Array substrate, display panel and manufacturing method of array substrate
By setting a smaller thickness in the display area for the first conductive layer of the array substrate and setting a larger thickness in the peripheral area for the adapter electrode, the high temperature afterimage and reliability and low yield in the prior art are solved. Problem, improving process stability.
Patent Information
- Application Number
- CN202410955147.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
When the prior art improves the contrast of the display panel, it will lead to problems such as high-temperature afterimage, reliability, yield and process stability.
By setting a smaller thickness for the electrode of the first conductive layer in the display area of the array substrate and setting a larger thickness for the adapter electrode in the peripheral area, the risk of the adapter electrode being broken at the through-hole slope is reduced, and the risk of the adapter electrode being broken is increased. Trust and yield.
Improve the high-temperature afterimage problem in the display area, and improve reliability, yield and process stability in the surrounding area.
Smart Images

Figure CN118919540A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of display technology, and in particular to an array substrate, a display panel and a method for manufacturing the array substrate. Background Art
[0002] Compared with the vertical alignment (VA) display mode, the advanced superdimensional switch (ADS) display mode has the problem of low contrast ratio (CR). The liquid crystal alignment force of the ADS display mode is weak, and the rotation of the liquid crystal is in-plane rotation. When light passes through the liquid crystal box, the direction of light travels in the non-optical axis direction of the liquid crystal, the scattering is relatively large, and the CR is about 1200. When light in the VA display mode passes through the liquid crystal box, the direction of light travels in the optical axis direction of the liquid crystal, the scattering is relatively small, and the CR is about 3000. However, when the display panel of the prior art improves the contrast, the display panel will have high-temperature afterimages, as well as low reliability, yield and process stability. Summary of the invention
[0003] The present invention provides an array substrate, a display panel and a method for manufacturing the array substrate, so as to improve the problems of the display panel in the prior art that when the contrast is improved, the display panel may have a high-temperature afterimage, and the reliability, yield and process stability may be low.
[0004] An embodiment of the present invention provides an array substrate having a display area and a peripheral area located outside the display area. The array substrate comprises: a substrate, a first conductive layer located on one side of the substrate;
[0005] The first conductive layer includes: a plurality of first electrodes and a plurality of switching electrodes; the first electrodes are located in the display area, and the switching electrodes are located in the peripheral area; in a direction perpendicular to the substrate, a maximum thickness of the first electrodes is smaller than a maximum thickness of the switching electrodes.
[0006] In a possible implementation, at an edge region of the peripheral area, in a direction perpendicular to the substrate, a thickness of the switching electrode in a portion of the edge region is smaller than a thickness in a middle region.
[0007] In a possible implementation, the array substrate further includes: a plurality of first signal lines, a plurality of second signal lines, and a plurality of first via holes located between the substrate and the switching electrode; the first signal lines are electrically connected to the second signal lines at the first via holes through the switching electrodes;
[0008] The orthographic projection of the switching electrode on the substrate covers the orthographic projection of the first via hole on the substrate.
[0009] In a possible implementation manner, a first insulating layer is provided between the first signal line and the switching electrode, a second insulating layer is provided between the second signal line and the switching electrode, the first insulating layer has a first sub-via, and the second insulating layer has a second sub-via;
[0010] The switching electrode is partially electrically connected to the first signal line through the first sub-via, and partially electrically connected to the second signal line through the second sub-via; the first via includes the first sub-via and the second sub-via.
[0011] In a possible implementation, the array substrate further includes: a plurality of transistors located in the display area, and a plurality of second via holes; the transistors include: a first electrode and a second electrode; the first electrode is electrically connected to the second electrode through the second via hole;
[0012] In a direction perpendicular to the substrate, a depth of the first sub-via hole is greater than a depth of the second via hole.
[0013] In a possible implementation manner, the first signal line includes: an initial signal line, a clock signal line, a high level signal line, or a low level signal line; the second signal line includes: a transfer line;
[0014] Alternatively, the first signal line includes: a gate output signal lead; the second signal line includes: a gate line;
[0015] Alternatively, the first signal line includes: a plurality of common electrode wirings; the second signal line includes: a ground line or a plurality of short-circuit loop lines.
[0016] In a possible implementation manner, in a direction perpendicular to the substrate, the maximum thickness of the first electrode is one quarter to three quarters of the maximum thickness of the switching electrode.
[0017] In a possible implementation, the array substrate includes: a first metal structure layer located between the substrate and the transfer electrode; the first metal structure layer includes: a first sub-metal layer, and a second sub-metal layer located on a side of a portion of the first sub-metal layer away from the substrate and in contact with the first sub-metal layer;
[0018] The first metal structure layer includes: multiple first-type signal lines and multiple second-type signal lines; the minimum line width of the first-type signal lines is smaller than the minimum line width of the second-type signal lines; the first-type signal lines include: the first sub-metal layer; the second-type signal lines include: the first sub-metal layer and the second sub-metal layer.
[0019] In a possible implementation, the peripheral area includes: a binding area located at one side of the display area;
[0020] The first type of signal lines include: gate lines and third signal lines; the gate lines are located in the display area, and the third signal lines are located in the binding area; the second type of signal lines are located in the peripheral areas other than the binding area.
