Golf cart battery and positive plate and preparation method thereof

By using a specially formulated lead paste and precise curing process on the positive electrode plate of the golf cart battery, the problem of short battery life was solved, the plate strength was improved and the stability of active materials was enhanced, thus extending the battery's lifespan.

CN118919637APending Publication Date: 2024-11-08HUBEI CAMEL HAIXIA STORAGE BATTERY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411235797.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing golf cart batteries have a short lifespan under deep discharge cycle conditions, mainly because the active material of the positive electrode plate constantly changes in volume due to the conversion between lead dioxide and lead sulfate, causing the lead paste to loosen and resulting in capacity decay.

Method used

The positive electrode lead paste, formulated with a specific formula, includes dilute sulfuric acid, deionized water, short fibers, tetrabasic lead sulfate, stannous sulfate, waterborne fluorocarbon emulsion resin, and waterborne acrylic emulsion. Through precise curing processes, it forms fine and uniform tetrabasic lead sulfate seed crystals and improves interfacial properties, enhances electrode bonding strength, and prevents active material from falling off.

Benefits of technology

It significantly extends the lifespan of golf cart batteries, increasing the 100% deep discharge cycle life from 400 cycles to over 850 cycles, an improvement of more than 110%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919637A_ABST
    Figure CN118919637A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a positive plate of a golf cart battery. The preparation method comprises the following steps: preparing positive lead plaster, wherein the positive lead plaster is prepared from the following raw materials in percentage by weight: 4-8% of dilute sulfuric acid, 5-10% of deionized water, 0.1-0.3% of short fiber, 2-5% of tetrabasic lead sulfate, 0.1-0.6% of stannous mono-sulphate, 0.5-0.8% of water-based fluorocarbon emulsion resin, 0.05-0.1% of water-based acrylate emulsion and the balance of lead powder; coating positive electrode lead paste on the positive electrode alloy plate grid and rolling; carrying out curing treatment on the rolled positive electrode alloy plate grid to prepare a positive electrode plate; the curing treatment comprises the following steps: keeping the positive plate at the temperature of 65-68 DEG C and the relative humidity of 98-100% for 5 hours; keeping the temperature at 82-85 DEG C and the relative humidity at 85-90% for 8 hours; keeping for 6-8 hours at the temperature of 62-65 DEG C and the relative humidity of 98-100%; and keeping for 18-20 hours at the temperature of 80 + / -5 DEG C and the relative humidity of 0-20%. The service life of the battery is effectively prolonged, and the problem that the service life of the battery of the golf cart is short in a deep discharge recycling state is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of secondary batteries, and in particular relates to a golf cart battery. Background Art

[0002] Golf cart batteries provide power for golf carts. The performance of batteries is directly related to the running status of vehicles. The core component of batteries is the plate, which is the main factor affecting the life of batteries. The traditional method for preparing lead paste for golf cart batteries is to mix lead powder, dilute sulfuric acid solution, deionized water, and additives in a certain proportion in a paste machine in the order of dry mixing, adding water, adding acid, and mixing to make lead paste, and then apply the lead paste on the grid to obtain the green plate after curing; then assemble the positive plate, negative plate, and separator, add acid to obtain the lead-acid battery. During the battery's charge and discharge cycle, the active substance component of the positive plate lead paste is lead dioxide, which is converted into lead sulfate during discharge, and is converted from lead sulfate to lead dioxide during charging. Because the positive lead paste is constantly converted between lead dioxide and lead sulfate, the volume ratio of lead dioxide to lead sulfate is quite different, and the volume of the positive lead paste is constantly expanding and contracting, which leads to loosening of the lead paste, causing the battery capacity to decay and battery failure. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a positive plate of a long-life golf cart battery, so as to solve the problem that the existing golf cart battery has a short battery life under deep discharge cycle use.

