Positive electrode material and preparation method thereof, positive electrode plate and lithium-sulfur battery
By using porous carbon conductive agents and phosphorus pentasulfide and sulfur powder in the positive electrode of lithium sulfur battery, a solid electrolyte of lithium phosphorus sulfur is formed to form an efficient ionic conductive network, and the problems of low ionic conductivity and insufficient specific capacity in lithium sulfur batteries are solved, and the problem of low ionic conductivity and insufficient specific capacity in lithium sulfur batteries is achieved. Higher specific capacity and cycle stability.
Patent Information
- Application Number
- CN202410961403.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
The existing all-solid lithium-sulfur battery positive electrode system has poor performance under high loads, and cannot effectively utilize the full performance of sulfur as an active substance, resulting in the problems of low ionic conductivity and low specific capacity.
Porous carbon conductive agent, diphosphate pentasulfide and sulfur powder are used as active substances, and lithium phosphorus and sulfur solid electrolyte is generated by ball mill mixing and sintering to form an efficient ionic conductivity network, and the ionic conductivity of the positive electrode material and the utilization rate of the active substance are improved.
The specific capacity of lithium-sulfur batteries is significantly improved under high area loading, and the stability of battery circulation is ensured, which improves the overall performance of the positive electrode material.
Smart Images

Figure CN118919639A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of electrochemical technology, and in particular to a positive electrode material and a preparation method thereof, a positive electrode sheet and a lithium-sulfur battery. Background Art
[0002] Among the many new lithium battery systems, lithium-sulfur batteries are a hot research system recently. Compared with traditional transition metal oxide systems, the specific capacity of lithium-sulfur batteries is much higher than other battery systems. The specific capacity of up to 1675mAh / g makes the lithium-sulfur battery system far ahead of all lithium battery systems. Although its average discharge voltage is low, its energy density is still at a high level. The all-solid-state lithium-sulfur battery system avoids many problems in traditional liquid lithium-sulfur batteries, including the shuttle effect and lithium metal pulverization.
[0003] The existing all-solid-state lithium-sulfur battery cathode system is mostly prepared with complex materials and processes, and the performance is poor at high loading, and it is unable to exert the full performance of sulfur as an active substance. In view of this, it is necessary to provide a cathode material that can ensure the cycle stability of the battery. Summary of the invention
[0004] The present application provides a positive electrode material and a preparation method thereof, a positive electrode plate and a lithium-sulfur battery, the purpose of which is to improve the problems of poor ion conductivity and low specific capacity existing in lithium-sulfur batteries.
[0005] The first aspect of the present application provides a positive electrode material, comprising the following raw materials in parts by weight: 10 parts of porous carbon conductive agent, 7 to 14 parts of additives, 38 to 44 parts of active substances, and 32 to 40 parts of solid electrolytes; wherein the active substances include sulfur powder; and the additives include one or both of phosphorus pentasulfide and phosphorus trisulfide.
[0006] The lithium sulfide generated by the elemental sulfur in the present application and lithium ions during battery discharge can be in situ generated with additives as lithium phosphorus sulfur (Li3PS4) solid electrolyte. The lithium phosphorus sulfur solid electrolyte can not only enable most of the active substances to participate in the charge and discharge cycle, improve the utilization rate of the active substances, form an ion conductive network, and lithium ions can be conducted faster, but also improve the ion conductivity of the positive electrode material, so that at a high area loading, the assembled all-solid-state battery can improve the specific capacity of the lithium-sulfur battery while ensuring the stability of the cycle.
[0007] In some embodiments, the porous carbon conductive agent includes one or more of Ketjen black, acetylene black, carbon black, graphite, carbon fiber, and activated carbon.
[0008] The use of porous carbon conductive agent is conducive to better adhesion of phosphorus pentasulfide to the surface and better penetration of active substances into the pores.
[0009] In some embodiments, the solid electrolyte includes one or more of lithium phosphorus sulfur chlorine, lithium phosphorus sulfur, lithium germanium phosphorus sulfur, and lithium lanthanum zirconium oxygen.
