Erbium-ytterbium co-doped beta-Ta2O5 green up-conversion luminescent material and preparation method thereof

By doping Erbium-ytterbium co-doped β-Ta2O5 green upconversion luminescent material in β-Ta2O5 matrix, the stability and safety problems of NaYF4:Er3+/Yb3+ phosphor were solved, and a higher level of Fluorescence intensity and temperature sensitivity are suitable for photothermal sensing.

CN118909629AActive Publication Date: 2024-11-08DALIAN MARITIME UNIVERSITY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410965988.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

NaYF4:Er3+/Yb3+ upconverting phosphor has insufficient chemical stability and potential toxicity that limit its widespread use, especially in areas where long-term stability and safety are required, such as in vivo implantation and environmental monitoring, and material leakage may be environmentally friendly. and adverse effects of organisms.

Method used

Erbium ytterbium co-doped β-Ta2O5 green upconversion luminescent material is used to improve the chemical stability and safety of the material by doping Er3+ and Yb3+ ions in the β-Ta2O5 matrix, and prepare it by solvent molten salt method to control the morphology For a uniform columnar structure, a pickling step is introduced to remove solvent residues and impurities.

Benefits of technology

Significantly improves the chemical stability and safety of the material, enhances the green upconversion fluorescence intensity, has higher temperature sensitivity, and can replace commercial NaYF4:Er3+/Yb3+ phosphors in the field of photothermal sensing, providing higher Application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909629A_ABST
    Figure CN118909629A_ABST
Patent Text Reader

Abstract

The invention discloses an erbium-ytterbium co-doped beta-Ta2O5 green up-conversion luminescent material and a preparation method thereof, the luminescent material takes beta-Ta2O5 as a matrix, Er < 3 + > and Yb < 3 + > are doped in the matrix, the chemical formula of the luminescent material is beta-Ta2O5: aEr < 3 + > / bYb < 3 + >, a: b = 1: 2-15, and a = 0.003-0.01. The preparation method comprises the steps of raw material mixing, grinding, sintering, suction filtration, drying and the like. The erbium-ytterbium co-doped beta-Ta2O5 green up-conversion luminescent material prepared by the invention takes beta-Ta2O5 as a matrix, is co-doped with Er < 3 + > and Yb < 3 + >, is higher in chemical stability and lower in toxicity, has remarkably enhanced green up-conversion fluorescence intensity, is more sensitive to temperature, and effectively improves the instability and safety problems of NaYF4: Er < 3 + > / Yb < 3 + > fluorescent powder due to the characteristics; therefore, the material has a good application prospect in the specific fields of photo-thermal sensing and the like, and is expected to replace a commercial fluorescent powder product NaYF4: Er < 3 + > / Yb < 3 + >.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of up-conversion luminescent materials, and in particular to an erbium-ytterbium co-doped beta-Ta2O5 green up-conversion luminescent material and a preparation method thereof. Background Art

[0002] In the field of optical materials, rare earth-doped upconversion phosphors have attracted much attention due to their unique energy conversion mechanism, which is the ability to convert long-wavelength, low-energy light into short-wavelength, high-energy light. 3+ / Yb 3+ Upconversion phosphors stand out in many applications with their excellent fluorescence efficiency, high quantum yield and good luminescence stability, especially in biomedical imaging, high-efficiency solar cells, photocatalytic reaction promotion, non-contact temperature measurement systems, advanced anti-counterfeiting technology and optical regulation to promote plant growth, showing great application potential.

[0003] However, despite the NaYF4:Er 3+ / Yb 3+ Phosphors have many advantages, but their lack of chemical stability and potential toxicity have become key factors limiting their further widespread application. Fluoride matrix materials are prone to hydrolysis or corrosion in aqueous solutions and certain chemical environments, resulting in decreased fluorescence performance or even failure, which poses a severe challenge to application fields that require long-term stability and safety of materials (such as implantation in organisms, long-term environmental monitoring, etc.). In addition, the toxicity of fluoride, especially when the material is leaked or handled improperly, may have adverse effects on the environment and organisms, increasing the risk and cost of use. Summary of the invention

[0004] The present invention provides an Er-Yb co-doped β-Ta2O5 green up-conversion luminescent material and a preparation method thereof, wherein the β-Ta2O5 matrix with higher chemical stability and lower toxicity is used to replace the fluoride. 3+ and Yb 3+ By effectively doping rare earth ions, the chemical stability and safety of the material can be significantly improved on the basis of enhancing the original up-conversion luminescence performance, thus overcoming the shortcomings of fluoride-based phosphors.

