0006] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a thermally conductive silicone gasket, comprising the following components in parts by mass: 5-30 parts of vinyl silicone oil of a first viscosity, 1-20 parts of vinyl silicone oil of a second viscosity, 1-10 parts of vinyl silicone oil of a third viscosity, 50-150 parts of thermally conductive filler, 2-10 parts of vinyl raw rubber, 0.1-0.5 parts of platinum catalyst, and 3-8 parts of coupling agent; the thermally conductive filler comprises alumina with a particle size of 100-120 μm; alumina with a particle size of 40-70 μm and alumina with a particle size of 3-10 μm.

[0007] Optionally, the aluminum oxide content of the 100-120 μm particle size is 20-40%, the aluminum oxide content of the 40-70 μm particle size is 10-30%, and the aluminum oxide content of the 3-10 μm particle size is 10-30%.

[0008] Optionally, the first viscosity is 10-20 cps, the second viscosity is 500-1000 cps, and the third viscosity is 10000-20000 cps.

[0009] Optionally, the mass ratio of the total mass of the vinyl silicone oil of the first viscosity, the vinyl silicone oil of the second viscosity and the vinyl silicone oil of the third viscosity to the thermal conductive filler is 1:3-1:5.

[0010] Optionally, the viscosity of the vinyl rubber is 10000-20000 cps.

[0011] Optionally, the thermally conductive filler further includes one or more of boron nitride, silicon carbide, graphene and zinc oxide; and the coupling agent is one or more of a silane coupling agent, an aluminate coupling agent, a phthalate coupling agent and a phosphate coupling agent.

[0012] The second aspect of the present invention provides a method for preparing the thermally conductive silicone gasket provided by the first aspect of the present invention, the method comprising: The vinyl silicone oil of the first viscosity, the vinyl silicone oil of the second viscosity, the vinyl silicone oil of the third viscosity, the thermal conductive filler and the vinyl raw rubber are mixed and stirred to be uniformly dispersed, and then a coupling agent is added to carry out stirring reaction to obtain a thermal conductive silicone solution; The thermally conductive silicone solution and the platinum catalyst are evenly mixed, and then cured and vulcanized to obtain a thermally conductive silicone gasket.

[0013] Optionally, the mass ratio of the thermally conductive silica gel solution to the platinum catalyst is 1:0.001-0.005.

[0014] Optionally, the stirring speed is 80-120 r / min, and the stirring reaction time is 1-3 h.

[0015] Optionally, the curing temperature is 55-85°C, and the time is 1-2h; the vulcanization temperature is 75~110°C, and the time is 0.5~1.5h.

[0016] Optionally, the vulcanizing agent used for the vulcanization includes one or more of a di-pentadienyl vulcanizing agent, a di-tetra-pentadienyl vulcanizing agent and a platinum vulcanizing agent.

[0017] Through the above technical scheme, the present invention optimizes the formula of thermally conductive fillers by compounding thermally conductive fillers of different particle sizes, which can achieve low cost, high thermal conductivity, and stable dispersion, thereby effectively improving the thermal conductivity of the thermally conductive silicone gasket; at the same time, the filling amount of the thermally conductive filler is moderate, which can meet the thermal conductivity requirements of the silicone gasket without affecting the mechanical properties, and improve the reliability and life of the thermally conductive silicone gasket. And by using vinyl silicone oil and vinyl raw rubber of different viscosities, the flexibility of the thermally conductive silicone gasket can be guaranteed, so that the thermally conductive silicone sheet of the present invention can meet various special requirements.

[0018] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings: Figure 1 It is a schematic diagram of the thermal conductive silicone gasket of the present invention when in use. DETAILED DESCRIPTION

[0020] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0021] The first aspect of the present invention provides a thermally conductive silicone gasket, comprising the following components in parts by mass: 5-30 parts of vinyl silicone oil of a first viscosity, 1-20 parts of vinyl silicone oil of a second viscosity, 1-10 parts of vinyl silicone oil of a third viscosity, 50-150 parts of thermally conductive filler, 2-10 parts of vinyl raw rubber, 0.1-0.5 parts of platinum catalyst, and 3-8 parts of coupling agent; the thermally conductive filler comprises alumina with a particle size of 100-120 μm; alumina with a particle size of 40-70 μm and alumina with a particle size of 3-10 μm.

