Semiconductor device with metal gate structure and manufacturing method thereof

By forming a multi-layer dielectric structure in a semiconductor device and combining high-k and low-k dielectric layers, the problem of increasing parasitic capacitance in semiconductor devices is solved, the switching speed of the device is improved and power consumption is reduced.

CN118919490APending Publication Date: 2024-11-08TAIWAN SEMICONDUCTOR MANUFACTURING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311777699.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-10-17
Filing Date
2023-12-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

As semiconductor technology develops to a smaller geometric structure, the parasitic capacitance between the metal gate structure and the source/drain contact becomes more prominent, and existing methods are difficult to effectively reduce, affecting the switching speed and power consumption of the device.

Method used

By forming a multi-layer dielectric structure in a semiconductor device, including a high-k dielectric layer and a low-k dielectric layer, a multi-layer dielectric layer is formed between the gate structure and the source/drain contact through a deposition and etching process, reducing the whole Dielectric constant, reducing parasitic capacitance.

Benefits of technology

It effectively reduces the parasitic capacitance between the gate structure and the source/drain contact, improves the switching speed of the device and reduces power consumption, and is suitable for smaller transistor technology nodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919490A_ABST
    Figure CN118919490A_ABST
Patent Text Reader

Abstract

The invention relates to a semiconductor device with a metal gate structure and a manufacturing method thereof. A method includes alternately stacking a first semiconductor layer and a second semiconductor layer over a substrate; patterning the first semiconductor layer and the second semiconductor layer into fin structures; forming a dummy gate structure across the fin structure; depositing a gate spacer over sidewalls of the dummy gate structure; removing the dummy gate structure to form a recess; removing the first semiconductor layer; depositing an interface layer surrounding the second semiconductor layer; depositing a high-k dielectric layer over the interface layer and over sidewalls of the gate spacer; depositing a first gate electrode over the high-k dielectric layer; recessing the first gate electrode and the high-k dielectric layer to expose top portions of sidewalls of the gate spacer; depositing a low-k dielectric layer over the recessed high-k dielectric layer; and depositing a second gate electrode over the first gate electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a semiconductor device having a metal gate structure and a method for manufacturing the same. Background Art

[0002] The semiconductor integrated circuit (IC) industry has experienced exponential growth. Technological advances in IC materials and design have produced successive generations of ICs, each with smaller and more complex circuits than the previous one. Over the course of IC evolution, functional density (i.e., the number of interconnected devices per chip area) has generally increased, while geometry size (i.e., the smallest component (or line) that can be created using a manufacturing process) has decreased. This scaling down process generally provides benefits by increasing production efficiency and reducing associated costs. Such scaling down also increases the complexity of processing and manufacturing ICs.

[0003] For example, it is important to reduce parasitic capacitance between conductive features of transistors, such as parasitic capacitance between metal gate structures and source / drain contacts, thereby increasing device switching speed, reducing switching power consumption, and / or reducing coupled noise of transistors. Certain low-k materials with a dielectric constant less than about 5.0 (e.g., a dielectric constant lower than the dielectric constant of silicon oxide (about 3.9)) are suggested as insulating materials for various dielectric layers (e.g., gate spacers and interlayer dielectric (ILD) layers) outside the gate structure, which can provide a lower relative permittivity to reduce parasitic capacitance. However, as semiconductor technology develops to smaller geometries, the distance between the metal gate structure and the source / drain contacts is further reduced, and the relatively high dielectric constant of (one or more) dielectric materials (e.g., high-k dielectric layers) inside the gate structure becomes a factor that should no longer be omitted, resulting in large parasitic capacitance. Therefore, although existing transistor formation methods are generally sufficient for their intended purposes, these existing methods are not completely satisfactory in all aspects due to the continuous reduction of transistor dimensions to technology nodes below 10nm. Summary of the invention

[0004] According to one aspect of the present disclosure, a method for manufacturing a semiconductor device is provided, comprising: alternately stacking a first semiconductor layer and a second semiconductor layer on a substrate; patterning the first semiconductor layer and the second semiconductor layer into a fin structure; forming a dummy gate structure across the fin structure; depositing a gate spacer on a sidewall of the dummy gate structure; laterally recessing an end portion of the first semiconductor layer; forming an internal spacer on an end portion of the first semiconductor layer; removing the dummy gate structure to form a recess, the recess exposing the sidewall of the gate spacer; removing the first semiconductor layer to form a gap between the second semiconductor layers; depositing an interfacial layer around each of the second semiconductor layers; depositing a high-k dielectric layer on the interfacial layer and on the sidewall of the gate spacer; depositing a first gate electrode on the high-k dielectric layer; recessing the first gate electrode; recessing the high-k dielectric layer to expose a top portion of the sidewall of the gate spacer; depositing a low-k dielectric layer on the recessed high-k dielectric layer and on the exposed top portion of the sidewall of the gate spacer; and depositing a second gate electrode on the first gate electrode.

[0005] According to another aspect of the present disclosure, a method for manufacturing a semiconductor device is provided, comprising: forming a vertically stacked channel member suspended above a substrate; forming an epitaxial material adjacent to opposite ends of the channel member; depositing a gate dielectric layer surrounding the channel member; depositing a first gate electrode above the gate dielectric layer; recessing the first gate electrode and the gate dielectric layer; forming a spacer layer above the gate dielectric layer, wherein the dielectric constant of the spacer layer is less than the dielectric constant of the gate dielectric layer; depositing a second gate electrode above the first gate electrode, wherein the spacer layer is disposed on the sidewalls of the second gate electrode; and forming a contact portion above the epitaxial material, wherein the spacer layer is stacked laterally between the contact portion and the second gate electrode.

[0006] According to another aspect of the present disclosure, a semiconductor device is provided, comprising: a semiconductor channel component vertically stacked on a substrate; a gate stack, wherein the gate stack comprises a high-k dielectric layer surrounding the semiconductor channel component, a first gate electrode on the high-k dielectric layer, a second gate electrode on the first gate electrode, and a low-k dielectric layer disposed on a sidewall of the second gate electrode and on the high-k dielectric layer; a gate spacer disposed on the sidewall of the gate stack; a source / drain feature adjacent to the semiconductor channel component; and a source / drain contact disposed on the source / drain feature, wherein the low-k dielectric layer is laterally stacked between the source / drain contact and the second gate electrode. BRIEF DESCRIPTION OF THE DRAWINGS

[0007] When read in conjunction with the accompanying drawings, various aspects of the present disclosure can be best understood from the following detailed description. It should be noted that, in accordance with standard practice in the industry, various features are not drawn to scale. In fact, for the sake of clarity of discussion, the size of various features may be arbitrarily increased or reduced.

[0008] Figure 1 A flow chart of a method of forming a semiconductor device according to various aspects of the present disclosure is shown.

[0009] Figure 2 , Figure 3 , Figure 4 , Figure 5 , Figure 6 , Figure 7 , Figure 8 , Fig. 9 , Fig.10 , Fig.11 , Fig.12 , Fig.13 , Fig.14 , Fig.15 and Fig.16 The present invention shows various aspects of the present disclosure. Figure 1 A perspective view of a semiconductor structure during a manufacturing stage of a method.

[0010] Fig.17 , Fig.18 , Fig.19 , Fig. 20 , Fig.21 , Fig. 22 , Fig.23 , Fig.24 , Fig.25 , Fig.26 , Fig. 27 , Fig.28 , Fig.29 and Fig.30 According to various aspects of the present disclosure, Figure 1 A cross-sectional view of a semiconductor structure during a fabrication stage of a method. DETAILED DESCRIPTION

[0011] The following disclosure provides many different embodiments or examples for implementing the different features of the provided subject matter. Specific examples of components and arrangements are described below to simplify the present disclosure. Of course, these are merely examples and are not intended to be limiting. For example, in the following description, forming a first feature on or above a second feature may include an embodiment in which the first feature and the second feature are formed in direct contact, and may also include an embodiment in which an additional feature may be formed between the first feature and the second feature so that the first feature and the second feature may not be in direct contact. In addition, the present disclosure may repeat reference numerals and / or letters in various examples. This repetition is for the purpose of simplicity and clarity, and does not itself indicate the relationship between the various embodiments and / or configurations discussed.

[0012] In addition, spatially relative terms (e.g., "below," "below," "below," "above," "upper," etc.) may be used herein to facilitate description of the relationship of one element or feature shown in the figures relative to another (one or more) elements or (one or more) features. These spatially relative terms are intended to cover different orientations of the device in use or operation other than the orientation shown in the figures. The device may be oriented in other ways (rotated 90 degrees or in other orientations), and the spatially relative descriptors used herein should also be interpreted accordingly. In addition, when a number or a range of numbers is described using "about," "approximately," etc., the term is intended to include numbers that fall within the range of + / -10% of the described number, unless otherwise specified. For example, the term "about 5nm" encompasses a size range from 4.5nm to 5.5nm.

[0013] The present disclosure generally relates to a semiconductor device and a method of forming the same. More specifically, the present disclosure relates to providing a method and structure for reducing parasitic capacitance between a gate structure and a source / drain contact of a field effect transistor (FET) (e.g., a fin FET (FinFET) or a gate-all-around (GAA) transistor) in semiconductor manufacturing.