[0005] In order to achieve the above object, the technical solution of the present invention is:

[0006] An erbium-ytterbium co-doped β-Ta2O5 green up-conversion luminescent material, with β-Ta2O5 as a matrix, and Er doped in the matrix 3+ and Yb 3+ .

[0007] Furthermore, the chemical formula of the luminescent material is β-Ta2O5:aEr 3+ / bYb 3+ , where a:b=1:2~15, a=0.003~0.01.

[0008] Furthermore, the chemical formula of the luminescent material is β-Ta2O5:0.01Er 3+ / 0.02Yb 3+ .

[0009] Furthermore, the chemical formula of the luminescent material is β-Ta2O5:0.0038Er 3+ / 0.05Yb 3+ .

[0010] To achieve the above object, the present invention also provides a method for preparing an Er-Yb co-doped β-Ta2O5 green up-conversion luminescent material, characterized in that it comprises the following steps:

[0011] S1: weigh raw materials Ta2O5, Er2O3 and Yb2O3, mix them evenly and grind them thoroughly;

[0012] S2: Add B2O3 and Sr(NO3)2 to the ground material in S1 and mix them thoroughly. The amount of B2O3 added is 1.5 to 8 times the mass of Ta2O5, and the molar ratio of B2O3 to Sr(NO3)2 is 1:0.0015 to 0.006;

[0013] S3: sintering the mixed materials in S2 at 800-1200° C. for 18-30 hours;

[0014] S4: The product sintered in S3 is subjected to solid-liquid separation, and the solid is dried to obtain a luminescent material.

[0015] Furthermore, the molar ratio of the weighed raw materials Ta2O5, Er2O3 and Yb2O3 is Ta2O5:Er2O3:Yb2O3=1:a:b.

[0016] Furthermore, the luminescent material obtained by drying in S4 is subjected to acid washing treatment in an acid solution with a pH value of 0 to 4 for 5 to 7 hours, followed by solid-liquid separation, and the solid is dried to obtain the acid-washed luminescent material.

[0017] Furthermore, the acid solution is HCl solution.

[0018] Furthermore, the drying time is 1 to 4 hours.

[0019] Furthermore, the purity of Er2O3, Yb2O3 and Ta2O5 is above 99.9%.

[0020] In summary, the present invention has the following beneficial effects:

[0021] First, the matrix β-Ta2O5 used in the present invention is a layered structure composed of TaO6 and TaO7 units. β-Ta2O5 has low phonon energy and is very suitable for doping Er. 3+ / Yb 3+ As an upconversion fluorescent material, β-Ta2O5 has stronger stability and biosafety than fluoride.

[0022] Second, the green up-conversion phosphor prepared by the present invention has good green up-conversion fluorescence intensity. Under 980nm laser excitation, it presents high-brightness pure green fluorescence. The green up-conversion fluorescence integral intensity reaches the commercial phosphor product NaYF4:Er 3+ / Yb 3+ 86.7%.

[0023] Third, the green upconversion luminescent material prepared by the present invention has higher temperature sensitivity. The maximum relative temperature sensitivity calculated by the fluorescence intensity branching ratio technique (LIR) is 0.01145K. -1 The results show that the luminescent material prepared by the present invention has good application prospects in specific fields such as photothermal sensing and is expected to replace the commercial NaYF4:Er 3+ / Yb 3+ Phosphor.

