Etching method of semiconductor structure

By combining dry etching with electrolytic UV light using a mixed gas of HBr and Ar, the damage problem of low dielectric constant materials during the etching process was solved, the reliability and mechanical properties of semiconductor structures were improved, the dielectric constant K value was reduced, and the morphology of the dielectric layer was improved.

CN118919408APending Publication Date: 2024-11-08GTA SEMICON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411008675.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the semiconductor manufacturing process, materials with low dielectric constants are damaged during etching, affecting the reliability and mechanical properties of the semiconductor structure.

Method used

A dry etching method is adopted, which combines electrolysis of HBr and Ar mixed gas with UV light excitation to release the pore-forming agent in the dielectric layer, so that Si, O and C bonds are rebonded, reducing damage during the etching process. Furthermore, impurities from the dry etching process are removed by cleaning, and etching parameters are optimized to protect the dielectric layer.

Benefits of technology

It effectively reduces the damage to low dielectric constant materials, improves the reliability and mechanical properties of semiconductor structures, reduces the dielectric constant K value, and improves the morphology of the dielectric layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919408A_ABST
    Figure CN118919408A_ABST
Patent Text Reader

Abstract

The invention provides an etching method of a semiconductor structure, and belongs to the field of semiconductors, and the method specifically comprises the steps: S1, removing a hard mask layer on the surface of a target etching region of a substrate to be etched through dry etching; s2, performing dry etching on the dielectric layer at the target etching area according to preset parameters to form an etching pattern; s3, performing dry etching on the photoresist layer; s4, after mixed gas electrolysis, UV light is excited to release the pore-foaming agent in the dielectric layer, so that the Si bond, the O bond and the C bond in the dielectric layer are bonded again; s5, performing dry etching on the exposed etching stop layer until the substrate layer is exposed; and S6, cleaning and removing impurities on the inner wall of the hole under the dry etching process to obtain the semiconductor structure. According to the processing scheme, damage to the low-dielectric-constant material in the etching process is reduced, the product reliability is improved, and the mechanical performance of the material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of semiconductors, and in particular to an etching method for a semiconductor structure. Background Art

[0002] In the semiconductor manufacturing process, as the critical dimensions of the back-end metal wiring process gradually decrease, the spacing between metal trenches also gradually decreases. During the use of semiconductor devices, parasitic capacitance will form between metal trenches, affecting the service life of the device. In order to reduce parasitic capacitance, the dielectric layer material between the semiconductor back-end uses a low dielectric constant (Low-k) dielectric.

[0003] In the process of semiconductor etching, after the pattern formed by photolithography is transferred, the photoresist needs to be removed by ashing. In the process of removing the photoresist, the low dielectric constant material will also be damaged, resulting in damage to the sidewalls of the through holes formed in the semiconductor structure. Figure 1 As shown, the shaded area is a through hole formed in the semiconductor structure. There are multiple steps in the shaded area. These steps are the damage formed, and these damages will affect the reliability of the semiconductor structure.

[0004] Therefore, a method to reduce the damage of low dielectric constant materials is urgently needed. Summary of the invention

[0005] Therefore, in order to overcome the above-mentioned shortcomings of the prior art, the present invention provides a method for etching a semiconductor structure, which can reduce the damage to the low dielectric constant material during the etching process, improve product reliability, and improve the mechanical properties of the material.

[0006] In order to achieve the above-mentioned purpose, the present invention provides an etching method for a semiconductor structure, comprising: S1, dry etching to remove a hard mask layer on the surface of a target etching area of ​​a substrate to be etched, wherein the substrate to be etched comprises at least a substrate layer, an etching stop layer, a dielectric layer, a hard mask layer and a photoresist layer from bottom to top, and the dielectric layer has a porogen; S2, dry etching the dielectric layer at the target etching area according to predetermined parameters to form an etching pattern; S3, dry etching the photoresist layer; S4, releasing the porogen in the dielectric layer by exciting UV light after mixed gas electrolysis to allow Si bonds, O bonds, and C bonds in the dielectric layer to re-bond, thereby reducing problems such as a high K value caused during the etching process; S5, dry etching the exposed etching stop layer until the substrate layer is exposed; S6, cleaning and removing impurities on the inner wall of the opening under the dry etching process to obtain a semiconductor structure.

[0007] In one embodiment, in S4, the mixed gas is a mixed gas of HBr and Ar.

[0008] In one of the embodiments, in S4, the content of HBr in the mixed gas is 5% to 30%, the content of Ar in the mixed gas is 70% to 95%, and the flow rate of the mixed gas is 200 sccm to 600 sccm.

