Improved IBC solar cell and preparation method thereof
By preparing boron-doped floating junction FFE layer, back tunneling oxide layer and doped amorphous silicon layer in IBC crystalline silicon solar cells, the problem of insufficient back carrier collection performance is solved, and the short-circuit current density and open circuit are improved Voltage improves the conversion efficiency of solar cells.
Patent Information
- Application Number
- CN202411007182.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-08
AI Technical Summary
The carrier collection performance of existing IBC crystal silicon solar cells on the back p+ emitter and n+ back surface field is poor, resulting in carrier recombination loss and affecting the short-circuit current density and conversion efficiency.
The boron-doped floating junction FFE layer was prepared on the front surface of the IBC crystalline silicon solar cell, and the carriers were pumped to the back p+ and n+ regions using the voltage gradient pumping effect of the FFE layer, combining the back tunneling oxide layer and doped amorphous Silicon layer, enhancing carrier collection capability.
The short-circuit current density and open-circuit voltage of IBC solar cells are improved, the conversion efficiency is improved, the short-circuit current density is increased by 0.2~0.5mA/cm2, the open-circuit voltage is increased by 5~15mV, and the conversion efficiency is increased by 0.2~0.4%.
Smart Images

Figure CN118919595A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a technology in the field of crystalline silicon solar cells, in particular to an improved interdigitated back contact (IBC) solar cell and a preparation method thereof. Background Art
[0002] Finger-type back-contact crystalline silicon solar cells have a higher short-circuit current density potential because there is no metal electrode covering the front side. However, the back side of the current IBC crystalline silicon solar cell is distributed in a finger-type manner. + The emitter and n + The back surface field is not superior in terms of carrier collection, and there are also more carrier recombination losses in the contact area with the metal electrode. The existing all-aluminum passivated back contact solar cells only use tunneling oxide layers and doped polysilicon layers, which cannot solve the passivation problem on the back of IBC cells. Summary of the invention
[0003] In view of the above-mentioned deficiencies in the prior art, the present invention proposes an improved IBC solar cell and a preparation method thereof, wherein a boron-doped floating junction FFE layer is prepared on the front surface of the IBC crystalline silicon solar cell, and a pumping effect formed by voltage gradients in different regions of the FFE layer is used to pump carriers in the field region of the back surface of the cell to the emitter region over a long distance, thereby increasing the carrier transmission distance and allowing more photogenerated carriers to enter the back surface of the silicon wafer. + and n + The area is effectively collected to obtain a higher short-circuit current density, thereby improving the conversion efficiency of the solar cell.
[0004] The present invention is achieved through the following technical solutions:
[0005] The present invention relates to an improved IBC solar cell, comprising: an n-type crystalline silicon substrate, p-type crystalline silicon substrates arranged in sequence on the front surface of the substrate, + The floating junction FFE layer, the aluminum oxide passivation layer and the hydrogenated silicon nitride anti-reflection layer and the tunneling oxide layer, n + Amorphous silicon layer, n + Microcrystalline silicon layer, p + Amorphous silicon layer, p + Microcrystalline silicon layer, hydrogenated silicon nitride anti-reflection layer and metal electrode.
[0006] The n-type crystalline silicon substrate is an n-type Cz single crystal silicon wafer with a crystal orientation of (100).
[0007] The p + The boron doping concentration in the floating junction FFE layer is 5×10 18 ~1×10 20 cm -3 The doping junction depth is 0.5~1.5μm.
[0008] The p + Amorphous silicon layer and p + The boron doping concentration in the microcrystalline silicon layer is 1×10 19 ~2×10 20 cm -3 , with thicknesses of 5~50nm and 20~150nm respectively.
[0009] The n + Amorphous silicon layer and n + The phosphorus doping concentration in the microcrystalline silicon layer is 5×10 19 ~1×10 21 cm -3 , with thicknesses of 5~50nm and 20~150nm respectively.
[0010] The tunneling oxide layer is SiO 2 or Al 2 O 3 Structure, thickness is 1 to 2 nm.
