Preparation method of modified soybean fiber, bed core and mattress
By modifying soybean dregs, using the first and second modification additives and bamboo fibers, combined with pH adjustment and cooking technology, the top-breaking strength and elasticity of soybean fibers are significantly improved, and the strength of existing soybean fiber fabrics is solved. The problem of insufficient length extends the service life of the bed core and mattress.
Patent Information
- Application Number
- CN202410923180.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The top breaking strength of existing soybean fiber fabrics is low, resulting in textiles being easily damaged and affecting their service life.
Using soybean dregs as raw materials, the treatment of the first modification additive, bamboo fiber and the second modification additive, combined with specific pH conditions and cooking treatment, significantly improve the top-breaking strength and elasticity of the soybean fiber, and enhance the mechanical properties of the fiber. .
The modified soybean fibers prepared have high top-breaking strength and good elasticity, extend the service life of the bed core and mattress, and significantly improve the mechanical properties of textiles.
Smart Images

Figure BDA0004937295500000061
Abstract
Description
Technical Field
[0001] The invention belongs to the field of textile technology, and particularly relates to a preparation method of modified soybean fiber, a bed core and a mattress. Background Art
[0002] Soybean fiber fabrics have better warmth retention and skin-friendliness than cotton, and are known as "the healthy and comfortable fiber of the new century" and "good fabrics that the skin likes." Therefore, soybean fiber is widely used in the textile field.
[0003] However, the existing soybean fiber fabrics used for clothing or bedding have good skin affinity, but have poor strength. The existing soybean fiber has low bursting strength, which makes soybean fiber textiles prone to damage and other problems.
[0004] Therefore, there is an urgent need to provide a new modified soybean fiber with high bursting strength, which is beneficial to the application of soybean fiber in the textile field. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a preparation method of modified soybean fiber, a bed core, and a mattress. The modified soybean fiber prepared by the preparation method of the present invention has high bursting strength and good elasticity. The modified soybean fiber is applied to the textile field, such as bed cores and mattresses, which is conducive to improving the service life of the bed core and mattress.
[0006] The present invention uses soybean residue as raw material, and after a first modification aid and bamboo fiber, a second modification aid, and a specific pH condition treatment and a steaming treatment, the soybean residue of the present invention has high bursting strength and elasticity. Among them, through the treatment of the second modification aid, the compatibility of bamboo fiber and soybean fiber can be significantly improved, so that the modified soybean fiber finally obtained has good mechanical properties. When the first modification aid is added, the soybean residue is steamed, so that the protein in the soybean residue is separated from the fiber, and the strength of the separated fiber is strengthened and the fiber surface groups are activated. When the second modification aid and bamboo fiber are added, the performance of the bamboo fiber is better integrated, so that the modified soybean fiber finally obtained has good mechanical properties.
[0007] A first aspect of the present invention provides a method for preparing modified soybean fiber.
[0008] Specifically, a method for preparing modified soybean fiber comprises the following steps:
[0009] Mixing soybean residue, water and the first modification aid, adjusting the pH to 10.5-11.5 for the first time, steaming, cooling after the steaming, adding bamboo fiber and the second modification aid, stirring, centrifuging to obtain a precipitate, dissolving the precipitate in water, adjusting the pH to 6.5-7.5 for the second time, centrifuging, and drying the obtained precipitate to obtain the modified soybean fiber;
[0010] The first modification aid includes sodium alginate, potassium carbonate, and a silane coupling agent;
[0011] The second modification aid includes sodium alginate, sodium dodecyl sulfate and potassium acetate.
[0012] Preferably, the mesh size of the soybean residue is 150-250 mesh, and more preferably 180-200 mesh.
[0013] Preferably, the first modifying aid, by weight, comprises 5-20 parts of sodium alginate, 1-3 parts of potassium carbonate, and 3-10 parts of silane coupling agent; further preferably, the first modifying aid, by weight, comprises 6-15 parts of sodium alginate, 1-2 parts of potassium carbonate, and 3-8 parts of silane coupling agent.
[0014] Preferably, the second modifying aid, calculated by weight, includes 4-15 parts of sodium alginate, 2-10 parts of sodium dodecyl sulfate, and 1-7 parts of potassium acetate; further preferably, the second modifying aid, calculated by weight, includes 4-12 parts of sodium alginate, 2-8 parts of sodium dodecyl sulfate, and 1-5 parts of potassium acetate.
