Heat resistant film
Through the polyester-based elastomer of hard and soft segments, combining aromatic dicarboxylic acids and aliphatic polycarbonate, the problem of difficulty in taking into account both dilation and heat resistance at high temperatures is solved, and high efficiency is achieved surface protection effect.
Patent Information
- Application Number
- CN202410929031.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2020-06-05
- Filing Date
- 2021-05-25
- Publication Date
- 2024-11-08
AI Technical Summary
The existing heat-resistant films are prone to defects such as deflection, wrinkles and pressing marks during high temperature treatment, and it is difficult to take into account both heat resistance and expansion.
Polyester-based elastomer bonded with hard segments and soft segments. The hard segment is formed by aromatic dicarboxylic acid, aliphatic diol or alicyclic diols. The soft segment is mainly composed of aliphatic polycarbonate , the weight ratio of the hard chain segment exceeds 50%, and is bonded through an ester bond or isocyanate compound, with a melting point between 195 and 240°C to achieve high heat resistance and dilation.
It achieves uniform stretchability and heat resistance at high temperatures, reduces deflection and wrinkle phenomena, and is suitable for surface protection of semiconductor cutting processes and other products.
Smart Images

Figure BDA0004939103780000131 
Figure BDA0004939103780000141
Abstract
Description
[0001] This application is a divisional application. The filing date of the parent application is May 25, 2021. The international application number is PCT / JP2021 / 019791. The application number entering the Chinese national phase is 202180035949.3. The name of the invention is heat-resistant film. Technical Field
[0002] The present invention relates to a heat-resistant film suitable for protecting the surface state of plastic products, glass products, ceramic products, etc. after conducting electricity, decorating, etc., or suitable for fixing semiconductors, etc. when they are cut and separated to obtain chips. Background Art
[0003] Plastic products, glass products, ceramic products, etc. are not only flat but also have curved surfaces and concave and convex shapes. Films protecting these products are required to have adaptability in various applications. For example, an adhesive sheet with an adhesive laminated on a film is required to have conformability, and therefore uniform conformability within the surface is required.
[0004] In addition, the semiconductor manufacturing process includes: a dicing process to cut wafers and substrates into chips; an expansion process to widen the intervals between the individual chips so that they can be easily picked up by suction fixtures; and a chip picking process. There are various expectations for protective films, adhesive sheets, etc. that can reduce the load at this time in each process.
[0005] In the dicing process, in order to fix the wafer, substrate, etc., and prevent the position shift and chip scattering during dicing by the blade, etc., appropriate rigidity is required, and in the expansion process, stretchability is required to expand the chip spacing evenly. In addition, the high performance of TSV (silicon wafer through hole) stacking multiple semiconductor chips is also being improved, the process of directly applying sealing materials through transfer molding is simplified, and the high temperature treatment of the wafer reaches 150°C or more. Therefore, heat resistance is required for the surface protection film and the base material used for the dicing tape.
[0006] In particular, a multilayer film is disclosed, characterized in that a resin composition containing, for example, a vinyl aromatic hydrocarbon or a hydrogenated conjugated diene copolymer and a polypropylene resin is laminated on a substrate of a surface protection film or an adhesive sheet as a dicing tape in a semiconductor process, thereby forming the multilayer film. However, although the expansibility is sufficient, there are problems such as the following: deflection due to the weight of the wafer; wrinkles and pressing marks on the substrate due to the heating process in the coating process of the adhesive layer, etc., and also due to the high temperature treatment as described above (Patent Document 1).
[0007] Polyester resin is a raw material with a high glass transition temperature and excellent heat resistance. Focusing on this, an amorphous polyester is disclosed, wherein the glass transition temperature of the amorphous polyester is set to 0 to 50° C. in order to obtain a certain degree of extensibility. However, even if it is extended, it cannot maintain tension, so it is easy to bend, and when the glass transition temperature is exceeded, the elastic modulus decreases.
[0008] In addition, a method of laminating polyester resins having glass transition temperatures of -100 to 0°C and 0 to 100°C is disclosed. However, since the method basically includes layers having low melting points or softening points, when a high temperature treatment is performed, there are problems such as wrinkles and pressure marks, and deflection due to the weight of the wafer (Patent Documents 2 to 3).
[0009] Regarding polyester elastomers, block copolymers formed by bonding hard segments formed by polyester and soft segments mainly formed by alicyclic diols are known, wherein the polyester is formed by aromatic dicarboxylic acids, aliphatic diols or alicyclic diols. These polyester elastomers have high heat resistance compared to polystyrene elastomers, polyolefin elastomers, polyamide elastomers, etc., and are exhibited in various applications. However, many block copolymers will show a yield point at a low elongation of 10 to 25%, so when this value is exceeded, uniform stretching becomes difficult. In response to these problems, if countermeasures such as increasing the ratio of soft segments are taken, heat resistance will be reduced, and it will not be possible to achieve a balance between heat resistance and expansion.