[0024] Fourth, the present invention adopts the solvent molten salt method, and realizes precise control of the preparation process of the luminescent material by finely adjusting various synthesis parameters, and adjusts its morphology into a uniform columnar structure. This uniform columnar structure not only gives the material higher physical stability, but also helps to improve the transmission path and efficiency of photons, thereby enhancing the photoelectric conversion performance.

[0025] Fifth, the introduction of an acid washing step in the preparation method effectively removes solvent residues and impurities on the surface of the material, thereby significantly improving the purity of the final product. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0027] Figure 1 It is the X-ray diffraction result diagram of the luminescent materials prepared in Examples 1 to 6 of the present invention.

[0028] Figure 2 It is the up-conversion fluorescence spectra of the luminescent materials prepared in Examples 2, 4, 5 and 6 under 980nm laser excitation.

[0029] Figure 3 It is a comparison diagram of up-conversion fluorescence spectra of the luminescent materials prepared in Examples 1 and 2 under 980nm laser excitation.

[0030] Figure 4 It is a comparison diagram of up-conversion fluorescence spectra of the luminescent materials prepared in Examples 3 and 4 under 980nm laser excitation.

[0031] Figure 5 These are scanning electron microscope test images of the luminescent materials prepared in Examples 3, 4, and 5.

[0032] Figure 6 The luminescent material prepared in Example 5 and NaYF4:Er 3+ / Yb 3+ Up-conversion fluorescence spectra.

[0033] Figure 7 It is the temperature-variable up-conversion fluorescence spectrum of the luminescent material prepared in Example 5 under 980nm laser excitation.

[0034] Figure 8 This is a graph showing the relationship between the fluorescence branching ratio LIR value and temperature of the luminescent material prepared in Example 5.

[0035] Fig. 9 This is a graph showing the relationship between the relative temperature sensitivity of the luminescent material prepared in Example 5 and temperature. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] The present invention provides an Er-Yb co-doped β-Ta2O5 green up-conversion luminescent material and a preparation method thereof, wherein the β-Ta2O5 matrix with higher chemical stability and lower toxicity is used to replace the fluoride. 3+ and Yb 3+ By effectively doping rare earth ions, the chemical stability and safety of the material can be significantly improved on the basis of enhancing the original up-conversion luminescence performance, thus overcoming the shortcomings of fluoride-based phosphors.

[0038] In order to achieve the above object, the technical solution of the present invention is:

[0039] An erbium-ytterbium co-doped β-Ta2O5 green up-conversion luminescent material, with β-Ta2O5 as a matrix, and Er doped in the matrix 3+ and Yb 3+ .

[0040] Furthermore, the chemical formula of the luminescent material is β-Ta2O5:aEr 3+ / bYb 3+ , where a:b=1:2~15, a=0.003~0.01.

[0041] β-Ta2O5 has stronger stability and biosafety than fluoride. It has a layered structure consisting of TaO6 and TaO7 units and has low phonon energy, making it very suitable as a matrix for Er doping. 3+ / Yb 3+ As an up-conversion fluorescent material, the fluorescence integral intensity of the up-conversion green light of the prepared fluorescent material can reach that of the commercial phosphor product NaYF4:Er 3+ / Yb 3+ More than 18.8%.

[0042] Furthermore, the chemical formula of the up-conversion luminescent material is β-Ta2O5:0.01Er 3+ / 0.02Yb 3+ .

[0043] After optimizing the co-doping ratio of erbium and ytterbium, the fluorescence integrated intensity of the upconverted green light of the prepared fluorescent material can reach that of the commercial phosphor product NaYF4:Er 3+ / Yb 3+ 49.4%.

[0044] Furthermore, the chemical formula of the up-conversion luminescent material is β-Ta2O5:0.0038Er 3+ / 0.05Yb 3+ .

[0045] After optimizing the co-doping ratio of erbium and ytterbium, the prepared fluorescent material exhibits high-brightness pure green fluorescence under 980nm laser excitation, and the integrated intensity reaches that of the commercial phosphor product NaYF4:Er 3+ / Yb 3+ It also has higher temperature sensitivity, and the maximum relative temperature sensitivity calculated using the fluorescence intensity branching ratio technique (LIR) is 0.01145K. -1 , has good application prospects in specific fields such as photothermal sensing, and is expected to replace commercial NaYF4:Er 3+ / Yb 3+ Phosphor.

