Preparation method of semiconductor structure and semiconductor structure

By forming target trenches in semiconductor device manufacturing and covering the first and second isolation layers respectively, the problem of hollow defects in high aspect ratio processes is solved, the isolation and stability are improved, the leakage phenomenon is reduced, and the semiconductor structure is improved yield.

CN118919486APending Publication Date: 2024-11-08GTA SEMICON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410996447.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

During semiconductor device manufacturing, high aspect ratio processes are prone to hollow defects when filling shallow trenches, resulting in reduced isolation and device stability, and leakage problems.

Method used

By forming a dielectric material stack on the top surface of the substrate, partial substrate and dielectric material are removed to form a target trench whose length is greater than the isolation trench, the first and second isolation trench are formed to cover the inner surface and side walls of the trench, Avoid hollow formation and improve filling effect.

Benefits of technology

It effectively avoids hollow defects when filling the isolation layer in the trench, improves the isolation and device stability of the semiconductor structure, reduces the occurrence of leakage, and improves the yield of the semiconductor structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919486A_ABST
    Figure CN118919486A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a semiconductor structure and the semiconductor structure. The preparation method of the semiconductor structure comprises the following steps: providing a substrate, and forming a dielectric material lamination layer on the top surface of the substrate; removing a part of the substrate to form an isolation groove; a part of the dielectric material lamination is removed to form a dielectric lamination and a target groove, the target groove is located over the isolation groove, the length of the target groove in the first direction is larger than that of the isolation groove in the first direction, and the first direction is the direction parallel to the substrate; forming a first isolation layer, wherein the first isolation layer covers the inner surface of the isolation groove, the side wall of the target groove and the top surface of the dielectric lamination layer; and forming a second isolation layer on the surface of the first isolation layer, wherein the first isolation layer and the second isolation layer form a target isolation layer. The preparation method of the semiconductor structure at least can avoid a cavity formed when the isolation layer is filled in the groove.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor manufacturing, and in particular to a method for preparing a semiconductor structure and a semiconductor structure. Background Art

[0002] As semiconductor process technology continues to develop, the size of semiconductor devices continues to shrink, and the process of ultra-large-scale integrated circuits becomes more and more complex. As the size of the active area continues to shrink, the size of shallow trench isolation also becomes smaller and smaller, making trench filling more and more difficult.

[0003] Usually, the filling effect of the trench is improved by continuously improving the filling capability of the equipment and process or adjusting the etching morphology. High aspect ratio process (HARP) is often used to deposit a filling isolation layer in a shallow trench with a high aspect ratio. The filling capability of the high aspect ratio process is better for the trench.

[0004] However, since the high aspect ratio process is limited by the selectivity of the substrate and the ability of the process to maintain shape, as well as being affected by the poor morphology of the previous layer, the high aspect ratio process is prone to produce void defects in the middle of the trench during the trench filling process. The void defects will cause a significant reduction in shallow trench isolation and device stability, leading to problems such as device leakage. Summary of the invention

[0005] Based on this, the embodiments of the present application provide a method for preparing a semiconductor structure and a semiconductor structure, which can at least avoid voids formed when an isolation layer is filled in a trench.

[0006] According to some embodiments, the present application provides a method for preparing a semiconductor structure, the method comprising: providing a substrate and forming a dielectric material stack on the top surface of the substrate; removing a portion of the substrate to form an isolation trench; removing a portion of the dielectric material stack to form a dielectric stack and a target trench, the target trench being located directly above the isolation trench, and the length of the target trench along a first direction being greater than the length of the isolation trench along the first direction, the first direction being a direction parallel to the substrate; forming a first isolation layer, the first isolation layer covering the inner surface of the isolation trench, the sidewall of the target trench and the top surface of the dielectric stack; forming a second isolation layer on the surface of the first isolation layer, the first isolation layer and the second isolation layer constituting a target isolation layer.

[0007] In the preparation method of the above-mentioned semiconductor structure, a dielectric material stack is formed on the top surface of the substrate; a portion of the substrate is removed to form an isolation groove; a portion of the dielectric material stack is removed to form a dielectric stack and a target groove, and then a first isolation layer covering the inner surface of the isolation groove, the sidewall of the target groove and the top surface of the dielectric stack is formed. Since the length of the target groove along the first direction is greater than the length of the isolation groove along the first direction, a larger opening is opened for the subsequent formation of the first isolation layer, which can avoid the occurrence of voids during the formation of the first isolation layer, and a second isolation layer is formed on the surface of the first isolation layer. The first isolation layer and the second isolation layer constitute the target isolation layer. The target isolation layer is formed by separately forming the first isolation layer and the second isolation layer, which avoids the occurrence of voids during the one-time filling process of the groove to form the target isolation layer, thereby improving the isolation and device stability of the semiconductor structure, and helping to avoid leakage, thereby improving the yield of the semiconductor structure.