[0010] Prior art literature
[0011] Patent Literature
[0012] Patent Document 1: Japanese Patent Application Publication No. 2009-094418
[0013] Patent Document 2: Japanese Patent Application Publication No. 2003-092273
[0014] Patent Document 3: Japanese Patent Application Publication No. 2017-034618 Summary of the invention
[0015] Problems to be solved by the invention
[0016] The present invention aims to provide a heat-resistant film suitable for protecting the surface state of plastic products, glass products, ceramic products, etc. after conducting electricity, decorating, etc., or suitable for fixing chips when cutting and separating wafers, etc. in a semiconductor manufacturing process.
[0017] Means used to solve problems
[0018] Means for Solving the Problems The present inventors have conducted intensive studies to solve the above-mentioned problems and have completed the following invention.
[0019] [1] A heat-resistant film comprising a thermoplastic resin, wherein the thermoplastic resin is a polyester elastomer in which a hard segment and a soft segment are bonded together,
[0020] The hard segment has a polyester unit formed by an aromatic dicarboxylic acid and an aliphatic diol or an alicyclic diol.
[0021] The soft segment is mainly formed by aliphatic polycarbonate.
[0022] The weight ratio of the hard segment contained in the polyester elastomer exceeds 50%,
[0023] The film containing the thermoplastic resin has an elastic modulus of 30 to 500 MPa, an elongation at break of 200 to 700%, and a ratio F50 / F25 of stress F50 at 50% elongation to stress F25 at 25% elongation of 1.05 or more.
[0024] [2] The heat-resistant film described above, characterized in that the hard segment of the polyester elastomer contains a polybutylene terephthalate unit, and the melting point of the polyester elastomer is 195 to 220°C.
[0025] [3] The heat-resistant film described above, characterized in that the hard segment of the polyester elastomer contains polybutylene naphthalate units, and the melting point of the polyester elastomer is 210 to 240°C.
[0026] [4] The above-mentioned heat-resistant film, which is used as a protective film.
[0027] [5] A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive on at least one surface of the heat-resistant film.
[0028] Effects of the Invention
[0029] The heat-resistant film of the present invention is formed of a specific polyester-based elastomer. In particular, since the soft segment of the present invention is included, a heat-resistant film having excellent heat resistance and high expandability can be obtained. DETAILED DESCRIPTION
[0030] The heat-resistant film of the present invention is mainly suitable for use as a dicing tape for fixing semiconductors when they are cut and separated to obtain chips. In addition, it can cope with the heat treatment in the coating process of the adhesive layer, etc., has excellent stretchability and sufficient expansion, and can be used as a surface protection film for protecting the surface state of plastic products, glass products, ceramic products, etc. after conducting electricity, decoration, etc. In addition, an adhesive sheet with an adhesive can be provided.
[0031] The heat-resistant film of the present invention has the compound and structure described below.
[0032] <Polyester elastomer>
[0033] The polyester elastomer used for the heat-resistant film of the present invention is formed by bonding a hard segment comprising polyester formed of an aromatic dicarboxylic acid and an aliphatic diol or an alicyclic diol to a soft segment mainly comprising an aliphatic polycarbonate.
[0034] The aromatic dicarboxylic acid forming the polyester of the hard segment in the polyester-based elastomer can widely use a general aromatic dicarboxylic acid. Specifically, as the aromatic dicarboxylic acid, terephthalic acid or naphthalene dicarboxylic acid is desirable. In addition, these compounds can be included as the main component of the aromatic dicarboxylic acid of the present invention.
[0035] As other acid components, there can be mentioned aromatic dicarboxylic acids such as biphenyl dicarboxylic acid, isophthalic acid, and sodium 5-sulfoisophthalic acid, alicyclic dicarboxylic acids such as cyclohexane dicarboxylic acid and tetrahydrophthalic anhydride, and acid components obtained by adding aliphatic dicarboxylic acids such as succinic acid, glutaric acid, adipic acid, azelaic acid, sebacic acid, dodecanedioic acid, dimer acid, and hydrogenated dimer acid to the aromatic dicarboxylic acids such as biphenyl dicarboxylic acid, isophthalic acid, and 5-sulfoisophthalic acid, etc. It should be noted that these aliphatic dicarboxylic acids are used within a range that does not significantly reduce the melting point of the resin, and the amount thereof is less than 30 mol%, preferably less than 20 mol%, of the total acid components.
