Method for deeply removing impurities from secondary zinc oxide
Through the granulation and two-stage treatment process of zinc oxide, combined with ball milling treatment, the problem of difficult removal of impurities such as fluorine and chlorine in zinc oxide is solved, and the efficient and economical deep removal effect is achieved, satisfying zinc smelting Strict requirements for impurity content.
Patent Information
- Application Number
- CN202410946052.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art is difficult to effectively and economically remove impurities such as fluorine and chlorine in zinc oxide, resulting in increased zinc smelting costs and low production efficiency.
Griting technology is used to make zinc oxide into notched square-like pellets, and through two-stage processes of low-temperature pretreatment and high-temperature roasting, the volatilization of moisture forms a channel to promote the discharge of impurities, combined with ball milling to improve impurity detachment. Derate.
The deep removal of impurities such as fluorine and chlorine in zinc oxide has been achieved, reaching a removal rate of 98.5% or above, reducing production costs, meeting the strict requirements of zinc electrolysis for impurity content, and improving the recovery rate of zinc and The degree of mechanization of the smelting system.
Smart Images

Figure CN118910413A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgy and chemical engineering, and in particular to a method for deep impurity removal of zinc oxide. Background Art
[0002] The zinc hydrometallurgy process involves zinc electrolysis. During zinc electrolysis, impurity elements such as As, Sb, Pb, F, and Cl can cause zinc electrolysis plates to burn, increase zinc electrolysis energy consumption, or reduce the quality of precipitated zinc, thereby increasing the production cost of zinc smelting. For example, fluoride ions destroy the aluminum oxide film on the surface of the cathode aluminum plate, forming a zinc-aluminum solid solution that makes it difficult to peel the zinc sheet, resulting in increased consumption of the cathode aluminum plate, which affects the production capacity of the enterprise. In severe cases, it causes production to stop. At the same time, fluorine is a highly toxic substance. A high fluorine content will deteriorate the working environment of the workshop and affect the health of the employees of the enterprise. Chlorine mainly affects the anode lead plate during the electrolysis process, causing the quality of the precipitated zinc to deteriorate and increasing production costs. Impurities such as arsenic and antimony can cause the precipitated zinc to burn, and the precipitated zinc to become black and brittle. In severe cases, it will dissolve back and deteriorate the entire electrolysis, leading to a production stoppage.
[0003] With the advancement of zinc smelting technology, zinc electrolysis has become increasingly large-scale, and the requirements for impurities in the electrolysis process have become more and more stringent, especially for impurities such as As, Sb, F, and Cl. For example, in the zinc hydrometallurgical process, the impurity element content in the new solution is required to meet the requirements of As≤0.0002g / L, Sb≤0.0002g / L, Cl≤0.3g / L, and F≤0.03g / L. The quality requirements of zinc oxide entering hydrometallurgy are that F and Cl meet Cl≤0.08% and F≤0.006%.
[0004] With the progress of zinc smelting and the expansion of zinc production, the supply of zinc sulfide concentrate is becoming increasingly exhausted. Secondary zinc oxide, as an important secondary resource, has become another supplement to zinc hydrometallurgical raw materials and has entered the vision of zinc smelting enterprises. Secondary zinc oxide usually refers to zinc oxide containing a certain amount of impurity elements, especially relatively high content of F and Cl. There are 6 main types: 1. Zinc oxide dust produced by the volatilization of hydrometallurgical zinc leaching slag through a rotary kiln; 2. Hot-dip galvanizing ash; 3. Zinc oxide dust produced by the recycling process of galvanized steel scrap; 4. Zinc oxide dust produced by a lead fuming furnace; 5. Zinc oxide dust, a by-product of brass smelting; 6. Zinc oxide dust produced by the reduction and volatilization of blast furnace dust in a short furnace.
[0005] At present, the zinc oxide smoke produced by short furnace reduction and volatilization of blast furnace dust in steelmaking has the characteristics of less valuable recoverable metals such as lead, indium, silver, cadmium, cobalt, and nickel, but higher content of impurity elements such as As, Sb, Pb, F, and Cl. In particular, the content of F and Cl exceeds 0.45% and 8.5% respectively, which is difficult to remove completely in one method during the enterprise's pretreatment and impurity removal process.