[0021] In a possible implementation manner, the first sub-metal layer includes copper; and the second sub-metal layer includes a stacked structure of molybdenum / titanium / nickel.
[0022] In a possible implementation manner, the first electrode is a pixel electrode; and the array substrate further includes a common electrode layer located on a side of the first conductive layer facing the substrate.
[0023] An embodiment of the present invention further provides a display panel, comprising the array substrate provided by the embodiment of the present invention, and further comprising: an opposite substrate arranged opposite to the array substrate.
[0024] The embodiment of the present invention further provides a method for manufacturing the array substrate provided by the embodiment of the present invention, the manufacturing method comprising:
[0025] providing a substrate;
[0026] A first conductive layer including a plurality of first electrodes and a plurality of switching electrodes is formed on one side of the substrate, and the maximum thickness of the first electrodes is smaller than the maximum thickness of the switching electrodes.
[0027] In a possible implementation manner, forming a first conductive layer including a plurality of first electrodes and a plurality of switching electrodes on one side of the substrate includes:
[0028] forming a first conductive film on one side of the substrate;
[0029] Coating photoresist, and exposing the display area by a marking machine or an auxiliary exposure device, and after development, etching, and stripping, only the first conductive film in the peripheral area is retained;
[0030] A second conductive film is formed, and the second conductive film and the first conductive film in the peripheral area are patterned together to form the first electrode in the display area and the switching electrode in the peripheral area.
[0031] In a possible implementation manner, forming a first conductive layer including a plurality of first electrodes and a plurality of switching electrodes on one side of the substrate includes:
[0032] forming a third conductive film on one side of the substrate;
[0033] Coating photoresist, and exposing the display area by a marking machine or an auxiliary exposure device, and after development, only retaining the photoresist in the peripheral area;
[0034] Controlling etching time to thin the third conductive film in the display area;
[0035] The photoresist is stripped off, and the third conductive film is patterned to form the first electrode located in the display area and the switching electrode located in the peripheral area.
[0036] In a possible implementation manner, forming a first conductive layer including a plurality of first electrodes and a plurality of switching electrodes on one side of the substrate includes:
[0037] forming a fourth conductive film on one side of the substrate;
[0038] Coating photoresist, using a half-tone mask in the display area and a full-tone mask in the peripheral area, so that the thickness of the photoresist in the peripheral area is greater than the thickness of the photoresist in the display area;
[0039] Under the shielding of the photoresist, the fourth conductive film is patterned to form the first electrode located in the display area and the switching electrode located in the peripheral area.
[0040] The beneficial effects of the embodiments of the present invention are as follows: In the embodiments of the present invention, by making the thickness of the first electrode of the first conductive layer in the display area smaller, the high-temperature afterimage problem in the display area can be improved, while the thickness of the transfer electrode in the peripheral area is larger, which can reduce the risk of breakage of the transfer electrode at the peripheral via climbing point, thereby improving the reliability, yield and process stability in the peripheral area. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1A This is a picture of the burnt part of the adapter hole;
[0042] Figure 1B Schematic diagram of MTD process to reduce gate line width and MTD peeling;
[0043] Figure 2 One of the cross-sectional structural schematic diagrams of an array substrate provided in an embodiment of the present invention;
[0044] Figure 3 A partial schematic diagram of an array substrate provided by an embodiment of the present invention;
[0045] Figure 4 A second schematic diagram of a cross-sectional structure of an array substrate provided in an embodiment of the present invention;
[0046] Figure 5A schematic top view of an array substrate provided by an embodiment of the present invention;
[0047] Figure 6 A schematic diagram of the manufacturing process of an array substrate provided in an embodiment of the present invention;
[0048] Fig. 7A This is a schematic diagram of a marking machine or an auxiliary exposure device after exposure and development for the first time according to an embodiment of the present invention;
[0049] Figure 7B This is a schematic diagram of the display area and the binding area after etching according to an embodiment of the present invention;
[0050] Figure 7C A schematic diagram of a film layer after a gate line layer is formed according to an embodiment of the present invention;
[0051] Fig.7D This is a schematic diagram of a second marking machine or auxiliary exposure equipment after exposure and development according to an embodiment of the present invention;
[0052] Fig. 7E This is a schematic diagram of the first conductive layer after etching and photoresist stripping according to an embodiment of the present invention;
[0053] Figure 7F This is one of the schematic diagrams of the final array substrate of an embodiment of the present invention;
[0054] Fig. 8A This is a schematic diagram of etching a portion of the first conductive film in the display area according to an embodiment of the present invention;
[0055] Figure 8B This is the second schematic diagram of the final array substrate according to the embodiment of the present invention;
[0056] Fig.9A This is a schematic diagram of an array substrate of a first conductive layer after gray tone masking according to an embodiment of the present invention;
[0057] Fig. 9B This is the third schematic diagram of the final array substrate according to an embodiment of the present invention. DETAILED DESCRIPTION
[0058] In order to make the purpose, technical solution and advantages of the embodiments of the present disclosure clearer, the technical solution of the embodiments of the present disclosure will be clearly and completely described below in conjunction with the drawings of the embodiments of the present disclosure. Obviously, the described embodiments are part of the embodiments of the present disclosure, not all of the embodiments. Based on the described embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present disclosure.