[0046] The present invention also provides a method for preparing an erbium-ytterbium co-doped β-Ta2O5 green up-conversion luminescent material, which is characterized by comprising the following steps:

[0047] S1: weigh raw materials Ta2O5, Er2O3 and Yb2O3, mix them evenly and grind them thoroughly;

[0048] S2: Add B2O3 and Sr(NO3)2 to the ground material in S1 and mix them thoroughly. The amount of B2O3 added is 1.5 to 8 times the mass of Ta2O5, and the molar ratio of B2O3 to Sr(NO3)2 is 1:0.0015 to 0.006;

[0049] S3: sintering the mixed materials in S2 at 800-1200° C. for 18-30 hours;

[0050] S4: The product sintered in S3 is subjected to solid-liquid separation, and the solid is dried to obtain a luminescent material.

[0051] Furthermore, the molar ratio of the weighed raw materials Ta2O5, Er2O3 and Yb2O3 is Ta2O5:Er2O3:Yb2O3=1:a:b.

[0052] This scheme uses the solvent molten salt method to prepare Er-Yb co-doped β-Ta2O5 green upconversion luminescent material. By finely adjusting various synthesis parameters, the luminescent material preparation process is precisely controlled, and its morphology is adjusted to a uniform columnar structure. This uniform columnar structure not only gives the material higher physical stability, but also helps to improve the transmission path and efficiency of photons, thereby enhancing the photoelectric conversion performance.

[0053] Furthermore, the luminescent material obtained by drying in S4 is subjected to acid washing treatment in an acid solution with a pH value of 0 to 4 for 5 to 7 hours, followed by solid-liquid separation, and the solid is dried to obtain the acid-washed luminescent material.

[0054] In the preparation method of this scheme, the liquid B2O3 and Sr(NO3)2 solvents are removed by solid-liquid separation at high temperature, and a pickling step is introduced into the dried product to further remove the solvent residues and impurities on the surface of the material, thereby significantly improving the purity of the final product.

[0055] Furthermore, the acid solution is HCl solution.

[0056] Furthermore, the drying time is 1 to 4 hours.

[0057] Furthermore, the purity of Er2O3, Yb2O3 and Ta2O5 is above 99.9%.

[0058] Through the above-mentioned preferred preparation process parameters, precise control of the processing of Er-Yb co-doped β-Ta2O5 green upconversion luminescent material is achieved. The prepared luminescent material has high purity and high safety, better chemical stability, lower toxicity, significantly enhanced green upconversion fluorescence intensity, and is more sensitive to temperature, which improves the NaYF4:Er 3+ / Yb 3+ The instability and safety issues of phosphors have good application prospects in specific fields such as photothermal sensing and are expected to replace commercial NaYF4:Er 3+ / Yb 3+ Phosphor.

[0059] Example 1

[0060] Preparation of Erbium-Ytterbium Co-doped β-Ta2O5 Green Upconversion Luminescent Material by Solvent Molten Salt Method:

[0061] S1: Molar ratio 5+ :Er 3+ :Yb 3+ =2:0.01:0.02, weigh 2g Ta2O5, 0.0087g Er2O3, 0.0178g Yb2O3 respectively, mix well and grind thoroughly for 30min;

[0062] S2: Add 15g of B2O3 and 0.0958g of Sr(NO3)2 to the ground material in S1 and mix thoroughly. The amount of B2O3 added is 7.5 times the mass of Ta2O5, and the molar ratio of B2O3 to Sr(NO3)2 is 1:0.0015;

[0063] S3: sintering the mixed materials in S2 at 1000° C. for 30 hours;

[0064] S4: After filtering the product sintered in S3, place it in an oven and dry it at 80° C. for 2 hours to obtain a luminescent material.