[0006] At present, there are two main methods for pretreatment and impurity removal of zinc oxide: roasting method and alkali washing method. In roasting method, fluoride and chloride in zinc oxide undergo physical and chemical changes in a multi-chamber furnace at a high temperature of about 700℃ and a certain negative pressure in the furnace, so that fluorine and chlorine compounds are desorbed and return to the gas phase, low-boiling fluorine and chlorine compounds are volatilized, and fluorine and chlorine compounds of lead and zinc are decomposed into gaseous state, which enter the flue gas system along with furnace gas and zinc oxide smoke and are removed. However, the multi-chamber furnace equipment of this method has high one-time investment and high energy consumption, and the equipment is easy to damage and has high maintenance cost. It is mainly used for impurity removal of zinc oxide raw materials with F and Cl contents below 0.2% and 1% respectively, and the removal rate of F and Cl is less than 85%. For zinc oxide smoke with high fluorine and chlorine content, the removal effect is poor. The alkaline washing method utilizes the principle of double decomposition reaction, taking advantage of the fact that alkali metals and halogen compounds are easily soluble in water, while lead and zinc react with alkali or carbonate ions to generate compounds that are insoluble in weak alkalis to achieve the purpose of separation from fluorine and chlorine. Alkaline washing for fluorine and chlorine removal has the advantages of simple equipment and operation, and low cost. However, a single alkaline washing process is difficult to remove completely, and the amount of wastewater is large, and the zinc loss rate is high.
[0007] Traditional rotary kilns can use reduction-oxidation method to treat zinc-containing slag to recover valuable metals such as zinc, lead, indium and silver in the slag. At high temperature of 1100℃~1300℃, valuable metals such as zinc, lead, indium and silver in the zinc-containing slag (mainly in oxide state, and partly in sulfide state) are reduced to metals by carbon monoxide and volatilize into flue gas, and are oxidized into zinc oxide and the like in the flue gas. They leave the volatilization kiln with the flue gas and are collected in the dust collector. At the same time, the impurity elements F and Cl are removed. The removal rates of F and Cl are often only 80-90% and 55-65% respectively. Therefore, it is difficult to effectively remove F and Cl for zinc oxide with high F and Cl content by traditional methods.
[0008] For example, the Chinese patent for a method for efficiently removing F and Cl from zinc oxide ash and producing electrolytic zinc (CN101649396B) adopts a rotary kiln roasting method, and sulfuric acid is added before and after the zinc oxide is granulated. The corrosiveness of sulfuric acid increases the loss and depreciation of the rotary kiln, so the economic efficiency is not high and it is difficult to promote. The invention patent for a method for removing fluorine, chlorine and valuable metals from zinc oxide (CN104773751A) overcomes the shortcomings of adding sulfuric acid to corrode the equipment, and the temperature is controlled between 950-1000°C, the temperature is reduced to a certain extent, and the energy consumption and production cost are reduced to a certain extent, but the direct recovery rate of zinc is only 93wt%, and the fluorine in the roasted sand is ≤0.03wt%, and the chlorine is ≤0.50wt%. The roasted sand cannot be directly used for zinc hydrometallurgy to recover the zinc therein, and it is necessary to add a defluorination and dechlorination process again before the electrolytic zinc process, which increases the production cost. At the same time, the material processing time is long, which occupies a large amount of working capital. The invention patents of a smelting method for defluorinating and chlorinating zinc oxide containing fluorine and chlorine and enriching valuable metals (CN103924091A) and a smelting method for defluorinating and chlorinating zinc oxide (CN113122734A) can better remove fluorine and chlorine and enrich valuable metals, and the F and Cl contents in zinc oxide are removed to fluorine ≤ 0.01% and chlorine ≤ 0.05%, respectively. However, these two methods require "reaction temperature 1200-1300°C" and "total sulfur is 0.5 to 2.5 times the theoretical calculated amount", which are relatively high requirements. Therefore, this method has the disadvantages of long process, low production efficiency, high investment and technical transformation costs, high energy consumption, high dust, and zinc direct recovery rate of only 90%. At the same time, there are special requirements for the sulfur content in the zinc oxide raw material.
[0009] Therefore, how to find an efficient, environmentally friendly, low-cost one-time deep treatment method for zinc oxide powder with F and Cl contents reaching or exceeding 0.45% and 8.5% respectively to meet the requirements of electrolytic zinc raw materials is a problem that needs to be solved before us. At the same time, it is also necessary to formulate corresponding recycling technology routes based on the material's phase properties, physical properties (such as particle size, tap density, bulk density, etc.) and the production status of the enterprise. Therefore, it is imperative to seek a more economical, environmentally friendly, energy-saving and efficient method for deep removal of zinc oxide impurities such as arsenic, antimony, fluorine, and chlorine. Summary of the invention
[0010] The technical problem to be solved by the present invention is to provide a method for deep impurity removal of zinc oxide which is economical, efficient, energy-saving and environmentally friendly and can effectively remove impurities such as arsenic, antimony, fluorine and chlorine.