[0059] Unless otherwise defined, the technical terms or scientific terms used in the present disclosure should be understood by people with ordinary skills in the field to which the present disclosure belongs. The "first", "second" and similar words used in the present disclosure do not indicate any order, quantity or importance, but are only used to distinguish different components. "Include" or "comprise" and similar words mean that the elements or objects appearing before the word cover the elements or objects listed after the word and their equivalents, without excluding other elements or objects. "Connect" or "connected" and similar words are not limited to physical or mechanical connections, but can include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.
[0060] As used herein, "approximately" or "substantially the same" includes the stated value and means within an acceptable range of deviation for the particular value as determined by one of ordinary skill in the art taking into account the measurement in question and the errors associated with the measurement of the particular quantity (i.e., the limitations of the measurement system). For example, "substantially the same" may mean that the difference relative to the stated value is within one or more standard deviations, or within ±30%, 20%, 10%, 5%.
[0061] In the accompanying drawings, the thickness of layers, films, panels, regions, etc., is exaggerated for clarity. Exemplary embodiments are described herein with reference to cross-sectional views as schematic diagrams of idealized embodiments. In this way, deviations from the shapes of the figures as a result of, for example, manufacturing techniques and / or tolerances will be expected. Thus, the embodiments described herein should not be interpreted as being limited to the specific shapes of the regions as shown herein, but include deviations in shape caused by, for example, manufacturing. For example, a region illustrated or described as flat may typically have rough and / or nonlinear features. In addition, the illustrated sharp corners may be rounded. Thus, the regions shown in the figures are schematic in nature, and their shapes are not intended to illustrate the precise shapes of the regions, and are not intended to limit the scope of the claims.
[0062] In order to keep the following description of the embodiments of the present disclosure clear and concise, the present disclosure omits detailed descriptions of well-known functions and well-known components.
[0063] See also Figure 2 , an embodiment of the present invention provides an array substrate having a display area AA and a peripheral area BB located outside the display area AA, the array substrate comprising: a substrate 1, a first conductive layer 2 located on one side of the substrate 1;
[0064] The first conductive layer 2 includes: a plurality of first electrodes 21 and a plurality of switching electrodes 22; the first electrodes 21 are located in the display area AA, and the switching electrodes 22 are located in the peripheral area BB; in a direction perpendicular to the substrate 1, the maximum thickness h1 of the first electrodes 21 is less than the maximum thickness h2 of the switching electrodes 22. Optionally, the first conductive layer 2 may be a pixel electrode layer; the first electrodes 21 may be pixel electrodes.
[0065] Actual product and technology development has verified that the thinning of the first conductive layer (for example, the material of the first conductive layer is indium tin oxide (ITO)) has a clear effect of improving the contrast and high temperature afterimage of the display panel. Thinning to The contrast ratio is increased by 40; for example, the thickness of the first conductive layer (such as the material is indium tin oxide) is Thinning to The contrast ratio can be improved by 63. The mechanism is speculated to be that reducing the thickness of the first conductive layer can reduce the impact of the overall unevenness of the first conductive layer on the upper film layer (for example, the alignment film layer) (that is, because the first conductive layer is a patterned film layer, some areas have patterns, and some areas do not have patterns, which will make the first conductive layer as a whole have an uneven structure, and a thinner first conductive layer will reduce the impact of unevenness on the upper alignment film layer), thereby reducing the proportion of weak areas of friction (Rubbing) of the upper alignment film layer. However, the thinning of the first conductive layer will lead to an increase in the square resistance (especially P-ITO). The thickness of the first conductive layer (such as the material is indium tin oxide) is increased by Reduce to After annealing, the sheet resistance increases 2 to 3 times.
[0066] In the peripheral area of the display panel, especially the clock signal line (CLK line) and the frame start signal line (STV line) of the gate drive circuit GOA, the current is relatively large. Due to wiring requirements, some signal lines need to pass through the switching electrode on the same layer as the first electrode at some positions and change layers through the switching hole (for example, Figure 3 As shown, on the input side of the gate drive circuit GOA, the clock signal line CLK needs to be switched to the adapter line Z to provide a signal for the gate drive circuit GOA). The adapter electrode will be thinner at the climbing part of the adapter hole. Under the action of large current, the adapter electrode at the adapter hole is prone to burning and corrosion. In harsh environments such as high temperature and high humidity, it causes problems such as reliability and yield (such as Figure 1AAs shown in the figure). In addition, the ITO film on the tray surface of the magnetron sputtering equipment absorbs water vapor, which will affect the resistance. As the tray service life increases, the resistance effect becomes more significant. After the first conductive layer is thinned, the film thickness of the first conductive layer and other process fluctuations have a more obvious impact on the product. Therefore, in order to improve contrast and high-temperature afterimages, reliability, yield and process stability have become issues that need to be addressed.