[0065] Example 2

[0066] Preparation of Erbium-Ytterbium Co-doped β-Ta2O5 Green Upconversion Luminescent Material by Solvent Molten Salt Method:

[0067] S1: Molar ratio 5+ :Er 3+ :Yb 3+ =2:0.01:0.02, weigh 2g Ta2O5, 0.0087g Er2O3, 0.0178g Yb2O3 respectively, mix well and grind thoroughly for 30min;

[0068] S2: Add 15g of B2O3 and 0.0958 of Sr(NO3)2 to the ground material in S1 and mix thoroughly. The amount of B2O3 added is 7.5 times the mass of Ta2O5, and the molar ratio of B2O3 to Sr(NO3)2 is 1:0.0015;

[0069] S3: sintering the mixed materials in S2 at 1000° C. for 30 hours;

[0070] S4: After filtering the product sintered in S3, place it in an oven and dry it at 80°C for 2h;

[0071] S5: The dried sample is placed in a pH 4 HCl solution for pickling for 6 hours, and then the sample is filtered and then placed in an oven for drying at 80° C. for 2 hours to obtain a luminescent material.

[0072] Example 3

[0073] Preparation of Erbium-Ytterbium Co-doped β-Ta2O5 Green Upconversion Luminescent Material by Solvent Molten Salt Method:

[0074] S1: Molar ratio 5+ :Er 3+ :Yb 3+ =2:0.01:0.02, weigh 2g Ta2O5, 0.0087g Er2O3, 0.0178g Yb2O3 respectively, mix well and grind thoroughly for 30min;

[0075] S2: Add 3g of B2O3 and 0.0479g of Sr(NO3)2 to the ground material in S1 and mix thoroughly. The amount of B2O3 added is 1.5 times the mass of Ta2O5, and the molar ratio of B2O3 to Sr(NO3)2 is 1:0.0038;

[0076] S3: sintering the mixed materials in S2 at 1100° C. for 18 hours;

[0077] S4: After filtering the product sintered in S3, place it in an oven and dry it at 80° C. for 2 hours to obtain a luminescent material.

[0078] Example 4

[0079] Preparation of Erbium-Ytterbium Co-doped β-Ta2O5 Green Upconversion Luminescent Material by Solvent Molten Salt Method:

[0080] S1: Molar ratio 5+ :Er 3+ :Yb 3+=2:0.01:0.02, weigh 2g Ta2O5, 0.0087g Er2O3, 0.0178g Yb2O3 respectively, mix well and grind thoroughly for 30min;

[0081] S2: Add 15g of B2O3 and 0.2395g of Sr(NO3)2 to the ground material in S1 and mix them thoroughly. The amount of B2O3 added is 7.5 times the mass of Ta2O5, and the molar ratio of B2O3 to Sr(NO3)2 is 1:0.0038;

[0082] S3: sintering the mixed materials in S2 at 1100° C. for 18 hours;

[0083] S4: After filtering the product sintered in S3, place it in an oven and dry it at 80°C for 2h;

[0084] S5: The dried sample is placed in a pH 2 HCl solution for pickling for 6 hours, and then the sample is filtered and then placed in an oven for drying at 80° C. for 2 hours to obtain a luminescent material.

[0085] Example 5

[0086] Preparation of Erbium-Ytterbium Co-doped β-Ta2O5 Green Upconversion Luminescent Material by Solvent Molten Salt Method:

[0087] S1: Molar ratio 5+ :Er 3+ :Yb 3+ =2:0.0038:0.05, weigh 2g of Ta2O5, 0.0033g of Er2O3, and 0.0446g of Yb2O3 respectively, mix them evenly, and grind them thoroughly for 30min;

[0088] S2: Add 15g of B2O3 and 0.2395g of Sr(NO3)2 to the ground material in S1 and mix them thoroughly. The amount of B2O3 added is 7.5 times the mass of Ta2O5, and the molar ratio of B2O3 to Sr(NO3)2 is 1:0.0038;

[0089] S3: sintering the mixed materials in S2 at 1100° C. for 24 hours;

[0090] S4: After filtering the product sintered in S3, place it in an oven and dry it at 80°C for 2h;

[0091] S5: The dried sample is placed in a pH 0 HCl solution for pickling for 6 hours, and then the sample is filtered and then placed in an oven for drying at 80° C. for 2 hours to obtain a luminescent material.