[0036] The aliphatic diol or alicyclic diol forming the polyester of the hard segment is not particularly limited, but is preferably an alkylene glycol having 2 to 8 carbon atoms. Specifically, ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, etc. are mentioned, and 1,4-butanediol and 1,4-cyclohexanedimethanol are most preferred. In addition, these compounds may be included as the main component of the diol of the present invention.
[0037] Therefore, the polyester as the hard segment preferably mainly contains butylene terephthalate units or butylene naphthalate units from the viewpoints of physical properties, moldability, and cost performance.
[0038] The aliphatic diol forming the soft segment in the polyester elastomer used for the heat-resistant film of the present invention is preferably aliphatic polycarbonate diol having a low melting point (e.g., 70°C or less) and a low glass transition temperature. For example, the aliphatic polycarbonate diol formed from 1,6-hexanediol has a glass transition temperature as low as about -60°C and a melting point of about 50°C, so that stretchability at room temperature can be obtained, which is suitable. In addition, for example, the aliphatic polycarbonate diol obtained by copolymerizing an appropriate amount of 3-methyl-1,5-pentanediol with the above-mentioned aliphatic polycarbonate diol has a slightly higher glass transition temperature than the original aliphatic polycarbonate diol, but the melting point is lowered or it becomes amorphous, which is equivalent to a good aliphatic polycarbonate diol. For example, an aliphatic polycarbonate diol composed of 1,9-nonanediol and 2-methyl-1,8-octanediol has a melting point of about 30° C. and a sufficiently low glass transition temperature of about −70° C., and thus is also a good aliphatic polycarbonate diol.
[0039] These aliphatic polycarbonate diols may be copolymerized with a small amount of other diols, dicarboxylic acids, ester compounds, ether compounds, etc. Examples of copolymer components include: diols such as dimer alcohol (Japanese: ダイマージオール), hydrogenated dimer alcohol, and their modified products, dicarboxylic acids such as dimer acid and hydrogenated dimer acid, polyesters formed from aliphatic, aromatic, or alicyclic dicarboxylic acids and diols, or polyesters formed from oligoesters, ε-caprolactone, etc., or oligoesters, polyalkylene glycols such as polytetramethylene glycol and polyoxyethylene glycol, or oligoalkylene glycols, etc., which can be used to a degree that does not substantially eliminate the effect of the aliphatic polycarbonate segment. In addition, substances mainly containing aliphatic diol residues having 2 to 12 carbon atoms, such as ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 2,2-dimethyl-1,3-propylene glycol, 3-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 1,9-nonanediol, and 2-methyl-1,8-octanediol, and particularly aliphatic diols having 5 to 12 carbon atoms are preferred from the viewpoint of heat resistance and elongation. These components may be used alone or in combination of two or more as required.
[0040] Furthermore, copolymer components such as polyalkylene glycols such as polyethylene glycol and polyoxytetramethylene glycol, and polyesters such as polycaprolactone and polybutylene adipate may be introduced as soft segments to the extent that the effects of the invention are not lost.
[0041] In the polyester elastomer used for the heat-resistant film of the present invention, for the mass ratio of the hard segment and the soft segment containing polyester, when the mass ratio of the hard segment becomes higher, the stretchability sometimes decreases, and when the mass ratio of the soft segment becomes higher, the heat resistance sometimes decreases. Here, the hard segment is formed by an aromatic dicarboxylic acid and an aliphatic diol or an alicyclic diol, and the soft segment contains an aliphatic polycarbonate and a copolymer component used as needed. Therefore, usually, the hard segment: soft segment = 40:60 to 80:20. It is preferred that the weight ratio of the hard segment contained in the polyester elastomer is greater than the weight ratio of the soft segment, and the weight ratio of the hard segment contained in the polyester elastomer exceeds 50%. For example, hard segment: soft segment = 50.1:49.9 to 70:30, 55:45 to 75:25 is a preferred range. In addition, in one embodiment, hard segment: soft segment = 55:45 to 70:30.
[0042] In the polyester elastomer used for the heat-resistant film of the present invention, it is preferred that the hard segment comprising polyester and the soft segment mainly comprising aliphatic polycarbonate are in a state where the units forming the hard segment and / or the soft segment are directly bonded via ester bonds or carbonate bonds, and the hard segment is formed from an aromatic dicarboxylic acid and an aliphatic diol or an alicyclic diol.
[0043] In addition, the hard segment and the soft segment in the polyester elastomer are more preferably bonded via a chain extender such as an isocyanate compound. In this case, it is desirable that 0.5 to 10 parts by mass of a polycarbodiimide compound is contained, for example, 0.5 to 6 parts by mass of a polycarbodiimide compound is contained, more preferably 1.0 to 3.0 parts by mass of a polycarbodiimide compound, relative to 100 parts by mass of a substance obtained by repeatedly subjecting the polyester forming the hard segment, the polycarbonate forming the soft segment, and various copolymer components used as needed to molten state for a certain period of time to ester exchange reaction and depolymerization reaction (hereinafter sometimes referred to as a blocked reaction product).