[0067] In the embodiment of the present invention, by making the thickness of the first electrode 21 of the first conductive layer 2 in the display area AA smaller, the high-temperature afterimage problem in the display area AA can be improved, while the thickness of the transfer electrode 22 in the peripheral area BB is larger, which can reduce the risk of disconnection of the transfer electrode 22 at the peripheral via climbing point, thereby improving the reliability, yield and process stability in the peripheral area.
[0068] In a possible implementation, the array substrate may further include an alignment film layer located on a side of the first conductive layer 2 facing away from the substrate 1 and in contact with the first conductive layer 2 .
[0069] In one possible implementation, see Figure 2 As shown, at the edge region of the peripheral area BB, in a direction perpendicular to the substrate 1 , the thickness h21 of the switching electrode 22 in a portion of the edge region is smaller than the thickness h22 in the middle region.
[0070] In a specific implementation, when the thickness h21 of the switching electrode 22 in a portion of the edge region is smaller than the thickness h22 in the middle region, the maximum thickness h2 of the switching electrode 22 may be the thickness h22 in the middle region.
[0071] In one possible implementation, see Figure 4 As shown, at the edge region of the peripheral area BB, in the direction perpendicular to the substrate 1 , the thickness h21 of the switching electrode 22 in a portion of the edge region may also be equal to the thickness h22 in the middle region.
[0072] In one possible implementation, see Figure 2 or Figure 4 As shown, the array substrate also includes: a plurality of first signal lines L1, a plurality of second signal lines L2, and a plurality of first via holes K1 located between the substrate 1 and the switching electrode 22; the first signal line L1 is electrically connected to the second signal line L2 at the first via hole K1 through the switching electrode 22; the orthographic projection of the switching electrode 22 on the substrate 1 covers the orthographic projection of the first via hole K1 on the substrate 1.
[0073] In a possible implementation, the first signal line L1 and the second signal line L2 are located in different layers. In a possible implementation, the first signal line L1 can be in the same layer as the gate line, and the second signal line L2 can be in the same layer as the data line; in another possible implementation, the first signal line L1 can be in the same layer as the data line, and the second signal line L2 can be in the same layer as the gate line.
[0074] In a possible implementation, the first signal line L1 includes: an initial signal line STV, a clock signal line CLK, a high-level signal line VGH, or a low-level signal line VGL; the second signal line L2 includes: a transfer line; that is, the initial signal line STV, the clock signal line CLK, the high-level signal line VGH, or the low-level signal line VGL are electrically connected to the transfer line through the transfer electrode 22, and optionally, the initial signal line STV, the clock signal line CLK, the high-level signal line VGH, or the low-level signal line VGL provide a signal to the gate drive circuit GOA through the transfer line. Optionally, the transfer line may include multiple transfer lines, and the initial signal line STV, the clock signal line CLK, the high-level signal line VGH, or the low-level signal line VGL respectively correspond to different transfer lines; optionally, the extension direction of the first signal line L1 and the second signal line L2 are different, for example, the extension direction of the first signal line L1 and the second signal line L2 can be perpendicular, for example, as Figure 3 As shown, the first signal line L1 includes a clock signal line CLK, the second signal line L2 includes a switching line Z, and the clock signal line CLK and the switching line Z are perpendicular to each other in their extending directions.
[0075] In a possible implementation, the first signal line L1 includes: a gate output signal lead; the second signal line includes: a gate line. That is, the gate output signal lead is electrically connected to the gate line through a transfer electrode. Optionally, the gate drive circuit GOA can transmit the signal to the gate line through the gate output signal line lead. Optionally, the gate output signal lead and the gate line can have the same extension direction, and the two can be located in different layers. Optionally, for example, the gate output signal line lead can be in the same layer as the data line.
[0076] In a possible implementation, the first signal line L1 includes: a plurality of common electrode lines; the second signal line L2 includes: a ground line or a plurality of short-circuit loops. Optionally, the common electrode lines are electrically connected to the ground lines or short-circuit loops at some locations through transfer electrodes to achieve static discharge and provide static protection for the display panel.
[0077] It should be noted that the above is only a specific example of the types of the first signal line L1 and the second signal line L2. In specific implementation, in the embodiment of the present invention, the first signal line L1 may also include other routings besides the routings described above, and the second signal line L2 may also include other routings besides the routings described above. The embodiment of the present invention is not limited to this.
[0078] In one possible implementation, see Figure 2 or Figure 4 As shown, there is a first insulating layer F1 between the first signal line L1 and the switching electrode 22, there is a second insulating layer F2 between the second signal line L2 and the switching electrode 22, the first insulating layer F1 has a first sub-via K11, and the second insulating layer F2 has a second sub-via K12; part of the switching electrode 22 is electrically connected to the first signal line L1 through the first sub-via K11, and part of it is electrically connected to the second signal line L2 through the second sub-via K12; the first via K1 includes a first sub-via K11 and a second sub-via K12.
[0079] In one possible implementation, combining Figure 2 or Figure 4 As shown, the first insulating layer F1 may include a second insulating layer F2; optionally, the first insulating layer F1 may include: a gate insulating layer 91, and a passivation layer 92 located on a side of the gate insulating layer 91 away from the substrate 1; the second insulating layer F2 may include only the passivation layer 92.
