Ternary positive electrode material and preparation method thereof

By covering the calcium borate layer on the surface of the ternary positive electrode material, the stability problem of nickel-rich ternary layered transition metal oxides in lithium-ion batteries is solved, and high power and long cycle performance are improved .

CN118919636AInactive Publication Date: 2024-11-08HEFEI GUOXUAN HIGH TECH POWER ENERGY

Patent Information

Application Number
CN202411135571.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Nickel-rich ternary layered transition metal oxides in lithium-ion batteries have caused material dissolution and solid electrolyte film formation due to electrolyte erosion, resulting in increased internal resistance, limiting their commercial application.

Method used

By uniformly coating the calcium borate (Ca2B2O6) layer on the surface of the ternary positive electrode material, the electronegative attraction boron and calcium elements are used to form a stable conductive coating layer, preventing side reactions between the material and the electrolyte and promoting the transmission of lithium ions .

Benefits of technology

It significantly improves the cycling performance and rate performance of the battery, reduces the side reaction between the surface of the positive electrode material and the electrolyte, and enhances the stability and conductivity of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a ternary positive electrode material and a preparation method thereof. The preparation method of the ternary positive electrode material comprises the following steps: adding the ternary positive electrode material into a calcium salt solution, stirring, and adding a tetrahydroborate solution; after the reaction is completed, drying a reaction system to obtain powder; and sintering the powder in an inert atmosphere. The coating layer of the ternary positive electrode material prepared by the method is calcium borate, and the coating layer has good physical and chemical stability, so that the physical and chemical stability of the surface of the material can be effectively improved, and side reaction of an electrolyte and the positive electrode material is effectively reduced. Meanwhile, the coating layer prepared by the method is uniform in coating, the uniform coating layer is more beneficial to keeping the positive electrode material stable in the charge-discharge process, side reaction is more effectively prevented, and the positive electrode material has excellent cycle performance while having good gram capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a ternary positive electrode material and a preparation method thereof, belonging to the technical field of lithium ion batteries. Background Art

[0002] In recent years, with the demand for high energy density batteries, batteries have become thinner and lighter. Nickel (Ni)-rich ternary layered transition metal oxides (LiNi x Co y M 1-x-y O2, M = Mn or Al) has become a hot topic of research due to its superior energy density and low cost. However, the application of Ni-rich ternary layered transition metal oxides mainly faces the following problems: (1) The erosion of the electrolyte causes the dissolution of part of the transition metal in the material; (2) After the decomposition of the electrolyte at the positive electrode, a solid electrolyte (CEI) film will be formed, resulting in an increase in internal resistance. It is precisely because of the existence of these defects that the commercial application of Ni-rich ternary layered transition metal oxides is subject to certain restrictions.

[0003] In order to solve the above problems, coating is a very effective means. By coating a layer of inorganic metal oxide on the surface of the ternary positive electrode material, the side reaction between the material and the electrolyte can be effectively avoided, thereby enhancing the stability of the material and improving the cycle performance of the battery. At the same time, if the coating material has good conductivity, it can effectively improve the transmission of lithium ions, thereby improving the power performance of the positive electrode material. Summary of the invention

[0004] The purpose of the present invention is to provide a high-power long-cycle ternary positive electrode material coated with a high-stability conductive coating layer, and the preparation process is carried out in a non-aqueous solution. The coating layer is coated evenly, and the uniform coating layer is more conducive to the positive electrode material to remain stable during the charge and discharge process, and more effectively prevent the occurrence of side reactions. While having good gram capacity, it also has excellent cycle performance.