[0044] The above-mentioned polycarbodiimide compound can be obtained, for example, by the decarbonation reaction of a diisocyanate compound. As the diisocyanate used, 4,4'-diphenylmethane diisocyanate, 4,4'-diphenyldimethylmethane diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 1,5-naphthalene diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, cyclohexane-1,4-diisocyanate, xylylene diisocyanate, isophorone diisocyanate, methylcyclohexane diisocyanate, tetramethylxylylene diisocyanate, 1,3,5-triisopropylbenzene-2,4-diisocyanate, etc. can be used alone or by copolymerizing two or more thereof. In addition, a branched structure can be introduced, and functional groups other than carbodiimide groups and isocyanate groups can be introduced by copolymerization. The terminal isocyanate may be used as it is, or the degree of polymerization may be controlled by reacting the terminal isocyanate, or a part of the terminal isocyanate may be blocked.
[0045] Among such polycarbodiimide compounds, alicyclic polycarbodiimides having dicyclohexylmethane diisocyanate, cyclohexane-1,4-diisocyanate, isophorone diisocyanate, etc. as main raw materials are preferred. In addition, polycarbodiimide compounds having an isocyanate group at the end and an isocyanate group content of about 0.5 to 4% by mass are preferred from the perspectives of stability and handling, and the isocyanate group content is more preferably about 1 to 3% by mass.
[0046] Particularly preferred are polycarbodiimides derived from dicyclohexylmethane diisocyanate or isophorone diisocyanate and having an isocyanate group content of 0.5 to 4% by mass, and more preferably polycarbodiimides having an isocyanate group content of 1 to 3% by mass. It should be noted that the isocyanate group content can be measured by a conventional method (a method of dissolving with an amine and back titrating with hydrochloric acid).
[0047] In addition, from the perspective of thermal stability, the number of carbodiimide groups of the carbodiimide compound is preferably 2 to 50, and more preferably 5 to 30. In addition, in the case of such a degree of polymerization, it is solid at room temperature, so it is excellent in operability and compatibility when mixed with a polyester elastomer by powdering, so it is preferred from the perspective of being able to expect a uniform reaction and resistance to oozing out. It should be noted that the number of carbodiimide groups is the number of carbodiimides in the polycarbodiimide compound, and if it is a polycarbodiimide obtained from a diisocyanate compound, it is equivalent to the degree of polymerization. Usually, polycarbodiimide is a mixture of molecules of various lengths, and the number of carbodiimide groups is expressed as an average value. The number of carbodiimide groups can also be measured by conventional methods (dissolving with amines and back titrating with hydrochloric acid) as described above.
[0048] By using such a polycarbodiimide compound having an isocyanate group content of 0.5 to 4% by mass and a carbodiimide group number of 2 to 50, the MFR based on JIS K 7210 "Plastics - Method for determining the melt flow rate (MFR) and melt volume flow rate (MVR) of thermoplastics" is adjusted to 1 to 10 g / 10 minutes, and the occurrence of ejection unevenness can be suppressed during melt extrusion such as film formation.
[0049] In addition, a molecule containing two or more glycidyl groups, a weight average molecular weight of 4,000 to 25,000, and an epoxy value of 400 to 780 equivalents / 10 6 In this case, the reactive compound is preferably contained in an amount of 0.1 to 30 parts by mass, more preferably 0.5 to 5 parts by mass.
[0050] Regarding the composition obtained by this formulation, when the reduced viscosity before and after forming such as film formation is compared, the reduced viscosity after forming can be maintained, and the generation of foreign matter such as gel-like matter can be suppressed. In addition, although the mechanism is not clear, the ratio F50 / F25 of the stress F50 at an elongation of 50% to the stress F25 at an elongation of 25% becomes larger, thereby obtaining uniform stretchability.
[0051] Here, in the heat-resistant film of the present invention, the ratio F50 / F25 of the stress F50 at an elongation of 50% to the stress F25 at an elongation of 25% is 1.05 or more, for example, 2.0 or less. In one embodiment, F50 / F25 may be 1.05 or more and 1.6 or less.
[0052] By setting F50 / F25 within such a range, abnormalities such as wrinkles and distortion are less likely to occur when stretching is performed in one direction or in a plurality of directions.