[0014] In the formation of FETs, it is important to increase device switching speed, reduce switching power consumption, and reduce coupled noise. Parasitic capacitance generally has a negative impact on these parameters, especially the parasitic capacitance between the gate structure and the source / drain contacts. For example, in a ring oscillator circuit including an odd number of inverter stages connected in a ring, parasitic capacitance may increase the effective load of each inverter stage within the ring oscillator. As a result, it takes longer for the output to propagate through each stage, thereby reducing the speed of the circuit.

[0015] Parasitic capacitance exists in a capacitor-like structure that includes two conductive features with an insulating material between them. The dielectric constant of the insulating material (which is a measure of the ability of the insulating material to store electrical energy in the form of an electric field) directly affects the parasitic capacitance of the structure. In a FET, the gate electrode and adjacent source / drain contacts (which are two conductive features) within a metal gate structure and the insulating material between them (usually a multilayer structure including an interlayer dielectric (ILD) layer, a gate spacer, and a gate dielectric layer) form this structure. Certain low-k materials (whose dielectric constants are lower than that of silicon oxide) have been suggested as insulator materials for various dielectric layers (e.g., gate spacers and / or ILD layers) outside the gate structure, which can provide lower dielectric constants to reduce parasitic capacitance. As semiconductor technology evolves to smaller geometries, the distance between the gate electrode and the source / drain contacts within the metal gate structure is reduced, and the portion of the gate dielectric layer in the multilayer insulating material increases, making it impossible to ignore the high dielectric constant of the gate dielectric layer when estimating parasitic capacitance. Generally, the gate dielectric layer includes (one or more) high dielectric constant (high-k) materials for better electrostatic control of the channel and suppression of leakage current when the FET is in the OFF state. However, (one or more) high-k materials in the gate dielectric layer lead to greater parasitic capacitance.

[0016] Therefore, parasitic capacitance in FETs becomes more problematic as transistor dimensions continue to shrink to technology nodes of 10 nm and below. The present disclosure aims to provide solutions that further reduce the effective dielectric constant of the insulating material between the gate structure and the source / drain contacts in order to reduce parasitic capacitance.

[0017] Some exemplary embodiments of the present disclosure relate to, but are not limited to, multi-gate devices. Multi-gate devices have been introduced to improve gate control by increasing gate-channel coupling, reducing OFF-state current, and reducing short channel effects (SCE). One such multi-gate device that has been introduced is a fin field effect transistor (FinFET). FinFET is named after a fin structure that extends from a substrate (on which the fin structure is formed), and the fin structure is used to form a FET channel. Another multi-gate device introduced to partially address the performance challenges associated with FinFET is a gate all-around (GAA) transistor. GAA transistors are named after a gate structure that can extend around a channel region (e.g., a nanosheet stack) to provide control of the channel on four sides. GAA transistors are compatible with conventional complementary metal oxide semiconductor (CMOS) processes, and the structure of GAA transistors allows GAA transistors to be actively expanded while maintaining gate control and mitigating SCE. The following disclosure will continue to use one or more GAA examples to illustrate various embodiments of the present disclosure. However, it should be understood that the present application should not be limited to a particular type of device unless otherwise stated. For example, various aspects of the present disclosure may also be applicable to FinFET or planar FET based implementations.

[0018] Figure 1 A flow chart of a method 10 for forming a semiconductor device according to the present disclosure is shown. The method 10 is an example, and the method 10 is not intended to limit the present disclosure beyond what is explicitly recited in the claims. Other operations may be provided before, during, and after the method 10, and some of the operations described may be replaced, eliminated, or relocated for other embodiments of the method. Figure 2-Figure 30 Method 10 is described, Figure 2-Figure 30 Perspective and cross-sectional views of a semiconductor device 100 during various manufacturing steps according to some embodiments of method 10 are shown. The semiconductor device 100 may be an intermediate device manufactured during processing of an integrated circuit (IC) or a portion thereof, which may include: static random access memory (SRAM) and / or logic circuits; passive components, such as resistors, capacitors, and inductors; and active components, such as p-type FETs (pFETs), n-type FETs (nFETs), metal oxide semiconductor field effect transistors (MOSFETs), and complementary metal oxide semiconductor (CMOS) transistors, bipolar transistors, high voltage transistors, high frequency transistors, other memory cells, and combinations thereof. In addition, various features (including transistors, gate stacks, active regions, isolation structures, and other features) in various embodiments of the present disclosure are provided for simplicity and ease of understanding, and do not necessarily limit these embodiments to any type of device, any number of devices, any number of regions, or any configuration of structures or regions.

[0019] refer to Figure 1 and Figure 2 , in operation 12, method 10 ( Figure 1 ) provides (or receives) a precursor of the semiconductor device 100. For ease of discussion, the precursor of the semiconductor device 100 is also referred to as the device 100. The device 100 may include a substrate 101 and various features formed in or on the substrate 101. In some embodiments, the substrate 101 includes a crystalline silicon substrate (e.g., a wafer). Depending on the design requirements, the substrate 101 may include various doped regions (e.g., a p-type well and / or an n-type well). In some embodiments, the doped region may be doped with a p-type or n-type dopant. For example, the doped region may be doped with a p-type dopant (e.g., boron or BF2), an n-type dopant (e.g., phosphorus or arsenic), and / or a combination thereof. The doped region may be configured for an n-type transistor, or may be configured for a p-type transistor. In some embodiments, an anti-punch-through (APT) implantation is performed on a top portion of the substrate 101 to form an APT region. The conductivity type of the dopant implanted into the APT region is the same as that of the doped region (or well). The APT region may extend below subsequently formed source / drain regions and serve to reduce leakage from the source / drain regions to the substrate 101. The source / drain region(s) may be referred to individually or collectively as a source or drain, depending on the context. For clarity, in Figure 1 The doped regions and APT regions are not shown in the following figures. In some alternative embodiments, the substrate 101 includes an elemental semiconductor (e.g., silicon or germanium), a compound semiconductor (e.g., silicon carbide, gallium sulfide, gallium phosphide, indium phosphide, indium arsenide, and indium antimonide), an alloy semiconductor (e.g., SiGe, GaAsP, AlInAs, AlGaAs, GaInAs, GaInP, and GaInAsP), or a combination thereof.

[0020] The device 100 includes a semiconductor stack 102 formed on a substrate 101. The semiconductor stack 102 may include a plurality of first layers 104 and a plurality of second layers 106 alternately stacked along the Z direction. Figure 2 Only three first layers 104 and three second layers 106 are shown in the figure, but the embodiments of the present disclosure are not limited thereto. In other embodiments, the number of the first layer 104 and the second layer 106 is adjusted as needed, for example, one, two, four, or more first layers 104 and second layers 106.

[0021] In some embodiments, the first layer 104 and the second layer 106 include different materials. For example, the first layer 104 is a SiGe layer having a germanium atomic percentage in a range between about 15% and 40%, and the second layer 106 is a germanium-free Si layer. However, the embodiments of the present disclosure are not limited thereto, and in other embodiments, the first layer 104 and the second layer 106 include materials with different etching selectivities. In some embodiments, the first layer 104 and the second layer 106 are formed by an epitaxial growth process, such as a molecular beam epitaxy (MBE) process, a metal organic chemical vapor deposition (MOCVD) process, and the like. In this case, the first layer 104 is an epitaxial SiGe layer, and the second layer 106 is an epitaxial Si layer. In some alternative embodiments, the first layer 104 and the second layer 106 are formed by appropriate deposition, such as chemical vapor deposition (CVD), atomic layer deposition (ALD), and the like. In this case, the first layer 104 is a polycrystalline SiGe layer, and the second layer 106 is a polycrystalline Si layer.

[0022] The first layer 104 and the second layer 106 may have the same or different thicknesses. In some embodiments, the first layer 104 has the same thickness T1, and the second layer 106 has the same thickness T2. In some embodiments, the thickness T1 ranges from about 5 nm to about 20 nm, and the second thickness T2 ranges from about 5 nm to about 20 nm. Alternatively, the first layer 104 from top to bottom may have different thicknesses, and the second layer 106 from top to bottom may have different thicknesses.

[0023] The device 100 also includes a mask layer 108 formed on the semiconductor stack 102. The mask layer 108 may include a single-layer structure, a two-layer structure, or a multi-layer structure. For example, the mask layer 108 includes a silicon oxide (SiO) layer and a silicon nitride (SiN) layer on the SiO layer. In some embodiments, the mask layer 108 is formed by CVD, ALD, etc.

[0024] refer to Figure 1 and Figure 3, in operation 14, the method 10 patterns the mask layer 108, the semiconductor stack 102 of the first layer 104 and the second layer 106, and the top portion of the substrate 101 to form the fin 110. In some embodiments, the mask layer 108 is patterned to form a plurality of mask strips 109. The semiconductor stack 102 and the substrate 101 are then patterned by using the mask strips 109 as masks to form a plurality of trenches 118. In this case, a stack of a plurality of fin bases 111 and a plurality of semiconductor strips 112 on the fin bases 111 are formed between the trenches 118. The trenches 118 extend into the substrate 101 and have longitudinal directions parallel to each other. Here, the stack of semiconductor strips 112 is referred to as a nanosheet stack 112, and the combination of the fin base 111 and the nanosheet stack 112 thereon is referred to as a fin 110. As Figure 3 As shown, the nanosheet stack 112 includes a plurality of first nanosheets 114 and a plurality of second nanosheets 116 alternately stacked along the Z direction and extending along the Y direction.