[0092] Example 6

[0093] Preparation of Erbium-Ytterbium Co-doped β-Ta2O5 Green Upconversion Luminescent Material by Solvent Molten Salt Method:

[0094] S1: Molar ratio 5+ :Er 3+ :Yb 3+ =2:0.01:0.02, weigh 2g Ta2O5, 0.0087g Er2O3, 0.0178g Yb2O3 respectively, mix well and grind thoroughly for 30min;

[0095] S2: Add 15g of B2O3 and 0.3831g of Sr(NO3)2 to the ground material in S1 and mix thoroughly. The amount of B2O3 added is 7.5 times the mass of Ta2O5, and the molar ratio of B2O3 to Sr(NO3)2 is 1:0.006;

[0096] S3: sintering the mixed materials in S2 at 1200° C. for 18 hours;

[0097] S4: After filtering the product sintered in S3, place it in an oven and dry it at 80°C for 2h;

[0098] S5: The dried sample is placed in a pH 0 HCl solution for pickling for 6 hours, and then the sample is filtered and then placed in an oven for drying at 80° C. for 2 hours to obtain a luminescent material.

[0099] The specific experimental conditions of each embodiment are shown in Table 1:

[0100] Table 1 List of experimental conditions corresponding to each embodiment

[0101]

[0102] Test and result analysis

[0103] (1) X-ray diffraction (XRD) test and results

[0104] Examples 1, 2, 3, 4, 5, 6 with different Sr(NO3)2 solvent amounts and different Er 3+ / Yb 3+ The luminescent material samples prepared by the molten salt method with a content of 2.5-1.5 were subjected to X-ray diffraction test, and the results were as follows: Figure 1 shown.

[0105] The results show that Erbium-ytterbium co-doped β-Ta2O5 green upconversion luminescent material with target fluorescence intensity was successfully prepared under the preparation conditions provided by the present invention using B2O3 and Sr(NO3)2 as solvent molten salt method.

[0106] Comparison of the diffraction patterns of the luminescent material samples prepared in Examples 1, 2, 3, and 4 shows that there will be certain B2O3 residues on the surface of the grown crystals, but they can be removed by acid washing, further improving the purity of the samples.

[0107] The diffraction patterns of the luminescent material samples prepared in Examples 2, 4, and 6 show that when the Sr(NO3)2 content increases, hexagonal SrTa4O 11 Phase impurities.

[0108] The diffraction pattern of the luminescent material sample prepared in Example 5 shows that the luminescent material crystal grown under the preparation conditions is pure β-Ta2O5 phase, contains almost no B2O3 residue, and only a small amount of SrTa4O 11 Phase impurities exist.

[0109] (2) Upconversion spectrum test and result analysis

[0110] In the spectral test within the green up-conversion wavelength range conducted on the luminescent material samples prepared in Examples 1 to 6, the results (eg Figures 2 to 4 Specifically, the luminescent material samples prepared in the six embodiments all successfully exhibited green up-conversion luminescence characteristics and had a certain fluorescence intensity, which indicates that these luminescent material samples can effectively convert low-energy photons into green high-energy photons under specific excitation conditions. Among them, the luminescent material sample prepared in Example 5 showed stronger performance in green up-conversion fluorescence intensity, and its fluorescence intensity was significantly higher than that of the other embodiments, which reflects the optimization effect of Example 5 in preparation process or formula.

[0111] Figure 3 and Figure 4 This indicates that the pickling treatment can further improve the fluorescence intensity of the sample. The fluorescence intensities of the samples prepared in Example 2 and Example 4 after the pickling treatment are 1.65 times and 1.82 times of the samples prepared in Example 1 and Example 3 without the pickling treatment, respectively.