[0008] In some embodiments, before forming the first isolation layer, the method further includes: forming a repair layer, the repair layer covering the inner surface of the isolation trench, the sidewall of the target trench, and the top surface of the dielectric stack;

[0009] The first isolation layer is formed, including: forming the first isolation layer on the surface of the repair layer, wherein the thickness of the first isolation layer at the bottom of the isolation trench is greater than the thickness of the repair layer.

[0010] In some embodiments, a portion of the dielectric material stack is removed to form a dielectric stack and a target trench, including: removing a portion of the dielectric material stack to form an initial trench in the dielectric material stack, the initial trench being located directly above the isolation trench, and the length of the initial trench along a first direction is the same as the length of the top opening of the isolation trench along the first direction; etching the dielectric material stack located on the sidewalls of the initial trench to form the dielectric stack and the target trench.

[0011] In some embodiments, a first isolation layer is formed on the surface of the repair layer, including: forming an initial isolation layer and a first filling groove on the surface of the repair layer, the initial isolation layer conformally covers the surface of the repair layer, the first filling groove is located between opposite outer walls of the initial isolation layer, and the thickness of the initial isolation layer is greater than the thickness of the repair layer; removing part of the initial isolation layer to form a first isolation layer and a second filling groove, the second filling groove is located between opposite outer walls of the first isolation layer, and the length of the second filling groove top opening along the first direction is greater than the length of the first filling groove top opening along the first direction.

[0012] In some embodiments, forming the second isolation layer on the surface of the first isolation layer includes: forming the second isolation layer at least in the second filling trench.

[0013] In some embodiments, forming an initial isolation layer on the surface of the repair layer includes: forming the initial isolation layer on the surface of the repair layer using a predetermined deposition process;

[0014] Forming a second isolation layer on the surface of the first isolation layer includes: forming the second isolation layer on the surface of the first isolation layer using a preset deposition process.

[0015] In some embodiments, the predetermined deposition process includes a sub-atmospheric pressure chemical vapor deposition process; the reaction raw materials of the predetermined deposition process include ozone and tetraethyl orthosilicate.

[0016] In some embodiments, the material of the target isolation layer includes silicon oxide.

[0017] In some embodiments, removing a portion of the initial isolation layer to form a first isolation layer and a second filled trench includes: etching the initial isolation layer and annealing the resulting structure to form the first isolation layer and the second filled trench.

[0018] According to some embodiments, the present application further provides a semiconductor structure, which is prepared using the method for preparing the semiconductor structure in any of the above embodiments.

[0019] In the above semiconductor structure, since the semiconductor structure is prepared by the preparation method of the semiconductor structure in any of the above embodiments. In the process of forming the semiconductor structure, a dielectric material stack is formed on the top surface of the substrate; a portion of the substrate is removed to form an isolation groove; a portion of the dielectric material stack is removed to form a dielectric stack and a target groove, and then a first isolation layer covering the inner surface of the isolation groove, the sidewall of the target groove and the top surface of the dielectric stack is formed. Since the length of the target groove along the first direction is greater than the length of the isolation groove along the first direction, a larger opening is opened for the subsequent formation of the first isolation layer, which can avoid the occurrence of voids in the process of forming the first isolation layer, and a second isolation layer is formed on the surface of the first isolation layer. The first isolation layer and the second isolation layer constitute the target isolation layer. The target isolation layer is formed by forming the first isolation layer and the second isolation layer respectively, which avoids the occurrence of voids in the process of filling the groove to form the target isolation layer at one time, improves the isolation and device stability of the semiconductor structure, and is conducive to avoiding leakage, thereby improving the yield of the semiconductor structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 A schematic diagram of a structure with a void defect in a semiconductor structure;

[0021] Figure 2 A schematic flow chart of a method for preparing a semiconductor structure provided by an embodiment;

[0022] Figure 3A schematic cross-sectional view of a structure obtained in step S10 in a method for preparing a semiconductor structure provided in an embodiment;

[0023] Figure 4 A schematic cross-sectional view of a structure obtained in step S51 in a method for preparing a semiconductor structure provided in an embodiment;