[0025] In some embodiments, the fins 110 may be patterned using any suitable method. For example, these structures may be patterned using one or more photolithography processes, including double patterning or multi-patterning processes. Typically, double patterning or multi-patterning processes combine photolithography and self-alignment processes, allowing for the creation of patterns with gaps, such as gaps smaller than those obtainable using a single, direct photolithography process. For example, in one embodiment, a sacrificial layer is formed over a substrate and patterned using a photolithography process. Spacers are formed next to the patterned sacrificial layer using a self-alignment process. The sacrificial layer is then removed, and the remaining spacers may be used to pattern the fins 110.

[0026] Although in Figure 3 Only two fins 110 are shown in the figure, but the embodiments of the present disclosure are not limited thereto. In other embodiments, the number of fins 110 can be adjusted as needed, such as one fin, three fins, four fins, or more fins. In addition, Figure 3 The mask strip 109 shown in FIG. 1 has a flat top surface. However, the embodiments of the present disclosure are not limited thereto. In other embodiments, the mask strip 109 may have a rounded top surface due to high aspect ratio etching.

[0027] refer to Figure 1 and Figure 4, in operation 16, method 10 forms an insulating layer 113 in the trench 118. In some embodiments, an insulating material is formed on the substrate 101 to cover the fin 110 and fill the trench 118. In addition to the fin 110, the insulating material further covers the mask strip 109. The insulating material may include silicon oxide, silicon nitride, silicon oxynitride, a spin-on dielectric material, or a low-k dielectric material. Here, the low-k dielectric material is typically a dielectric material having a dielectric constant lower than 5.0, for example, a dielectric constant lower than the dielectric constant of silicon oxide (approximately 3.9). The insulating material may be formed by flowable chemical vapor deposition (FCVD), high density plasma chemical vapor deposition (HDP-CVD), sub-atmospheric pressure CVD (SACVD), or spin. A planarization process may be performed to remove the insulating material and a portion of the mask strip 109 until the fin 110 is exposed. In this case, as Figure 4 As shown, the top surface 110t of the fin 110 is substantially coplanar with the top surface 113t of the planarized insulating layer 113. In some embodiments, the planarization process includes chemical mechanical polishing (CMP), an etch-back process, a combination thereof, and the like.

[0028] refer to Figure 1 and Figure 5 In operation 18, the method 10 recesses the insulating layer 113 to form a plurality of isolation regions 115. After the insulating layer 113 is recessed, the fin 110 protrudes relative to the top surface 115t of the isolation region 115. That is, the top surface 115t of the isolation region 115 may be lower than the top surface 110t of the fin 110. In some embodiments, the nanosheet stack 112 is exposed by the isolation region 115. That is, the top surface 115t of the isolation region 115 may be substantially coplanar with the bottom surface 112bt of the nanosheet stack 112, or lower than the bottom surface 112bt of the nanosheet stack 112. In addition, the top surface 115t of the isolation region 115 may have a planar surface (as shown), a convex surface, a concave surface (e.g., a dish shape), or a combination thereof. In some embodiments, the insulating layer 113 is recessed by using an appropriate etching process, for example, a wet etching process using hydrofluoric acid (HF), a dry etching process, or a combination thereof. In some embodiments, the height difference between the top surface 110t of the fin 110 and the top surface 115t of the isolation region 115 is in a range from about 30nm to about 100nm. In some embodiments, the isolation region 115 may be a shallow trench isolation (STI) region, a deep trench isolation (DTI) region, etc.

[0029] refer to Figure 1 and Figure 6In operation 20, the method 10 forms a dummy dielectric layer 120 on the substrate 101. In some embodiments, the dummy dielectric layer 120 conformally covers the surface of the nanosheet stack 112 and the top surface 115t of the isolation region 115. In some embodiments, the dummy dielectric layer 120 includes silicon oxide, silicon nitride, silicon oxynitride, etc., and can be formed by CVD, ALD, etc. The dummy dielectric layer 120 and the isolation region 115 can have the same or different dielectric materials.

[0030] refer to Figure 1 and Figure 7 , in operation 22, method 10 forms a dummy gate stack 122 over a portion of the nanosheet stack 112 and a portion of the isolation region 115. The dummy gate stack 122 may extend along an X direction perpendicular to the extension direction of the nanosheet stack 112. That is, the dummy gate stack 122 may be formed to span the nanosheet stack 112. Specifically, the dummy gate stack 122 may include a dummy gate electrode 124, and a portion of the dummy dielectric layer 120 covered by the dummy gate electrode 124. Here, the portion of the dummy dielectric layer 120 covered by the dummy gate electrode 124 is referred to as a dummy gate dielectric layer 120m. In some embodiments, the dummy gate electrode 124 includes a silicon-containing material, such as polycrystalline silicon, amorphous silicon, or a combination thereof. The dummy gate electrode 124 may be formed using a suitable process (e.g., ALD, CVD, PVD, electroplating, or a combination thereof). Although Figure 7 The dummy gate electrode 124 shown in the figure is a single-layer structure, but the embodiments of the present disclosure are not limited thereto. In other embodiments, the dummy gate electrode 124 can be a multi-layer structure. The dummy gate stack 122 can also include a hard mask layer 126 on the dummy gate electrode 124. In some embodiments, the hard mask layer 126 includes a single-layer structure, a two-layer structure, or a multi-layer structure. For example, Figure 7 As shown, the hard mask layer 126 includes a silicon oxide layer 126 a and a silicon nitride layer 126 b disposed on the silicon oxide layer 126 a .

[0031] Still reference Figure 7, the gate spacer 128 is also formed on the sidewall of the dummy gate stack 122. Similar to the dummy gate stack 122, the gate spacer 128 is also formed across the nanosheet stack 112. In some embodiments, the gate spacer 128 is formed of one or more dielectric materials, for example, SiCN, SiC, SiOCN, SiOC, SiON, or a combination thereof. In order to implement some embodiments, the gate spacer 128 may include a low-k material having a k value less than about 5.0, for example, about 3.9 or even less. For example, in some embodiments, the gate spacer 128 may include a porous dielectric material, an extremely low-k (ELK) dielectric material (e.g., SiCOH), etc. The gate spacer 128 may or may not include an air gap (not shown) to further reduce its k value. The low-k material of the gate spacer 128 is used to advantageously reduce the parasitic capacitance between the subsequently formed metal gate structure and the (one or more) source / drain contacts, particularly in advanced node technologies where the metal gate structure and the (one or more) source / drain contacts are close to each other. In some embodiments, the gate spacer 128 has a thickness ranging from about 1 nm to about 10 nm. Figure 7 The gate spacer 128 shown in FIG. 1 is a single-layer structure, but the embodiments of the present disclosure are not limited thereto. In other embodiments, the gate spacer 128 may be a multi-layer structure. For example, the spacer 128 may include a silicon oxide layer and a silicon nitride layer disposed on the silicon oxide layer. The dummy gate stack 122 and the gate spacer 128 cover the middle portion of the nanosheet stack 112 and expose the opposite end portions that are not covered.

[0032] refer to Figure 1 and Figure 8 , in operation 24, the method 10 recesses the end portion of the nanosheet stack 112 to form a recess 130. Here, the recess 130 may be referred to as a source / drain recess 130. In some embodiments, the end portion of the nanosheet stack 112 may be removed by an anisotropic etching process, an isotropic etching process, or a combination thereof. In some embodiments, the source / drain recess 130 further extends into the fin substrate 111 and is lower than the top surface 115t of the isolation region 115. In other words, the end portion of the nanosheet stack 112 is completely removed, and the top portion of the fin substrate 111 is further removed. In this case, as Figure 8As shown, the bottom surface 14bt of the source / drain recess 130 is lower than the top surface 115t of the isolation region 115. In some embodiments, some portions of the dummy dielectric layer 120 are removed, and other portions of the dummy dielectric layer 120 may remain above the isolation region 115 and aligned with the edge of the isolation region 115, wherein the source / drain recess 130 is formed between these other portions of the dummy dielectric layer 120. The gate spacer 128 may cover the sidewalls of the dummy gate stack 122, which includes the dummy gate dielectric layer 120m, the dummy gate electrode 124, and the hard mask layer 126.

[0033] refer to Figure 1 and Fig. 9 , in operation 26, the method 10 forms an internal spacer 132 at opposite end portions of the first nanosheet 114. In some embodiments, the opposite end portions of the first nanosheet 114 exposed in the source / drain recess 130 are selectively and partially recessed to form an internal spacer recess (not shown), while the second nanosheet 116 is substantially unetched. In embodiments where the second nanosheet 116 substantially includes silicon (Si) and the first nanosheet 114 substantially includes silicon germanium (SiGe), the selective and partial recessing of the first nanosheet 114 may include a SiGe oxidation process followed by SiGe oxide removal. The SiGe oxidation process may include the use of ozone (O3). In some other embodiments, the selective recessing may be a selective isotropic etching process (e.g., a selective dry etching process or a selective wet etching process), and the extent to which the first nanosheet 114 is recessed is controlled by the duration of the etching process. The selective dry etching process may include the use of one or more fluorine-based etchants, such as fluorine gas or hydrofluorocarbons. The selective wet etching process may include a hydrofluoride (HF) or NH4OH etchant. After forming the internal spacer recess, an internal spacer material layer is deposited on the semiconductor device 100, which is included in the internal spacer recess. The internal spacer material layer may include silicon oxide, silicon nitride, silicon oxycarbide, silicon oxycarbonitride, silicon carbonitride, metal nitride, or a suitable dielectric material. The deposited internal spacer material layer is then etched back to remove excess internal spacer material layer on the gate spacer 128 and on the sidewall of the second nanosheet 116, thereby forming an internal spacer 132.