[0053] For the polyester-based elastomer formed by bonding a hard segment comprising polyester and a soft segment mainly comprising aliphatic polycarbonate contained in the heat-resistant film of the present invention, when the melting point is low, heat resistance may be problematic, and when it is high, elongation may be reduced. In one embodiment, the melting point of the polyester-based elastomer is 195°C or higher, and when the hard segment comprises a polybutylene terephthalate unit, the melting point is preferably 195 to 220°C. In addition, when the hard segment comprises a polybutylene naphthalate unit, the melting point is preferably 210 to 240°C.
[0054] In addition, the polyester elastomer may be added with known inorganic compound particles such as silica, talc, zeolite, aluminum borate, etc., organic compound particles such as polymethyl methacrylate, melamine formaldehyde resin, melamine urea resin, polyester resin, etc., within the range not impairing the purpose. However, organic lubricants such as hydrocarbons such as liquid paraffin, paraffin, synthetic polyethylene wax, aliphatic and higher alcohols such as stearic acid, stearyl alcohol, fatty acid amides such as stearic acid amide, oleic acid amide, and erucic acid amide have concerns about contamination due to bleeding, so it is important that the extract obtained by Soxhlet extraction with chloroform based on JIS K6229 "Method for determining rubber-solvent extract (quantitative)" is 1 wt% or less, and substantially no organic lubricants are contained. When added, each organic lubricant is preferably 0.5 wt% or less, and further 0.1 wt% or less.
[0055] The raw materials used for the polyester elastomer are not particularly limited and may be derived from petroleum or plants. However, from the viewpoint of the environment, those derived from plants are preferred.
[0056] <Filmization>
[0057] The heat-resistant film of the present invention is obtained by flake-forming a polyester-based elastomer formed by bonding a hard segment and a soft segment by melt extrusion or the like, wherein the hard segment comprises polyester, and the polyester is formed by an aromatic dicarboxylic acid and an aliphatic diol or an alicyclic diol, and the soft segment mainly comprises an aliphatic polycarbonate.
[0058] As melt extrusion, it is extruded from a single-screw or twin-screw extruder through a T-die in the form of a sheet. The extruded sheet is pressed to the surface of a metal roller in which cooling water and oil are circulated by an air knife, an air chamber, a hard rubber roller, a steel belt, a metal roller, etc., and is cooled and solidified. In addition, the two sides of the sheet can be clamped with a steel belt for cooling and solidification. In addition, the above-mentioned sheet can also be obtained in the form of a sheet of different layers by using a feed head or a multi-manifold. It should be noted that, as required, the above-mentioned sheet can be stretched along a single axis or a double axis. When the total stretch ratio is high, the stretchability is sometimes impaired. When it is low, the thickness variation sometimes becomes larger, so it is preferably 3 to 12 times.
[0059] <Structure of heat-resistant film>
[0060] The heat-resistant film of the present invention can be formed by similar polyester elastomers, different types of elastomers, polyester resins, different types of resins, etc. to form A: single layer, A / B, A / B / A, A / B / C and other layer structures. In addition, in order to avoid problems such as interlayer peeling, other resin layers can be further arranged between the layers.
[0061] In such a configuration, when the static friction coefficient of at least one side is low, problems such as winding misalignment occur when the roller is wound, and when the static friction coefficient is high, wrinkles and the like sometimes remain, so the lower limit is preferably 0.10 or more, and more preferably 0.15 or more. In addition, the upper limit is preferably 0.9 or less, and in particular, when used in a dicing tape for a semiconductor process, uniform expansibility may not be obtained in the expansion process, so it is more preferably 0.5 or less.
[0062] <Thickness of heat-resistant film>
[0063] The heat-resistant film of the present invention depends on the method of use, but when the overall thickness is small, the stiffness is small, and when the overall thickness is large, sometimes there will be problems with handling. In particular, when used in a dicing tape for a semiconductor process, there is a concern that a break may occur due to defects occurring during the cutting process and / or sometimes uniform expansibility cannot be obtained, so the overall thickness is preferably 60 μm or more, more preferably 80 μm or more. In addition, from the viewpoint of handling, it is preferably 180 μm or less.
[0064] The thermoplastic resin film of the present invention cannot be stretched when the elastic modulus is large, and the stiffness becomes small when the elastic modulus is small, so it is preferably 30 to 500 MPa, more preferably 30 to 100 MPa. It should be noted that the elongation at break can be 200 to 700%, for example, 350 to 700%.
[0065] <Adhesive>
[0066] In one embodiment, an adhesive sheet having an adhesive on at least one side of the heat-resistant film of the present invention is provided. The adhesive that can be used for the adhesive sheet of the present invention can include (meth) acrylic adhesives, silicone adhesives, urethane adhesives, olefin adhesives, styrene adhesives, etc. It can be selected based on the surface protection film that protects the surface state after the implementation of conduction, decoration, etc. in plastic products, glass products, ceramic products, etc., and the object of application. In addition, for the dicing tape that fixes the wafers, etc. when they are cut and separated by semiconductor processes, etc. to obtain chips, among these, it is preferred that the (meth) acrylic adhesive that can easily adjust the adhesive force.