[0024] Figure 5 A schematic cross-sectional view of a structure obtained in step S52 in a method for preparing a semiconductor structure provided in an embodiment;

[0025] Figure 6 A schematic cross-sectional view of a structure obtained in step S60 in a method for preparing a semiconductor structure provided in an embodiment;

[0026] Figure 7 A schematic cross-sectional view of a structure obtained in step S711 in a method for preparing a semiconductor structure provided in an embodiment;

[0027] Figure 8 A schematic cross-sectional view of a structure obtained in step S712 in a method for preparing a semiconductor structure provided in an embodiment;

[0028] Fig. 9 The cross-sectional view of the structure obtained in step S90 in a method for preparing a semiconductor structure provided by an embodiment is a schematic diagram.

[0029] Explanation of the reference numerals: V, void; 10, substrate; 11, isolation trench; 20, dielectric stack; 201, dielectric material stack; 21, first dielectric layer; 211, first dielectric material layer; 22, second dielectric layer; 221, second dielectric material layer; 23, target trench; 231, initial trench; 30, target isolation layer; 31, first isolation layer; 311, initial isolation layer; 312, first filled trench; 32, second isolation layer; 321, second filled trench; 40, repair layer. DETAILED DESCRIPTION

[0030] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. Preferred embodiments of the present invention are provided in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0032] In the case of using “including”, “having”, and “comprising” described herein, another component may be added unless a clear limiting term such as “only”, “consisting of”, etc. is used. Unless mentioned otherwise, a term in the singular form may include a plural form and should not be understood as being one in number.

[0033] Spatially relative terms such as "under," "beneath," "below," "under," "above," "above," and the like may be used herein to describe the relationship of an element or feature shown in the figures to other elements or features. It should be understood that, in addition to the orientations shown in the figures, spatially relative terms also include different orientations of the device in use and operation. For example, if the device in the accompanying drawings is flipped, an element or feature described as "under other elements" or "under it" or "under it" will be oriented as being "above" the other elements or features. Thus, the exemplary terms "under" and "under" may include both upper and lower orientations. In addition, the device may also include additional orientations (e.g., rotated 90 degrees or other orientations), and the spatial descriptors used herein are interpreted accordingly.

[0034] It should be understood that although the terms first, second, third, etc. can be used to describe various elements, components, regions, layers, doping types and / or parts, these elements, components, regions, layers, doping types and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer, doping type or part from another element, component, region, layer, doping type or part. Therefore, without departing from the teachings of the present disclosure, the first element, component, region, layer, doping type or part discussed below can be represented as a second element, component, region, layer or part.

[0035] In addition, in order to clearly indicate the multiple layers and regions in the drawings, the thickness of each layer and each region in the drawings are enlarged to clearly illustrate the relative positions between the layers and the distribution of each region. When a layer, film, region, plate, etc. is expressed as being located on the "side" of another part, the expression includes not only the case where it is "directly" above the other part, but also the case where there are other layers in between. And, it is understood that when a layer, film, region, plate, etc. is expressed as being located on the "side" of another part, it generally refers to the side located directly above the other part.

[0036] Embodiments of the invention are described herein with reference to cross-sectional views that are schematic representations of idealized embodiments (and intermediate structures) of the present disclosure, such that variations in the shapes shown due to, for example, manufacturing techniques and / or tolerances are anticipated. Thus, embodiments of the present disclosure should not be limited to the specific shapes of the regions shown herein, but rather include deviations in shapes due to, for example, manufacturing techniques. Thus, the regions shown in the figures are schematic in nature, their shapes do not represent the actual shapes of the regions of the device, and do not limit the scope of the present disclosure.

[0037] See also Figure 1 A shallow trench is formed in the substrate 10 and the dielectric stack 20 on the substrate 10. The dielectric stack 20 usually includes a first dielectric layer 21 and a second dielectric layer 22. When depositing and filling the target isolation layer 30 in the shallow trench, a high aspect ratio process (HARP) is usually used. The high aspect ratio process has a better filling ability for the trench. However, since the high aspect ratio process is limited by the selectivity of the substrate 10 and the ability of process conformality, as well as the influence of the poor morphology of the previous layer, the high aspect ratio process is prone to produce a void V (void) defect in the middle part of the trench during the trench filling process. The void V defect will greatly reduce the isolation of the shallow trench and the stability of the device, resulting in problems such as device leakage.

[0038] Based on this, the embodiments of the present application provide a method for preparing a semiconductor structure and a semiconductor structure, which can at least avoid voids formed when an isolation layer is filled in a trench.