[0034] refer to Figure 1 and Fig.10In operation 28, the method 10 epitaxially grows a strained material 140 (or a highly doped low resistance material) from the source / drain recess 130. In some embodiments, the strained material 140 is used to apply strain or stress to the second nanosheet 116 and the fin substrate 111. Here, the strained material 140 may be referred to as a source / drain region 140 or a source / drain feature 140. In this case, the strained material 140 includes a source disposed on one side of the dummy gate stack 122 and a drain disposed on the other side of the dummy gate stack 122. The source covers one end of the fin substrate 111, and the drain covers the other end of the fin substrate 111. The source / drain region 140 is adjacent to and electrically connected to the second nanosheet 116, while the source / drain region 140 is electrically isolated from the first nanosheet 114 by the internal spacer 132. In some embodiments, the source / drain region 140 extends beyond the top surface of the nanosheet stack 112. However, the embodiments of the present disclosure are not limited thereto, and in other embodiments, the top surface of the source / drain region 140 is substantially aligned with the top surface of the nanosheet stack 112 .

[0035] The source / drain region 140 includes any acceptable material, such as a material suitable for a p-type transistor or an n-type transistor. For example, the source / drain region 140 may include SiGe, SiGeB, Ge, GeSn, etc., which are suitable for p-type transistors. In some alternative embodiments, the source / drain region 140 may include silicon, SiC, SiCP, SiP, etc., which are suitable for n-type transistors. In some embodiments, the source / drain region 140 is formed by MOCVD, MBE, ALD, etc. The source / drain region 140 may include one or more semiconductor material layers. For example, the source / drain region 140 may include a bottom semiconductor material layer, an intermediate semiconductor material layer, and a capping semiconductor material layer. Any number of semiconductor material layers may be used for the source / drain region 140. Each semiconductor material layer may be formed of different semiconductor materials and may be doped to different dopant concentrations. In embodiments where the source / drain region 140 includes three semiconductor material layers, a bottom semiconductor material layer may be deposited, a middle semiconductor material layer may be deposited over the bottom semiconductor material layer, and a capping semiconductor material layer may be deposited over the middle semiconductor material layer.

[0036] In some embodiments, the source / drain region 140 is doped with a conductive dopant. For example, the source / drain region 140 (e.g., SiGe) can be epitaxially grown with a p-type dopant for use in a strained p-type transistor. That is, the source / drain region 140 is doped with a p-type dopant to serve as the source and drain of a p-type transistor. The p-type dopant includes boron or BF2, and the source / drain region 140 can be epitaxially grown by an LPCVD process using in-situ doping. As described above, the source / drain region 140 can be epitaxially grown with multiple layers of different doping concentrations, for example, a SiGe:B bottom layer with a Ge atomic percentage of about 45% to 55% and a boron concentration of about 1×10 21 / cm 3 About 2×10 21 / cm 3 ; an intermediate layer of SiGe:B, wherein the Ge atomic percentage is about 45% to 60% and the boron concentration is about 8×10 20 / cm 3 About 3×10 21 / cm 3 and a capping layer of SiGe:B, wherein the Ge atomic percentage is about 25% to 45% and the boron concentration is about 1×10 20 / cm 3 About 8×10 20 / cm 3 In some alternative embodiments, the source / drain region 140 (e.g., SiC, SiP, a combination of SiC / SiP, or SiCP) is epitaxially grown with n-type dopants for use in strained n-type transistors. That is, the source / drain region 140 is doped with n-type dopants to serve as the source and drain of the n-type transistor. The n-type dopant includes arsenic and / or phosphorus, and the source / drain region 140 can be epitaxially grown using an LPCVD process using in-situ doping. In some embodiments, the source / drain region 140 is epitaxially grown with multiple layers of different doping concentrations, for example, a bottom layer of Si:P with a phosphorus concentration of about 1×10 21 / cm 3 About 2×10 21 / cm 3 ; Si:P intermediate layer, wherein the phosphorus concentration is about 1×10 21 / cm 3 About 4×10 21 / cm 3 ; and a capping layer of Si:As, wherein the arsenic concentration is about 1×10 20 / cm 3 About 1×10 21 / cm 3 .

[0037] Due to the epitaxial growth process used to form the source / drain region 140, the cross-section of the source / drain region 140 may have a rhombus or pentagonal shape. However, the embodiments of the present disclosure are not limited thereto. In other embodiments, the cross-section of the source / drain region 140 may also have a hexagonal, columnar, or rod-like shape. In some embodiments, as shown in FIG. Fig.10 As shown, after the epitaxial growth process is completed, adjacent source / drain regions 140 are separated from each other. Alternatively, adjacent source / drain regions 140 may be merged.

[0038] refer to Figure 1 and Fig.11 In operation 30, the method 10 forms an interlayer dielectric (ILD) layer 144 over the device 100. A contact etch stop layer (CESL) may also be formed between the source / drain regions 140 and the ILD layer 144. For clarity, Fig.11 CESL is not shown in FIG. In addition, in order to show the features behind the front portion of ILD layer 144, Fig.11 Some front portions of the ILD layer 144 are not shown in the following figures so that internal features can be shown. It is understood that the unshown portions of the ILD layer 144 are still present.

[0039] In some embodiments, the CESL conformally covers the sidewalls of the source / drain regions 140 and the outer sidewalls of the gate spacer 128. The CESL may include silicon nitride, silicon oxynitride, silicon nitride containing oxygen (O) or carbon (C) elements, and / or other materials; and may be formed by CVD, PVD (physical vapor deposition), ALD, or other suitable methods.

[0040] The ILD layer 144 includes silicon oxide, silicon nitride, silicon oxynitride, phosphosilicate glass (PSG), borophosphosilicate glass (BPSG), spin-on glass (SOG), fluorinated silicon glass (FSG), carbon-doped silicon oxide (e.g., SiCOH), SiOCN, SiOC, SiC, polyimide, and / or combinations thereof. In some other embodiments, the ILD layer 144 includes a low-k dielectric material. Examples of low-k dielectric materials include BLACK. (Applied Materials, Santa Clara, California), Xerogel, Aerogel, Amorphous Fluorinated Carbon, Parylene, BCB (Bisbenzocyclobutene), Flare, (Dow Chemical Company, Michigan), hydrogen silsesquioxane (HSQ), or fluorinated silicon oxide (SiOF), and / or combinations thereof. In alternative embodiments, the ILD layer 144 includes one or more dielectric materials and / or one or more dielectric layers. In some embodiments, the ILD layer 144 is formed to a suitable thickness by FCVD, CVD, HDPCVD, SACVD, spin coating, sputtering, or other suitable methods. For example, the interlayer dielectric material layer is initially formed to cover the isolation region 115, the dummy gate stack 122, and the gate spacer 128. Subsequently, the thickness of the interlayer dielectric material layer is reduced until the dummy gate stack 122 is exposed, thereby forming the ILD layer 144. The process of reducing the thickness of the interlayer dielectric material layer can be achieved by a chemical mechanical polishing (CMP) process, an etching process, or other suitable processes. In this case, the top surface of the ILD layer 144 can be coplanar with the top surface of the dummy gate stack 122.

[0041] Still reference Figure 1 and Fig.11 In operation 32, the method 10 removes the dummy gate stack 122 to form a gate trench 146. The ILD layer 144 and the CESL can protect the source / drain region 140 during the removal of the dummy gate stack 122. The dummy gate stack 122 can be removed by using plasma dry etching and / or wet etching. When the dummy gate electrode is polysilicon and the ILD layer 144 is silicon oxide, a wet etchant (e.g., TMAH solution) can be used to selectively remove the dummy gate electrode. Thereafter, the dummy gate dielectric layer is removed by using another plasma dry etching and / or wet etching.

[0042] refer to Figure 1 and Fig.12 In operation 34, the method 10 performs an etching process to remove the first nanosheet 114. In this case, the first nanosheet 114 may be completely removed to form a plurality of gaps 148 between the second nanosheets 116, as shown in FIG. Fig.13 shown. Fig.13 A clearer view of a portion of the stacked nanosheets 116 is shown. Fig.12 The ILD 144, source / drain regions 140, and gate spacers 128 are not shown. Fig.13, but these features still exist. Therefore, the second nanosheets 116 are separated from each other by gaps 148. In addition, the bottom-most second nanosheet 116 can also be separated from the fin substrate 111 by gaps 148. As a result, the second nanosheet 116 is suspended. In some embodiments, the height of the gap 148 ranges from about 5nm to about 20nm. In the present embodiment, the second nanosheet 116 includes silicon, and the first nanosheet 114 includes silicon germanium. The first nanosheet 114 can be selectively removed by oxidizing the first nanosheet 114 using a suitable oxidant (e.g., ozone). Thereafter, the oxidized first nanosheet 114 can be selectively removed from the gate trench 146. In some embodiments, the etching process includes a dry etching process to selectively remove the first nanosheet 114, for example, by applying HCl gas at a temperature of about 20°C to about 300°C, or by applying a gas mixture of CF4, SF6, and CHF3. The opposite ends of the suspended second nanosheet 116 are connected to the source / drain region 140. The suspended second nanosheet 116 may be referred to as a channel member 116 hereinafter. The etching process may be referred to as a channel member releasing process. The top surface 110 t of the fin 110 is referred to as a channel top surface 116 t , which is the top surface of the topmost channel member 116 .