[0112] (3) Scanning electron microscope (SEM) test and result analysis

[0113] The samples of the luminescent materials prepared in Examples 3, 4, and 5 were scanned by electron microscope, and SEM images were generated. Figure 5 The results show that compared with Example 3, the luminescent material sample prepared by adding the acid washing process in Example 4 can remove some small particles and residual B2O3 on the surface of the large crystal. In addition to acid washing, Example 5 also adjusts the Er 3+ / Yb 3+The concentration formula, the crystal morphology of the prepared luminescent material sample is a columnar structure, which provides a more direct transmission channel, reduces the scattering and loss of photons inside the material, and thus greatly improves the photoelectric transmission efficiency. In addition, the acid washing step reduces the solvent residue and ensures the purity of the prepared luminescent material sample.

[0114] (4) 980nm laser excitation test and upconversion spectrum analysis

[0115] Under 980nm laser excitation, the existing commercial NaYF4:Er 3+ / Yb 3+ The green phosphor was tested and compared with the luminescent material samples prepared in the examples for fluorescence performance. The results are shown in Table 2:

[0116] Table 2 Fluorescence intensity of each example for commercial product NaYF4:Er 3+ / Yb 3+ Proportion

[0117] Sample No. <![CDATA[Fluorescence intensity vs. proportion (%) of NaYF4:Er 3+ / Yb 3+ green phosphor]]> Example 1 18.8 Example 2 31.1 Example 3 27.1 Example 4 49.4 Example 5 86.7 Example 6 37.9

[0118] The fluorescence integrated intensity of the up-conversion green light of the samples prepared in Examples 1 to 6 can reach that of the commercial phosphor product NaYF4:Er 3+ / Yb 3+ The up-conversion fluorescence spectrum of the sample prepared in Example 5 is as follows Figure 6 As shown in the figure, the fluorescence integrated intensity of the upconverted green light can reach that of the commercial phosphor product NaYF4:Er 3+ / Yb 3+ 86.7%.

[0119] (5) Analysis of the test results of variable temperature upconversion spectroscopy excited by 980nm laser

[0120] Under 980nm laser excitation, the luminescent material sample prepared in Example 5 was tested for variable temperature upconversion fluorescence spectrum, and the LIR value and relative temperature sensitivity S R The relationship between temperature.

[0121] The spectrum test results are as follows Figure 7 As shown. In the temperature range of 303 to 723K, Er 3+ Ionic 2 H 11 / 2 → 4 I 15 / 2 , 4 S 3 / 2 → 4 I 15 / 2 and 4 F 9 / 2 → 4 I15 / 2 The transition emission decreases with increasing temperature.

[0122] Based on the characteristic that the fluorescence integral intensity of the transition of two thermally coupled energy levels of rare earth ions to the ground state emission is only related to temperature, it is also called LIR technology. The sensitivity of LIR value to temperature determines the application prospect of fluorescent materials in the field of photothermal. The relationship curve between LIR value and temperature T of the luminescent material sample prepared in Example 5 can be calculated by the following formula:

[0123]

[0124] I H For Er 3+ of 2 H 11 / 2 → 4 I 15 / 2 Emission fluorescence integrated intensity value;

[0125] I S For Er 3+ of 4 S 3 / 2 → 4 I 15 / 2 The value of the integrated intensity of emitted fluorescence; B is a constant, k B is the Boltzmann constant, ΔE is 2 H 11 / 2 and 4 S 3 / 2 The band gap between energy levels.

[0126] The fitted function is LIR = 32.99exp(-1050.11 / T), see Figure 8 , indicating that the LIR value increases with the increase of temperature, with a one-to-one correspondence and a high sensitivity.

[0127] Relative temperature sensitivity S of the luminescent material sample prepared in Example 5 R The relationship curve between temperature T can be calculated by the following formula:

[0128]

[0129] The results are as follows Fig. 9 As shown, it shows that the sample has a maximum relative temperature sensitivity of 0.01145K at 303K. -1 , while the commercial NaYF4:Er 3+ / Yb 3+ The maximum absolute sensitivity of the phosphor at 363K is 0.00368K -1, which means that the luminescent material sample prepared in Example 5 can more accurately sense and respond to temperature changes, thereby improving the accuracy and reliability of sensing and having better application prospects in the field of photothermal sensing.