[0022] The present invention optimizes the formula of the thermally conductive filler by compounding thermally conductive fillers of different particle sizes, which can effectively improve the thermal conductivity of the thermally conductive silicone gasket; by using vinyl silicone oil and vinyl raw rubber of different viscosities, the flexibility of the thermally conductive silicone gasket can be ensured, so that the thermally conductive silicone sheet can meet various special requirements.

[0023] According to the present invention, optionally, the content of alumina in the particle size of 100-120 μm is 20-40%, the content of alumina in the particle size of 40-70 μm is 10-30%, and the content of alumina in the particle size of 3-10 μm is 10-30%. The present invention can more effectively fill the gaps in the silica gel system, increase the contact between the thermally conductive filler particles, and thus effectively improve the thermal conductivity by selecting thermally conductive fillers of different particle sizes and reasonably matching them in proportion.

[0024] According to the present invention, optionally, the first viscosity is 10-20 cps, the second viscosity is 500-1000 cps, and the third viscosity is 10000-20000 cps. The present invention can ensure the flexibility of the silicone gasket by using high-viscosity, medium-viscosity and low-viscosity vinyl silicone oil, making it more widely applicable.

[0025] According to the present invention, optionally, the mass ratio of the total mass of the vinyl silicone oil of the first viscosity, the vinyl silicone oil of the second viscosity, and the vinyl silicone oil of the third viscosity to the thermally conductive filler is 1:3 to 1:5. Through the above embodiment, the filling amount of the thermally conductive filler in the silicone matrix is ​​moderate, and the thermal conductivity coefficient requirement of the silicone gasket can be met without affecting the mechanical properties, thereby improving the reliability and life of the thermally conductive silicone gasket, and obtaining a thermally conductive silicone gasket with better thermal conductivity and mechanical properties.

[0026] According to the present invention, optionally, the viscosity of the vinyl rubber is 10000-20000 cps. The viscosity of the vinyl rubber of the present invention is within the above range, and can be matched with vinyl silicone oils of different viscosities to improve the flexibility of the thermally conductive silicone gasket.

[0027] According to the present invention, optionally, the thermally conductive filler further includes one or more of boron nitride, silicon carbide, graphene and zinc oxide; the coupling agent is one or more of a silane coupling agent, an aluminate coupling agent, a phthalate coupling agent and a phosphate coupling agent.

[0028] The second aspect of the present invention provides a method for preparing the thermally conductive silicone gasket provided by the first aspect of the present invention, the method comprising: The vinyl silicone oil of the first viscosity, the vinyl silicone oil of the second viscosity, the vinyl silicone oil of the third viscosity, the thermal conductive filler and the vinyl raw rubber are mixed and stirred to be uniformly dispersed, and then a coupling agent is added to carry out stirring reaction to obtain a thermal conductive silicone solution; The thermally conductive silicone solution and the platinum catalyst are evenly mixed, and then cured and vulcanized to obtain a thermally conductive silicone gasket.

[0029] According to the present invention, optionally, the mass ratio of the thermally conductive silicone solution to the platinum catalyst is 1:0.001-0.005. Through the above embodiment, the thermally conductive silicone solution can be cross-linked under the action of the platinum catalyst and cured to form a stable thermally conductive silicone gasket.

[0030] According to the present invention, optionally, the stirring speed is 80-120 r / min, and the stirring reaction time is 1-3 h.

[0031] According to the present invention, optionally, the curing temperature is 55-85°C and the time is 1-2h; the vulcanization temperature is 75~110°C and the time is 0.5~1.5h; the vulcanizing agent used in the vulcanization includes one or more of dipentadienyl vulcanizer, ditetrabenzyl vulcanizer and platinum vulcanizer. Through vulcanization treatment, the silicone molecules can undergo cross-linking reaction, promoting the linear molecules to form a three-dimensional network structure, improving the strength of the elastomer, increasing the mechanical properties, and improving the fracture strength.

[0032] According to the present invention, optionally, the thermal conductivity of the thermally conductive silicone gasket obtained by the preparation method of the present invention is 10-15 W / m·k; the Shore hardness is 60-70; the elongation at break is 30%-60%; the volume resistivity is 1*10 15 Ω / cm.