[0043] refer to Figure 1 and Fig.14 At operation 36 , method 10 forms a gate dielectric layer 152 in gate trenches 146 and gaps 148 . Fig.15 1 is a diagram showing a clearer view of the gate dielectric layer 152 surrounding the channel member 116. In some embodiments, the gate dielectric layer 152 includes an interface layer 152a formed on the surface of the channel member 116 and the top surface of the fin substrate 111, and a high-k dielectric layer 152b surrounding the interface layer 152a and the underlying channel member 116. The high-k dielectric layer 152b is also disposed on the opposite sidewall surfaces of the gate spacer 128 in the gate trench 146 (e.g., Fig.17as shown). The interface layer 152a is very thin and is made of, for example, SiO2, SiOx (0 < x < 2), or a combination thereof. In some embodiments, the interface layer 152a is formed by applying an oxidant on the surface of the channel member 116. For example, a liquid containing hydrogen peroxide can be applied or supplied on the surface of the channel member 116 to form the interface layer 152a. The high-k dielectric layer 152b can include a dielectric material having a high dielectric constant. Examples of high-k dielectric materials include HfO2, HfSiO, HfSiON, HfTaO, HfTiO, HfZrO, zirconia, lanthanum oxide, alumina, titanium oxide, hafnium oxide-aluminum oxide (HfO2-Al2O3) alloy, other suitable high-k dielectric materials, and / or combinations thereof. The high-k dielectric layer 152b can be formed by CVD, ALD, or any suitable method. In one embodiment, the high-k dielectric layer 152b is formed by using a highly conformal deposition process such as ALD to ensure that a high-k dielectric layer with a uniform thickness is formed around each channel member 116. In some embodiments, the thickness of the high-k dielectric layer 152b ranges from about 0.5 nm to about 3 nm.

[0044] Reference Figure 1 and Fig.16 , in operation 38, method 10 forms a gate electrode 154 on the gate dielectric layer 152 and then planarizes it by using, for example, a CMP process until the top surface of the ILD layer 144 is exposed. Fig.17 Corresponding to Fig.16 a non-complete cross-sectional view of the device 100 taken along line A-A' in. In this case, the gate electrode 154 and the gate dielectric layer 152 constitute the gate stack 150. The gate electrode 154 can include various conductive materials, such as polysilicon, aluminum, copper, titanium, tantalum, tungsten, cobalt, molybdenum, tantalum nitride, nickel silicide, cobalt silicide, TiN, WN, TiAl, TiAlN, TaCN, TaC, TaSiN, metal alloys, other suitable materials, and / or combinations thereof. The gate electrode 154 can include one or more conductive material layers, such as a work function layer and a metal fill layer (not shown separately). The metal fill layer serves as a conductive filler that completely fills the remaining space of the gate trench 146.

[0045] The work function layer can be used to provide the desired work function of the transistor to improve device performance, including improved threshold voltage. In some embodiments, the work function layer is used to form a PMOS device. The work function layer is a p-type work function layer. The p-type work function layer can provide a work function value suitable for the device, for example, equal to or greater than about 4.8 eV. The p-type work function layer can include a metal, a metal carbide, a metal nitride, other suitable materials, or a combination thereof. For example, the p-type metal includes tantalum nitride, tungsten nitride, titanium, titanium nitride, one or more other suitable materials, or a combination thereof. In some other embodiments, the work function layer is used to form an NMOS device. The work function layer is an n-type work function layer. The n-type work function layer can provide a work function value suitable for the device, for example, equal to or less than about 4.5 eV. The n-type work function layer can include a metal, a metal carbide, a metal nitride, or a combination thereof. For example, the n-type work function layer includes titanium nitride, tantalum, tantalum nitride, one or more other suitable materials, or a combination thereof. In some embodiments, the n-type work function layer is an aluminum-containing layer. The aluminum-containing layer may be made of or include the following: TiAlC, TiAlO, TiAlN, one or more other suitable materials, or a combination thereof. The work function layer may also be made of or include the following: hafnium, zirconium, titanium, tantalum, aluminum, metal carbides (e.g., hafnium carbide, zirconium carbide, titanium carbide, aluminum carbide), aluminum compounds, ruthenium, palladium, platinum, cobalt, nickel, conductive metal oxides, or a combination thereof. The thickness and / or composition of the work function layer may be fine-tuned to adjust the work function level. The work function layer may be deposited on the gate dielectric layer 152 using an ALD process, a CVD process, a PVD process, an electroplating process, an electroless plating process, one or more other applicable processes, or a combination thereof.

[0046] In some embodiments, a barrier layer (not shown) is formed before the work function layer to connect the gate dielectric layer 152 to the subsequently formed work function layer interface. The barrier layer can also be used to prevent diffusion between the gate dielectric layer 152 and the subsequently formed work function layer. The barrier layer can be made of or include a metal-containing material. The metal-containing material can include titanium nitride, tantalum nitride, one or more other suitable materials, or a combination thereof. The barrier layer can be deposited using an ALD process, a CVD process, a PVD process, an electroplating process, an electroless plating process, one or more other applicable processes, or a combination thereof.

[0047] In some embodiments, the metal filling layer is made of or includes a metal material. The metal material may include tungsten, ruthenium, aluminum, copper, cobalt, titanium, TiN, TiAl, TiAlC, one or more other suitable materials, or a combination thereof. The metal filling layer may be deposited on the work function layer using a CVD process, an ALD process, a PVD process, an electroplating process, an electroless plating process, a spin coating process, one or more other applicable processes, or a combination thereof.

[0048] In some embodiments, before forming the conductive layer, a barrier layer (not shown) is formed on the work function layer. The barrier layer can be used to prevent the subsequently formed metal filling layer from diffusing or penetrating into the work function layer. The barrier layer can be made of or include the following items: tantalum nitride, titanium nitride, one or more other suitable materials, or a combination thereof. The barrier layer can be deposited using an ALD process, a PVD process, an electroplating process, an electroless plating process, one or more other applicable processes, or a combination thereof.

[0049] In some embodiments, the metal fill layer does not extend into gap 148 because gap 148 is small and is already filled with other features such as gate dielectric layer 152 and work function layer. Fig.17 In the incomplete cross-sectional view along line AA' shown, the bottom surface of the metal filling layer may be higher than the trench top surface 116t. However, the embodiments of the present disclosure are not limited thereto. In some other embodiments, a portion of the metal filling layer extends into the gap 148 having a larger space.

[0050] For clarity, combined Figure 18-Figure 30 Subsequent steps of method 10 of forming device 100 are described, wherein Figure 18-Figure 23 and Figure 26-Figure 30 Corresponds to Fig.16 A non-complete cross-sectional view of the device 100 along line AA' in FIG. 1 , and Figure 24-25 Corresponds to Fig.16 FIG. 1 is a non-complete cross-sectional view of the device 100 along line BB′.

[0051] refer to Figure 1 and Fig.18 In operation 40, the method 10 etches back the gate electrode 154 to form a recess 160. In some embodiments, the etch-back process can be a dry etching process, which includes using an oxygen-containing gas, hydrogen, nitrogen, a fluorine-containing gas (e.g., CF4, SF6, CH2F2, CHF3, CH3F, C4F6 and / or C2F6), a chlorine-containing gas (e.g., Cl2, CHCl3, CCl4 and / or BCl), a bromine-containing gas (e.g., HBr and / or CHBR), an iodine-containing gas (e.g., CF3I), other suitable gases and / or plasmas, and / or combinations thereof. The etchant is selected so that the high-k dielectric layer 152b is substantially intact and remains on the opposite sidewall surfaces of the gate spacer 128. The recessed top surface 154t of the gate electrode 154 can have a concave (e.g., dished) profile. In some embodiments, the remaining gate height (denoted as GH, measured from the bottom of the recess to the channel top surface 116t) is in a range from about 1 nm to about 20 nm.

[0052] refer to Figure 1 and Fig.19 In operation 42, the method 10 etches back the high-k dielectric layer 152b to expose the opposite sidewall surface of the gate spacer 128 in the recess 160. In some embodiments, the insulating layer 113 is recessed by using an appropriate etching process, for example, a selective wet etching process, a selective dry etching process, or a combination thereof. The selective dry etching process may include using one or more fluorine-based etchants, such as fluorine gas or hydrofluorocarbons. The selective wet etching process may include hydrogen fluoride (HF) or NH4OH etchants. The etchant is selected to leave the gate spacer 128 and the recessed gate electrode 154 substantially intact. The amount of etching back of the high-k dielectric layer 152b may be controlled by an etching timer. In some embodiments, as shown by the corner region 162 highlighted by the dashed box, the high-k dielectric layer 152b may have a protruding portion that is higher than the recessed top surface 154t by a vertical distance ΔH2. In various embodiments, ΔH2 is less than about 2nm. It is not arbitrary that ΔH2 is less than about 2nm. If the protruding portion of the high-k dielectric layer 152b is greater than about 2 nm, the remaining high-k material between the metal gate structure and the subsequently formed source / drain contacts is still excessive and increases parasitic capacitance. Fig.19 As shown in , in the alternative corner region 162 ', the high-k dielectric layer 152b can be recessed to be below the recessed gate electrode 154 by a vertical distance ΔH3. In some embodiments, ΔH3 can range from about 0.1nm to about 2nm. To implement some embodiments, the recessed top surface of the high-k dielectric layer 152b is further below the lowest point of the concavity of the recessed top surface 154t of the recessed gate electrode 154. In some embodiments, operations 40 and 42 can be performed simultaneously so that the gate electrode 154 and the high-k dielectric layer 152b are recessed together by an etching process.