[0011] The present invention relates to a method for preparing the above-mentioned improved IBC solar cell, comprising the following steps:
[0012] Step 1, preparing an industrial-grade n-type Cz single crystal silicon wafer with a crystal orientation of (100) as a crystalline silicon substrate, the thickness of the silicon wafer is 100-150 μm, and the resistivity is 0.5-2 Ω·cm; using a KOH solution to remove the damage layer on the surface of the crystalline silicon substrate caused by wire cutting;
[0013] Step 2, after texturing the n-type crystalline silicon substrate with a KOH solution, a pre-treated silicon wafer is obtained by standard RCA cleaning;
[0014] Step 3: Apply BCl to the front side of the silicon wafer 3 The p-type nanostructured ... + Floating knot FFE layer.
[0015] Step 4: After etching the edges of the silicon wafer obtained in step 3, the back surface of the silicon wafer is polished with a KOH solution, and a SiO2 layer with a thickness of 1 to 2 nm is obtained by high-temperature thermal oxidation technology, plasma enhanced chemical vapor deposition (PECVD) or atomic layer deposition (ALD). 2 Layer or Al 2 O 3 layer;
[0016] Step 5: insert the back side of the silicon wafer obtained in step 4 into the first mask, and deposit a p-type film with a thickness of 5 to 50 nm by PECVD. + Amorphous silicon, doping concentration 1×10 19 ~2×1020 cm -3 and p with a thickness of 20 to 150 nm + Microcrystalline silicon, doping concentration 1×10 19 ~2×10 20 cm -3 .
[0017] The sequential deposition means: firstly setting the power of the power supply to 3-5 kW, the deposition temperature to 150-250°C, the deposition pressure to 200-300 Pa, and introducing a mixed gas of silane, borane and hydrogen to deposit a p-type film with a thickness of 5-50 nm. + Amorphous silicon, the power supply is 7-10kW, the deposition temperature is 300-450℃, the deposition pressure is 300-400Pa, and a mixed gas of silane, borane and hydrogen is introduced to deposit a p-type silicon with a thickness of 20-150nm. + Microcrystalline silicon, doping concentration 1×10 19 ~2×10 20 cm -3 .
[0018] Step 6: Take out the first mask from the back of the silicon wafer obtained in step 5 and insert the second mask, and use PECVD to deposit n-type films with a thickness of 5 to 50 nm. + Amorphous silicon, doping concentration 5×10 19 ~1×10 21 cm -3 and a thickness of 20 to 150 nm + Microcrystalline silicon, doping concentration 5×10 19 ~1×10 21 cm -3 .
[0019] The holes of the mask are distributed in an interdigitated manner.
[0020] The sequential deposition means: firstly setting the power of the power supply to 3-5 kW, the deposition temperature to 150-250° C., the deposition pressure to 200-300 Pa, and introducing a mixed gas of silane, phosphine and hydrogen to deposit a layer of n-type nanoparticles with a thickness of 5-50 nm. + Amorphous silicon, doping concentration 5×10 19 ~1×10 21 cm -3 Then set the power supply to 7-10kW, the deposition temperature to 300-450°C, the deposition pressure to 300-400Pa, and introduce a mixed gas of silane, phosphine and hydrogen to deposit a thickness of 20-150nm. + Microcrystalline silicon, doping concentration 5×10 19 ~1×10 21 cm -3 .n +Amorphous silicon and n + Deposition principle of microcrystalline silicon and p + Same area.
[0021] When the deposition thickness is 5 to 50 nm, + When amorphous silicon is used, the flow rate ratio of phosphine gas in the mixed gas is 3-8%; when the deposition thickness is 20-150nm, the + In the case of microcrystalline silicon, the flow rate ratio of phosphine gas in the mixed gas is 1 to 4%.
[0022] Step 7: After removing the back borosilicate glass and phosphosilicate glass from the silicon wafer obtained in Steps 5 and 6 and cleaning it, SiN with a thickness of 80 to 100 nm is deposited in the corresponding area. x :H anti-reflection layer.
[0023] Step 8: After removing the borosilicate glass from the front side of the silicon wafer obtained in step 7 and cleaning it, an ALD device and a PECVD device are used to deposit an Al 2 O 3 Passivation layer and SiN with a thickness of 70-80nm x :H anti-reflection layer.