[0033] The present invention is further illustrated by the following examples, but the present invention is not limited thereto.

[0034] Example 1 Take 9 parts of 15cps vinyl silicone oil; 15 parts of 800cps vinyl silicone oil; 6 parts of 15000cps vinyl silicone oil; 108 parts of thermal conductive filler; 7 parts of vinyl rubber; the thermal conductive filler contains 30% of 120μm alumina, 20% of 60μm alumina and 20% of 5μm alumina, stir and disperse them evenly at a low speed of 100r / min, add 5 parts of KH570 silane coupling agent, until it is completely dissolved, and gradually add 5% graphene powder, 15% zinc oxide powder and 10% silicon carbide powder of thermal conductive filler, stir and react at constant temperature for 2 hours, and the solution for thermal conductive silicone gasket is obtained. The above silicone liquid is divided into two parts, one part is solidified into sheets, and the other part is tested using a thermal conductivity tester. The curing process is as follows: 100 parts of the thermal conductive silicone solution are mixed evenly with 0.2 parts of platinum catalyst to make it cross-linked under the action of platinum catalyst, then coated on the surface of release PET, cured at 60°C for 1.5 hours, and then vulcanized at 95°C for 1 hour using platinum vulcanizer to obtain a uniform and complete thermal conductive silicone gasket. The overall thermal conductivity is tested to be 15W / m·k; the elongation at break is 55%; the volume resistivity is 1*10 15 Ω / cm.

[0035] Example 2 Take 9 parts of 15cps vinyl silicone oil; 15 parts of 800cps vinyl silicone oil; 6 parts of 15000cps vinyl silicone oil; 108 parts of thermal conductive filler; 7 parts of vinyl rubber; the thermal conductive filler contains 30% of 120μm alumina, 20% of 60μm alumina and 20% of 5μm alumina, stir and disperse them evenly at a low speed of 100r / min, add 5 parts of KH570 silane coupling agent, until it is completely dissolved, and gradually add 5% graphene powder and 25% zinc oxide powder of thermal conductive filler, stir and react at constant temperature for 2 hours, and the solution for thermal conductive silicone gasket is obtained. The above silicone liquid is divided into two parts, one part is solidified into sheets, and the other part is tested using a thermal conductivity tester. The curing process is as follows: 100 parts of the thermal conductive silicone solution are mixed evenly with 0.2 parts of platinum catalyst to make it cross-linked under the action of platinum catalyst, then coated on the surface of release PET, cured at 60°C for 1.5 hours, and then vulcanized at 95°C with platinum vulcanizer for 1 hour to obtain a uniform and complete thermal conductive silicone gasket. The overall thermal conductivity is tested to be 10W / m·k; the elongation at break is 40%; the volume resistivity is 1*10 15 Ω / cm.

[0036] Example 3 Take 9 parts of 15cps vinyl silicone oil; 15 parts of 800cps vinyl silicone oil; 6 parts of 15000cps vinyl silicone oil; 108 parts of thermal conductive filler; 7 parts of vinyl rubber; the thermal conductive filler contains 30% of 120μm alumina, 20% of 60μm alumina and 20% of 5μm alumina, stir and disperse them evenly at a low speed of 100r / min, add 5 parts of KH570 silane coupling agent, until it is completely dissolved, and gradually add 5% graphene powder and 25% silicon carbide powder of thermal conductive filler, stir and react at constant temperature for 2 hours, and the solution for thermal conductive silicone gasket is obtained. The above silicone liquid is divided into two parts, one part is solidified into sheets, and the other part is tested using a thermal conductivity tester. The curing process is as follows: 100 parts of the thermal conductive silicone solution are mixed evenly with 0.2 parts of platinum catalyst to make it cross-linked under the action of platinum catalyst, then coated on the surface of release PET, cured at 60°C for 1.5 hours, and then vulcanized at 95°C with platinum vulcanizer for 1 hour to obtain a uniform and complete thermal conductive silicone gasket. The overall thermal conductivity is 13W / m·k; the elongation at break is 45%; the volume resistivity is 1*10 15 Ω / cm.

[0037] Comparative Example 1 The preparation of the thermally conductive silicone gasket in this comparative example is the same as that in Example 1, except that 30 parts of 800cps vinyl silicone oil and only 60μm particle size powder are contained in the alumina thermal conductive filler. The overall thermal conductivity is 8W / m·k; the elongation at break is 35%; the volume resistivity is 1*10 15 Ω / cm.