[0080] In a possible implementation manner, the orthographic projection of the first sub-via K11 on the substrate 1 does not overlap with the orthographic projection of the second sub-via K12 on the substrate 1; in a possible implementation manner, Figure 2 or Figure 4 As shown, in the direction perpendicular to the substrate 1 , the depth of the first sub-via hole K11 may be greater than the depth d3 of the second sub-via hole K12 .
[0081] In one possible implementation, see Figure 2 or Figure 4 As shown, the array substrate also includes: a plurality of transistors T located in the display area AA, and a plurality of second via holes K2; the transistor T includes: a first electrode 61, and a second electrode 62; optionally, the first electrode 61 may be a source electrode, and the second electrode 62 may be a drain electrode; the first electrode 21 is electrically connected to the second electrode 62 through the second via hole K2; in a direction perpendicular to the substrate 1, a depth d1 of the first sub-via hole K11 is greater than a depth d2 of the second via hole K2.
[0082] In the embodiment of the present invention, in the display area AA, although a plurality of via holes (such as the second via hole K2) are also provided, the first electrode 21 also has a slope at the second via hole K2, but since the depth of the second via hole K2 is relatively small, compared with the first via hole K1 with a deeper portion in the non-display area BB, the risk of the first electrode 21 breaking when climbing at the second via hole K2 is relatively low. Therefore, the first electrode 21 in the display area AA can be made thinner to improve the high-temperature afterimage problem in the display area AA.
[0083] In one possible implementation, see Figure 2 or Figure 4 As shown, in the direction perpendicular to the substrate 1, the maximum thickness h1 of the first electrode 21 is one quarter to three quarters of the maximum thickness of the switching electrode h2. In a possible implementation, in the direction perpendicular to the substrate 1, the maximum thickness h1 of the first electrode 21 is one half of the maximum thickness of the switching electrode h2.
[0084] For large-size display panels, the gate layer is often made of thick copper, but copper is easily corroded, and stubborn problems such as gate line breakage (Gate Open, GO) and via corrosion may occur. Optionally, the gate layer (Gate layer) is a two-layer structure of MoNb / Cu. In order to improve copper corrosion and bubble defects and increase reliability life, an alloy layer (for example, Mo / Ti / Ni, MTD alloy layer, and other alloy layers such as Mo / Ti) is optionally added above the copper layer. The MTD alloy layer has good corrosion resistance and oxidation resistance. However, the metal surface energy of the MTD alloy layer is relatively large, and the contact angle with the photoresist is reduced. In thick copper, especially in the half-tone mask process, the MTD alloy layer may be drilled or peeled, resulting in line narrowing (Line small) or even line breakage (Line Open) phenomenon, such as Figure 1B Moreover, in the display area AA, the line width of the gate line at the position where it overlaps with the data line is generally 6μm to 7μm. In addition, the wiring of the gate line layer in the fan-out area and the bonding area (COF Bonding) is also narrow (except for the fanout area and COF Bonding, the line width of the gate line layer in other peripheral areas is generally >30μm (which can be compensated by design)), and the setting of the MTD alloy layer will further increase the line width of this part of the wiring, and the risk of wire breakage will be further increased. Based on this, in an embodiment of the present invention, the array substrate includes: a first metal structure layer M1 located between the substrate 1 and the transfer electrode 22; the first metal structure layer M includes: a first sub-metal layer M01, and a second sub-metal layer M02 located on a side of the first sub-metal layer M01 away from the substrate 1 and in contact with the first sub-metal layer M01; the first metal structure layer M includes: a plurality of first-class signal lines, and a plurality of second-class signal lines; the minimum line width of the first-class signal line is less than the minimum line width of the second-class signal line; the first-class signal line includes: a first sub-metal layer M01; the second-class signal line includes: a first sub-metal layer M01 and a second sub-metal layer M02. Optionally, the first metal structure layer M1 can be a gate line layer. Optionally, the first sub-metal layer M01 includes: copper; the second sub-metal layer M02 includes a stacked molybdenum / titanium / nickel (i.e., an MTD alloy layer).
[0085] In an embodiment of the present invention, the first-category signal line with a smaller line width is made to include only the first sub-metal layer M01, and the second-category signal line with a larger line width is made to include: the first sub-metal layer M01 and the second sub-metal layer M02, thereby avoiding the risk of the first-category signal line being further narrowed and the occurrence of line breakage due to the provision of the second sub-metal layer M02. As for the second-category signal line with a larger line width, the second sub-metal layer M02 is provided, and the good corrosion resistance and oxidation resistance of the second sub-metal layer M02 are utilized to improve the corrosion / bubble problem of the first sub-metal layer M01 and enhance the reliability life.
[0086] In a possible implementation, the peripheral area BB includes: a binding area BB1 located on one side of the display area AA; optionally, the binding area BB1 may include a plurality of binding terminals; the first type of signal line includes: a gate line 3, and a third signal line 4; the gate line 3 is located in the display area AA, and the third signal line 4 is located in the binding area BB1; optionally, the third signal line 4 may be a routing line in a fan-shaped area; the second type of signal line is located in other peripheral areas BB except the binding area BB1, for example, Figure 5 As shown, if the binding area BB1 is located at the lower side of the display area AA, the second type signal lines can be located in the binding opposite side area on the upper side of the display area AA, and in the peripheral area on the left or right side of the display area AA.