[0011] In order to solve the above technical problems, the present invention provides a method for deep impurity removal of zinc oxide, comprising the following steps:
[0012] Add water to zinc oxide and mix to form square zinc oxide particles with notches;
[0013] The secondary zinc oxide granules are sent to the pretreatment section with a lifting plate in the rotary kiln for low-temperature stirring pretreatment to obtain the pretreated secondary zinc oxide material;
[0014] The pre-treated zinc oxide material is sent to the high temperature section of the rotary kiln for high temperature roasting to obtain zinc oxide roasted sand;
[0015] The process of recovering valuable metals from zinc oxide roasted sand after ball milling.
[0016] Furthermore, the secondary zinc oxide is a secondary zinc oxide with a medium particle size of ≤15 μm, and the mass of water added to the secondary zinc oxide is 5.2-7.2 wt % of the mass of the secondary zinc oxide.
[0017] Furthermore, the notched square-shaped zinc oxide particles have a side length of 7.5 to 10.5 mm and a notch depth of 2 to 4 mm.
[0018] Furthermore, during the low-temperature pretreatment of the secondary zinc oxide particles, natural gas is used as fuel for heating or electric heating is used for heating.
[0019] Furthermore, the treatment temperature of the low-temperature pretreatment of the secondary zinc oxide particles is controlled at 510-580° C., the time is 0.3-1.5 h, and the inlet wind pressure of the rotary kiln pretreatment section is controlled at 1800-2000 Pa.
[0020] Furthermore, the copying plates in the pretreatment section of the rotary kiln are uniformly welded on the inner circumference of the treatment section. There are 8 to 14 copying plates on the inner circumference of the treatment section. Each copying plate is 3 to 6 mm thick, 13 to 18 mm long, and 46 to 54 mm high.
[0021] Furthermore, the pretreated secondary zinc oxide material is roasted in the high temperature section of the rotary kiln at a temperature of 830 to 930° C. for a time of 1.8 to 2.8 hours.
[0022] Furthermore, smoke dust containing impurities such as F, Cl, As and Sb is generated by roasting the pretreated secondary zinc oxide material in the high temperature section of the rotary kiln and is discharged after being cooled and dust-collected along with the kiln tail gas and meeting the standards.
[0023] Furthermore, the zinc oxide roasted sand is ball-milled to D90≤63 μm and then sent to a zinc hydrometallurgical system to recover valuable metals.
[0024] Furthermore, the medium particle size of the zinc oxide roasted sand after ball milling is ≥380 meshes.
[0025] The invention provides a method for deep impurity removal of zinc secondary oxide. The method comprises the following steps: firstly, water is added to the zinc secondary oxide for granulation. This method can not only solve the dust pollution in the subsequent impurity removal process and the generation of a large amount of dust by the zinc secondary oxide during pretreatment and high-temperature roasting, thereby improving the direct recovery rate of zinc, but also enable the impurity elements such as F, Cl, As and Sb to enter the smoke from the zinc secondary oxide at a shorter distance, thereby improving the removal rate of F, Cl, As and Sb.
[0026] In addition, the present invention provides a method for deep impurity removal of secondary zinc oxide. During granulation, the secondary zinc oxide is granulated into square-like particles with notches. In the subsequent low-temperature pretreatment and high-temperature roasting steps, the water added to the secondary zinc oxide for granulation will volatilize when heated, and will form the shortest distance channel in the square-like secondary zinc oxide particles with notches, which can be used as a channel for the discharge of impurity elements such as arsenic, antimony, fluorine, and chlorine, which is conducive to the discharge of impurities such as arsenic, antimony, fluorine, and chlorine into smoke with the shortest distance, thereby maximizing the removal rate of impurities such as arsenic, antimony, fluorine, and chlorine, and can quickly remove high-content fluorine and chlorine in the secondary zinc oxide that are difficult to remove under environmentally friendly and low-cost conditions.