[0038] Comparative Example 2 The preparation of the thermally conductive silicone gasket in this comparative example is the same as that in Example 1, except that no thermally conductive filler graphene powder is added. The overall thermal conductivity is 5W / m·k; the elongation at break is 20%; the volume resistivity is 1*10 17 Ω / cm.

[0039] Comparative Example 3 The preparation of the thermally conductive silicone gasket in this comparative example is the same as that in Example 1, except that no silane coupling agent is added. The overall thermal conductivity is 10W / m·k; the elongation at break is 25%; the volume resistivity is 5*10 16 Ω / cm.

[0040] Comparative Example 4 The preparation of the thermally conductive silicone gasket in this comparative example is the same as that in Example 1, except that it is not subjected to vulcanization treatment. The overall thermal conductivity is tested to be 12 W / m·k; the elongation at break is 5%; the volume resistivity is 5*10 15 Ω / cm.

[0041] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0042] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0043] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A thermally conductive silicone gasket, characterized in that: The invention comprises the following components in parts by weight: 5-30 parts of vinyl silicone oil of the first viscosity, 1-20 parts of vinyl silicone oil of the second viscosity, 1-10 parts of vinyl silicone oil of the third viscosity, 50-150 parts of thermal conductive filler, 2-10 parts of vinyl raw rubber, 0.1-0.5 parts of platinum catalyst, and 3-8 parts of coupling agent; The thermal conductive filler includes aluminum oxide with a particle size of 100-120 μm, aluminum oxide with a particle size of 40-70 μm and aluminum oxide with a particle size of 3-10 μm.

2. The thermally conductive silicone gasket according to claim 1, wherein: The content of alumina with a particle size of 100-120 μm is 20-40%, the content of alumina with a particle size of 40-70 μm is 10-30%, and the content of alumina with a particle size of 3-10 μm is 10-30%.

3. The thermally conductive silicone gasket according to claim 1, wherein: The first viscosity is 10-20 cps, the second viscosity is 500-1000 cps, and the third viscosity is 10000-20000 cps.

4. The thermally conductive silicone gasket according to claim 1, wherein: The mass ratio of the total mass of the vinyl silicone oil of the first viscosity, the vinyl silicone oil of the second viscosity and the vinyl silicone oil of the third viscosity to the mass of the thermal conductive filler is 1:3-1:

5.

5. The thermally conductive silicone gasket according to claim 1, wherein: The viscosity of the vinyl rubber is 10000-20000 cps.

6. The thermally conductive silicone gasket according to claim 1, wherein: The thermally conductive filler further comprises one or more of boron nitride, graphene, silicon carbide and zinc oxide; The coupling agent is one or more of a silane coupling agent, an aluminate coupling agent, a phthalate coupling agent and a phosphate coupling agent.

7. A method for preparing the thermally conductive silicone gasket according to any one of claims 1 to 6, characterized in that: The method includes: The vinyl silicone oil of the first viscosity, the vinyl silicone oil of the second viscosity, the vinyl silicone oil of the third viscosity, the thermal conductive filler and the vinyl raw rubber are mixed and stirred to be uniformly dispersed, and then a coupling agent is added to carry out stirring reaction to obtain a thermal conductive silicone solution; The thermally conductive silicone solution and the platinum catalyst are evenly mixed, and then cured and vulcanized to obtain a thermally conductive silicone gasket.

8. The method according to claim 7, wherein: The mass ratio of the thermally conductive silica gel solution to the platinum catalyst is 1:0.001-0.

005.

9. The method according to claim 7, wherein: The stirring speed is 80-120 r / min, and the stirring reaction time is 1-3 h.

10. The method according to claim 7, wherein: The curing temperature is 55-85°C and the curing time is 1-2h; The vulcanization temperature is 75-110°C and the time is 0.5-1.5h; The vulcanizing agent used in the vulcanization includes one or more of a di-pentadienyl vulcanizing agent, a di-tetra-pentadienyl vulcanizing agent and a platinum vulcanizing agent.

Citation Information

Cited By

  • Insulating high-thermal-conductivity flexible silica gel sheet and preparation method thereof

    CN121673840A