[0039] See also Figure 2 According to some embodiments, a method for preparing a semiconductor structure is provided, the method comprising:

[0040] Step S10, providing a substrate, and forming a dielectric material stack on the top surface of the substrate;

[0041] Step S30, removing part of the substrate to form an isolation trench;

[0042] Step S50, removing part of the dielectric material stack to form a dielectric stack and a target trench, wherein the target trench is located directly above the isolation trench, and the length of the target trench along a first direction is greater than the length of the isolation trench along the first direction, and the first direction is a direction parallel to the substrate;

[0043] Step S70, forming a first isolation layer, wherein the first isolation layer covers the inner surface of the isolation trench, the sidewall of the target trench, and the top surface of the dielectric stack;

[0044] Step S90 , forming a second isolation layer on the surface of the first isolation layer, wherein the first isolation layer and the second isolation layer constitute a target isolation layer.

[0045] In the preparation method of the above-mentioned semiconductor structure, a dielectric material stack is formed on the top surface of the substrate; a portion of the substrate is removed to form an isolation groove; a portion of the dielectric material stack is removed to form a dielectric stack and a target groove, and then a first isolation layer covering the inner surface of the isolation groove, the sidewall of the target groove and the top surface of the dielectric stack is formed. Since the length of the target groove along the first direction is greater than the length of the isolation groove along the first direction, a larger opening is opened for the subsequent formation of the first isolation layer, which can avoid the occurrence of voids during the formation of the first isolation layer, and a second isolation layer is formed on the surface of the first isolation layer. The first isolation layer and the second isolation layer constitute the target isolation layer. The target isolation layer is formed by separately forming the first isolation layer and the second isolation layer, which avoids the occurrence of voids during the one-time filling process of the groove to form the target isolation layer, thereby improving the isolation and device stability of the semiconductor structure, and helping to avoid leakage, thereby improving the yield of the semiconductor structure.

[0046] In some embodiments, step S50, removing a portion of the dielectric material stack to form a dielectric stack and a target trench, includes:

[0047] Step S51, removing part of the dielectric material stack to form an initial trench in the dielectric material stack, wherein the initial trench is located directly above the isolation trench, and the length of the initial trench along the first direction is the same as the length of the top opening of the isolation trench along the first direction;

[0048] Step S52 , etching the dielectric material stack located on the sidewall of the initial trench to form a dielectric stack and a target trench.

[0049] In some embodiments, before step S70, forming the first isolation layer, the method further includes:

[0050] Step S60, forming a repair layer, wherein the repair layer covers the inner surface of the isolation trench, the sidewall of the target trench, and the top surface of the dielectric stack;

[0051] In some embodiments, step S70, forming a first isolation layer, includes:

[0052] Step S71 , forming a first isolation layer on the surface of the repair layer, wherein the thickness of the first isolation layer at the bottom of the isolation trench is greater than the thickness of the repair layer.

[0053] In some embodiments, step S71, forming a first isolation layer on the surface of the repair layer, comprises:

[0054] Step S711, forming an initial isolation layer and a first filling trench on the surface of the repair layer, wherein the initial isolation layer conformally covers the surface of the repair layer, the first filling trench is located between opposite outer side walls of the initial isolation layer, and the thickness of the initial isolation layer is greater than the thickness of the repair layer;

[0055] Step S712, remove part of the initial isolation layer to form a first isolation layer and a second filled trench, the second filled trench is located between the opposite outer side walls of the first isolation layer, and the length of the top opening of the second filled trench along the first direction is greater than the length of the top opening of the first filled trench along the first direction.

[0056] In some embodiments, step S711, forming an initial isolation layer on the surface of the repair layer, comprises:

[0057] Step S7111, forming an initial isolation layer on the surface of the repair layer using a preset deposition process;

[0058] In some embodiments, step S712, removing a portion of the initial isolation layer to form a first isolation layer and a second filling trench, includes:

[0059] Step S7121, etching the initial isolation layer and annealing the resulting structure to form a first isolation layer and a second filling trench.

[0060] In some embodiments, step S90, forming a second isolation layer on the surface of the first isolation layer, comprises:

[0061] Step S901: forming a second isolation layer on the surface of the first isolation layer by using a preset deposition process.

[0062] In some embodiments, the predetermined deposition process includes a sub-atmospheric pressure chemical vapor deposition process; the reaction raw materials of the predetermined deposition process include ozone and tetraethyl orthosilicate.