[0053] refer to Figure 1 and Fig. 20In operation 44, the method 10 deposits a low-k spacer layer 164 over the bottom and sidewall surfaces of the recess 160 and over the top surface of the ILD layer 144. The low-k spacer layer 164 covers the high-k dielectric layer 152b and the recessed gate electrode 154. The low-k spacer layer 164 may include a low-k material having a k value less than 5.0, such as less than about 3.9 or even less than about 2.5. For example, in some embodiments, the low-k spacer layer 164 may include silicon carbonitride (SiCN), SiONC, a porous dielectric material, an extremely low-k (ELK) dielectric material (e.g., SiCO, SiCOH), etc. The low-k spacer layer 164 may optionally include an air gap (not shown) to further reduce its k value. In one example, the dielectric constant of the porous low-k dielectric material is less than about 2.0. The low-k dielectric material of the low-k spacer layer 164 replaces the high-k dielectric material of the high-k dielectric layer 152b and is used to advantageously reduce the parasitic capacitance between the metal gate structure and the subsequently formed source / drain contacts. In some embodiments, the gate spacer 128, the low-k spacer layer 164, and the high-k dielectric layer 152b include dielectric materials that are different from each other. With respect to the dielectric constant, the k value of the low-k spacer layer 164 can be less than or higher than the k value of the gate spacer 128, depending on specific device performance considerations, and both are less than the k value of the high-k dielectric layer 152b. In some embodiments, the low-k spacer layer 164 is blanket (or conformally) deposited, for example, in an ALD process, wherein during the ALD process, a precursor for forming the low-k spacer layer 164 is applied in a cyclic manner. The thickness of the low-k spacer layer 164 can be controlled by adjusting the number of deposition cycles performed in the deposition chamber during the ALD process. In some embodiments, the low-k spacer layer 164 has a thickness ranging from about 0.5 nm to about 1.5 nm.

[0054] refer to Figure 1 and Fig.21In operation 46, the method 10 performs an etching process for destroying the horizontal portion of the low-k spacer layer 164 and removing most of the horizontal portion of the low-k spacer layer 164. The etching process is also referred to as a breakthrough (BT) etching process. In some embodiments, the BT etching process may include an anisotropic dry etching process, etc. In some embodiments, the BT etching process is a reactive ion etching (RIE) process using an etching process gas including the following items: CHF3, Ar, CF4, N2, O2, CH2F2, SF3, etc., or a combination thereof. The RIE process may be performed under the following conditions: an etching time between about 2 seconds and about 20 seconds, a pressure between about 2mTorr and about 30mTorr, a temperature between about 10°C and about 100°C, a radio frequency (RF) power between about 100W and about 1500W, and a voltage bias between about 10V and about 800V. Alternatively, the BT etching process may include a selective wet etching process using hydrogen fluoride (HF) or NH4OH etchant. In the illustrated embodiment, after the BT etching process, some portions of the low-k spacer layer 164 remain on the opposite sidewall surfaces of the gate spacer 128, and the protruding portion of the high-k dielectric layer 152b (if present) and the recessed gate electrode 154 are exposed again in the recess 160. In some embodiments, the thickness of the remaining portion of the low-k spacer layer 164 ranges from about 0.5nm to about 1.3nm. To implement some embodiments, the thickness of the remaining portion of the low-k spacer layer 164 is greater than the thickness of the high-k dielectric layer 152b. The greater thickness of the low-k spacer layer 164 increases the lateral distance between the metal gate structure and the subsequently formed source / drain contacts, and further reduces parasitic capacitance. In some alternative embodiments, the thickness of the remaining portion of the low-k spacer layer 164 is less than the thickness of the high-k dielectric layer 152b.

[0055] refer to Figure 1 and Fig. 22In operation 48, the method 10 forms a conductive layer 166 filling the recess 160. The conductive layer 166 is made of or includes a metal material. The metal material may include tungsten, ruthenium, aluminum, copper, cobalt, titanium, TiAl, TiAlC, one or more other suitable materials, or a combination thereof. In some embodiments, the conductive layer 166 and the metal filling layer of the recessed gate electrode 154 include different metal materials. For example, compared to the metal filling layer of the recessed gate electrode 154, the conductive layer 166 may include a metal material with a lower resistivity, thereby reducing the overall resistance of the metal gate structure. In some embodiments, the conductive layer 166 and the metal filling layer of the recessed gate electrode 154 include (one or more) the same metal material. The conductive layer 166 may be deposited on the recessed gate electrode 154 using a CVD process, an ALD process, a PVD process, an electroplating process, an electroless plating process, a spin coating process, one or more other suitable processes, or a combination thereof. The conductive layer 166 may also cover the top surface of the ILD layer 144. The device 100 is then planarized by using, for example, a CMP process until the top surface of the ILD layer 144 is exposed. Fig.23 . In the illustrated embodiment, the conductive layer 166 is in physical contact with the low-k spacer layer 164, the protruding portion of the high-k dielectric layer 152b (if present), and the recessed gate electrode 154. The recessed gate electrode 154 is also referred to as the first gate electrode 154, and the conductive layer 166 is also referred to as the second gate electrode 166. The gate dielectric layer 152, the first gate electrode 154, and the second gate electrode 166 together define a gate stack 150, which is also referred to as a metal gate stack 150 or a metal gate structure 150.

[0056] As taken along the longitudinal axis of the gate stack 150 Fig.24 As shown in the cross-sectional view of , the gate dielectric layer 152 surrounds each channel member 116, the first gate electrode 154 further surrounds the gate dielectric layer 152 and fills the vertical space between adjacent channel members 116, and the second gate electrode 166 is deposited on the top surface of the first gate electrode 154. Note that during the etch-back of the first gate electrode 154, byproducts (e.g., TiCl4 and / or AlF3) may remain at the interface between the first gate electrode 154 and the second gate electrode 166 as isolation islands 168 of impurities. Alternatively, the impurities may form a thin film between the first gate electrode 154 and the second gate electrode 166. Similarly, during the etch-back of the high-k dielectric layer 152b, byproducts (e.g., hafnium-containing byproducts, such as HfCl4 and / or HfFx) may remain at the interface between the high-k dielectric layer 152b and the low-k spacer layer 164 as isolation islands of impurities ( Fig.23Alternatively, the hafnium-containing impurity may form a thin film between the high-k dielectric layer 152 b and the low-k spacer layer 164 . Fig.25 is a cross-sectional view taken along the longitudinal axis of the gate stack 150 . Fig.25 Many aspects of the device 100 are similar to Fig.24 One difference is that during the etch back of the first gate electrode 154, the recess 160 in the XZ plane may extend below the channel top surface 116t in the corner region due to the etch loading effect. Fig.25 In the illustrated embodiment, the bottom-most portion of the second gate electrode 166 can extend down to a location between the top-most channel member 116 and the intermediate channel members 116 .

[0057] refer to Figure 1 and Fig.26 In operation 50, method 10 forms a gate contact 172, a source / drain contact 174, and a source / drain contact via 176. In some embodiments, a first patterned mask (not shown) is formed over the ILD layer 144 having an opening over the source / drain region 140. An etching process etches the ILD layer 144 through the opening and exposes the source / drain region 140 in the trench. A silicide feature 170 is formed over the source / drain region 140 in a silicide formation process. The silicide features 170 may include titanium silicide (TiSi), nickel silicide (NiSi), tungsten silicide (WSi), nickel platinum silicide (NiPtSi), nickel platinum germanium silicide (NiPtGeSi), nickel germanium silicide (NiGeSi), ytterbium silicide (YbSi), platinum silicide (PtSi), iridium silicide (IrSi), erbium silicide (ErSi), cobalt silicide (CoSi), combinations thereof, or other suitable compounds. Subsequently, source / drain contacts 174 are formed in the trenches and land on the silicide features 170 by depositing a conductive material in the trenches. The conductive material may include any suitable material, such as W, Co, Ru, Cu, Ta, Ti, Al, Mo, other suitable conductive materials, or combinations thereof, and may be deposited by any suitable method, such as CVD, PVD, ALD, electroplating, other suitable methods, or combinations thereof. Alternatively, silicide formation may be skipped and the source / drain contacts 174 may directly contact the source / drain features 140.

[0058] After forming the source / drain contacts 174, an ILD layer 178 is deposited on the ILD layer 144. In some embodiments, the ILD layer 178 includes silicon oxide, silicon nitride, silicon oxynitride, phosphosilicate glass (PSG), borophosphosilicate glass (BPSG), spin glass (SOG), fluorinated silicon glass (FSG), carbon-doped silicon oxide (e.g., SiCOH), polyimide, and / or a combination thereof. In some other embodiments, the ILD layer 178 includes a low-k dielectric material. In some embodiments, the ILD layers 144 and 178 include different dielectric materials. The ILD layer 178 can be formed to a suitable thickness by FCVD, CVD, HDPCVD, SACVD, spin coating, sputtering, or other suitable methods.