[0067] There is no particular restriction on the thickness of the adhesive layer using the above-mentioned adhesive. When used as a dicing tape for fixing chips when wafers are cut and separated through a semiconductor process; and when used as a surface protective film for protecting the surface state of plastic products, glass products, ceramic products, etc. after conduction, decoration, etc. are performed, the thickness of the adhesive layer is preferably 1 to 50 μm, and more preferably 3 to 30 μm, from the viewpoint of the adhesive strength, the uniformity of the thickness of the adhesive layer, etc.
[0068] Example
[0069] Hereinafter, the present invention will be described in more detail with reference to the examples. It should be noted that the present invention is not limited to the following examples, and can be implemented by adding modifications within the scope consistent with the gist of the present invention, and these are all included in the technical scope of the present invention.
[0070] The evaluation methods of physical properties in Examples are as follows.
[0071] (1) Number average molecular weight
[0072] Dissolve the aliphatic polycarbonate diol sample in deuterated chloroform (CDCl 3 ) and measure H-NMR, thereby calculating the terminal group and obtaining it by the following formula.
[0073] Number average molecular weight = 1000000 / ((end group weight (equivalent / ton)) / 2)
[0074] (2) Reduced viscosity
[0075] Based on JIS K 7367-5:1998 "Method for determining viscosity of polymer dilute solution using plastic capillary viscometer -", phenol / tetrachloroethane = 60 / 40 was used.
[0076] The viscosity of the mixed solvent containing 1% (mass %) was measured using an Ostwald viscometer and was defined as the reduced viscosity.
[0077] (3) Tm (melting point)
[0078] The melting peak temperature in a curve obtained by DSC (differential scanning calorimetry) based on JIS K 7121: 1987 "Determination of transition temperatures of plastics" was used.
[0079] (4) Soft (chain segment) amount
[0080] Using a Fourier transform nuclear magnetic resonance apparatus (AVANCE-NEO500 manufactured by BRUKER, Germany), after dissolving in a solvent (deuterated chloroform / trifluoroacetic acid = 85 / 15 volume %) at a concentration of 3 to 5 volume %, proton NMR measurement was performed at 25°C, and the mass ratio of the hard segment to the soft segment was determined and calculated based on the signal intensity ratio of the methylene peaks adjacent to various oxygen in the molecular structure.
[0081] (5)Film thickness
[0082] The thickness was determined based on JIS K 7130:1999 "Plastic film and sheet - Measurement of thickness (Method A)".
[0083] (6) Strength, elongation, elastic modulus, F25, F50
[0084] Based on JIS K 7127:1999 "Plastics - Test methods for tensile properties -", the strength, elongation and elastic modulus are calculated from the tensile strength, tensile elongation at break and tensile elastic modulus, and 25% and 50% are set as the specified strains, and the tensile stresses are set as F25 and F50. It should be noted that the index of expansion is represented by the stress ratio F50 / F25 at the above specified strain.
[0085] (7) Coating properties
[0086] Butyl acrylate / acrylic acid = 90 / 10 was copolymerized in a toluene solution by a conventional method, and 80 parts by weight of commercially available dipentaerythritol hexaacrylate "KAYARAD DPHA: manufactured by Nippon Kayaku", 5 parts by weight of a photopolymerization initiator "Omnirad 184: manufactured by IGM Resins RV", and 5 parts by weight of a polyisocyanate compound "Coronate L: manufactured by Tosoh" were added to the obtained solution containing an acrylic copolymer (weight average molecular weight 500,000). The obtained adhesive solution was applied to a commercially available release film "E7002: manufactured by Toyobo" so that the adhesive thickness was about 10 μm, and then laminated to the heat-resistant film (Example) of the present invention or the general-purpose film (Comparative Example) to obtain an adhesive sheet. The obtained adhesive sheet was evaluated by the following items.
[0087] ◎The single piece of adhesive sheet has no curling
[0088] ○ The single piece of adhesive sheet curls, but this can be solved by adjusting the tension of the sheet.
[0089] △The single piece of adhesive sheet curls, which is difficult to deal with by adjusting the tension of the sheet
[0090] ×It is difficult to adjust the tension of the sheets during bonding, and the thickness of the adhesive on the individual sheets is uneven
[0091] (8) Expandability
[0092] The adhesive sheet was fixed to a 6-inch cutting frame with double-sided tape, and the center point and the concentric circles of 50 mm and 100 mm in diameter were drawn. Then, the sheet was expanded with an expander (stage: temperature 30°C, rising speed 50 mm / min, holding 60 sec) in a manner that the elongation was specified relative to the inner diameter of the cutting frame. The sheet was measured at a spacing of 45 degrees relative to the concentric circles, and the following evaluation was performed based on the obtained elongation. It should be noted that the specified elongation is obtained by the following formula.