[0087] In one possible implementation, see Figure 2 As shown, the first electrode 21 is a pixel electrode; the array substrate further includes a common electrode layer 5 located on the side of the first conductive layer 2 facing the substrate 1. That is, the display panel provided in the embodiment of the present invention can be a display panel in the ADS mode.
[0088] Based on the same inventive concept, an embodiment of the present invention further provides a display panel, including the array substrate provided by the embodiment of the present invention, and further including: an opposite substrate arranged opposite to the array substrate.
[0089] In a possible implementation, the display panel further includes a liquid crystal layer located between the array substrate and the opposite substrate. Optionally, the liquid crystal in the liquid crystal layer is negative liquid crystal.
[0090] In a possible implementation manner, the display panel provided by the embodiment of the present invention is a display panel in an ADS display mode.
[0091] In a possible implementation manner, the display panel provided by the embodiment of the present invention is a large-size display panel, wherein the gate line material includes copper, wherein the thickness of the copper is in the range of
[0092] Based on the same inventive concept, the embodiment of the present invention further provides a method for manufacturing an array substrate as provided in the embodiment of the present invention, see Figure 6 As shown, the production method includes:
[0093] Step S100, providing a substrate;
[0094] Step S200: forming a first conductive layer including a plurality of first electrodes and a plurality of switching electrodes on one side of the substrate, and making the maximum thickness of the first electrodes smaller than the maximum thickness of the switching electrodes.
[0095] In a possible implementation, regarding step S200, forming a first conductive layer including a plurality of first electrodes and a plurality of transfer electrodes on one side of the substrate includes:
[0096] A first conductive film is formed on one side of the substrate; optionally, a first conductive film may be deposited by magnetron sputtering. The first conductive film (the material may be indium tin oxide); specifically, before forming the first conductive film on one side of the substrate, a common electrode layer 5 (VA and IPS modes do not need to be deposited), a first sub-metal layer M01 (which may be a copper layer), and a second sub-metal layer M02 (which may be an MTD alloy layer) may be deposited on the substrate 1; wherein, optionally, the thickness range of the common electrode layer 5 may be The thickness of the Cu layer can range from The thickness of the MTD alloy layer can range from Then, photoresist coating is performed, and the thickness range can be about 1.0μm to 2.2μm (the thickness of each film layer here is not limited to the range in the text, such as the thickness of photoresist, which can be above 1.0μm in mass production, and there will be coating problems below 1.0μm). No mask is required, and a marking machine (Titler) or auxiliary exposure (Lex-I) is used to expose the display AA area and the binding area BB1. After development, Fig. 7A After that, the etching time is controlled to etch the second sub-metal layer M02 (which may be an MTD alloy layer) showing the AA region and the binding region BB1, and the photoresist is stripped to obtain the following Figure 7B Then, the mask (HGA Mask), the first sub-metal layer M01 (which can be a copper layer) etching, the common electrode layer 5 etching, ashing (HGA Ashing), the second sub-metal layer M02 (which can be an MTD alloy layer) etching and Gate STR are sequentially performed, and the following is obtained after Gate STR Figure 7C The film layer structure shown shows that there is no MTD alloy layer in the AA area and the binding area BB1, avoiding the Line Small and Line Open problems, and other surrounding areas contain MTD alloy layers; then, the normal data line layer and via process;
[0097] The photoresist is coated, and the display area is exposed by a marking machine or an auxiliary exposure device, and after development, etching, and stripping, only the first conductive film in the peripheral area is retained; the photoresist is normally coated, and the display area AA is exposed by a marking machine (Titler) or an auxiliary exposure (Lex-I device) without an exposure machine. After development, the display area AA is not covered by the photoresist, and the peripheral area is covered by the photoresist, such as Fig.7D As shown; after the first conductive film etching, photoresist stripping and other processes, the display area AA is not covered by the first conductive film, and the peripheral area is completely covered with the first conductive film;
[0098] A second conductive film is formed, and the second conductive film and the first conductive film in the peripheral area are patterned together to form a first electrode located in the display area and a switching electrode located in the peripheral area. Specifically, the second conductive film can be deposited in sequence (the material can be indium tin oxide, and the thickness can be ), coating, exposure, development, etching, photoresist stripping, annealing and other processes, and finally completing all the processes of the array substrate, forming a difference in thickness of the first electrode 21 in the display area AA and the thickness of the transfer electrode 22 in the peripheral area BB. Fig. 7E and Figure 7F shown.
[0099] In the embodiment of the present invention, no new mask plate is required, and it is compatible with existing products. The width range of the peripheral area of conventional products is 6mm to 8mm, and that of narrow-frame products is 4.5mm to 5.5mm. The accuracy, repeatability and stability of the Titler exposure equipment can meet the requirements. Optionally, the power of the light-emitting diode (LED) lamp is divided into 256 segments, each segment corresponds to an independently controlled small LED lamp, and the regional exposure is achieved by controlling the power of the LED lamps at various locations, and the illumination range is 10mj to 30mj. The exposure boundary is located at the center of the auxiliary pixel (Dummy Pixel) of the peripheral area BB (including the left side GL of the gate drive circuit, the right side GR of the gate drive circuit, the binding side DP, and the binding opposite side DPO). The number of Dummy Pixels is generally 0.5 to 1, which can ensure exposure accuracy; the film thickness position of the first conductive layer includes all peripheral vias, such as GOA signal line transfer holes, CLK transfer holes, Fanout transfer holes and other holes; the location of the MTD alloy layer does not include the binding area BB1.