[0015] Preferably, the silane coupling agent includes silane coupling agent KH560 or silane coupling agent KH570.
[0016] Preferably, the cooking temperature is 100-115°C, more preferably 110-115°C.
[0017] Preferably, the cooking time is 30-55 minutes, more preferably 45-50 minutes.
[0018] Preferably, the cooling refers to cooling to 40-60°C, more preferably 50-55°C.
[0019] Preferably, the rotation speed during centrifugation is 4000-8000 rpm, more preferably 5000-8000 rpm.
[0020] Preferably, the centrifugation time is 10-20 minutes, more preferably 15-20 minutes.
[0021] Preferably, the drying is spray drying.
[0022] Preferably, the pH is adjusted using sodium hydroxide solution or hydrochloric acid, for example, a sodium hydroxide solution or hydrochloric acid with a concentration of 0.5-1.5 mol / L is used to adjust the pH.
[0023] Preferably, the weight ratio of the soybean residue, water and the first modification aid is 100:(5-40):(0.5-5); further preferably, the weight ratio of the soybean residue, water and the first modification aid is 100:(5-30):(0.5-3).
[0024] Preferably, the weight ratio of the soybean residue to the bamboo fiber and the second modifying agent is 100:(1-5):(0.5-2); further preferably, the weight ratio of the soybean residue to the bamboo fiber and the second modifying agent is 100:(1-3):(0.5-1.5).
[0025] A second aspect of the present invention provides a modified soybean fiber.
[0026] A modified soybean fiber is prepared by the above preparation method.
[0027] The third aspect of the present invention provides an application of modified soybean fiber.
[0028] A fabric is obtained by spinning the modified soybean fiber to obtain warp yarn and weft yarn, and the warp yarn and weft yarn are woven to obtain the fabric.
[0029] A bed core comprises the modified soybean fiber.
[0030] A mattress comprises the modified soybean fiber.
[0031] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0032] The present invention uses soybean residue as raw material, and undergoes a first modification aid, bamboo fiber, a second modification aid, and a specific pH condition treatment and a steaming treatment, so that the soybean residue of the present invention has high bursting strength and elasticity. Among them, the treatment with the second modification aid can significantly improve the compatibility of bamboo fiber and soybean fiber, so that the modified soybean fiber finally obtained has good mechanical properties. DETAILED DESCRIPTION
[0033] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.
[0034] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.
[0035] Example 1
[0036] A method for preparing modified soybean fiber comprises the following steps:
[0037] The soybean residue, water and the first modification aid are mixed, the pH value is adjusted to 11 for the first time with 1 mol / L sodium hydroxide solution, and the mixture is steamed (autoclaved) at 110°C for 40 minutes. After the steaming is completed, the mixture is cooled to 50°C, bamboo fiber (the length of the bamboo fiber is 12±2 mm) and the second modification aid are added, and the mixture is stirred for 30 minutes, and then centrifuged (the speed during the centrifugation is 5000 rpm and the centrifugation time is 15 minutes) to obtain a precipitate, which is dissolved in water, the pH value is adjusted to 6.5 for the second time with 0.5 mol / L hydrochloric acid, and the mixture is centrifuged (the speed during the centrifugation is 4000 rpm and the centrifugation time is 15 minutes), and the obtained precipitate is spray-dried to obtain modified soybean fiber;
[0038] The first modification aid is composed of the following components by weight: 6 parts of sodium alginate, 2.5 parts of potassium carbonate, and 5 parts of silane coupling agent KH560;
[0039] The second modification aid is composed of the following components by weight: 5 parts of sodium alginate, 4 parts of sodium dodecyl sulfate, and 1.5 parts of potassium acetate;
[0040] The weight ratio of soybean residue, water and the first modifying aid is 100:40:2.
[0041] The weight ratio of soybean residue, bamboo fiber and the second modification auxiliary agent is 100:1.5:1.