[0063] In some embodiments, the material of the target isolation layer includes silicon oxide.

[0064] In some embodiments, step S90, forming a second isolation layer on the surface of the first isolation layer, comprises:

[0065] Step S91, forming a second isolation layer at least in the second filling trench.

[0066] In the above embodiments of the present disclosure, unless otherwise specified herein, the execution of each step in the method is not strictly limited in order, and these steps may not necessarily be executed in the order described, and may be executed in other ways. Moreover, at least a part of any step may include multiple sub-steps or multiple stages, and these sub-steps or stages are not necessarily executed at the same time, but may be executed at different times, and the execution order of these sub-steps or stages is not necessarily sequential, but may be executed in turn or alternately with other steps or at least a part of the sub-steps or stages of other steps.

[0067] In order to more clearly illustrate the method for preparing the semiconductor structure provided by the above embodiment, Figures 2 to 9 The method is described in detail.

[0068] like Figure 3 As shown, in step S10 , a substrate 10 is provided, and a dielectric material stack 201 is formed on the top surface of the substrate 10 .

[0069] As an example, in the embodiment of the present disclosure, the substrate 10 can be made of semiconductor material, insulating material, conductor material or any combination of their material types. The substrate 10 can be a single-layer structure or a multi-layer structure. For example, the substrate 10 can be a silicon (Si) substrate 10, a silicon germanium (SiGe) substrate 10, a silicon germanium carbon (SiGeC) substrate 10, a silicon carbide (SiC) substrate 10, a gallium arsenide (GaAs) substrate 10, an indium arsenide (InAs) substrate 10, an indium phosphide (InP) substrate 10 or other III / V semiconductor substrates 10 or II / VI semiconductor substrates 10. Alternatively, for example, the substrate 10 can be a layered substrate 10 including a stack of Si and SiGe, a stack of Si and SiC, a silicon on insulator (SOI) or a silicon germanium on an insulator. Those skilled in the art can select the type of substrate 10 according to the type of transistor formed on the substrate 10, so the type of substrate 10 should not limit the scope of protection of the present disclosure.

[0070] In some embodiments, the dielectric material stack 201 may include a first dielectric material layer 211 and a second dielectric material layer 221 stacked in a direction perpendicular to the substrate 10. The direction perpendicular to the substrate 10 may be understood as follows: Figure 3 The Y direction is shown. For example, the materials of the first dielectric material layer 211 and the second dielectric material layer 221 are different. For example, the material of the first dielectric material layer 211 can be silicon nitride, and the material of the second dielectric material layer 221 can be silicon oxide.

[0071] For example, the first dielectric material layer 211 and the second dielectric material layer 221 can be formed by a deposition process or a thin film growth process. For example, the dielectric material stack 201 including the first dielectric material layer 211 and the second dielectric material layer 221 can be formed on the top surface of the substrate 10 by physical vapor deposition or chemical vapor deposition.

[0072] like Figure 4 As shown, in step S30 , a portion of the substrate 10 is removed to form an isolation trench 11 .

[0073] By way of example, an etching process may be used to remove a portion of the substrate 10 to form the isolation trench 11. In some embodiments, the isolation trench 11 may be a shallow trench. By way of example, the isolation trench 11 has a high aspect ratio.

[0074] like Figure 4 and Figure 5As shown, in step S50, a portion of the dielectric material stack 201 is removed to form a dielectric stack 20 and a target trench 23. The target trench 23 is located directly above the isolation trench 11, and the length of the target trench 23 along the first direction is greater than the length of the isolation trench 11 along the first direction. The first direction is a direction parallel to the substrate 10, that is, the first direction can be understood as follows Figure 4 The X direction is shown.

[0075] In some embodiments, step S50, removing a portion of the dielectric material stack 201 to form the dielectric stack 20 and the target trench 23, includes:

[0076] like Figure 4 As shown, in step S51, a portion of the dielectric material stack 201 is removed to form an initial trench 231 in the dielectric material stack 201. The initial trench 231 is located directly above the isolation trench 11, and the length of the initial trench 231 along the first direction is the same as the length of the top opening of the isolation trench 11 along the first direction.

[0077] For example, in step S30 and step S51, a one-time etching process can be used to simultaneously remove part of the substrate 10 and part of the dielectric material stack 201 to form the isolation trench 11 and the initial trench 231. It can be understood that the one-time etching process can be understood as completing the etching of different materials in a single etching step without the need for multiple etching operations, thereby improving the manufacturing efficiency of semiconductor devices, reducing processing steps, and reducing production costs. Alternatively, a step-by-step etching process can be used to remove part of the substrate 10 and part of the dielectric material stack 201 respectively.