[0100] In a possible implementation, regarding step S200, forming a first conductive layer including a plurality of first electrodes and a plurality of transfer electrodes on one side of the substrate includes:
[0101] forming a third conductive film on one side of the substrate;
[0102] Applying photoresist, and exposing the display area through a marking machine or an auxiliary exposure device, and after development, only the photoresist in the peripheral area is retained;
[0103] Controlling the etching time to reduce the thickness of the third conductive film in the display area;
[0104] The photoresist is stripped off, and the third conductive film is patterned to form a first electrode located in the display area and a switching electrode located in the peripheral area.
[0105] In the embodiment of the present invention, similar to Figure 7A-7F In the scheme shown, after the array substrate completes the Via photoresist stripping, magnetron sputtering is used to deposit ≥ The third conductive film (material can be indium oxide) is normally coated with photoresist, and the display area AA is exposed using a marking machine (Titler) or auxiliary exposure equipment without passing through an exposure machine (same as Figure 7A-7F As shown in the scheme), after development, the display area AA is not covered with photoresist, and the peripheral area BB is covered with photoresist (as shown in the scheme Fig. 8A As shown). Control the etching time of the third conductive film, and partially etch the third conductive film in the display area AA, and the remaining After the photoresist is stripped, the normal third conductive film coating, exposure, etching, stripping, annealing and other processes are directly carried out to finally form an array substrate. Figure 8B shown.
[0106] In a possible implementation, regarding step S200, forming a first conductive layer including a plurality of first electrodes and a plurality of transfer electrodes on one side of the substrate includes:
[0107] forming a fourth conductive film on one side of the substrate;
[0108] Coating photoresist, using a half-tone mask in the display area and a full-tone mask in the peripheral area, so that the thickness of the photoresist in the peripheral area is greater than the thickness of the photoresist in the display area;
[0109] Under the shielding of the photoresist, the fourth conductive film is patterned to form a first electrode located in the display area and a switching electrode located in the peripheral area.
[0110] In the embodiment of the present invention, similar to Figure 8A-8B In the scheme shown, after the array substrate completes the Via photoresist stripping, magnetron sputtering is used to deposit ≥ A fourth conductive film (the material may be indium tin oxide) is formed, and then a gray tone mask (HalfTone Mask) is used, that is, the first electrode (pixel electrode) of the display area AA adopts Halftone, and the via hole of the peripheral area BB adopts Full tone; the thickness of the photoresist film at the first electrode (pixel electrode) of the display area AA is about Afterwards, the fourth conductive film etching is performed to etch the area not covered by the photoresist, such as Fig.9A As shown, then, the photoresist on 2ITO Line is ashed by dry etching, and the photoresist PR in the peripheral area BB is still retained, and then the etching time is controlled to ensure that the remaining film thickness of the fourth conductive film of display AA is The fourth conductive film of the peripheral area BB ≥ Finally, the desired array substrate is obtained, such as Fig. 9B shown.
[0111] The beneficial effects of the embodiments of the present invention are as follows: In the embodiments of the present invention, by making the thickness of the first electrode 21 of the first conductive layer 2 in the display area AA smaller, the high-temperature afterimage problem in the display area AA can be improved, and the thickness of the transfer electrode 22 in the peripheral area BB is larger, which can reduce the risk of disconnection of the transfer electrode 22 at the peripheral via climbing, thereby improving the reliability, yield and process stability in the peripheral area.
[0112] Based on the same inventive concept, the embodiment of the present disclosure further provides a display device, including the above display panel provided by the embodiment of the present disclosure. The implementation of the display device can refer to the embodiment of the above display panel, and the repeated parts will not be repeated.
[0113] In specific implementation, in the embodiments of the present disclosure, the display device may be any product or component with a display function, such as a mobile phone, a tablet computer, a television, a monitor, a laptop computer, a digital photo frame, a navigator, etc. Other essential components of the display device are well understood by those skilled in the art, and are not described in detail here, nor should they be used as limitations to the present disclosure.
[0114] Although the preferred embodiments of the present disclosure have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications falling within the scope of the present disclosure.
[0115] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. An array substrate, comprising a display area and a peripheral area located outside the display area, characterized in that: The array substrate comprises: a substrate, a first conductive layer located on one side of the substrate; The first conductive layer includes: a plurality of first electrodes and a plurality of switching electrodes; the first electrodes are located in the display area, and the switching electrodes are located in the peripheral area; in a direction perpendicular to the substrate, a maximum thickness of the first electrodes is smaller than a maximum thickness of the switching electrodes.
2. The array substrate according to claim 1, characterized in that: At the edge region of the peripheral area, in a direction perpendicular to the substrate, the thickness of the switching electrode in a portion of the edge region is smaller than the thickness in the middle region.