[0059] After forming the ILD layer 178, a second patterned mask (not shown) is formed over the ILD layer 178, which has openings over the source / drain contacts 174 and the second gate electrode 166, respectively. The etching process etches through the ILD layer 178 through the openings and exposes the source / drain contacts 174 and the second gate electrode 166 in the trenches. Subsequently, source / drain contact vias 176 and gate contacts 172 are formed in the trenches by depositing a conductive material in the trenches, and fall on the source / drain contacts 174 and the second gate electrode 166, respectively. The conductive material may include any suitable material, such as W, Co, Ru, Cu, Ta, Ti, Al, Mo, other suitable conductive materials, or combinations thereof, and may be deposited by any suitable method, such as CVD, PVD, ALD, electroplating, other suitable methods, or combinations thereof. The conductive material forming the source / drain contact vias 176 and the gate contacts 172 may be different from the conductive material forming the source / drain contacts 174. Subsequently, a planarization process (eg, a CMP process) is performed to remove excess conductive material and expose the ILD layer 178 .

[0060] Still reference Fig.26, a multi-layer dielectric structure is stacked laterally between the gate stack 150 and the source / drain contacts 174. The multi-layer dielectric structure includes an ILD layer 144, a gate spacer 128, a high-k dielectric layer 152b that separates the first gate electrode 154 and the gate spacer 128 from contact, and a low-k spacer layer 164 that separates the second gate electrode 166 and the gate spacer 128 from contact. In some embodiments, the source / drain contacts 174 can be deposited on the sidewalls of the gate spacer 128 by a self-aligned formation process so that the multi-layer dielectric structure does not include the ILD layer 144. In either case, a large portion of the high-k dielectric layer 152b above the channel top surface 116t is replaced by the low-k spacer layer 164. Therefore, the overall dielectric constant of the multi-layer dielectric structure is reduced, which also reduces the parasitic capacitance between the gate stack 150 and the source / drain contacts 174. For example, by replacing a large portion of the high-k dielectric layer 152b above the channel top surface 116t with the low-k spacer layer 164, the parasitic capacitance can be reduced by about 30% to about 40%. In some embodiments, the ratio (H1 / H2) of the height H1 of the high-k dielectric layer 152b measured above the channel top surface 116t to the height H2 of the low-k spacer layer 164 is in the range of about 1:20 to about 1:2. This range is not arbitrary. If H1 / H2 is less than 1:20, the gate stack 150 may have an excessively large aspect ratio, increasing manufacturing difficulty; if H1 / H2 is greater than 1:2, the parasitic capacitance may not be effectively reduced because a large portion of the high-k dielectric layer 152b remains laterally between the gate stack 150 and the gate / drain contact 174.

[0061] Fig. 27 An alternative embodiment of device 100 is shown. Fig. 27 Many aspects of the device 100 are similar to Fig.26 The same or similar aspects in Fig. 27 In the embodiment, the low-k spacer layer 164 covers the protruding portion of the high-k dielectric layer 152b due to the greater thickness of the low-k spacer layer 164. In this alternative embodiment, the bottom surface of the low-k spacer layer 164 is in physical contact with the first gate electrode 154 and separates the high-k dielectric layer 152b from the second gate electrode 166 without contact.

[0062] Fig.28 Another alternative embodiment of device 100 is shown. Fig.28 Many aspects of the device 100 are similar to Fig.26 The same or similar aspects in Fig.28In the embodiment, the low-k spacer layer 164 is thinner than the high-k dielectric layer 152 b , so that the top surface of the high-k dielectric layer 152 b is not completely covered by the low-k spacer layer 164 and is in physical contact with the second gate electrode 166 .

[0063] Fig.29 Another alternative embodiment of device 100 is shown. Fig.29 Many aspects of the device 100 are similar to Fig.26 The same or similar aspects in Fig.29 In the embodiment, the high-k dielectric layer 152b is recessed to be below the recessed gate electrode 154 (also as shown in FIG. Fig.19 The low-k dielectric layer 152b is also not in contact with the second gate electrode 166.

[0064] Fig.30 Another alternative embodiment of device 100 is shown. Fig.30 Many aspects of the device 100 are similar to Fig.26 The same or similar aspects in Fig.30 In the embodiment, the high-k dielectric layer 152b is recessed to be below the recessed gate electrode 154 (also as shown in FIG. Fig.19 162'), and the void 180 (or air gap) is sealed by the bottom portion of the low-k spacer layer 164. The high-k dielectric layer 152b does not contact the second gate electrode 166. The void 180 is formed due to the limited gap filling ability of the low-k spacer layer 164 during the deposition of the low-k spacer layer 164 into the gap between the recessed high-k dielectric layer 152b and the recessed gate electrode 154. The void 180 can be located above the top surface of the source / drain region 140. The void 180 further reduces the overall dielectric constant of the multi-layer dielectric structure between the gate stack 150 and the source / drain contact 174, thereby generating smaller parasitic capacitance.

[0065] Although not intended to be limiting, one or more embodiments of the present disclosure provide many benefits to semiconductor devices and their formation. For example, embodiments of the present disclosure provide a multilayer dielectric structure stacked between a gate electrode and a source / drain contact of a metal gate structure, which effectively reduces the parasitic capacitance of the structure by including a low-k dielectric layer disposed on a recessed high-k dielectric layer. In addition, the formation of the barrier layer can be easily integrated into existing semiconductor manufacturing processes.

[0066] In one exemplary aspect, the present disclosure relates to a method for manufacturing a semiconductor device. The method includes: alternately stacking a first semiconductor layer and a second semiconductor layer on a substrate; patterning the first semiconductor layer and the second semiconductor layer into a fin structure; forming a dummy gate structure across the fin structure; depositing a gate spacer on a sidewall of the dummy gate structure; laterally recessing an end portion of the first semiconductor layer; forming an inner spacer on an end portion of the first semiconductor layer; removing the dummy gate structure to form a recess that exposes a sidewall of the gate spacer; removing the first semiconductor layer to form a gap between the second semiconductor layers; depositing an interfacial layer around each second semiconductor layer; depositing a high-k dielectric layer on the interfacial layer and on the sidewall of the gate spacer; depositing a first gate electrode on the high-k dielectric layer; recessing the first gate electrode; recessing the high-k dielectric layer to expose a top portion of the sidewall of the gate spacer; depositing a low-k dielectric layer on the recessed high-k dielectric layer and on the exposed top portion of the sidewall of the gate spacer; and depositing a second gate electrode on the first gate electrode. In some embodiments, the method further comprises: forming an epitaxial feature adjacent to an end portion of the second semiconductor layer; and forming a contact portion over the epitaxial feature and electrically coupled to the epitaxial feature, wherein the low-k dielectric layer is stacked laterally between the contact portion and the second gate electrode. In some embodiments, the topmost portion of the high-k dielectric layer is higher than the top surface of the recessed first gate electrode. In some embodiments, the topmost portion of the high-k dielectric layer is higher than the top surface of the recessed first gate electrode by a vertical distance less than about 2 nm. In some embodiments, the topmost portion of the high-k dielectric layer is lower than the top surface of the recessed first gate electrode. In some embodiments, the topmost portion of the high-k dielectric layer is lower than the top surface of the recessed first gate electrode by a vertical distance less than about 2 nm. In some embodiments, the low-k dielectric layer is thicker than the high-k dielectric layer. In some embodiments, the interface between the low-k dielectric layer and the high-k dielectric layer includes a hafnium-containing impurity. In some embodiments, the interface between the first gate electrode and the second gate electrode includes a titanium-containing or aluminum-containing impurity. In some embodiments, the dielectric constant value of the low-k dielectric layer is less than the gate spacer.

[0067] In another exemplary aspect, the present disclosure relates to a method. The method includes: forming a vertically stacked channel member suspended above a substrate; forming an epitaxial material adjacent to opposite ends of the channel member; depositing a gate dielectric layer surrounding the channel member; depositing a first gate electrode above the gate dielectric layer; recessing the first gate electrode and the gate dielectric layer; forming a spacer layer above the gate dielectric layer, wherein the dielectric constant of the spacer layer is less than the dielectric constant of the gate dielectric layer; depositing a second gate electrode above the first gate electrode, wherein the spacer layer is disposed on the sidewalls of the second gate electrode; and forming a contact portion above the epitaxial material, wherein the spacer layer is stacked laterally between the contact portion and the second gate electrode. In some embodiments, forming the spacer layer includes: conformally depositing the dielectric layer above the gate dielectric layer and the first gate electrode; and removing a horizontal portion of the dielectric layer to expose the first gate electrode, wherein a vertical portion of the dielectric layer remains as the spacer layer. In some embodiments, the method also includes: forming a gate spacer above the epitaxial material, wherein the gate spacer is in physical contact with the spacer layer. In some embodiments, the gate spacer is in physical contact with the gate dielectric layer. In some embodiments, the bottom surface of the second gate electrode is lower than the bottom surface of the spacer layer. In some embodiments, the dielectric constant of the spacer layer is less than about 2.5. In some embodiments, the spacer layer separates the gate dielectric layer from the second gate electrode without physically contacting it.

[0068] In another exemplary aspect, the present disclosure relates to a semiconductor device. The semiconductor device includes: a semiconductor channel component, stacked vertically on a substrate; and a gate stack. The gate stack includes a high-k dielectric layer surrounding the semiconductor channel component, a first gate electrode on the high-k dielectric layer, a second gate electrode on the first gate electrode, and a low-k dielectric layer disposed on the sidewall of the second gate electrode and on the high-k dielectric layer. The semiconductor device also includes: a gate spacer, disposed on the sidewall of the gate stack; a source / drain feature, adjacent to the semiconductor channel component; and a source / drain contact, disposed on the source / drain feature. The low-k dielectric layer is stacked laterally between the source / drain contact and the second gate electrode. In some embodiments, the gate spacer is in physical contact with the high-k dielectric layer and the low-k dielectric layer. In some embodiments, the bottom surface of the second gate electrode is lower than the top surface of the topmost semiconductor channel component of the semiconductor channel component.