[0078] like Figure 5 As shown, in step S52 , the dielectric material stack 201 located on the sidewall of the initial trench 231 is etched to form the dielectric stack 20 and the target trench 23 .

[0079] In the above embodiment, by etching the dielectric material stack 201 located on the sidewall of the initial trench 231, a target trench 23 with a larger opening is formed, which provides a larger window for forming subsequent structures and is conducive to forming a semiconductor structure with better morphology.

[0080] like Figure 6 As shown, in step S60 , a repair layer 40 is formed, and the repair layer 40 covers the inner surface of the isolation trench 11 , the sidewall of the target trench 23 , and the top surface of the dielectric stack 20 .

[0081] It can be understood that after the target groove 23 is formed, since the length of the target groove 23 along the first direction is greater than the length of the isolation groove 11 along the first direction, the edge area of ​​the substrate 10 located at the top corner of the isolation groove 11 will form a sharper pointed structure. By forming a repair layer 40 covering the inner surface of the isolation groove 11 and the side wall of the target groove 23, the above-mentioned pointed structure can be rounded, thereby reducing the electric field concentration in the edge area of ​​the substrate 10 to improve the performance and reliability of the device.

[0082] On the other hand, ion implantation is a commonly used semiconductor processing technology. It is very important to control the implantation depth. Avoiding penetration can ensure the performance and stability of the device. Forming the repair layer 40 can be used as a preventive measure to prevent the dopant in the ion implantation process from penetrating to an unexpected depth to ensure the accuracy and precision of the doping concentration. In addition, the junction leakage current may reduce the performance of the device, leading to problems such as increased power consumption and signal distortion. By controlling factors such as doping concentration and oxide quality, the junction leakage current can be reduced to improve the reliability and performance of the device.

[0083] For example, a high-temperature in-situ growth process can be used to form the repair layer 40. When the high-temperature in-situ growth process is used to form the repair layer 40, a silicon oxide layer can be formed on the exposed surface of the silicon substrate 10 as the repair layer 40, a silicon oxide layer can be formed on the exposed surface of the first dielectric layer 21 composed of silicon oxide as the repair layer 40, and a silicon oxide layer can be formed on the exposed surface of the second dielectric layer 22 composed of silicon nitride as the repair layer 40.

[0084] like Figure 7 As shown, in step S70 , a first isolation layer 31 is formed, and the first isolation layer 31 covers the inner surface of the isolation trench 11 , the sidewall of the target trench 23 , and the top surface of the dielectric stack 20 .

[0085] In step S71 , a first isolation layer 31 is formed on the surface of the repair layer 40 . The thickness of the first isolation layer 31 at the bottom of the isolation trench 11 is greater than the thickness of the repair layer 40 .

[0086] In some embodiments, step S71, forming a first isolation layer 31 on the surface of the repair layer 40, includes the following steps S711 and S712.

[0087] In some embodiments, step S711 , forming an initial isolation layer 311 on the surface of the repair layer 40 , includes step S7111 , forming the initial isolation layer 311 on the surface of the repair layer 40 using a preset deposition process.

[0088] like Figure 7As shown, in step S7111, an initial isolation layer 311 and a first filling trench 312 are formed on the surface of the repair layer 40, the initial isolation layer 311 conformally covers the surface of the repair layer 40, the first filling trench 312 is located between opposite outer side walls of the initial isolation layer 311, and the thickness of the initial isolation layer 311 is greater than the thickness of the repair layer 40. After the initial isolation layer 311 is formed on the surface of the repair layer 40, the isolation trench 11 is filled by 1 / 2 to 2 / 3.

[0089] In some embodiments, the preset deposition process includes a sub-atmospheric pressure chemical vapor deposition process. The sub-atmospheric pressure chemical vapor deposition process refers to a chemical vapor deposition reaction in which the pressure of the reaction gas is 500 torr to 600 torr when the deposition reaction is carried out in the chamber. The sub-atmospheric pressure chemical vapor deposition process has better step coverage and trench filling capabilities, and its reaction process is a pure chemical reaction without plasma damage. Based on the above advantages, the sub-atmospheric pressure chemical vapor deposition process is widely used in trench filling in the front-end-of-line (FEOL) of the semiconductor manufacturing process, such as shallow trench filling in shallow trench isolation structures.