[0009] In one embodiment, S1 dry etching, S2 dry etching, S3 dry etching, and S5 dry etching are reactive ion etching or plasma etching processes.

[0010] In one of the embodiments, during the S1 dry etching process, the gas flow ratio is CHF3:CF4:O2=0~100:200~300:0~20;

[0011] During the S2 dry etching process, the gas flow ratio is Ar:CF4:O2=600-900:200-300:0-20;

[0012] During the S3 dry etching process, the gas flow ratio is CO2:O2=200-500:200-500;

[0013] During the S5 dry etching process, the gas flow ratio is Ar:CF4:N2:O2=200-1000:20-120:0-300:0-30.

[0014] In one embodiment, the parameters of the dry etching include: the etching gas is CF4, CHF3, NF3, CH2F2 or C4F8, the dilution gas is N2, O2, CO, He or Ar, the gas flow rate of the etching gas is 10sccm to 200sccm, the gas flow rate of the dilution gas is 10sccm to 200sccm`, and the chamber pressure is 30mTorr to 200mTorr.

[0015] In one of the embodiments, in S6, during the process of treating the inner wall of the opening with at least one of nitrogen, hydrogen, oxygen, carbon monoxide and carbon dioxide, the gas flow rate is 300 sccm to 500 sccm, and the treatment time is 12s to 60s.

[0016] In one embodiment, the substrate to be etched has an oxide layer, the oxide layer is arranged between the dielectric layer and the etching stop layer, and there is S7 between S4 and S5, and the oxide layer is dry-etched.

[0017] In one embodiment, S7, the gas flow rate of the etching gas is 10 sccm to 200 sccm, the gas flow rate of the dilution gas is 10 sccm to 200 sccm, and the chamber pressure is 30 mTorr to 200 mTorr.

[0018] Compared with the prior art, the advantages of the present invention are: through process optimization, ultraviolet light is used to remove the porogen in the dielectric layer during the electrolysis process, and HBr and AR gases are used to rebond the Si-bonds, O-bonds, and C-bonds in the material, which not only reduces the degree of damage to the low dielectric constant material in the dielectric layer caused by oxygen-containing gases such as O2, CO2, CO, etc. used in the degumming process in the plasma state, thereby improving product reliability and improving the mechanical properties of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0020] Figure 1 It is a schematic diagram of a scanning electron microscope showing damage formed in a low dielectric layer after semiconductor etching in the prior art;

[0021] Figure 2 is a schematic flow chart of a method for etching a semiconductor structure in an embodiment of the present invention;

[0022] Figure 3 is a schematic diagram of the principle of the etching method of the semiconductor structure in an embodiment of the present invention;

[0023] Figure 4 Schematic diagram of a semiconductor structure obtained by scanning electron microscope in an embodiment of the present invention. DETAILED DESCRIPTION

[0024] The embodiments of the present application are described in detail below with reference to the accompanying drawings.

[0025] The following describes the implementation methods of the present application through specific examples, and those skilled in the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. The present application can also be implemented or applied through other different specific implementation methods, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present application. It should be noted that, in the absence of conflict, the following embodiments and the features in the embodiments can be combined with each other. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present application.

[0026] It should be noted that various aspects of the embodiments within the scope of protection of the present invention are described below. It should be apparent that the aspects described herein can be embodied in a wide variety of forms, and any specific structure and / or function described herein is merely illustrative. Based on the present application, it should be understood by those skilled in the art that an aspect described herein can be implemented independently of any other aspect, and two or more of these aspects can be combined in various ways. For example, any number and aspect described herein can be used to implement the device and / or practice the method. In addition, other structures and / or functionalities other than one or more of the aspects described herein can be used to implement this device and / or practice this method.

[0027] It should also be noted that the illustrations provided in the following embodiments are only schematic illustrations of the basic concept of the present application. The drawings only show components related to the present application rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0028] Additionally, in the following description, specific details are provided to facilitate a thorough understanding of the examples. However, it will be understood by those skilled in the art that the aspects described may be practiced without these specific details.

[0029] like Figure 1 As shown, an embodiment of the present application provides a method for etching a semiconductor structure, comprising the following steps:

[0030] S1, dry etching to remove the hard mask layer on the surface of the target etching area of ​​the substrate to be etched, the substrate to be etched includes at least a substrate layer, an etching stop layer, a dielectric layer, a hard mask layer and a photoresist layer from bottom to top, and the dielectric layer has a porogen.