[0093] Elongation (%) = (distance traveled by the stage × 2) / frame inner diameter × 100
[0094] ◎: The specified elongation is 65% or more in all directions, and the maximum difference is less than 2%
[0095] ○: The specified elongation is 65% or more in all directions, with a maximum difference of 2 to 5%
[0096] △: The elongation is 50-65% of the specified elongation in some directions, with a maximum difference of 2-5%
[0097] ×: The elongation is less than 50% of the specified elongation in some directions, or there is a difference of 5% or more at most
[0098] (9) Heat resistance
[0099] Based on JIS K 7206:1999 "Plastics - Thermoplastics - Method for determining Vicat softening temperature (A120 method)", the following evaluation was performed on samples having a thickness of 3 mm obtained by pressing the resins obtained in the following Examples and Comparative Examples.
[0100] ◎: Vicat softening point is above 180℃
[0101] △: Vicat softening point is 170~180℃
[0102] △: Vicat softening point is 160~170℃
[0103] ×: Vicat softening point is 160°C or less
[0104] Next, the present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited to the following Examples.
[0105] <Examples 1 and 2>
[0106] A mixture of commercially available 1,6-hexanediol type aliphatic polycarbonate diol (molecular weight 2000) and diphenyl carbonate was reacted at a temperature of 205°C and a pressure of 130 Pa for 2 hours, and the obtained preparation (number average molecular weight 10000) was polycondensed with PBT (polybutylene terephthalate) at elevated temperature and reduced pressure to obtain a resin having a specified soft segment mass ratio recorded in Table 1.
[0107] The obtained resin (suitable for layer A) is used, and a granular MB (masterbatch) based on the same resin and containing 15wt% of commercially available spherical silica (average particle size 12μm) is used, and a resin (suitable for layer B) in which the spherical silica is made to be 7500ppm using the masterbatch, so that the film thickness constituting A becomes 10% of the total thickness and has a structure constituting A / B. The film is extruded from a T-die by an extruder, pressed onto a cooling roller with an air knife, and then trimmed at the edge during the process to obtain a heat-resistant film with a total film thickness of 100μm of Examples 1 to 2, and the heat-resistant film is in the form of a roll with a width of 650mm and a roll length of 1000m.
[0108] In the above examples, sheeting was performed at a temperature about 10°C higher than the melting point for about 4 to 5 hours, but no abnormal pressure was observed in extrusion or ejection. Table 1 shows the properties of the resins used and the evaluation results of the heat-resistant films and rolls.
[0109] <Comparative Examples 1 and 2>
[0110] Comparative Example 1 and Comparative Example 2 were prepared in the same manner as in Example 1 except that resins under the conditions shown in Table 1 were used. Table 1 shows the physical properties of the obtained films.
[0111] <Examples 3 and 4>
[0112] A mixture of commercially available 1,6-hexanediol type aliphatic polycarbonate diol (molecular weight 2000) and diphenyl carbonate was reacted at a temperature of 205° C. and a pressure of 130 Pa for 2 hours, and a resin was obtained in the same manner as in Example 1 except that PBN (polybutylene naphthalate) was used for the obtained preparation (number average molecular weight 10000).
[0113] Furthermore, similarly to Example 1, a film was formed so that the film thickness of the component A was 10% of the total thickness and the structure of the component A / B was obtained to obtain a heat-resistant film roll having a total film thickness of 100 μm, a width of 650 mm, and a roll length of 1000 m.
[0114] In the above examples, sheeting was performed at a temperature about 10°C higher than the melting point for about 4 to 5 hours, but no abnormal pressure was observed in extrusion or ejection. Table 1 shows the properties of the resins used and the evaluation results of the heat-resistant films and rolls.
[0115] <Comparative Examples 3 and 4>
[0116] Comparative Examples 3 and 4 were prepared in the same manner as in Example 3 except that resins under the conditions shown in Table 1 were used. Table 1 shows the physical properties of the obtained films.
[0117] [Table 1]
[0118]
[0119] The adhesive sheet of the present invention is a heat-resistant film of a resin formed by bonding a hard segment of polyester and a soft segment mainly containing aliphatic polycarbonate, which is a polyester elastomer. The polyester is formed by aromatic dicarboxylic acid and aliphatic diol or alicyclic diol. In the embodiment, the tension is easily adjusted during the application of the adhesive, so the uneven film thickness of the adhesive caused by the lamination of the release film and the curling of the single sheet are reduced. In addition, in terms of expandability, uniform extension can be obtained even at a high elongation, and the high heat resistance that is a characteristic of the polyester elastomer is maintained.