[0090] In some embodiments, the reaction raw materials of the preset deposition process include ozone and tetraethyl orthosilicate. It can be understood that tetraethyl orthosilicate will produce two intermediates under the action of ozone, namely polysiloxane and silanols, wherein the dangling bonds of the hydrogen-oxygen bonds in the silanols have a higher electrical polarity and are easily absorbed and bonded with the surface of the substrate 10. Since silicon nitride and silicon oxynitride have multiple hydrogen-oxygen bonds on the surface (the bond energy of the hydrogen-oxygen bonds is about 499KJ / mol), and the dangling bonds of the multiple hydrogen bonds on the surface of silicon (the bond energy of the hydrogen bonds is about 30KJ / mol), compared with hydrogen-oxygen bonds, the hydrogen bonds are more active and more likely to react, so the preset deposition process is selective for the substrate, for example, the selectivity of the preset deposition process can be silicon, silicon nitride, silicon oxynitride, silicon oxide in descending order. Moreover, compared with the silicon oxide layer serving as the repair layer 40 located in the isolation trench 11, the area where the silicon oxynitride layer serving as the repair layer 40 is located is closer to the gas of the reaction source. Therefore, the thickness of the initial isolation layer 311 formed on the sidewall of the second dielectric layer 22 is greater than the thickness of the initial isolation layer 311 formed on the sidewall and bottom of the isolation trench 11.

[0091] Illustratively, the material of the initial isolation layer 311 includes silicon oxide.

[0092] like Figure 8As shown, step S712, part of the initial isolation layer 311 is removed to form a first isolation layer 31 and a second filling groove 321, the second filling groove 321 is located between the opposite outer walls of the first isolation layer 31, and the length of the top opening of the second filling groove 321 along the first direction is greater than the length of the top opening of the first filling groove 312 along the first direction.

[0093] In some embodiments, step S712 , removing a portion of the initial isolation layer 311 to form a first isolation layer 31 and a second filling trench 321 , includes step S7121 , etching the initial isolation layer 311 and annealing the resulting structure to form a first isolation layer 31 and a second filling trench 321 .

[0094] In some embodiments, the initial isolation layer 311 can be cyclically etched and the resulting structure can be annealed to form a first isolation layer 31 and a second filling groove 321, and the width of the second filling groove 321 at the opening is greater than the width of the first filling groove 312 at the opening. For example, nitrogen fluoride and ammonia can be used as reaction raw materials for the etching process, and ammonium fluoride can be generated under the action of plasma. Ammonium fluoride, as an etchant, can react with the initial isolation layer 311 composed of silicon oxide at low temperature to generate volatile fluorinated diammonium hexasilicate and water, and the product volatilizes at high temperature to achieve the removal of part of the initial isolation layer 311. Since the initial isolation layer 311 at the corner of the isolation groove 11 is thicker, it is correspondingly removed more, so that the width of the second filling groove 321 at the opening is greater than the width of the first filling groove 312 at the opening.

[0095] like Fig. 9 As shown, in step S90 , the second isolation layer 32 is formed on the surface of the first isolation layer 31 , and the first isolation layer 31 and the second isolation layer 32 constitute the target isolation layer 30 .

[0096] In some embodiments, step S90 of forming the second isolation layer 32 on the surface of the first isolation layer 31 includes step S901 of forming the second isolation layer 32 on the surface of the first isolation layer 31 by using a predetermined deposition process.

[0097] For example, in step S711 and step S901 , the same predetermined deposition process may be used to form the first isolation layer 31 and the second isolation layer 32 , respectively.

[0098] In some embodiments, the material of the second isolation layer 32 includes silicon oxide. Accordingly, the material of the target isolation layer 30 composed of the first isolation layer 31 and the second isolation layer 32 also includes silicon oxide.

[0099] like Fig. 9As shown, in some embodiments, step S90 , forming the second isolation layer 32 on the surface of the first isolation layer 31 , includes step S91 , forming the second isolation layer 32 at least in the second filling trench 321 .

[0100] Please refer to Fig. 9 According to some embodiments, a semiconductor structure is also provided, which is prepared using the method for preparing the semiconductor structure in any of the above embodiments.