[0027] Meanwhile, the invention provides a method for deep impurity removal of zinc oxide, which adopts a two-stage impurity removal process of low-temperature pretreatment and high-temperature roasting in the impurity removal process, so that compounds such as basic zinc fluoride, basic zinc chloride, basic lead fluoride and basic lead chloride in the zinc oxide are easily activated after the low-temperature pretreatment, which is beneficial to the deep removal of impurity elements such as F and Cl in the later high-temperature roasting process, and can make the removal rates of fluorine and chlorine in zinc oxide with high fluorine and chlorine content exceed 98.5% and 99% respectively, and make the contents of F and Cl in the zinc oxide roasted sand obtained after high-temperature roasting drop to below 0.08wt% and 0.006wt% respectively, meeting the current large-scale zinc electrolytic plate requirements for impurities As≤0.0002g / L, Sb≤0.0002g / L, Cl≤0.3g / L and F≤0.03g / L in the zinc liquid, and ensuring that zinc electrolysis in subsequent zinc hydrometallurgy and zinc extraction does not cause plate burning due to the impurity elements F, Cl, As and Sb. It can not only achieve the purpose of deep removal of F and Cl impurities, but also save energy and reduce production costs, while also not adding additional removal steps for arsenic, antimony, fluorine, chlorine and other impurities in the subsequent wet smelting zinc extraction process.
[0028] In addition, the method for deep impurity removal of zinc suboxide provided by the present invention not only solves the problem of deep impurity removal of zinc suboxide with high fluorine and chlorine contents reaching or exceeding 0.45wt% and 8.5wt%, but also has a small number of impurity removal process flows, high efficiency and high degree of mechanization, which greatly improves energy saving, environmental protection and economic benefits, and is conducive to large-scale promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1A flow chart of a method for deep impurity removal of zinc oxide provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0030] See also Figure 1 The method for deep impurity removal of zinc oxide provided by the embodiment of the present invention is very suitable for deep impurity removal of zinc oxide with fluorine and chlorine contents exceeding 0.45wt% and 8.5wt%, respectively. The specific steps are as follows:
[0031] Step 1) Granulation: Add water to zinc oxide and mix to form square zinc oxide granules with notches.
[0032] The secondary zinc oxide has a medium particle size of ≤15 μm, and the mass of water added to the secondary zinc oxide is 5.2-7.2 wt % of the mass of the secondary zinc oxide.
[0033] In addition, the side length of the notched square-shaped zinc oxide particles is 7.5 to 10.5 mm, and the notch depth is 2 to 4 mm.
[0034] The present invention granulates the secondary zinc oxide by adding water, which not only solves the dust pollution in the subsequent impurity removal process and the generation of a large amount of dust by the secondary zinc oxide in the subsequent low-temperature pretreatment and high-temperature roasting process, thereby improving the direct recovery rate of zinc, but also allows impurity elements such as F, Cl, As and Sb to enter the smoke from the secondary zinc oxide at a shorter distance, thereby improving the removal rate of F, Cl, As and Sb.
[0035] Moreover, the present invention granulates the secondary zinc oxide into square-like particles with notches. In the subsequent low-temperature pretreatment and high-temperature roasting process, the water added to the secondary zinc oxide will form the shortest distance channel in the square-like secondary zinc oxide particles with notches when it is heated and volatilized. The channel can be used as a channel for the discharge of impurity elements such as arsenic, antimony, fluorine, and chlorine, which is conducive to the discharge of impurities such as arsenic, antimony, fluorine, and chlorine into smoke with the shortest distance, thereby maximizing the removal rate of impurities such as arsenic, antimony, fluorine, and chlorine, and enabling the high content of fluorine and chlorine that are difficult to remove in the secondary zinc oxide to be quickly removed under environmentally friendly and low-cost conditions.
[0036] Step 2) Pretreatment: The secondary zinc oxide granules are sent to a pretreatment section with a lifting plate in a rotary kiln for low-temperature stirring pretreatment to obtain pretreated secondary zinc oxide materials.
[0037] Among them, during the low-temperature pretreatment of the secondary zinc oxide particles in the rotary kiln, natural gas can be burned as fuel to provide heat for the rotary kiln, or electric heating can be used to provide heat for the rotary kiln.
[0038] In order to reduce production costs, the present invention preferably uses natural gas combustion to provide heat energy for the rotary kiln.
[0039] As a specific implementation of the present invention, in order to ensure the direction and dust collection rate of the flue gas in the dust collection system, and to improve the removal rate of fluorine and chlorine and reduce the volatilization of zinc, the inlet wind pressure of the rotary kiln pretreatment section is controlled at 1800-2000Pa.
[0040] Furthermore, in order to achieve the best effect of low-temperature pretreatment of zinc oxide particles, the treatment temperature of low-temperature pretreatment of zinc oxide particles is controlled at 510-580° C., and the time is 0.3-1.5 h.