[0031] The substrate to be etched is formed with an etch stop layer on the substrate; a dielectric layer is formed on the etch stop layer; a hard mask layer is formed on the dielectric layer; the dielectric layer is subsequently etched using the hard mask layer as a mask to form an initial opening, and then the hard mask layer is removed; after removing the hard mask layer, the etch stop layer exposed by the initial opening is removed.

[0032] The substrate may be single crystal silicon, silicon, silicon germanium or other semiconductor materials.

[0033] The etch stop layer is used to stop the etching when etching the dielectric layer to form the initial opening. The thickness of the etch stop layer is 200 to The etch stop layer may be one layer or more than two layers. The etch stop layer of the substrate and the etch stop layer closest to the substrate may be of different materials. The substrate and the etch stop layer spaced apart may be of the same material or different materials. In a multi-layer etch stop layer, the two etch stop layers spaced apart may be of the same material or different materials. For example, when the etch stop layer is two layers, the stop layer at the lower layer is silicon dioxide, and the stop layer at the upper layer is polysilicon. The material of the etch stop layer is SiCN, SiCO or SiO2.

[0034] The dielectric layer is used to insulate the interconnect structures formed subsequently. The material of the dielectric layer can have a porous structure, and the material with a porous structure is a low-k dielectric material (a low-k dielectric material refers to a dielectric material with a relative dielectric constant greater than or equal to 2.6 and less than or equal to 3.9) or an ultra-low-k dielectric material (an ultra-low-k dielectric material refers to a dielectric material with a relative dielectric constant less than 2.6), thereby effectively reducing the parasitic capacitance between the interconnect structures formed, thereby reducing the back end of line (BEOL) RC delay.

[0035] The material of the dielectric layer can be SiOH, SiOCH, FSG (fluorine-doped silicon dioxide), BSG (boron-doped silicon dioxide), PSG (phosphorus-doped silicon dioxide), BPSG (boron-phosphorus-doped silicon dioxide), hydrogenated silsesquioxane (HSQ, (HSiO 1.5 ) n ) or methylsilsesquioxane (MSQ, (CH3SiO 1.5 ) n For example, the material of the dielectric layer may be an ultra-low-k dielectric material, the ultra-low-k dielectric material may be SiOCH, and the process for forming the dielectric layer may be a chemical vapor deposition process (Chemical Vapor Deposition, CVD for short) or a physical vapor deposition process.

[0036] The thickness of the dielectric layer is 1000 to

[0037] The hard mask layer is used to act as a mask during the etching process. Etching with the hard mask layer as a mask can better control the graphic morphology of the opening and make the formed opening morphology smoother. The material of the hard mask layer can be TEOS (tetraethyl silicate), TiN, Ti or CuN. The thickness of the hard mask layer is 100 to The process of forming the hard mask may be a physical vapor deposition process or a chemical vapor deposition process.

[0038] S2, dry etching the dielectric layer at the target etching area according to predetermined parameters to form an etching pattern.

[0039] The predetermined parameters may include an etching depth, an etching width, etc. of the dielectric layer at the target etching area.

[0040] The dielectric layer at the target etching area is dry-etched according to predetermined parameters to form an etching pattern. During the dry etching process, the change of light intensity is constantly detected, and the etching is terminated when a certain light intensity rises or falls significantly, thereby marking the completion of etching of a certain layer.

[0041] S3, dry etching the photoresist layer.

[0042] S4, through the electrolysis of mixed gas and then stimulating UV light to release the porogen in the dielectric layer, so that the Si bonds, O bonds, and C bonds in the dielectric layer can be re-bonded; so as to reduce the problems such as the increase of K value caused by the etching process.

[0043] The mixed gas is selected from gases that can excite UV light after electrolysis. In one embodiment, the mixed gas can be HBr and AR gas.

[0044] like Figure 3 As shown, ultraviolet light (UV) is released during the electrolysis of HBr and AR gases. The ultraviolet light (UV) releases the porogen in the dielectric layer, allowing the Si-bonds, O-bonds, and C-bonds in the material to re-bond, eliminating the impurity bonds in the ring structure in the dielectric layer (Lowk material), forming a porous structure, and changing the Si-O-Si bond from a cage-like shape to a mesh-like shape (only part of the mesh connection is shown in the equation), thereby reducing the K value.

[0045] This method can reduce the damage of oxygen-containing gases such as O2, CO2, CO, etc. used in the debonding process to the low dielectric constant material in the dielectric layer in the plasma state. The reaction mechanism of the damage here is:

[0046] Si-OH+O * →Si-O+H2O↑

[0047] Si-CH3+O * →Si-O+CO↑+H2O↑.

[0048] S5, dry etching the exposed etching stop layer until the substrate layer is exposed.