[0005] The present invention realizes the coating of the coating layer by electronegativity. First, under the effect of electronegativity, BH4 - The ions are uniformly adsorbed on the surface of the ternary cathode material and react to produce BO2 - , achieving uniform coating of boron, and then adsorbing positively charged Ca 2+, the uniform coating of calcium element is realized, and finally a calcium borate (Ca2B2O6) coating layer is obtained. Compared with the traditional wet coating method, in the present invention, through electronegativity attraction, the coating element can be more uniformly and completely coated on the surface of the ternary cathode material. The coating layer is calcium borate, which has good physical and chemical stability. The ternary cathode material coated with the highly stable conductive coating layer prepared by the present invention can effectively reduce the side reaction between the surface of the cathode material and the electrolyte, greatly improving the cycle performance of the battery. At the same time, compared with traditional inorganic metal oxides, fluorides, phosphates, etc., the coating layer has good conductivity, and the coating can well promote the transport of Li+, improving the rate performance of the lithium-ion battery.

[0006] Specifically, the preparation method of the ternary cathode material with a long cycle coated with a uniform coating layer provided by the present invention includes the following steps: Add the ternary cathode material into a solution of calcium salt, stir and then add a solution of tetrahydroborate; after the reaction is complete, dry the reaction system to obtain a powder; sinter the powder in an inert atmosphere to obtain the product.

[0007] The ternary cathode material is prepared according to the following method: uniformly mix the ternary cathode material precursor and the lithium source in a high-speed mixer, then sinter in a muffle furnace, and then cool, crush, and screen; Among them, the chemical formula of the ternary cathode material precursor is Ni x Co y Mn z (OH)2, 0.3 < x < 1, 0 < y < 0.4, 0 < z < 1, x + y + z = 1; preferably, 0.3 ≤ x ≤ 0.65, 0.05 ≤ y < 0.4, 0.05 ≤ z < 0.4, x + y + z = 1; The lithium source is one or both of lithium carbonate (Li2CO3) and lithium hydroxide (LiOH); The molar ratio of the sum of Ni, Co, and Mn elements in the ternary cathode material precursor to Li in the lithium source is 1:1.01 - 1.10, preferably 1:1.02 - 1.08; During the sintering process, the selected atmosphere is air or oxygen, preferably oxygen; The sintering temperature is 600 - 1000 °C, preferably 700 - 900 °C, and the sintering time is 5 - 20 h, preferably 10 - 16 h.

[0008] In the preparation method of the present invention, the calcium salt is calcium chloride or calcium nitrate; The solution of the calcium salt is prepared using an organic solvent; The addition amount of the calcium salt is: 1 g of the ternary cathode material: 0.5 - 9 mg of the calcium salt.

[0009] In the preparation method of the present invention, the tetrahydroborate is sodium tetrahydroborate, magnesium tetrahydroborate or potassium tetrahydroborate; The added amount of the tetrahydroborate is: 1g of the ternary positive electrode material: 0.15~2mg of the tetrahydroborate.

[0010] In the preparation method of the present invention, the stirring time is 1 to 4 hours; The reaction time is 1 to 4 hours.

[0011] In the preparation method of the present invention, the drying temperature is 100-150° C. and the drying time is 4-10 hours.

[0012] In the preparation method of the present invention, the sintering process is as follows: Heat up to 300-500℃ at a rate of 1-3℃ and keep warm for 1-4h, then cool naturally to room temperature; The inert atmosphere is nitrogen or argon.

[0013] The surface of the ternary positive electrode material prepared by the method of the present invention is coated with a Ca2B2O6 coating layer with a content of 100-1000ppm.

[0014] At present, the main electrolyte lithium salt in the electrolyte of lithium-ion batteries is lithium hexafluorophosphate (LiPF6). LiPF6 has poor thermal stability and is easy to hydrolyze with water to generate hydrogen fluoride (HF). HF will corrode the positive electrode material, dissolve the transition metal ions in the material, cause the crystal to undergo phase change, and the battery performance will deteriorate. By coating a layer of inorganic non-metallic oxide on the surface of the ternary layered transition metal oxide material, the reaction between the electrolyte and the electrolyte can be effectively reduced, thereby improving the stability of the lithium-ion battery in the cycle. The coating layer of the ternary positive electrode material prepared by the method of the present invention is calcium borate. Since the coating layer has good physicochemical stability, it can effectively improve the physicochemical stability of the material surface and effectively reduce the occurrence of side reactions between the electrolyte and the positive electrode material. At the same time, the coating layer prepared by the method is uniformly coated, and the uniform coating layer is more conducive to the stability of the positive electrode material during the charge and discharge process, more effectively preventing the occurrence of side reactions, and having good gram capacity while having excellent cycle performance; and the coating layer is a good lithium ion conductor, which can promote the diffusion of lithium ions and improve the power performance of the material. DETAILED DESCRIPTION

[0015] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.