[0004] To achieve the above object, the present invention provides the following technical solution: a method for preparing a positive electrode plate of a golf cart battery, comprising the following steps:

[0005] S1. Preparation of positive electrode lead paste:

[0006] The positive electrode lead paste formula is composed of the following raw materials by weight percentage: 4% to 8% of dilute sulfuric acid, 5% to 10% of deionized water, 0.1% to 0.3% of short fibers, 2% to 5% of tetrabasic lead sulfate, 0.1% to 0.6% of stannous sulfate, 0.5% to 0.8% of water-based fluorocarbon emulsion resin, 0.05% to 0.1% of water-based acrylic emulsion, and the rest is lead powder; short fibers are added to the lead paste, and the short fibers improve the physical strength of the plate and reduce the shedding speed of the active material.

[0007] S2, coating the positive electrode lead paste on the positive electrode alloy grid and rolling it;

[0008] S3, curing the rolled positive electrode alloy grid to obtain a positive electrode plate;

[0009] The curing process steps are as follows:

[0010] S3.1. The positive plate is kept at a temperature of 65-68°C and a relative humidity of 98-100% for 5 hours. The main function of this stage is to continue to oxidize the fine metal lead and gel the water-based fluorocarbon emulsion resin.

[0011] S3.2. The positive plate is kept at a temperature of 82-85°C and a relative humidity of 85-90% for 8 hours. The main function of this stage is to form a corrosion layer between the grid bars and the lead paste, solidify the active material of the positive plate, and plasticize the water-based fluorocarbon emulsion resin.

[0012] S3.3. The positive plate is kept at a temperature of 62-65°C and a relative humidity of 98-100% for 6-8 hours. The main function of this stage is to increase the bonding strength between the lead paste and the grid, further oxidize the fine metal lead, and increase the strength of the network plastic lattice formed by the water-based fluorocarbon emulsion resin plasticization and the water-based acrylic emulsion.

[0013] S3.4. The positive plate is kept at a temperature of 80±5°C and a relative humidity of 0-20% for 18-20 hours. The main function of this stage is to dry the positive plate, remove moisture from the plate, and plasticize the water-based fluorocarbon emulsion resin and stabilize the network plastic lattice generated by the water-based acrylic emulsion.

[0014] The specific steps of preparing the positive electrode lead paste are as follows:

[0015] S1.1: Weigh the raw materials according to the formula, add the lead powder into the fully automatic paste mixing machine, add tetrabasic lead sulfate, stannous sulfate, and short fibers, and stir for 2±0.5 minutes;

[0016] S1.2: Add deionized water into the paste mixing machine;

[0017] S1.3: Continue stirring for 2±0.5 minutes after adding deionized water;

[0018] S1.4: Add dilute sulfuric acid solution into the paste mixer within 15±2 minutes;

[0019] S1.5: Continue stirring for 5±1 minutes after adding the dilute sulfuric acid solution;

[0020] S1.6: Add water-based fluorocarbon emulsion resin and water-based acrylic emulsion. Use a sprayer to add the mixture of water-based fluorocarbon emulsion resin and water-based acrylic emulsion, stirring while adding. The mixture should be added within 2±0.5 minutes, and continued to stir for 5±1 minutes after adding.

[0021] S1.7: Prepare the paste to obtain positive electrode lead paste.

[0022] The crystal grain diameter of the tetrabasic lead sulfate is less than 10 μm.

[0023] The oxidation degree of the lead powder is between 50% and 70%.

[0024] The positive electrode alloy grid is made of lead-antimony-tin-selenium alloy.

[0025] The lead-antimony-tin-selenium alloy has an antimony content of 3.0%, a tin content of 0.2% to 0.3%, and a selenium content of 0.02% to 0.03%.

[0026] The present invention also provides a golf cart battery positive plate prepared by adopting the golf cart battery positive plate preparation method.

[0027] The present invention also provides a golf cart battery, comprising a positive electrode plate, a negative electrode plate, a separator, an electrolyte, and a shell. The positive electrode plate is prepared by the above-mentioned golf cart battery positive electrode plate preparation method. The positive electrode plate, the negative electrode plate, and the separator are stacked and assembled, and then acidified to obtain a golf cart battery.