[0024] Step 9, using a screen printing method to print the back surface of the silicon wafer obtained in step 8 + and n + Ag / Al paste and Ag paste were printed in different regions respectively, and finally the metal electrodes were prepared by co-sintering in an infrared belt sintering furnace. Technical Effects
[0025] The present invention adds a low-cost tunneling oxide layer and a doped amorphous silicon layer with excellent interface passivation on the basis of the IBC solar cell, thereby enhancing the back surface p of the IBC solar cell. + and n + The region's ability to collect carriers can increase the open-circuit voltage of the IBC solar cell; a floating junction FFE layer is added to the front surface, and the pumping effect generated by the voltage gradient of different regions of the FFE layer is used to increase the transmission distance of carriers, thereby increasing the short-circuit current density of the IBC solar cell; compared with the prior art, the present invention increases the short-circuit current density of the IBC solar cell by 0.2-0.5 mA / cm through the floating junction FFE layer. 2 ; Based on the tunneling oxide layer on the back of the IBC solar cell, adding a doped amorphous silicon structure can increase the open circuit voltage of the cell by 5 to 15 mV; the superposition of the two technologies can increase the conversion efficiency of the IBC solar cell by 0.2 to 0.4%. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a schematic diagram of the silicon wafer after texturing;
[0027] Figure 2 Prepare floating junction FFE layer for the front surface, and cover the back surface with tunnel oxide layer, p + Amorphous silicon layer, p + Microcrystalline silicon layer, n + Amorphous silicon layer and n + Schematic diagram of silicon wafer with microcrystalline silicon layer;
[0028] Figure 3 This is a schematic diagram of the final high-efficiency IBC crystalline silicon solar cell structure of the present invention;
[0029] In the figure: 1-n-type crystalline silicon substrate, 2-p + Floating junction FFE layer, 3-tunneling oxide layer, 4-n + Amorphous silicon layer, 5-n + Microcrystalline silicon layer, 6-p + Amorphous silicon layer, 7-p + microcrystalline silicon layer, 8-aluminum oxide passivation layer, 9 and 10-hydrogenated silicon nitride antireflection layers, 11-metal electrode;
[0030] Figure 4 Schematic diagram for simulating and analyzing the effects of back surface field and back emitter width ratio on the performance of IBC solar cells;
[0031] In the picture: W n+ Refers to the back surface field width, W p+ Refers to the back emitter width. DETAILED DESCRIPTION
[0032] like Figure 3 As shown in the figure, this embodiment relates to an improved IBC solar cell comprising: an n-type crystalline silicon substrate 1, a p-type crystalline silicon substrate 2 formed on the front surface thereof, + Floating junction FFE layer 2, aluminum oxide passivation layer 8, hydrogenated silicon nitride anti-reflection layer 9; tunneling oxide layer 3, n + Amorphous silicon layer 4, n + Microcrystalline silicon layer 5, p + Amorphous silicon layer 6, p + Microcrystalline silicon layer 7, hydrogenated silicon nitride anti-reflection layer 10, and metal electrode 11.
[0033] This embodiment relates to the above-mentioned IBC solar cell preparation method, comprising:
[0034] Step 1, prepare an industrial-grade n-type Cz single crystal silicon wafer with a crystal orientation of (100) as a crystalline silicon substrate, the thickness of the silicon wafer is selected to be 130 μm, and the resistivity is 0.8 Ω·cm; use a KOH solution to remove the damage layer on the surface of the crystalline silicon substrate caused by wire cutting;
[0035] Step 2, texturing the n-type crystalline silicon substrate obtained in step 1 with a KOH mixed solution, wherein: the concentration of the KOH solution is 1-3%, and the concentration of the isopropanol solution is 2-10%, and then performing standard RCA cleaning to obtain a pre-treated silicon wafer;
[0036] Step 3: Place the silicon wafers obtained in step 2 back-to-back into a conventional high-temperature diffusion furnace for BCl 3 Diffusion, forming p on the front + The floating junction FFE layer, where the driving and oxidation temperatures are set to 900°C and 950°C respectively; the boron doping concentration of the FFE layer is 2×10 19 cm -3 , doping junction depth is 0.6μm.