[0016] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0017] Embodiment 1: (1) Take 7000g NCM6506 precursor and 3040g Li2CO3 and mix them evenly using a high-speed mixer. Then put the mixed materials into a sagger and shake and compact them. Then cut the materials into cubes of the same size. (2) Place the sagger containing the material in a muffle furnace and heat it to 880°C at a heating rate of 2°C / min and keep it warm for 15 hours. At the same time, compressed air is continuously introduced during the entire reaction process with a gas flow rate of 0.6m 3 / h. After crushing and sieving, the uncoated ternary positive electrode material is obtained; (3) Add 16 mg of Ca(NO3)2 into 1 L of ethanol solution and continue stirring for 2 h to allow the Ca(NO3)2 to completely dissolve.

[0018] (4) Add 20 g of the ternary positive electrode material obtained in step (2) to the organic solution obtained in step (3), and then add 2 mL of NaBH4 solution (the effective content of NaBH4 is 3.5 mg) dropwise, stirring continuously during the addition process, and then continue stirring for 3 hours to allow the reaction to be sufficient to obtain a ternary material suspension.

[0019] (5) The ternary material suspension obtained in step (4) is placed in a constant temperature oven, the oven temperature is set to 120°C, and the drying time is 8 hours, after which a uniformly mixed solid powder is obtained.

[0020] (6) The solid powder obtained in step (5) was placed in a dry pot and then in a muffle furnace, argon gas was introduced, the heating parameters were set, the temperature was raised to 400°C at a heating rate of 2°C / min, and the temperature was kept for 3 hours. After screening, a uniformly coated NCM positive electrode material was obtained, wherein the content of the Ca2B2O6 coating layer was 100ppm.

[0021] Embodiment 2: (1) Take 7000g NCM6506 precursor and 3040g Li2CO3 and mix them evenly using a high-speed mixer. Then put the mixed materials into a sagger and shake and compact them. Then cut the materials into cubes of the same size. (2) Place the sagger containing the material in a muffle furnace and heat it to 880°C at a heating rate of 2°C / min and keep it warm for 15 hours. At the same time, compressed air is continuously introduced during the entire reaction process with a gas flow rate of 0.6m 3 / h. After crushing and sieving, the uncoated ternary positive electrode material is obtained; (3) Add 80 mg of Ca(NO3)2 into 1 L of ethanol solution and continue stirring for 2 h to allow the Ca(NO3)2 to completely dissolve.

[0022] (4) Add 20 g of the ternary positive electrode material obtained in step (2) to the organic solution obtained in step (3), and then add 10 mL of NaBH4 solution (the effective content of NaBH4 is 17.5 mg) dropwise, stirring continuously during the addition process, and then continue stirring for 3 hours to allow the reaction to complete, thereby obtaining a ternary material suspension.

[0023] (5) The ternary material suspension obtained in step (4) is placed in a constant temperature oven, the oven temperature is set to 120°C, and the drying time is 8 hours, after which a uniformly mixed solid powder is obtained.

[0024] (6) The solid powder obtained in step (5) was placed in a dry pot and then in a muffle furnace, argon gas was introduced, the heating parameters were set, the temperature was raised to 400°C at a heating rate of 2°C / min, and the temperature was kept for 3 hours. After screening, a uniformly coated NCM positive electrode material was obtained, wherein the content of the Ca2B2O6 coating layer was 500ppm.