[0130] In summary, the erbium-ytterbium co-doped β-Ta2O5 green upconversion luminescent material prepared by the present invention uses β-Ta2O5 as a matrix, has higher chemical stability and lower toxicity, has significantly enhanced green upconversion fluorescence intensity, and is more sensitive to temperature, thus improving the NaYF4:Er 3+ / Yb 3+ The instability and safety issues of phosphors have good application prospects in specific fields such as photothermal sensing and are expected to replace commercial NaYF4:Er 3+ / Yb 3+ Phosphor.

[0131] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. An Er-Yb co-doped β-Ta2O5 green up-conversion luminescent material, characterized in that: The luminescent material is based on β-Ta2O5, in which Er is doped 3+ and Yb 3+ .

2. The Erbium-Ytterbium co-doped β-Ta2O5 green up-conversion luminescent material according to claim 1, characterized in that: The chemical formula of the luminescent material is β-Ta2O5:aEr 3+ / bYb 3+ , where a:b=1:2~15, a=0.003~0.

01.

3. The Erbium-Ytterbium co-doped β-Ta2O5 green up-conversion luminescent material according to claim 2, characterized in that: The chemical formula of the luminescent material is β-Ta2O5:0.01Er 3+ / 0.02Yb 3+ .

4. The Erbium-Ytterbium co-doped β-Ta2O5 green up-conversion luminescent material according to claim 2, characterized in that: The chemical formula of the luminescent material is β-Ta2O5:0.0038Er 3+ / 0.05Yb 3+ .

5. A method for preparing the erbium-ytterbium co-doped β-Ta2O5 green up-conversion luminescent material according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1: weigh raw materials Ta2O5, Er2O3 and Yb2O3, mix them evenly and grind them thoroughly; S2: Add B2O3 and Sr(NO3)2 to the ground material in S1 and mix them thoroughly. The amount of B2O3 added is 1.5 to 8 times the mass of Ta2O5, and the molar ratio of B2O3 to Sr(NO3)2 is 1:0.0015 to 0.006; S3: sintering the mixed materials in S2 at 800-1200° C. for 18-30 hours; S4: The product sintered in S3 is subjected to solid-liquid separation, and the solid is dried to obtain a luminescent material.

6. The method for preparing the Er-Yb co-doped β-Ta2O5 green up-conversion luminescent material according to claim 5, characterized in that: The chemical formula of the luminescent material is β-Ta2O5:aEr 3+ / bYb 3+ , wherein a:b=1:2~15, a=0.003~0.01, and the molar ratio of the raw materials Ta2O5, Er2O3 and Yb2O3 is Ta2O5:Er2O3:Yb2O3=2:a:b.

7. The method for preparing the Er-Yb co-doped β-Ta2O5 green up-conversion luminescent material according to claim 5, characterized in that: The luminescent material obtained by drying in S4 is pickled in an acid solution with a pH value of 0 to 4 for 5 to 7 hours, followed by solid-liquid separation, and the solid is dried to obtain the acid-washed luminescent material.

8. The method for preparing the Er-Yb co-doped β-Ta2O5 green up-conversion luminescent material according to claim 7, characterized in that: The acid solution is HCl solution.

9. The method for preparing the Er-Yb co-doped β-Ta2O5 green up-conversion luminescent material according to claim 5, characterized in that: The drying time is 1 to 4 hours.

10. The method for preparing the Er-Yb co-doped β-Ta2O5 green up-conversion luminescent material according to claim 5, characterized in that: The purity of the Er2O3, Yb2O3 and Ta2O5 are all above 99.9%.

Citation Information

Patent Citations

  • Erbium-ytterbium-doped CaTa4O11 up-conversion fluorescent material and preparation method thereof

    CN116574510A

  • Method for preparing erbium-ytterbium-doped LaTa7O19 up-conversion fluorescent powder through molten salt method and application