[0042] Example 2
[0043] A method for preparing modified soybean fiber comprises the following steps:
[0044] The soybean residue, water and the first modification aid are mixed, the pH value is adjusted to 10.5 for the first time with 1 mol / L sodium hydroxide solution, and the mixture is steamed (autoclaved) at 105°C for 45 minutes. After the steaming is completed, the mixture is cooled to 55°C, bamboo fiber (the length of the bamboo fiber is 12±2 mm) and the second modification aid are added, and the mixture is stirred for 30 minutes, and then centrifuged (the speed during the centrifugation is 4000 rpm and the centrifugation time is 15 minutes) to obtain a precipitate, which is dissolved in water, the pH value is adjusted to 7.0 for the second time with 0.5 mol / L hydrochloric acid, and the mixture is centrifuged (the speed during the centrifugation is 4000 rpm and the centrifugation time is 15 minutes), and the obtained precipitate is spray-dried to obtain modified soybean fiber;
[0045] The first modification aid is composed of the following components by weight: 6.5 parts of sodium alginate, 2.2 parts of potassium carbonate, and 4.5 parts of silane coupling agent KH560;
[0046] The second modification aid is composed of the following components by weight: 5.5 parts of sodium alginate, 4.2 parts of sodium dodecyl sulfate, and 1.8 parts of potassium acetate;
[0047] The weight ratio of soybean residue, water and the first modifying agent is 100:38:2.1.
[0048] The weight ratio of soybean residue, bamboo fiber and the second modification auxiliary agent is 100:1.3:1.1.
[0049] Example 3
[0050] A method for preparing modified soybean fiber comprises the following steps:
[0051] The soybean residue, water and the first modification aid are mixed, the pH value is adjusted to 11 for the first time with 1 mol / L sodium hydroxide solution, and the mixture is steamed (autoclaved) at 110°C for 40 minutes. After the steaming is completed, the mixture is cooled to 60°C, bamboo fiber (the length of the bamboo fiber is 12±2 mm) and the second modification aid are added, and the mixture is stirred for 30 minutes, and then centrifuged (the speed during the centrifugation is 5000 rpm and the centrifugation time is 15 minutes) to obtain a precipitate, which is dissolved in water, the pH value is adjusted to 7.0 for the second time with 0.5 mol / L hydrochloric acid, and the mixture is centrifuged (the speed during the centrifugation is 4000 rpm and the centrifugation time is 15 minutes), and the obtained precipitate is spray-dried to obtain modified soybean fiber;
[0052] The first modification aid is composed of the following components by weight: 7 parts of sodium alginate, 2.8 parts of potassium carbonate, and 4.8 parts of silane coupling agent KH570;
[0053] The second modification aid is composed of the following components by weight: 6.1 parts of sodium alginate, 4.4 parts of sodium dodecyl sulfate, and 1.7 parts of potassium acetate;
[0054] The weight ratio of soybean residue, water and the first modifying agent is 100:35:1.7.
[0055] The weight ratio of soybean residue, bamboo fiber and the second modification auxiliary agent is 100:1.2:1.4.
[0056] Comparative Example 1
[0057] Compared with Example 1, the difference of Comparative Example 1 is that an equal amount of sodium alginate is used instead of potassium carbonate in Comparative Example 1, and the rest of the process is the same as that of Example 1.
[0058] Comparative Example 2
[0059] Compared with Example 1, the difference of Comparative Example 2 is that the silane coupling agent KH560 is replaced by an equal amount of sodium alginate in Comparative Example 2, and the rest of the process is the same as that of Example 1.
[0060] Comparative Example 3
[0061] Compared with Example 1, the difference of Comparative Example 3 is that the sodium alginate is used in Comparative Example 3 instead of sodium dodecyl sulfate and potassium acetate in equal amounts, and the rest of the process is the same as that of Example 1.
[0062] Comparative Example 4
[0063] Compared with Example 1, the difference of Comparative Example 4 is that the pH is adjusted to 8.5 for the first time and to 6.0 for the second time, and the rest of the process is the same as that of Example 1.
[0064] Application Example 1
[0065] The modified soybean fiber prepared in the above Example 1 is spun to obtain warp yarn and weft yarn, and the warp yarn and weft yarn are woven (this process is a conventional process in the field) to obtain a fabric, the imperial count of the warp yarn is 40s, and the imperial count of the weft yarn is 35s; the density of the fabric is 155 warp yarns and 105 weft yarns per square inch.