[0069] The features of several embodiments are summarized above so that those skilled in the art can better understand the various aspects of the present disclosure. Those skilled in the art should understand that they can easily use the present disclosure as a basis for designing or modifying other processes and structures to achieve the same purpose of the embodiments introduced herein and / or achieve the same advantages of the embodiments introduced herein. Those skilled in the art should also recognize that such equivalent constructions do not depart from the spirit and scope of the present disclosure, and they can make various changes, substitutions and modifications herein without departing from the spirit and scope of the present disclosure.

[0070] Example 1. A method for manufacturing a semiconductor device, comprising: alternately stacking a first semiconductor layer and a second semiconductor layer on a substrate; patterning the first semiconductor layer and the second semiconductor layer into a fin structure; forming a dummy gate structure across the fin structure; depositing a gate spacer on the sidewall of the dummy gate structure; laterally recessing an end portion of the first semiconductor layer; forming an internal spacer on an end portion of the first semiconductor layer; removing the dummy gate structure to form a recess, the recess exposing the sidewall of the gate spacer; removing the first semiconductor layer to form a gap between the second semiconductor layers; depositing an interfacial layer around each of the second semiconductor layers; depositing a high-k dielectric layer on the interfacial layer and on the sidewall of the gate spacer; depositing a first gate electrode on the high-k dielectric layer; recessing the first gate electrode; recessing the high-k dielectric layer to expose a top portion of the sidewall of the gate spacer; depositing a low-k dielectric layer on the recessed high-k dielectric layer and on the exposed top portion of the sidewall of the gate spacer; and depositing a second gate electrode on the first gate electrode.

[0071] Example 2. The method according to Example 1 further includes: forming an epitaxial feature adjacent to an end portion of the second semiconductor layer; and forming a contact portion above the epitaxial feature and electrically coupled to the epitaxial feature, wherein the low-k dielectric layer is laterally stacked between the contact portion and the second gate electrode.

[0072] Example 3. The method of Example 1, wherein a topmost portion of the high-k dielectric layer is higher than a top surface of the recessed first gate electrode.

[0073] Example 4. The method of Example 3, wherein a topmost portion of the high-k dielectric layer is a vertical distance higher than a top surface of the recessed first gate electrode that is less than 2 nm.

[0074] Example 5. The method of Example 1, wherein a topmost portion of the high-k dielectric layer is below a top surface of the recessed first gate electrode.

[0075] Example 6. The method of Example 5, wherein a topmost portion of the high-k dielectric layer is a vertical distance below a top surface of the recessed first gate electrode that is less than 2 nm.

[0076] Example 7. The method of Example 1, wherein the low-k dielectric layer is thicker than the high-k dielectric layer.

[0077] Example 8. The method of Example 1, wherein an interface between the low-k dielectric layer and the high-k dielectric layer includes a hafnium-containing impurity.

[0078] Example 9. The method of Example 1, wherein an interface between the first gate electrode and the second gate electrode includes titanium-containing or aluminum-containing impurities.

[0079] Example 10. The method of example 1, wherein the low-k dielectric layer has a dielectric constant value that is smaller than the gate spacer.

[0080] Example 11. A method for manufacturing a semiconductor device, comprising: forming a vertically stacked channel member suspended above a substrate; forming an epitaxial material adjacent to opposite ends of the channel member; depositing a gate dielectric layer surrounding the channel member; depositing a first gate electrode above the gate dielectric layer; recessing the first gate electrode and the gate dielectric layer; forming a spacer layer above the gate dielectric layer, wherein the dielectric constant of the spacer layer is less than the dielectric constant of the gate dielectric layer; depositing a second gate electrode above the first gate electrode, wherein the spacer layer is disposed on the sidewalls of the second gate electrode; and forming a contact portion above the epitaxial material, wherein the spacer layer is stacked laterally between the contact portion and the second gate electrode.

[0081] Example 12. A method according to Example 11, wherein forming the spacer layer includes: conformally depositing a dielectric layer over the gate dielectric layer and the first gate electrode; and removing a horizontal portion of the dielectric layer to expose the first gate electrode, wherein a vertical portion of the dielectric layer is retained as the spacer layer.

[0082] Example 13. The method of Example 11, further comprising: forming a gate spacer over the epitaxial material, wherein the gate spacer is in physical contact with the spacer layer.

[0083] Example 14. The method of Example 13, wherein the gate spacer is in physical contact with the gate dielectric layer.

[0084] Example 15. The method of Example 11, wherein a bottom surface of the second gate electrode is lower than a bottom surface of the spacer layer.

[0085] Example 16. The method of Example 11, wherein the dielectric constant of the spacer layer is less than 2.5.

[0086] Example 17. The method of Example 11, wherein the spacer layer separates the gate dielectric layer from the second gate electrode without physically contacting it.

[0087] Example 18. A semiconductor device comprising: a semiconductor channel component stacked vertically above a substrate; a gate stack, wherein the gate stack includes a high-k dielectric layer surrounding the semiconductor channel component, a first gate electrode above the high-k dielectric layer, a second gate electrode above the first gate electrode, and a low-k dielectric layer disposed on the sidewalls of the second gate electrode and above the high-k dielectric layer; a gate spacer disposed on the sidewalls of the gate stack; a source / drain feature adjacent to the semiconductor channel component; and a source / drain contact disposed on the source / drain feature, wherein the low-k dielectric layer is stacked laterally between the source / drain contact and the second gate electrode.

[0088] Example 19. The semiconductor device of Example 18, wherein the gate spacer is in physical contact with the high-k dielectric layer and the low-k dielectric layer.

[0089] Example 20. The semiconductor device of Example 18, wherein a bottom surface of the second gate electrode is lower than a top surface of a topmost one of the semiconductor channel components.

Claims

1. A method for manufacturing a semiconductor device, include: Alternatingly stacking first semiconductor layers and second semiconductor layers on a substrate; patterning the first semiconductor layer and the second semiconductor layer into a fin structure; forming a dummy gate structure across the fin structure; depositing a gate spacer on a sidewall of the dummy gate structure; laterally recessing an end portion of the first semiconductor layer; forming an inner spacer on an end portion of the first semiconductor layer; removing the dummy gate structure to form a recess, the recess exposing a sidewall of the gate spacer; removing the first semiconductor layer to form a gap between the second semiconductor layers; depositing an interfacial layer around each of the second semiconductor layers; depositing a high-k dielectric layer over the interfacial layer and over sidewalls of the gate spacers; depositing a first gate electrode over the high-k dielectric layer; recessing the first gate electrode; recessing the high-k dielectric layer to expose top portions of sidewalls of the gate spacers; depositing a low-k dielectric layer over the recessed high-k dielectric layer and over the exposed top portions of the sidewalls of the gate spacers; as well as A second gate electrode is deposited over the first gate electrode.

2. The method according to claim 1, further comprising: include: forming an epitaxial feature adjacent to an end portion of the second semiconductor layer; as well as A contact is formed over and electrically coupled to the epitaxial feature, wherein the low-k dielectric layer is stacked laterally between the contact and the second gate electrode.

3. The method according to claim 1, in, A topmost portion of the high-k dielectric layer is higher than a top surface of the recessed first gate electrode.

4. The method according to claim 3, in, A topmost portion of the high-k dielectric layer is vertically higher than a top surface of the recessed first gate electrode by a distance that is less than 2 nm.

5. The method according to claim 1, in, A topmost portion of the high-k dielectric layer is below a top surface of the recessed first gate electrode.

6. The method according to claim 5, in, A topmost portion of the high-k dielectric layer is a vertical distance below a top surface of the recessed first gate electrode that is less than 2 nm.

7. The method according to claim 1, in, The low-k dielectric layer is thicker than the high-k dielectric layer.

8. The method according to claim 1, in, An interface between the low-k dielectric layer and the high-k dielectric layer includes a hafnium-containing impurity.

9. A method of manufacturing a semiconductor device, include: forming a vertically stacked channel member suspended above a substrate; forming epitaxial material adjacent opposite ends of the channel member; depositing a gate dielectric layer surrounding the channel member; depositing a first gate electrode over the gate dielectric layer; recessing the first gate electrode and the gate dielectric layer; forming a spacer layer on the gate dielectric layer, wherein the dielectric constant of the spacer layer is less than the dielectric constant of the gate dielectric layer; depositing a second gate electrode over the first gate electrode, wherein the spacer layer is disposed on sidewalls of the second gate electrode; and A contact is formed over the epitaxial material, wherein the spacer layer is stacked laterally between the contact and the second gate electrode.

10. A semiconductor device, include: A semiconductor channel member is vertically stacked on the substrate; a gate stack, wherein the gate stack comprises a high-k dielectric layer surrounding the semiconductor channel member, a first gate electrode over the high-k dielectric layer, a second gate electrode over the first gate electrode, and a low-k dielectric layer disposed on a sidewall of the second gate electrode and over the high-k dielectric layer; a gate spacer disposed on a sidewall of the gate stack; a source / drain feature adjacent to the semiconductor channel member; and A source / drain contact is disposed on the source / drain feature, wherein the low-k dielectric layer is laterally stacked between the source / drain contact and the second gate electrode.