[0028] The present invention also provides a positive electrode lead paste for golf cart batteries. The positive electrode lead paste formula consists of the following raw materials in weight percentage: 4% to 8% of dilute sulfuric acid, 5% to 10% of deionized water, 0.1% to 0.3% of short fibers, 2% to 5% of tetrabasic lead sulfate, 0.1% to 0.6% of stannous sulfate, 0.5% to 0.8% of water-based fluorocarbon emulsion resin, 0.05% to 0.1% of water-based acrylic emulsion, and the remainder is lead powder.

[0029] The crystal diameter of the tetrabasic lead sulfate is less than 10 μm; the oxidation degree of the lead powder is between 50% and 70%.

[0030] Compared with the existing golf cart battery technology, the beneficial effects of the present invention are as follows:

[0031] In order to protect the positive electrode active material from softening during the life cycle, tetrabasic lead sulfate is added to the positive electrode lead paste of the present invention. The tetrabasic lead sulfate can provide crystal seeds. After the plate is cured, a large number of fine tetrabasic lead sulfate particles exist in the plate, which increases the content of tetrabasic lead sulfate in the plate. Tetrabasic lead sulfate can provide crystal seeds. The use of tetrabasic lead sulfate with a grain diameter of less than 10 μm can make the formed crystals small and evenly distributed, thereby increasing the battery life. In addition, the plate curing time can be reduced, the formation efficiency can be improved, and the cost can be reduced. In order to improve the utilization rate of the positive electrode active material, stannous sulfate is added to the positive electrode lead paste of the present invention. During the charge and discharge cycle of the battery, Sn2+ ions form non-stoichiometric The PbxSnyOn compound improves the interface characteristics and the particle bonding strength, thereby improving the utilization rate of the active material. In addition, stannous sulfate can also prevent the formation of a passivation layer between the grid and the active material, prevent the early capacity decay of the battery, and increase the service life of the battery. In order to protect the positive electrode active material from softening during the life cycle, an aqueous fluorocarbon emulsion resin is added to the positive electrode lead paste of the present invention. The aqueous fluorocarbon emulsion resin is added to the lead paste. After curing under the curing process conditions provided by the present invention, a cross-linked network plastic grid is formed inside the lead paste, which fixes the lead paste in the grid, increases the strength of the plate, avoids the early shedding of the active material during the cyclic use process, and causes the battery service life to end prematurely, thereby improving the service life of the battery.

[0032] Aqueous acrylic emulsion is added to the positive lead paste of the present invention. After the aqueous acrylic emulsion is mixed with the aqueous fluorocarbon emulsion resin, the strength and plasticity of the aqueous fluorocarbon emulsion resin are improved. After the lead paste is cured, the aqueous acrylic emulsion improves the elastic strength of the mesh plastic lattice structure, which can effectively provide a compression space for the volume change of the positive electrode active material between the conversion of lead dioxide and lead sulfate, and can still maintain the toughness of the mesh plastic lattice after multiple volume reciprocating compressions, thereby avoiding premature failure of the mesh plastic lattice structure caused by volume expansion changes during charge and discharge conversion of the active material, and avoiding premature end of the battery service life due to early shedding of the active material during cyclic use.

[0033] The golf cart battery made by the present invention has the effects of improving the strength of the lead paste, slowing down the loosening, softening and shedding of the active material lead dioxide in the positive lead paste, and extending the service life of the battery. The 100% DOD cycle life of the battery is increased from about 400 times to about 850 times, with an increase of more than 110%. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 The figure is a comparison chart of 100% DOD cycle life of Example 1 of the present invention and the existing ordinary golf cart battery. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] The techniques, methods and equipment known to ordinary technicians in the relevant field may not be discussed in detail, but where appropriate, the techniques, methods and equipment should be considered as part of the authorization specification. The experimental methods or test methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials are obtained from conventional commercial channels or prepared by conventional methods unless otherwise specified.