[0066] Application Example 2
[0067] The modified soybean fiber prepared in the above Example 2 is spun to obtain warp yarn and weft yarn, and the warp yarn and weft yarn are woven (this process is a conventional process in the field) to obtain a fabric, the imperial count of the warp yarn is 40s, and the imperial count of the weft yarn is 35s; the density of the fabric is 155 warp yarns and 105 weft yarns per square inch.
[0068] Application Example 3
[0069] The modified soybean fiber prepared in the above Example 3 is spun to obtain warp yarn and weft yarn, and the warp yarn and weft yarn are woven (this process is a conventional process in the field) to obtain a fabric, the imperial count of the warp yarn is 40s, and the imperial count of the weft yarn is 35s; the density of the fabric is 155 warp yarns and 105 weft yarns per square inch.
[0070] Comparative Application Examples 1-4
[0071] Compared with Application Example 1, the comparative application examples respectively use the modified soybean fibers of Comparative Examples 1-4 to replace the modified soybean fibers of Example 1, and the remaining processes are the same as those of Application Example 1 to obtain the fabrics corresponding to Comparative Application Examples 1-4.
[0072] Product effect testing
[0073] The bursting strength of the fabrics corresponding to the above application examples 1-2 and comparative application examples 1-4 was tested. The bursting strength was tested with reference to the standard GB / T19976-2005. The results are shown in Table 1.
[0074] Table 1
[0075]
[0076] It can be seen from Table 1 that the bursting strength of the fabric corresponding to the modified soybean fiber prepared in Examples 1-2 is significantly higher than that of Comparative Examples 1-3. It can be seen that the first modification aid and the second modification aid have a greater impact on the performance of the modified soybean fiber, and the two pH adjustments also have a certain impact on the performance of the modified soybean fiber.
[0077] Take the fabric prepared in Application Example 1 and stretch it in the warp direction of the fabric. The length of each stretch is 1.1 times the original length of the fabric in the warp direction. After the fabric corresponding to Application Example 1 is stretched 2000 times, the change rate of the original length of the fabric in the warp direction only increases by 1%. When the fabric of Application Example 1 is stretched according to this method, after 2000 times, the change rate of the original length of the fabric in the warp direction increases by 8%.
[0078] It can be seen that the modified soybean fiber prepared in the embodiment of the present invention has good elasticity.
[0079] A bed core includes the modified soybean fiber of Example 1.
[0080] A mattress comprises the modified soybean fiber of Example 1.
Claims
1. A method for preparing modified soybean fiber, characterized in that: The following steps are involved: Mixing soybean residue, water and a first modification aid, adjusting the pH to alkaline 10.5-11.5 for the first time, steaming, cooling after the steaming, adding bamboo fiber and a second modification aid, stirring, centrifuging to obtain a precipitate, dissolving the precipitate in water, adjusting the pH to 6.5-7.5 for the second time, centrifuging, and drying the obtained precipitate to obtain the modified soybean fiber; The first modification aid includes sodium alginate, potassium carbonate, and a silane coupling agent; The second modification aid includes sodium alginate, sodium dodecyl sulfate and potassium acetate.
2. The method for preparing modified soybean fiber according to claim 1, characterized in that: The mesh number of the soybean residue is 150-250 meshes.
3. The method for preparing modified soybean fiber according to claim 1, characterized in that: The first modification auxiliary agent includes, by weight, 5-20 parts of sodium alginate, 1-3 parts of potassium carbonate, and 3-10 parts of silane coupling agent.
4. The method for preparing modified soybean fiber according to claim 1, characterized in that: The second modification aid comprises, by weight, 4-15 parts of sodium alginate, 2-10 parts of sodium dodecyl sulfate, and 1-7 parts of potassium acetate.
5. The method for preparing modified soybean fiber according to claim 1, characterized in that: The cooking temperature is 100-115°C.
6. The method for preparing modified soybean fiber according to claim 1, characterized in that: The weight ratio of the soybean residue, water and the first modification aid is 100:(5-40):(0.5-5).
7. The method for preparing modified soybean fiber according to claim 1, characterized in that: The weight ratio of the soybean residue to the bamboo fiber and the second modification auxiliary agent is 100:(1-5):(0.5-2).
8. A modified soybean fiber, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 7.
9. A bed core, characterized in that: The modified soybean fiber according to claim 8 is included.
10. A mattress, characterized in that: The modified soybean fiber according to claim 8 is included.