[0101] In the above semiconductor structure, since the semiconductor structure is prepared by the preparation method of the semiconductor structure in any of the above embodiments. In the process of forming the semiconductor structure, a dielectric material stack is formed on the top surface of the substrate 10; a portion of the substrate 10 is removed to form an isolation groove; a portion of the dielectric material stack is removed to form a dielectric stack 20 and a target groove, and then a first isolation layer 31 covering the inner surface of the isolation groove, the sidewall of the target groove and the top surface of the dielectric stack 20 is formed. Since the length of the target groove along the first direction is greater than the length of the isolation groove along the first direction, a larger opening is opened for the subsequent formation of the first isolation layer 31, which can avoid the occurrence of voids in the formation process of the first isolation layer 31, and a second isolation layer 32 is formed on the surface of the first isolation layer 31. The first isolation layer 31 and the second isolation layer 32 constitute the target isolation layer 30. The target isolation layer 30 is formed by forming the first isolation layer 31 and the second isolation layer 32 respectively, which avoids the occurrence of voids in the process of filling the groove to form the target isolation layer 30 at one time, improves the isolation property and device stability of the semiconductor structure, and is conducive to avoiding leakage, thereby improving the yield of the semiconductor structure.

[0102] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0103] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a semiconductor structure, characterized in that: include: Providing a substrate, and forming a dielectric material stack on the top surface of the substrate; removing a portion of the substrate to form an isolation trench; Removing part of the dielectric material stack to form a dielectric stack and a target trench, wherein the target trench is located directly above the isolation trench, and the length of the target trench along a first direction is greater than the length of the isolation trench along the first direction, and the first direction is a direction parallel to the substrate; forming a first isolation layer, wherein the first isolation layer covers the inner surface of the isolation trench, the sidewall of the target trench, and the top surface of the dielectric stack; A second isolation layer is formed on the surface of the first isolation layer, and the first isolation layer and the second isolation layer constitute a target isolation layer.

2. The method for preparing a semiconductor structure according to claim 1, characterized in that: Before forming the first isolation layer, the method further includes: forming a repair layer, wherein the repair layer covers the inner surface of the isolation trench, the sidewall of the target trench, and the top surface of the dielectric stack; The forming of the first isolation layer comprises: The first isolation layer is formed on the surface of the repair layer, and the thickness of the first isolation layer located at the bottom of the isolation trench is greater than the thickness of the repair layer.

3. The method for preparing a semiconductor structure according to claim 1, characterized in that: The removing part of the dielectric material stack to form a dielectric stack and a target trench includes: Removing a portion of the dielectric material stack to form an initial trench in the dielectric material stack, wherein the initial trench is located directly above the isolation trench, and the length of the initial trench along the first direction is the same as the length of the top opening of the isolation trench along the first direction; The dielectric material stack located on the sidewall of the initial trench is etched to form the dielectric stack and the target trench.

4. The method for preparing a semiconductor structure according to claim 2, characterized in that: The forming of the first isolation layer on the surface of the repair layer comprises: forming an initial isolation layer and a first filling groove on the surface of the repair layer, wherein the initial isolation layer conformally covers the surface of the repair layer, the first filling groove is located between opposite outer side walls of the initial isolation layer, and the thickness of the initial isolation layer is greater than the thickness of the repair layer; A portion of the initial isolation layer is removed to form the first isolation layer and a second filling groove, wherein the second filling groove is located between the opposite outer side walls of the first isolation layer, and the length of the top opening of the second filling groove along the first direction is greater than the length of the top opening of the first filling groove along the first direction.

5. The method for preparing a semiconductor structure according to claim 4, characterized in that: The forming of the second isolation layer on the surface of the first isolation layer comprises: The second isolation layer is formed at least in the second filling trench.

6. The method for preparing a semiconductor structure according to claim 4, characterized in that: The step of forming an initial isolation layer on the surface of the repair layer comprises: forming an initial isolation layer on the surface of the repair layer by using a preset deposition process; The forming of the second isolation layer on the surface of the first isolation layer comprises: A second isolation layer is formed on the surface of the first isolation layer by using the preset deposition process.

7. The method for preparing a semiconductor structure according to claim 6, characterized in that: The preset deposition process includes a sub-atmospheric pressure chemical vapor deposition process; The reaction materials of the preset deposition process include ozone and tetraethyl orthosilicate.

8. The method for preparing a semiconductor structure according to any one of claims 1 to 7, characterized in that: The material of the target isolation layer includes silicon oxide.

9. The method for preparing a semiconductor structure according to claim 4, characterized in that: The removing part of the initial isolation layer to form the first isolation layer and the second filling trench comprises: The initial isolation layer is etched and the resulting structure is annealed to form the first isolation layer and the second filling trench.

10. A semiconductor structure, characterized in that: The semiconductor structure is prepared by the method for preparing the semiconductor structure according to any one of claims 1 to 9.