[0025] Embodiment 3: (1) Take 7000g NCM6506 precursor and 3040g Li2CO3 and mix them evenly using a high-speed mixer. Then put the mixed materials into a sagger and shake and compact them. Then cut the materials into cubes of the same size. (2) Place the sagger containing the material in a muffle furnace and heat it to 880°C at a heating rate of 2°C / min and keep it warm for 15 hours. At the same time, compressed air is continuously introduced during the entire reaction process with a gas flow rate of 0.6m 3 / h. After crushing and sieving, the uncoated ternary positive electrode material is obtained; (3) Add 84 mg of Ca(NO3)2 into 1 L of ethanol solution and continue stirring for 2 h to allow the Ca(NO3)2 to completely dissolve.

[0026] (4) Add 20 g of the ternary positive electrode material obtained in step (2) to the organic solution obtained in step (3), and then add 16 mL of NaBH4 solution (the effective content of NaBH4 is 28 mg) dropwise, stirring continuously during the addition process, and then continue stirring for 3 hours to allow the reaction to be sufficient to obtain a ternary material suspension.

[0027] (5) The ternary material suspension obtained in step (4) is placed in a constant temperature oven, the oven temperature is set to 120°C, and the drying time is 8 hours, after which a uniformly mixed solid powder is obtained.

[0028] (6) The solid powder obtained in step (5) was placed in a dry pot and then in a muffle furnace, argon gas was introduced, the heating parameters were set, the temperature was raised to 400°C at a heating rate of 2°C / min, and the temperature was kept for 3 hours. After screening, a uniformly coated NCM positive electrode material was obtained, wherein the content of the Ca2B2O6 coating layer was 800ppm.

[0029] Embodiment 4: (1) Take 7000g NCM6506 precursor and 3040g Li2CO3 and mix them evenly using a high-speed mixer. Then put the mixed materials into a sagger and shake and compact them. Then cut the materials into cubes of the same size. (2) Place the sagger containing the material in a muffle furnace and heat it to 880°C at a heating rate of 2°C / min and keep it warm for 15 hours. At the same time, compressed air is continuously introduced during the entire reaction process with a gas flow rate of 0.6m 3 / h. After crushing and sieving, the uncoated ternary positive electrode material is obtained; (3) Add 160 mg of Ca(NO3)2 into 1 L of ethanol solution and continue stirring for 2 h to allow the Ca(NO3)2 to completely dissolve.

[0030] (4) Add 20 g of the ternary cathode material obtained in step (2) to the organic solution obtained in step (3), and then add 20 mL of NaBH4 solution (the effective content of NaBH4 is 35 mg) dropwise, stirring continuously during the addition process, and then continue stirring for 3 h to allow the reaction to complete, thereby obtaining a ternary material suspension.

[0031] (5) The ternary material suspension obtained in step (4) is placed in a constant temperature oven, the oven temperature is set to 120°C, and the drying time is 8 hours, after which a uniformly mixed solid powder is obtained.

[0032] (6) The solid powder obtained in step (5) was placed in a dry pot and then in a muffle furnace, argon gas was introduced, the heating parameters were set, the temperature was raised to 400°C at a heating rate of 2°C / min, and the temperature was kept for 3 hours. After screening, a uniformly coated NCM positive electrode material was obtained, wherein the content of the Ca2B2O6 coating layer was 1000ppm.

[0033] Comparative Example 1: (1) Take 7000g NCM6506 precursor and 3040g Li2CO3 and mix them evenly using a high-speed mixer. Then put the mixed materials into a sagger and shake and compact them. Then cut the materials into cubes of the same size. (2) Place the sagger containing the material in a muffle furnace and heat it to 880°C at a heating rate of 2°C / min and keep it warm for 15 hours. At the same time, compressed air is continuously introduced during the entire reaction process with a gas flow rate of 0.6m 3 / h. After crushing and sieving, the uncoated ternary positive electrode material is obtained; (3) Add 32.8 mg of Ca2B2O6 into 1 L of ethanol solution and continue stirring for 2 h to allow the Ca2B2O6 to completely dissolve.