[0037] Step 4: After the silicon wafer obtained in step 3 is etched around the edges, the back surface of the silicon wafer is polished with a 16% KOH solution, and then a SiO2 layer with a thickness of 1.5 nm covering the entire back surface is generated under high temperature hot oxygen conditions. 2 layer;
[0038] Step 5, insert the back side of the silicon wafer obtained in step 4 into the first mask, and use PECVD equipment to deposit a doped amorphous silicon layer, wherein the power supply power is 4kW, the deposition temperature is 200°C, and the deposition pressure is 250Pa; silane, borane and hydrogen gases are introduced, wherein the borane gas flow ratio is 3%, and a p-type silicon layer with a thickness of 10nm is deposited. + Amorphous silicon, doping concentration 5×10 19 cm -3 ; Then, the doped microcrystalline silicon layer was deposited by the same PECVD equipment, where the power supply was 8kW, the deposition temperature was 400°C, the deposition pressure was 350Pa, silane, borane and hydrogen gases were introduced, where the borane gas flow ratio was 1%, and the deposition thickness was 100nm. + Microcrystalline silicon, doping concentration 8×10 19 cm -3 .
[0039] Step 6: Take out the first mask from the back of the silicon wafer obtained in step 5 and insert the second mask. The holes of the two masks are distributed in an interdigitated manner. Use the same PECVD equipment as in step 5 to deposit the doped amorphous silicon layer. Pass silane, phosphine and hydrogen gases. The phosphine gas flow rate ratio is 5%. Deposit a 10nm thick n-type silicon layer. + Amorphous silicon, doping concentration 1×10 20 cm -3 Then, the doped microcrystalline silicon layer is deposited using the same PECVD equipment as in step 5, and silane, phosphine and hydrogen gases are introduced, wherein the phosphine gas flow ratio is 2%, and the deposition thickness is 100nm. +Microcrystalline silicon, doping concentration 2.5×10 20 cm -3 .
[0040] Step 7: After removing the back borosilicate glass and phosphosilicate glass from the silicon wafer obtained in steps 5 and 6 and cleaning it, SiN is deposited in the corresponding area. x :H anti-reflection layer, thickness 95nm.
[0041] Step 8: After removing the borosilicate glass from the front side of the silicon wafer obtained in step 7 and cleaning it, Al is deposited using an ALD device and a PECVD device. 2 O 3 Passivation layer and SiN x :H anti-reflection layer, with thicknesses of 3nm and 75nm respectively.
[0042] Step 9, using a screen printing method to print the back surface of the silicon wafer obtained in step 8 + and n + Ag / Al paste and Ag paste are printed in different regions respectively, and finally co-sintered in an infrared belt sintering furnace.
[0043] After specific practical experiments, under the specific environment setting of room temperature and standard atmospheric pressure, the use of the floating junction FFE layer in this embodiment can increase the short-circuit current density of the IBC solar cell by 0.9 mA / cm 2 ; Based on the tunneling oxide layer on the back of the IBC solar cell, adding a doped amorphous silicon structure can increase the open circuit voltage of the cell by 12mV; the superposition of the two technologies can increase the conversion efficiency of the IBC solar cell by 1.4%. The specific improvement effect of the cell performance is affected by the precision control of the process conditions themselves and environmental factors.
[0044] In this embodiment, BCl is used on the front side of the silicon wafer. 3 The p-type nanostructured ... + The floating junction FFE layer, through the pumping effect, can use the voltage gradient formed by boron doping in the floating junction to transmit the minority holes in the n-type silicon wafer over a longer distance, especially to transmit the carriers in the back surface field region to the back emitter region through the floating junction over a long distance, so that they can be effectively collected by the back electrode. The advantage is that the back surface field and the back emitter can be kept the same width without reducing the cell efficiency, as shown in Table 1 and Figure 4 shown.
[0045] Table 1 Comparison of battery performance test results
[0046] In this embodiment, PECVD is used to sequentially deposit n-type nanoparticles with a thickness of 5 to 50 nm. + Amorphous silicon, doping concentration 5×1019 ~1×10 21 cm -3 and a thickness of 20 to 150 nm + Microcrystalline silicon, doping concentration 5×10 19 ~1×10 21 cm -3 , thus taking advantage of the thinness of the tunnel oxide layer and its sensitivity to the interface, a low-power p + The amorphous silicon layer can not only utilize the good interface passivation function of amorphous silicon, but also the low-power PECVD deposition method can reduce the bombardment damage to the tunnel oxide layer; then the p-type silicon is deposited under higher power and higher temperature conditions. + The microcrystalline silicon layer can not only increase its collection of carriers, but also retain p + The amorphous components of the amorphous silicon layer are shown in Table 2.