[0041] Pretreatment at a relatively low temperature of 510-580°C is beneficial to the volatilization of moisture added to the notched square-shaped zinc oxide particles during granulation. During the escape of the volatilized moisture from the notched square-shaped zinc oxide particles, the shortest channels are formed in the notched square-shaped zinc oxide particles. These channels can be used as channels for the discharge of impurity elements such as arsenic, antimony, fluorine, and chlorine, which is beneficial for the discharge of impurities such as arsenic, antimony, fluorine, and chlorine into the smoke with the shortest distance, thereby maximizing the removal rate of impurities such as arsenic, antimony, fluorine, and chlorine, and enabling the high content of fluorine and chlorine that is difficult to remove in zinc oxide to be quickly removed under environmentally friendly and low-cost conditions.
[0042] In addition, the low-temperature pretreatment can easily activate compounds such as basic zinc fluoride, basic zinc chloride, basic lead fluoride and basic lead chloride in the secondary zinc oxide after the low-temperature pretreatment, which is beneficial to the deep removal of impurity elements such as F and Cl in the subsequent high-temperature roasting process.
[0043] In order to ensure sufficient fluidity of the zinc oxide particles and to ensure that the zinc oxide particles are evenly heated in the rotary kiln, and then to ensure that the channels formed in the zinc oxide particles are unobstructed, and to ensure that the impurity elements F and Cl are fully removed, a copying plate is set in the pretreatment section of the rotary kiln, and the copying plate is evenly welded on the circumference inside the treatment section. When the secondary zinc oxide particles are subjected to low-temperature pretreatment, the rotating copying plate can cause the secondary zinc oxide particles to turn over, so that the secondary zinc oxide particles are heated more evenly, avoiding the consistency problem of the zinc oxide roasted sand obtained after subsequent roasting.
[0044] As a specific embodiment of the present invention, in order to facilitate the sufficient turning of the secondary zinc oxide particles and uniform heating, the number of scissor plates on the inner circumference of the processing section can be set to 8 to 14, each scissor plate having a thickness of 3 to 6 mm, a length of 13 to 18 mm, and a height of 46 to 54 mm.
[0045] The following reactions occur during the low-temperature pretreatment of zinc oxide pellets:
[0046] Basic zinc fluoride → ZnO + ZnF2 + H2O↑
[0047] Basic zinc chloride → ZnO + ZnCl2 + H2O↑
[0048] Basic lead fluoride → PbO + ZnF2 + H2O↑
[0049] Basic lead chloride → PbO + ZnF2 + H2O↑
[0050] Step 3) high temperature roasting: the pre-treated secondary zinc oxide material is sent to the high temperature section of the rotary kiln for high temperature roasting, and then cooled to obtain zinc oxide roasted sand.
[0051] The temperature of the pretreated secondary zinc oxide material in the high temperature section of the rotary kiln is 830-930° C., and the roasting time is 1.8-2.8 hours.
[0052] Among them, the chemical reaction of the pretreated secondary zinc oxide material during high temperature roasting in the high temperature section of the rotary kiln is as follows:
[0053] 2NaF+ZnO→Na2O+ZnF2↑
[0054] 2NaF+PbO→Na2O+PbF2↑
[0055] 2NaCl+ZnO→Na2O+ZnCl2↑
[0056] 2NaCl+PbO→Na2O+PbCl2↑
[0057] ZnF2+PbO→ZnO+PbF2↑
[0058] ZnCl2+PbO→ZnO+PbCl2↑
[0059] When basic zinc fluoride, basic zinc chloride, basic lead fluoride and basic lead chloride in the secondary zinc oxide are activated in the low-temperature pretreatment stage and then roasted at a temperature of 830-930°C for 1.8-2.8h, it is beneficial for impurity elements such as F and Cl to be discharged from the channels of the notched quasi-square secondary zinc oxide particles, so that the impurity elements such as F and Cl are deeply removed, and the removal rates of fluorine and chlorine in the secondary zinc oxide with high fluorine and chlorine contents can exceed 98.5% and 99% respectively, and the contents of F and Cl in the zinc oxide roasted sand obtained after high-temperature roasting are reduced to below 0.08wt% and 0.006wt% respectively, meeting the current large-scale zinc electrolytic plate requirements for impurities As≤0.0002g / L, Sb≤0.0002g / L, Cl≤0.3g / L, and F≤0.03g / L in the zinc liquid, ensuring that the zinc electrolysis in the subsequent zinc hydrometallurgy does not cause plate burning due to the impurity elements F, Cl, As and Sb.
[0060] Among them, the smoke dust containing impurities such as F, Cl, As and Sb is produced when the pretreated secondary zinc oxide material is roasted in the high temperature section of the rotary kiln, and is discharged after being cooled and dust-collected along with the kiln tail gas and meeting the standards.
[0061] Step 4) ball milling: the process of recovering valuable metals from the zinc oxide roasted sand after ball milling.