[0037] Example 1

[0038] The method for preparing the positive electrode plate of a golf cart battery provided in this embodiment comprises the following steps:

[0039] S1. Preparation of positive electrode lead paste:

[0040] The positive lead paste formula is composed of the following raw materials by weight percentage: 8% dilute sulfuric acid, 9% deionized water, 0.1% short fiber, 4% tetrabasic lead sulfate, 0.4% stannous sulfate, 0.8% water-based fluorocarbon emulsion resin, 0.08% water-based acrylic emulsion, and the rest is lead powder; the oxidation degree of the lead powder is 65% to 70%; the crystal diameter of the tetrabasic lead sulfate is less than 10 μm;

[0041] S1.1: Weigh the raw materials according to the above formula, add the lead powder into the fully automatic paste mixing machine, add tetrabasic lead sulfate, stannous sulfate, short fibers, and stir for 2 minutes;

[0042] S1.2: Add deionized water into the paste mixing machine;

[0043] S1.3: Continue stirring for 2 minutes after adding deionized water;

[0044] S1.4: Add dilute sulfuric acid solution into the paste mixer within 15 minutes;

[0045] S1.5: Continue stirring for 5 minutes after adding the dilute sulfuric acid solution;

[0046] S1.6: Add water-based fluorocarbon emulsion resin and water-based acrylic emulsion. Use a sprayer to add the mixture of water-based fluorocarbon emulsion resin and water-based acrylic emulsion, stirring while adding. The mixture should be added within 2 minutes, and stirring should be continued for 5 minutes after addition.

[0047] S1.7: Prepare the paste to obtain positive electrode lead paste.

[0048] S2, coating the positive electrode lead paste on the positive electrode alloy grid and rolling it;

[0049] S3, curing the positive electrode alloy grid and the lead paste to obtain a positive electrode plate;

[0050] The curing process steps are as follows:

[0051] S3.1. Keep the positive plate at 65°C and 98-100% relative humidity for 5 hours;

[0052] S3.2. The positive plate is kept at a temperature of 85°C and a relative humidity of 85-90% for 8 hours;

[0053] S3.3, the positive plate is kept at a temperature of 65°C and a relative humidity of 98-100% for 7 hours;

[0054] S3.4. The positive electrode plate is kept at a temperature of 80°C and a relative humidity of 0-20% for 20 hours.

[0055] Example 2

[0056] The method for preparing the positive electrode plate of a golf cart battery provided in this embodiment comprises the following steps:

[0057] S1. Preparation of positive electrode lead paste:

[0058] The positive lead paste formula is composed of the following raw materials by weight percentage: 7% dilute sulfuric acid, 10% deionized water, 0.1% short fiber, 3% tetrabasic lead sulfate, 0.3% stannous sulfate, 0.8% water-based fluorocarbon emulsion resin, 0.06% water-based acrylic emulsion, and the rest is lead powder; the oxidation degree of the lead powder is 65% to 70%; the crystal diameter of the tetrabasic lead sulfate is less than 10 μm;

[0059] S1.1: Weigh the raw materials according to the above formula, add the lead powder into the fully automatic paste mixing machine, add tetrabasic lead sulfate, stannous sulfate, short fibers, and stir for 2 minutes;

[0060] S1.2: Add deionized water into the paste mixing machine;

[0061] S1.3: Continue stirring for 2 minutes after adding deionized water;

[0062] S1.4: Add dilute sulfuric acid solution into the paste mixer within 15 minutes;

[0063] S1.5: Continue stirring for 5 minutes after adding the dilute sulfuric acid solution;

[0064] S1.6: Add water-based fluorocarbon emulsion resin and water-based acrylic emulsion. Use a sprayer to add the mixture of water-based fluorocarbon emulsion resin and water-based acrylic emulsion, stirring while adding. The mixture should be added within 2 minutes, and stirring should be continued for 5 minutes after addition.

[0065] S1.7: Prepare the paste to obtain positive electrode lead paste.