[0047] Table 2 Comparison of battery performance test results
[0048] When the deposition thickness is 5 to 50 nm, + When the amorphous silicon is used, the flow rate ratio of borane gas in the mixed gas is 2-5%; when the deposition thickness is 20-150nm, the + In the case of microcrystalline silicon, the flow rate ratio of borane gas in the mixed gas is 0.5-2%.
[0049] The IBC solar cell front surface floating junction FFE layer and the back surface p + and n + The combined use of tunneling silicon oxide and doped amorphous silicon in the region. The floating junction FFE layer has a "pumping effect" that can increase the carrier transmission distance, and can be prepared by methods such as high-temperature diffusion and ion implantation; the back tunneling silicon oxide has the advantages of high passivation and low preparation cost, and the doped amorphous silicon has excellent interface passivation characteristics and can protect the tunneling silicon oxide. Moreover, the floating junction FFE layer and the back tunneling silicon oxide and doped amorphous silicon are located on both sides of the battery, respectively. The processes are independent and do not affect each other, and their respective process parameters can be optimized to the greatest extent. During the process, it is necessary to prepare the front floating junction FFE layer first, and then prepare the back tunneling silicon oxide and doped amorphous silicon layer to ensure the integrity of the amorphous silicon.
[0050] The above-mentioned specific implementation can be partially adjusted in different ways by those skilled in the art without departing from the principle and purpose of the present invention. The protection scope of the present invention shall be based on the claims and shall not be limited by the above-mentioned specific implementation. Each implementation scheme within its scope shall be subject to the constraints of the present invention.
Claims
1. An improved IBC solar cell, characterized in that: include: n-type crystalline silicon substrate, a p-type + The floating junction FFE layer, the aluminum oxide passivation layer and the hydrogenated silicon nitride anti-reflection layer and the tunneling oxide layer, n + Amorphous silicon layer, n + Microcrystalline silicon layer, p + Amorphous silicon layer, p + Microcrystalline silicon layer, hydrogenated silicon nitride anti-reflection layer and metal electrode.
2. The improved IBC solar cell according to claim 1, characterized in that: The n-type crystalline silicon substrate is an n-type Cz single crystal silicon wafer with a crystal orientation of (100); The p + The boron doping concentration in the floating junction FFE layer is 5×10 18 ~1×10 20 cm -3 , the doping junction depth is 0.5~1.5μm; The p + Amorphous silicon layer and p + The boron doping concentration in the microcrystalline silicon layer is 1×10 19 ~2×10 20 cm -3 , with thicknesses of 5-50nm and 20-150nm respectively; The n + Amorphous silicon layer and n + The phosphorus doping concentration in the microcrystalline silicon layer is 5×10 19 ~1×10 21 cm -3 , with thicknesses of 5~50nm and 20~150nm respectively.