[0049] S6, cleaning and removing impurities from the inner wall of the opening during the dry etching process to obtain a semiconductor structure.

[0050] The dry etching procedure is set, S1 is the first dry etching, S2 is the second dry etching (also called main etching), S4 is the third dry etching, and S5 is the fourth dry etching. In addition, in the etching steps of S1 to S6, there is a stabilization process between each two adjacent steps, and each stabilization process time can be 2 to 8 seconds. In some embodiments, each stabilization process time is about 4 seconds.

[0051] In one embodiment, the parameters of the dry etching process include: the etching gas is CF4, CHF3, NF3, CH2F2 or C4F8, the dilution gas is N2, O2, CO, He or Ar, the gas flow rate of the etching gas is 10sccm to 400sccm, the gas flow rate of the dilution gas is 100ccm to 800sccm, and the chamber pressure is 30mTorr to 200mTorr.

[0052] The above method, through process optimization, uses ultraviolet light irradiation to remove the porogen in the dielectric layer during the electrolysis process, and uses HBr and AR gases to rebond the Si-bonds, O-bonds, and C-bonds in the material. This not only reduces the degree of damage to the low dielectric constant material in the dielectric layer caused by oxygen-containing gases such as O2, CO2, CO, etc. used in the degumming process in the plasma state, thereby improving product reliability, but also improving the mechanical properties of the material.

[0053] In one of the embodiments, in S4, the content of HBr in the mixed gas is 5% to 30%, the content of Ar in the mixed gas is 70% to 95%, and the flow rate of the mixed gas is 200 sccm to 600 sccm.

[0054] In one embodiment, S1 dry etching, S2 dry etching, S3 dry etching, and S5 dry etching are reactive ion etching or plasma etching processes.

[0055] In one of the embodiments, during the S1 dry etching process, the flow ratio of the gas is CHF3:CF4:O2=0~100:200~300:0~20;

[0056] During the S2 dry etching process, the gas flow ratio is Ar:CF4:O2=600-900:200-300:0-20;

[0057] In the S3 dry etching process, the gas flow ratio is CO2:O2=200-500:200-500;

[0058] During the S5 dry etching process, the gas flow ratio is Ar:CF4:N2:O2=200-1000:20-120:0-300:0-30.

[0059] In one of the embodiments, in S6, during the process of treating the inner wall of the opening with at least one of nitrogen, hydrogen, oxygen, carbon monoxide and carbon dioxide, the gas flow rate is 300 sccm to 500 sccm, and the treatment time is 12s to 60s.

[0060] In one embodiment, the substrate to be etched has an oxide layer, and the oxide layer is disposed between the dielectric layer and the hard mask layer.

[0061] There is S7 between S4 and S5 for dry etching the oxide layer.

[0062] In one embodiment, the substrate to be etched may further have an oxide layer, and the oxide layer is disposed between the dielectric layer and the etch stop layer.

[0063] The oxide layer serves as an etching buffer layer for etching the dielectric layer. Since the dielectric layer is a low-k dielectric material or an ultra-low-k dielectric material, it is soft and prone to over-etching, while the oxide layer has better density and hardness. Therefore, by forming an oxide layer on the etch stop layer, the thickness of the etched dielectric layer can be better controlled in the subsequent etching process. In this embodiment, the material of the oxide layer is silicon oxide, and the process for forming the oxide layer is a chemical vapor deposition process.

[0064] The dry etching in S7 may be a reactive ion etching or a plasma etching process. In the dry etching process in S7, the flow ratio of the gas is Ar:CF4:O2=600:80:15:5.

[0065] The parameters of the dry etching process include: a gas flow rate of the etching gas is 10 sccm to 200 sccm, a gas flow rate of the dilution gas is 10 sccm to 200 sccm, and a chamber pressure is 30 mTorr to 200 mTorr.

[0066] Example 1

[0067] S1, dry etching to remove the hard mask layer on the surface of the target etching area of ​​the substrate to be etched, the substrate to be etched includes at least a substrate layer, an etching stop layer, a dielectric layer, a hard mask layer and a photoresist layer from bottom to top, and the dielectric layer has a porogen.

[0068] Substrate silicon dioxide.

[0069] The thickness of the etch stop layer is The material of the etch stop layer is SiCN.

[0070] The material of the dielectric layer is SiCOH. The thickness of the dielectric layer is

[0071] The material of the hard mask is TEOS. The thickness of the hard mask layer is

[0072] The photoresist model is ARF, and the film thickness is

[0073] S2, dry etching the dielectric layer at the target etching area according to predetermined parameters to form an etching pattern.