[0062] Among them, the zinc oxide roasted sand is ball-milled to D90≤63μm and then sent to the zinc hydrometallurgy system to recover valuable metals such as zinc, indium, lead, and cadmium. Ball-milling the zinc oxide roasted sand to a maximum particle size of D90≤63μm can ensure the effective leaching of valuable metals in the subsequent zinc hydrometallurgy system.
[0063] In addition, the medium particle size of the zinc oxide roasted sand after ball milling is ≥380 mesh, so as to ensure the maximum recovery of the subsequent valuable metals such as zinc, indium, lead, cadmium, etc. in the zinc hydrometallurgical system.
[0064] The following is a detailed description of the method for deep impurity removal of zinc oxide provided by the present invention through examples and comparative examples.
[0065] Example 1
[0066] A deep impurity removal test of zinc oxide was carried out using high-fluorine and chlorine zinc oxide with the composition of Zn 61.35wt%, Fe 0.52wt%, Pb 1.46wt%, Cd 0.021wt%, Ca0.16wt%, F 0.53wt%, and Cl 9.78wt%.
[0067] 1. Granulation: Mix 7.2 wt% of water accounting for the weight of zinc oxide and zinc oxide with a medium particle size of 9.25 μm and granulate into a square-shaped zinc oxide material with a notch, with a side length of 10.5 mm and a notch depth of 4 mm;
[0068] 2. Pretreatment: Feed the notched square-shaped secondary zinc oxide material to the pretreatment section of the rotary kiln with a lifting plate, control the temperature to 580°C, the time to 0.3h, natural gas as fuel, and the inlet wind pressure to 1800Pa to obtain the pretreated secondary zinc oxide material;
[0069] 3. High temperature roasting: When the pretreated secondary zinc oxide material is fed to the high temperature section of the rotary kiln, the temperature is controlled at 930°C for 1.8 hours, and after cooling, zinc oxide roasted sand is obtained, in which the Cl and F contents are 0.072wt% and 0.0051wt% respectively;
[0070] 4. Ball milling: The zinc oxide roasted sand is ball milled to D90 = 58μm and then fed to the zinc hydrometallurgical system to recover the valuable metals zinc, indium, lead, cadmium, etc.
[0071] Through deep removal of impurities in high-fluorine and high-chlorine zinc oxide, it is calculated that the zinc recovery rate is 99.1%, and the fluorine and chlorine removal rates are more than 98.8% and 99.2% respectively; the zinc oxide roasted sand is leached and purified by the original process in the wet smelting process to obtain zinc liquid, and the impurity contents in the zinc liquid are As 0.00011g / L, Sb 0.00008g / L, Cl 0.21g / L, and F 0.025g / L, which meets the requirements of large-scale zinc electrolytic plates for zinc liquid.
[0072] Example 2
[0073] A deep impurity removal test of zinc oxide was carried out using high-fluorine and chlorine zinc oxide with the composition of Zn 61.35wt%, Fe 0.52wt%, Pb 1.46wt%, Cd 0.021wt%, Ca0.16wt%, F 0.53wt%, and Cl 9.78wt%.
[0074] 1. Granulation: Mix 5.2 wt% of water accounting for the weight of zinc oxide and zinc oxide with a medium particle size of 7.52 μm and granulate into a square-shaped zinc oxide material with a notch, with a side length of 7.5 mm and a notch depth of 2 mm;
[0075] 2. Pretreatment: Feed the notched square-shaped secondary zinc oxide material to the pretreatment section of the rotary kiln with a lifting plate, control the temperature to 510°C, the time to 1.5h, natural gas as fuel, and the inlet wind pressure to 2000Pa, to obtain the pretreated secondary zinc oxide material;
[0076] 3. High temperature roasting: when the pretreated secondary zinc oxide material is fed to the high temperature section of the rotary kiln, the temperature is controlled at 830°C for 2.8 hours, and after cooling, zinc oxide roasted sand is obtained, and the Cl and F contents in the roasted sand are 0.068wt% and 0.0042wt% respectively;
[0077] 4. Ball milling: The zinc oxide roasted sand is ball milled to D90 = 54μm and then fed to the zinc hydrometallurgical system to recover the valuable metals zinc, indium, lead, cadmium, etc.
[0078] Through deep removal of impurities in high-fluorine and high-chlorine zinc oxide, it is calculated that the zinc recovery rate is 99.21%, and the fluorine and chlorine removal rates are more than 99.1% and 99.3% respectively; zinc oxide roasted sand is leached and purified by the original process in wet smelting to obtain zinc liquid, and the impurity contents in the zinc liquid are As 0.00013g / L, Sb 0.00010g / L, Cl 0.24g / L, and F 0.022g / L, which meets the requirements of large-scale zinc electrolytic plates for zinc liquid.