[0066] S2, coating the positive electrode lead paste on the positive electrode alloy grid and rolling it;

[0067] S3, curing the positive electrode alloy grid and the lead paste to obtain a positive electrode plate;

[0068] The curing process steps are as follows:

[0069] S3.1. Keep the positive plate at 68°C and 98-100% relative humidity for 5 hours;

[0070] S3.2, the positive plate is kept at a temperature of 82°C and a relative humidity of 85-90% for 8 hours;

[0071] S3.3, the positive plate is kept at a temperature of 62°C and a relative humidity of 98-100% for 8 hours;

[0072] S3.4. The positive plate is kept at a temperature of 85°C and a relative humidity of 0-20% for 19 hours.

[0073] Example 3

[0074] The method for preparing the positive electrode plate of a golf cart battery provided in this embodiment comprises the following steps:

[0075] S1. Preparation of positive electrode lead paste:

[0076] The positive lead paste formula is composed of the following raw materials by weight percentage: 7% dilute sulfuric acid, 10% deionized water, 0.15% short fiber, 5% tetrabasic lead sulfate, 0.4% stannous sulfate, 0.6% water-based fluorocarbon emulsion resin, 0.1% water-based acrylic emulsion, and the rest is lead powder; the oxidation degree of the lead powder is 65% to 70%; the crystal diameter of the tetrabasic lead sulfate is less than 10 μm;

[0077] S1.1: Weigh the raw materials according to the above formula, add the lead powder into the fully automatic paste mixing machine, add tetrabasic lead sulfate, stannous sulfate, short fibers, and stir for 2 minutes;

[0078] S1.2: Add deionized water into the paste mixing machine;

[0079] S1.3: Continue stirring for 2 minutes after adding deionized water;

[0080] S1.4: Add dilute sulfuric acid solution into the paste mixer within 15 minutes;

[0081] S1.5: Continue stirring for 5 minutes after adding the dilute sulfuric acid solution;

[0082] S1.6: Add water-based fluorocarbon emulsion resin and water-based acrylic emulsion. Use a sprayer to add the mixture of water-based fluorocarbon emulsion resin and water-based acrylic emulsion, stirring while adding. The mixture should be added within 2 minutes, and stirring should be continued for 5 minutes after addition.

[0083] S1.7: Prepare the paste to obtain positive electrode lead paste.

[0084] S2, coating the positive electrode lead paste on the positive electrode alloy grid and rolling it;

[0085] S3, curing the positive electrode alloy grid and the lead paste to obtain a positive electrode plate;

[0086] The curing process steps are as follows:

[0087] S3.1. Keep the positive plate at 68°C and 98-100% relative humidity for 5 hours;

[0088] S3.2. The positive plate is kept at a temperature of 85°C and a relative humidity of 85-90% for 8 hours;

[0089] S3.3, the positive plate is kept at a temperature of 62°C and a relative humidity of 98-100% for 8 hours;

[0090] S3.4. The positive electrode plate is kept at a temperature of 80°C and a relative humidity of 0-20% for 20 hours.

[0091] The golf cart battery positive plate was made into battery examples 1, 2 and 3 (the battery models of examples 1, 2 and 3 were the same, and the number of plate structures and separator compositions were exactly the same), and an existing ordinary golf cart battery was used as a comparative example (the comparative example and examples 1-3 were equipped with batteries of the same model and structure), and then the corresponding battery performance tests were carried out respectively.

[0092]

[0093] It can be seen from the above table that the 5-hour rate capacity and 20-hour rate capacity of the embodiment of the present invention are substantially the same as those of ordinary golf cart batteries, but the battery life of the embodiment of the present invention is significantly longer than that of ordinary golf cart batteries.