[0074] S3, dry etching the photoresist layer.

[0075] S4, after electrolysis of a mixed gas of HBr and Ar, UV light is stimulated to release the porogen in the Low-k material to allow the Si bonds, O bonds, and C bonds in the dielectric layer to rebond.

[0076] S5, dry etching the exposed etching stop layer until the substrate layer is exposed.

[0077] S6, cleaning and removing impurities from the inner wall of the opening under the dry etching process to obtain a semiconductor structure. In the S1 dry etching process, the flow ratio of the gas is CHF3:CF4:O2=60:240:10;

[0078] During the S2 dry etching process, the gas flow ratio is Ar:C4F8:O2=900:200:8;

[0079] During the S3 dry etching process, the gas flow ratio is CO:O2=300:300;

[0080] During the S5 dry etching process, the gas flow ratio is Ar:CF4:N2:O2=600:80:15:5.

[0081] In S6, during the process of treating the inner wall of the opening, the flow rate of hydrogen and nitrogen is 400 / 100 ccm, and the treatment time is 12 s.

[0082] According to the above process parameters, Figure 4 The semiconductor structure shown in this SEM schematic and Figure 1 By comparing the dielectric layer morphology with the dielectric layer etched, we can see that the dielectric layer morphology changes from rough to smooth after etching, and the edge roughness is reduced by at least 50%. Figure 1 3.7 down to Figure 4 2.8.

[0083] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed in the present application should be included in the protection scope of the present application.

Claims

1. A method for etching a semiconductor structure, characterized in that: include: S1, dry etching to remove the hard mask layer on the surface of the target etching area of ​​the substrate to be etched, wherein the substrate to be etched comprises at least a substrate layer, an etching stop layer, a dielectric layer, a hard mask layer and a photoresist layer from bottom to top, and the dielectric layer has a porogen; S2, dry etching the dielectric layer at the target etching area according to predetermined parameters to form an etching pattern; S3, dry etching the photoresist layer; S4, after electrolysis of the mixed gas, UV light is stimulated to release the porogen in the dielectric layer, so that the Si bonds, O bonds, and C bonds in the dielectric layer are rebonded; S5, dry-etching the exposed etching stop layer until the substrate layer is exposed; S6, cleaning and removing impurities from the inner wall of the opening during the dry etching process to obtain a semiconductor structure.

2. The etching method according to claim 1, characterized in that: In S4, the mixed gas is a mixed gas of HBr and Ar.

3. The etching method according to claim 2, characterized in that: In S4, the content of HBr in the mixed gas is 5% to 30%, the content of Ar in the mixed gas is 70% to 95%, and the flow rate of the mixed gas is 200 sccm to 600 sccm.

4. The etching method according to claim 1, characterized in that: S1 dry etching, S2 dry etching, S3 dry etching, and S5 dry etching are reactive ion etching or plasma etching processes.

5. The etching method according to claim 1, characterized in that: During the S1 dry etching process, the gas flow ratio is CHF3:CF4:O2=0-100:200-300:0-20; During the S2 dry etching process, the gas flow ratio is Ar:CF4:O2=600-900:200-300:0-20; During the S3 dry etching process, the gas flow ratio is CO2:O2=200-500:200-500; During the S5 dry etching process, the gas flow ratio is Ar:CF4:N2:O2=200-1000:20-120:0-300:0-30.

6. The etching method according to claim 1, characterized in that: The parameters of the dry etching include: the etching gas is CF4, CHF3, NF3, CH2F2 or C4F8, the dilution gas is He or Ar, the gas flow rate of the etching gas is 10 sccm to 400 sccm, the gas flow rate of the dilution gas is 100 sccm to 800 sccm, and the chamber pressure is 30 mTorr to 200 mTorr.

7. The etching method according to claim 1, characterized in that: In S6, in the process of treating the inner wall of the opening with at least one gas selected from nitrogen, hydrogen, oxygen, carbon monoxide and carbon dioxide, the gas flow rate is 300 sccm to 500 sccm and the treatment time is 12 s to 60 s.

8. The etching method according to claim 1, characterized in that: The substrate to be etched has an oxide layer, and the oxide layer is arranged between the dielectric layer and the etching stop layer. There is also step S7 between S4 and S5 for dry etching the oxide layer.

9. The etching method according to claim 8, characterized in that: S7, the gas flow rate of the etching gas is 10 sccm to 200 sccm, the gas flow rate of the dilution gas is 10 sccm to 200 sccm, and the chamber pressure is 30 mTorr to 200 mTorr.