[0079] Example 3
[0080] A deep impurity removal test of zinc oxide was carried out using high-fluorine and chlorine zinc oxide with the composition of Zn 61.35wt%, Fe 0.52wt%, Pb 1.46wt%, Cd 0.021wt%, Ca0.16wt%, F 0.53wt%, and Cl 9.78wt%.
[0081] 1. Granulation: Mix 6.2 wt% of water accounting for the weight of zinc oxide and zinc oxide with a medium particle size of 5.37 μm and granulate into a square-shaped zinc oxide material with a notch, with a side length of 9.5 mm and a notch depth of 3 mm;
[0082] 2. Pretreatment: Feed the notched square-shaped secondary zinc oxide material to the pretreatment section of the rotary kiln with a lifting plate, control the temperature to 550°C, the time to 1.0h, natural gas as fuel, and the inlet wind pressure to 1900Pa, to obtain the pretreated secondary zinc oxide material;
[0083] 3. High temperature roasting: When the pretreated secondary zinc oxide material is fed to the high temperature section of the rotary kiln, the temperature is controlled at 900°C for 2.2 hours, and after cooling, zinc oxide roasted sand is obtained, in which the Cl and F contents are 0.064wt% and 0.0049wt% respectively;
[0084] 4. Ball milling: The zinc oxide roasted sand is ball milled to D90 = 43μm and then fed to the zinc hydrometallurgical system to recover the valuable metals zinc, indium, lead, cadmium, etc.
[0085] Through deep removal of impurities in high-fluorine and high-chlorine zinc oxide, it is calculated that the zinc recovery rate is 99.16%, and the fluorine and chlorine removal rates are more than 99.2% and 99.1% respectively; zinc oxide roasted sand is leached and purified by the original process in wet smelting to obtain zinc liquid, and the impurity contents in the zinc liquid are As 0.00015g / L, Sb 0.00009g / L, Cl 0.26g / L, and F 0.019g / L, which meets the requirements of large-scale zinc electrolytic plates for zinc liquid.
[0086] Comparative Example 1
[0087] A deep impurity removal test of zinc oxide was carried out using high-fluorine and chlorine zinc oxide with the composition of Zn 61.35wt%, Fe 0.52wt%, Pb 1.46wt%, Cd 0.021wt%, Ca0.16wt%, F 0.53wt%, and Cl 9.78wt%.
[0088] The secondary zinc oxide is granulated into a particle size of 5 mm, and then the weight ratio of the sum of the added water to the raw material secondary zinc oxide is 9:91. The drying time is 2 days, and then the spherical material obtained by granulation is sent to a rotary kiln for roasting at a temperature of 950-1000° C. to remove F and Cl. The F and Cl contents in the roasted sand are 0.05wt% and 0.51wt% respectively, the F and Cl removal rates are 91.70% and 95.39%, and the total zinc recovery rate is 98.51%.
[0089] Compared with Examples 1 to 3 of the present invention, the removal rate of F and Cl and the recovery rate of zinc in Comparative Example 1 are significantly lower than those in Examples 1 to 3 of the present invention. The roasted sand obtained in Comparative Example 1 was ball-milled and then transferred to zinc hydrometallurgy to extract zinc. During the zinc electrolysis process, a large area of scorched plate appeared, the lead content in the precipitated zinc was significantly higher, and chlorine was enriched inside the electrolysis plant, which endangered the health of employees, seriously affected normal production, and significantly increased production costs.
[0090] Comparative Example 2
[0091] A deep impurity removal test of zinc oxide was carried out using high-fluorine and chlorine zinc oxide with the composition of Zn 61.35wt%, Fe 0.52wt%, Pb 1.46wt%, Cd 0.021wt%, Ca0.16wt%, F 0.53wt%, and Cl 9.78wt%.
[0092] The raw material high-fluorine and high-chlorine zinc oxide is fed into a rotary kiln and roasted with natural gas. The zinc oxide is mixed with high-temperature fuel in a mass ratio of 8:1 and roasted at 1120°C for 1.5 hours to obtain a solid residue. The contents of F and Cl in the solid residue are 0.035wt% and 0.18wt%, respectively. The removal rates of F and Cl are 94.19% and 98.38%, and the total recovery rate of zinc is 97.62%.