3. The array substrate according to claim 1, characterized in that: The array substrate further includes: a plurality of first signal lines, a plurality of second signal lines, and a plurality of first via holes located between the substrate and the switching electrode; the first signal lines are electrically connected to the second signal lines at the first via holes through the switching electrodes; The orthographic projection of the switching electrode on the substrate covers the orthographic projection of the first via hole on the substrate.
4. The array substrate according to claim 3, characterized in that: A first insulating layer is provided between the first signal line and the switching electrode, a second insulating layer is provided between the second signal line and the switching electrode, the first insulating layer has a first sub-via, and the second insulating layer has a second sub-via; The switching electrode is partially electrically connected to the first signal line through the first sub-via, and partially electrically connected to the second signal line through the second sub-via; the first via includes the first sub-via and the second sub-via.
5. The array substrate according to claim 4, characterized in that: The array substrate further comprises: a plurality of transistors located in the display area, and a plurality of second via holes; the transistors comprise: a first electrode and a second electrode; the first electrode is electrically connected to the second electrode through the second via hole; In a direction perpendicular to the substrate, a depth of the first sub-via hole is greater than a depth of the second via hole.
6. The array substrate according to claim 3, characterized in that: The first signal line includes: an initial signal line, a clock signal line, a high level signal line, or a low level signal line; the second signal line includes: a transfer line; Alternatively, the first signal line includes: a gate output signal lead; the second signal line includes: a gate line; Alternatively, the first signal line includes: a plurality of common electrode wirings; the second signal line includes: a ground line or a plurality of short-circuit loop lines.
7. The array substrate according to claim 1, wherein: In a direction perpendicular to the substrate, the maximum thickness of the first electrode is one quarter to three quarters of the maximum thickness of the switching electrode.
8. The array substrate according to any one of claims 1 to 7, characterized in that: The array substrate comprises: a first metal structure layer located between the substrate and the transfer electrode; the first metal structure layer comprises: a first sub-metal layer, and a second sub-metal layer located on a side of a portion of the first sub-metal layer away from the substrate and in contact with the first sub-metal layer; The first metal structure layer includes: multiple first-type signal lines and multiple second-type signal lines; the minimum line width of the first-type signal lines is smaller than the minimum line width of the second-type signal lines; the first-type signal lines include: the first sub-metal layer; the second-type signal lines include: the first sub-metal layer and the second sub-metal layer.
9. The array substrate according to claim 8, characterized in that: The peripheral area includes: a binding area located on one side of the display area; The first type of signal lines include: gate lines and third signal lines; the gate lines are located in the display area, and the third signal lines are located in the binding area; the second type of signal lines are located in the peripheral areas other than the binding area.
10. The array substrate according to claim 8, characterized in that: The first sub-metal layer includes copper; the second sub-metal layer includes molybdenum / titanium / nickel in a stacked arrangement.
11. The array substrate according to claim 1, characterized in that: The first electrode is a pixel electrode; the array substrate further comprises a common electrode layer located on a side of the first conductive layer facing the substrate.
12. A display panel, characterized in that: It comprises the array substrate as claimed in any one of claims 1 to 11, and further comprises: an opposite substrate arranged opposite to the array substrate.
13. A method for manufacturing an array substrate according to any one of claims 1 to 11, characterized in that: The production method comprises: providing a substrate; A first conductive layer including a plurality of first electrodes and a plurality of switching electrodes is formed on one side of the substrate, and the maximum thickness of the first electrodes is smaller than the maximum thickness of the switching electrodes.
14. The method according to claim 13, characterized in that: The first conductive layer including a plurality of first electrodes and a plurality of transfer electrodes is formed on one side of the substrate, comprising: forming a first conductive film on one side of the substrate; Coating photoresist, and exposing the display area by a marking machine or an auxiliary exposure device, and after development, etching, and stripping, only the first conductive film in the peripheral area is retained; A second conductive film is formed, and the second conductive film and the first conductive film in the peripheral area are patterned together to form the first electrode in the display area and the switching electrode in the peripheral area.
15. The method according to claim 13, characterized in that: The first conductive layer including a plurality of first electrodes and a plurality of transfer electrodes is formed on one side of the substrate, comprising: forming a third conductive film on one side of the substrate; Coating photoresist, and exposing the display area by a marking machine or an auxiliary exposure device, and after development, only retaining the photoresist in the peripheral area; Controlling etching time to thin the third conductive film in the display area; The photoresist is stripped off, and the third conductive film is patterned to form the first electrode located in the display area and the switching electrode located in the peripheral area.
16. The method according to claim 13, characterized in that: The first conductive layer including a plurality of first electrodes and a plurality of transfer electrodes is formed on one side of the substrate, comprising: forming a fourth conductive film on one side of the substrate; Coating photoresist, using a half-tone mask in the display area and a full-tone mask in the peripheral area, so that the thickness of the photoresist in the peripheral area is greater than the thickness of the photoresist in the display area; Under the shielding of the photoresist, the fourth conductive film is patterned to form the first electrode located in the display area and the switching electrode located in the peripheral area.