[0120] <Examples 5 to 12>
[0121] A mixture of commercially available 1,6-hexanediol type aliphatic polycarbonate diol (molecular weight 2000) and diphenyl carbonate described in Examples 1 to 4 is reacted at a temperature of 205°C and a pressure of 130 Pa for 2 hours, and the resulting preparation (number average molecular weight 10000) is polycondensed with PBT (polybutylene terephthalate) or PBN (polybutylene naphthalate) at an elevated temperature and reduced pressure to obtain a resin having a specified soft segment mass ratio.
[0122] Using the obtained resin (resin suitable for layer A), a granular MB (masterbatch) based on the same resin and containing 15 wt% of commercially available spherical silica (average particle size 12 μm), and a resin (suitable for layer B) obtained by using the masterbatch and containing 7500 ppm of spherical silica, and except that a carbodiimide compound ("Carbodilite LA-1") was supplied by side feeding in a prescribed amount during the extrusion of the resin suitable for layer A and the resin suitable for layer B, a heat-resistant film was prepared in the same manner as in Example 1. Specifically, the film thickness of the composition A was 10% of the total thickness and the composition A / B structure was formed, extruded from a T-die by an extruder, pressed onto a cooling roll by an air knife, and trimmed at the edges in the process to obtain heat-resistant films of Examples 5 to 12 with a total film thickness of 100 μm, and the heat-resistant films were in the form of rolls with a width of 650 mm and a roll length of 1000 m.
[0123] Table 2 shows the properties of the resins in Examples 5 to 12 and the evaluation results of the sheets and rolls of the resins.
[0124] [Table 2]
[0125]
[0126] The adhesive sheet of the present invention is a heat-resistant film of a resin formed by bonding a hard segment of polyester containing polyester and a soft segment mainly containing aliphatic polycarbonate, wherein the polyester is formed by aromatic dicarboxylic acid and aliphatic diol or alicyclic diol. Although the mechanism of the development is unclear, the expansion property is improved by adding a polycarbodiimide compound, and the reduced viscosity corresponding to the molecular weight is increased, so that the chance of whitening on the cooling roll when obtaining the heat-resistant film is reduced, and the temperature management of the cooling roll becomes easy.
[0127] About 2 g of samples were collected for Examples 1 to 12 and Comparative Examples 1 to 4, cut into pieces and subjected to Soxhlet extraction with chloroform (extraction for 4 hours), and the extract was confirmed to be 0.6 wt % or less.
[0128] Industrial Applicability
[0129] The adhesive sheet of the present invention is a heat-resistant film of a polyester elastomer, and has high heat resistance as its characteristic. In addition, by making the predetermined soft segment used in the polyester elastomer an appropriate amount, it is stable even in processing steps such as coating, and in terms of expansibility, it can be uniformly stretched even at a high elongation, so it is suitable as a surface protection film for protecting the surface state of plastic products, glass products, ceramic products, etc. after conducting electricity, decoration, etc., and is particularly suitable as a surface protection film in semiconductor processes or a dicing tape.
Claims
1. A heat-resistant film comprising a thermoplastic resin, wherein the thermoplastic resin is a polyester elastomer formed by bonding a hard segment and a soft segment, The hard segment has a polyester unit formed by an aromatic dicarboxylic acid and an aliphatic diol or an alicyclic diol. The soft segment is mainly formed by aliphatic polycarbonate. The weight ratio of the hard segment to the soft segment in the polyester elastomer, i.e., hard segment:soft segment, is 50.1:49.9 to 70:
30. The heat-resistant film containing the thermoplastic resin has a two-layer structure consisting of layer A and layer B. The elastic modulus of the heat-resistant film is 30MPa to 500MPa, the elongation at break is 200% to 700%, and the ratio F50 / F25 of the stress F50 at an elongation of 50% to the stress F25 at an elongation of 25% is greater than 1.
05.
2. The heat-resistant film according to claim 1, characterized in that The hard segment of the polyester elastomer includes a polybutylene terephthalate unit, and the melting point of the polyester elastomer is 195° C. to 220° C.
3. The heat-resistant film according to claim 1, characterized in that The hard segment of the polyester elastomer includes a polybutylene naphthalate unit, and the melting point of the polyester elastomer is 210° C. to 240° C. 4 . The heat-resistant film according to claim 1 , which is used for a protective film. 5 . An adhesive sheet comprising an adhesive on at least one surface of the heat-resistant film according to claim 1 .