[0093] Compared with Examples 1 to 3 of the present invention, the removal rate of F and Cl and the recovery rate of zinc in Comparative Example 2 are significantly lower than those in Examples 1 to 3 of the present invention. The calcined sand obtained in Comparative Example 2 was ball-milled and then transferred to zinc hydrometallurgy for zinc extraction. During the zinc electrolysis process, the plate burning phenomenon occurred, and the lead content in the precipitated zinc was high.
[0094] By comparing the embodiments 1-3 of the present invention with the comparative examples 1-2, it can be seen that the method for deep impurity removal of zinc oxide provided by the embodiments of the present invention is to firstly granulate the zinc oxide with water into square-shaped zinc oxide particles with gaps for zinc oxide with fluorine and chlorine contents exceeding 0.45wt% and 8.5wt%, and then perform a two-stage treatment process of low-temperature pretreatment and high-temperature roasting on the square-shaped zinc oxide particles with gaps to perform deep impurity removal, which can maximize the removal rate of harmful impurity elements such as arsenic, antimony, fluorine, and chlorine, and can reduce the content of F and Cl in zinc oxide roasted sand to below 0.08wt% and 0.006wt%, respectively, and make the removal rate of fluorine and chlorine in high-fluorine and chlorine zinc oxide exceed 98.5% and 99%, respectively. Finally, the obtained zinc oxide roasted sand is ball-milled and sent to the zinc hydrometallurgical system to recover valuable metals such as zinc, indium, lead, and cadmium, which can reduce the slag rate of leached slag in the process of zinc oxide roasted sand leaching, improve the leaching rate of zinc, and reduce the production cost.
[0095] Moreover, the method for deep impurity removal of zinc oxide provided by the embodiment of the present invention has the advantages of fewer process flows, high efficiency and high degree of mechanization, and has greatly improved energy saving, environmental protection and economic benefits, which is conducive to large-scale promotion and application.
[0096] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for deep impurity removal of zinc oxide, characterized in that: The steps include: Add water to zinc oxide and mix to form square zinc oxide particles with notches; The secondary zinc oxide granules are sent to the pretreatment section with a lifting plate in the rotary kiln for low-temperature stirring pretreatment to obtain the pretreated secondary zinc oxide material; The pre-treated zinc oxide material is sent to the high temperature section of the rotary kiln for high temperature roasting to obtain zinc oxide roasted sand; The process of recovering valuable metals from zinc oxide roasted sand after ball milling.
2. The method for deep impurity removal of zinc oxide according to claim 1, wherein: The secondary zinc oxide is a secondary zinc oxide with a medium particle size of ≤15 μm, and the mass of water added to the secondary zinc oxide is 5.2-7.2 wt % of the mass of the secondary zinc oxide.
3. The method for deep impurity removal of secondary zinc oxide according to claim 2, wherein: The side length of the notched square-shaped zinc oxide particles is 7.5 to 10.5 mm, and the notch depth is 2 to 4 mm.
4. The method for deep impurity removal of zinc oxide according to claim 1, wherein: During the low-temperature pretreatment of the secondary zinc oxide particles, natural gas is used as fuel for heating or electric heating is used for heating.
5. The method for deep impurity removal of secondary zinc oxide according to claim 4, characterized in that: The treatment temperature of the low-temperature pretreatment of the secondary zinc oxide particles is controlled at 510-580° C., the time is 0.3-1.5 hours, and the inlet wind pressure of the rotary kiln pretreatment section is controlled at 1800-2000 Pa.
6. The method for deep impurity removal of zinc oxide according to claim 5, characterized in that: The copying plates in the rotary kiln pretreatment section are uniformly welded on the inner circumference of the treatment section. There are 8 to 14 copying plates on the inner circumference of the treatment section. Each copying plate has a thickness of 3 to 6 mm, a length of 13 to 18 mm, and a height of 46 to 54 mm.
7. The method for deep impurity removal of zinc oxide according to claim 1, characterized in that: The pretreated secondary zinc oxide material is roasted in the high temperature section of the rotary kiln at a temperature of 830-930° C. for a time of 1.8-2.8 hours.
8. The method for deep impurity removal of zinc oxide according to claim 7, characterized in that: The smoke dust containing impurities of F, Cl, As and Sb generated by the pretreated secondary zinc oxide material being roasted in the high temperature section of the rotary kiln is discharged after being cooled and dust-collected along with the kiln tail smoke and meets the standards.
9. The method for deep impurity removal of zinc oxide according to claim 1, characterized in that: The zinc oxide roasted sand is ball-milled to a D90≤63 μm and then sent to a zinc hydrometallurgical system to recover valuable metals.
10. The method for deep impurity removal of zinc oxide according to claim 9, characterized in that: The zinc oxide roasted sand has a medium particle size of ≥380 meshes after ball milling.