[0034] (4) Add 20 g of the ternary positive electrode material obtained in step (2) to the organic solution obtained in step (3), and continue stirring for 3 h to allow the reaction to complete, thereby obtaining a ternary material suspension.

[0035] (5) The ternary material suspension obtained in step (4) is placed in a constant temperature oven, the oven temperature is set to 120°C, and the drying time is 8 hours, after which a uniformly mixed solid powder is obtained.

[0036] (6) The solid powder obtained in step (5) was placed in a dry pot and then in a muffle furnace, argon gas was introduced, the heating parameters were set, the temperature was raised to 400°C at a heating rate of 2°C / min, and the temperature was kept for 3 hours. After screening, a uniformly coated NCM positive electrode material was obtained, wherein the content of the Ca2B2O6 coating layer was 800ppm.

[0037] The positive electrode materials, conductive carbon black, and PVDF obtained in each embodiment and comparative example were mixed in a ratio of 90:5:5, and NMP was used as a solvent to mix them evenly, and then they were evenly coated on aluminum foil to make button batteries to test their electrochemical properties. The test was carried out at room temperature 25°C, and the first four weeks were charged and discharged at 0.2C / 0.2C, 0.33C / 0.33C, 1C / 1C, and 0.2C / 0.2C, respectively, and then at 1C / 1C for 50 cycles. The button battery performance data is shown in Table 1.

[0038] Table 1 Performance of different lithium-ion batteries

[0039] From the comparison of the electrical performance data of Example 3 and Comparative Example 1, it can be seen that compared with the traditional wet coating, at the same coating amount, the gram capacity, rate performance and cycle performance of the material prepared by the method of the present invention are significantly better than those of the ordinary wet coating sample. From Examples 1-4, it can be seen that within a certain range, as the coating amount increases, the cycle performance of the material becomes better and the gram capacity is also increased.

Claims

1. A method for preparing a ternary positive electrode material, comprising the following steps: The ternary positive electrode material is added to a calcium salt solution, and after stirring, a tetrahydroborate solution is added; after the reaction is complete, the reaction system is dried to obtain a powder; and the powder is placed in an inert atmosphere for sintering.

2. The preparation method according to claim 1, characterized in that: The calcium salt is calcium chloride or calcium nitrate; Using an organic solvent to prepare a solution of the calcium salt; The added amount of the calcium salt is: 1g of the ternary positive electrode material: 0.5~9mg of the calcium salt.

3. The preparation method according to claim 1 or 2, characterized in that: The tetrahydroborate is sodium tetrahydroborate, magnesium tetrahydroborate or potassium tetrahydroborate; The added amount of the tetrahydroborate is: 1g of the ternary positive electrode material: 0.15~2mg of the tetrahydroborate.

4. The preparation method according to any one of claims 1 to 3, characterized in that: The stirring time is 1 to 4 hours; The reaction time is 1 to 4 hours.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The drying temperature is 100-150° C. and the drying time is 4-10 hours.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The sintering process is as follows: Heat up to 300-500℃ at a rate of 1-3℃ and keep warm for 1-4h, then cool naturally to room temperature; The inert atmosphere is nitrogen or argon.

7. The ternary cathode material prepared by the method according to any one of claims 1 to 6; The surface of the ternary positive electrode material is coated with a Ca2B2O6 coating layer with a content of 100-1000ppm.

8. A lithium-ion battery using the ternary positive electrode material according to claim 7.

Citation Information

Patent Citations

  • Cathode active material and preparation method thereof, cathode material and lithium ion battery

    CN102569774A

  • Preparation method of single-crystal high-nickel low-cobalt or cobalt-free positive electrode material

    CN113629254A

  • Preparation method and application of single-crystal high-nickel ternary material with completely modified surface

    CN114261996A

  • Calcium phosphate coated high-nickel ternary positive electrode material as well as preparation method and application thereof

    CN114566647A

  • Method for completely coating surface of positive electrode material of lithium ion battery

    CN115465901A

Cited By

  • Composite coated ternary material as well as preparation method and application thereof

    CN120749143A