3. A method for preparing the improved IBC solar cell according to claim 1 or 2, characterized in that: The following steps are involved: Step 1, preparing an industrial-grade n-type Cz single crystal silicon wafer with a crystal orientation of (100) as a crystalline silicon substrate, the thickness of the silicon wafer is 100-150 μm, and the resistivity is 0.5-2 Ω·cm; using a KOH solution to remove the damage layer on the surface of the crystalline silicon substrate caused by wire cutting; Step 2, after texturing the n-type crystalline silicon substrate with a KOH solution, a pre-treated silicon wafer is obtained by standard RCA cleaning; Step 3: Form a p-type silicon wafer on the front side by BCl3 diffusion or high temperature annealing after boron ion implantation. + Floating knot FFE layer; Step 4, after etching the edges of the silicon wafer obtained in step 3, polishing the back surface of the silicon wafer with a KOH solution, and obtaining a SiO2 layer or Al2O3 layer with a thickness of 1 to 2 nm by high-temperature thermal oxidation technology, plasma enhanced chemical vapor deposition (PECVD) or atomic layer deposition (ALD); Step 5: insert the back side of the silicon wafer obtained in step 4 into the first mask, and deposit a p-type film with a thickness of 5 to 50 nm by PECVD. + Amorphous silicon, doping concentration 1×10 19 ~2×10 20 cm -3 and p with a thickness of 20 to 150 nm + Microcrystalline silicon, doping concentration 1×10 19 ~2×10 20 cm -3 ; Step 6: Take out the first mask from the back of the silicon wafer obtained in step 5 and insert the second mask, and use PECVD to deposit n-type films with a thickness of 5 to 50 nm. + Amorphous silicon, doping concentration 5×10 19 ~1×10 21 cm -3 and a thickness of 20 to 150 nm + Microcrystalline silicon, doping concentration 5×10 19 ~1×10 21 cm -3 ; Step 7: After removing the back borosilicate glass and phosphosilicate glass from the silicon wafer obtained in Steps 5 and 6 and cleaning it, SiN with a thickness of 80 to 100 nm is deposited in the corresponding area. x :H anti-reflection layer; Step 8: After removing the borosilicate glass from the front side of the silicon wafer obtained in step 7 and cleaning it, an Al2O3 passivation layer with a thickness of 2 to 5 nm and a SiN layer with a thickness of 70 to 80 nm are deposited using an ALD device and a PECVD device respectively. x :H anti-reflection layer; Step 9, using a screen printing method to print the back surface of the silicon wafer obtained in step 8 + and n + Ag / Al paste and Ag paste were printed in different regions respectively, and finally the metal electrodes were prepared by co-sintering in an infrared belt sintering furnace.
4. The preparation method according to claim 3, characterized in that: The sequential deposition in step 5 means: firstly setting the power supply to 3-5 kW, the deposition temperature to 150-250° C., the deposition pressure to 200-300 Pa, and introducing a mixed gas of silane, borane and hydrogen to deposit a p-type layer with a thickness of 5-50 nm; + Amorphous silicon, the power supply is 7-10kW, the deposition temperature is 300-450℃, the deposition pressure is 300-400Pa, and a mixed gas of silane, borane and hydrogen is introduced to deposit a p-type silicon with a thickness of 20-150nm. + Microcrystalline silicon, doping concentration 1×10 19 ~2×10 20 cm -3 .
5. The preparation method according to claim 4, characterized in that: When the deposition thickness is 5 to 50 nm, + When the amorphous silicon is used, the flow rate ratio of borane gas in the mixed gas is 2-5%; when the deposition thickness is 20-150nm, the + In the case of microcrystalline silicon, the flow rate ratio of borane gas in the mixed gas is 0.5-2%.
6. The preparation method according to claim 3, characterized in that: The holes of the mask are distributed in an interdigitated manner.
7. The preparation method according to claim 3, characterized in that: The sequential deposition in step 6 means: firstly setting the power supply to 3-5 kW, the deposition temperature to 150-250° C., the deposition pressure to 200-300 Pa, and introducing a mixed gas of silane, phosphine and hydrogen to deposit a layer of n-type nanoparticles with a thickness of 5-50 nm. + Amorphous silicon, doping concentration 5×10 19 ~1×10 21 cm -3 Then set the power supply to 7-10kW, the deposition temperature to 300-450°C, the deposition pressure to 300-400Pa, and introduce a mixed gas of silane, phosphine and hydrogen to deposit a thickness of 20-150nm. + Microcrystalline silicon, doping concentration 5×10 19 ~1×10 21 cm -3 , n + Amorphous silicon and n + Deposition principle of microcrystalline silicon and p + Same area.
8. The preparation method according to claim 7, characterized in that: When the deposition thickness is 5 to 50 nm, + When amorphous silicon is used, the flow rate ratio of phosphine gas in the mixed gas is 3-8%; when the deposition thickness is 20-150nm, the + In the case of microcrystalline silicon, the flow rate ratio of phosphine gas in the mixed gas is 1 to 4%.
Citation Information
Patent Citations
Topcon passivated IBC battery and preparation method thereof
CN110459638A
IBC solar cell structure and preparation process thereof
CN111987225A
Efficient P-type IBC battery and preparation method thereof
CN114725225A
Interdigital back contact battery and preparation method thereof
CN117080314A
Solar battery and method for manufacture thereof
JP2008010746A
Cited By
Back contact cell and etching‑free manufacturing method therefor, and cell assembly
WO2026183998A1