[0094] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that changes, modifications and substitutions may be made to the embodiments without departing from the principles of the present invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a positive electrode plate for a golf cart battery, characterized in that: The following steps are involved: S1. Preparation of positive electrode lead paste: The positive lead paste formula is composed of the following raw materials by weight percentage: 4% to 8% dilute sulfuric acid, 5% to 10% deionized water, 0.1% to 0.3% short fibers, 2% to 5% tetrabasic lead sulfate, 0.1% to 0.6% stannous sulfate, 0.5% to 0.8% water-based fluorocarbon emulsion resin, 0.05% to 0.1% water-based acrylic emulsion, and the rest is lead powder; S2, coating the positive electrode lead paste on the positive electrode alloy grid and rolling it; S3, curing the rolled positive electrode alloy grid to obtain a positive electrode plate; The curing process steps are as follows: S3.

1. Keep the positive plate at a temperature of 65-68°C and a relative humidity of 98-100% for 5 hours; S3.2, the positive plate is kept at a temperature of 82-85°C and a relative humidity of 85-90% for 8 hours; S3.3, keep the positive plate at a temperature of 62-65°C and a relative humidity of 98-100% for 6-8 hours; S3.

4. Maintain the positive plate at a temperature of 80±5°C and a relative humidity of 0-20% for 18-20 hours.

2. The method for preparing a positive electrode plate for a golf cart battery according to claim 1, characterized in that: The specific steps of preparing the positive electrode lead paste are as follows: S1.1: Weigh the raw materials according to the formula, add the lead powder into the fully automatic paste mixing machine, add tetrabasic lead sulfate, stannous sulfate, and short fibers, and stir for 2±0.5 minutes; S1.2: Add deionized water into the paste mixing machine; S1.3: Continue stirring for 2±0.5 minutes after adding deionized water; S1.4: Add dilute sulfuric acid solution into the paste mixer within 15±2 minutes; S1.5: Continue stirring for 5±1 minutes after adding the dilute sulfuric acid solution; S1.6: Add water-based fluorocarbon emulsion resin and water-based acrylic emulsion. Use a sprayer to add the mixture of water-based fluorocarbon emulsion resin and water-based acrylic emulsion, stirring while adding. The mixture should be added within 2±0.5 minutes, and continued to stir for 5±1 minutes after adding. S1.7: Prepare the paste to obtain positive electrode lead paste.

3. The method for preparing a positive electrode plate for a golf cart battery according to claim 1, characterized in that: The crystal grain diameter of the tetrabasic lead sulfate is less than 10 μm.

4. The method for preparing a positive electrode plate for a golf cart battery according to claim 1, characterized in that: The oxidation degree of the lead powder is between 50% and 70%.

5. The method for preparing a positive electrode plate for a golf cart battery according to claim 1, characterized in that: The positive electrode alloy grid is made of lead-antimony-tin-selenium alloy.

6. The method for preparing the positive electrode plate of a golf cart battery according to claim 5, characterized in that: The lead-antimony-tin-selenium alloy has an antimony content of 3.0%, a tin content of 0.2% to 0.3%, and a selenium content of 0.02% to 0.03%.

7. A golf cart battery positive plate prepared by the method for preparing a golf cart battery positive plate according to any one of claims 1 to 6.

8. A golf cart battery, comprising a positive plate, a negative plate, a separator, an electrolyte, and a casing, characterized in that: The positive electrode plate is a positive electrode plate prepared by the method for preparing a positive electrode plate for a golf cart battery according to any one of claims 1 to 6.

9. A positive electrode lead paste for a golf cart battery, characterized in that: The positive electrode lead paste formula is composed of the following raw materials by weight percentage: 4% to 8% of dilute sulfuric acid, 5% to 10% of deionized water, 0.1% to 0.3% of short fibers, 2% to 5% of tetrabasic lead sulfate, 0.1% to 0.6% of stannous sulfate, 0.5% to 0.8% of water-based fluorocarbon emulsion resin, 0.05% to 0.1% of water-based acrylic emulsion, and the rest is lead powder.

10. The positive electrode lead paste for golf cart battery according to claim 9, characterized in that: The crystal diameter of the tetrabasic lead sulfate is less than 10 μm; the oxidation degree of the lead powder is between 50% and 70%.