[0010] The second aspect of the present application provides a method for preparing the above-mentioned positive electrode material, comprising: ball-milling and mixing a porous carbon conductive agent and an additive, and then performing a first sintering treatment to obtain a first intermediate product; ball-milling and mixing the first intermediate product and an active substance, and then performing a second sintering treatment to obtain a second intermediate product; ball-milling and mixing the second intermediate product and a solid electrolyte to obtain a positive electrode material.
[0011] In some embodiments, the temperature of the first sintering process is 300°C to 420°C.
[0012] In some embodiments, the temperature of the first sintering process is 380°C to 400°C.
[0013] In some embodiments, the first sintering process lasts for 4 hours to 5 hours.
[0014] In some embodiments, the temperature of the second sintering process is 150°C to 160°C.
[0015] In some embodiments, the second sintering process lasts for 10 hours to 12 hours.
[0016] In some embodiments, the ball milling mixing time is 3 h to 7 h.
[0017] A third aspect of the present application provides a positive electrode plate, comprising the positive electrode material of the first aspect or the positive electrode material prepared according to the method of the second aspect.
[0018] A fourth aspect of the present application provides a lithium-sulfur battery, comprising the positive electrode plate of the third aspect. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application will be briefly introduced below. Obviously, the drawings described below are only some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work.
[0020] Figure 1 This is an X-ray photoelectron spectroscopy analysis diagram of the first intermediate product provided in Example 1 of the present application.
[0021] Figure 2 This is an X-ray photoelectron spectrum analysis diagram of the second intermediate product provided in Example 1 of the present application.
[0022] Figure 3 This is an X-ray photoelectron spectroscopy analysis diagram of the positive electrode material provided in Example 1 of the present application.
[0023] Figure 4 The lithium-sulfur battery of Example 1 of the present application and the lithium-sulfur battery of Comparative Example 1 are compared at a rate of 0.1C and an active material area loading of 4 mg / cm 2 The specific capacity comparison chart below.
[0024] Figure 5 The lithium-sulfur battery of Example 1 of the present application and the lithium-sulfur battery of Comparative Example 1 are shown in Figure 1 at different rates and with an active material area loading of 4 mg / cm 2 The specific capacity comparison chart below. DETAILED DESCRIPTION
[0025] In order to make the invention purpose, technical scheme and beneficial technical effect of the present application clearer, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the embodiments described in this specification are only for explaining the present application, not for limiting the present application.
[0026] For simplicity, only some numerical ranges are explicitly disclosed herein. However, any lower limit can be combined with any upper limit to form an unambiguous range; and any lower limit can be combined with other lower limits to form an unambiguous range, and any upper limit can be combined with any other upper limit to form an unambiguous range. In addition, although not explicitly stated, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unambiguous range.
[0027] In the description of this article, it should be noted that, unless otherwise specified, “above” and “below” are inclusive of the number itself, and the “multiple” in “one or more” and “one or more” means more than two (or more).
[0028] For lithium metal anode, it has the lowest voltage (-3.04V) and ultra-high specific capacity (3860mAh / g), which also makes its potential very huge. However, due to the insufficient safety of lithium metal anode, most of the current commercial lithium-ion batteries use graphite anode. At the same time, the positive electrode material usually uses transition metal oxides, which are based on the principle of intercalation reaction. The current specific capacity has gradually approached its bottleneck, and the room for improvement is extremely limited. The cost of transition metal oxides has remained high due to the relatively expensive cobalt element, which also limits the large-scale application of lithium-ion batteries. Finally, the safety issues of lithium-ion batteries have gradually attracted everyone's attention. The high-frequency spontaneous combustion accidents of electric vehicles and the safety issues of mobile phone batteries are difficult to satisfy people.
[0029] After the traditional solid-state lithium-sulfur battery combines sulfur and carbon, the sulfur does not fully participate in the battery cycle due to the low ionic conductivity of sulfur and the discharge product lithium sulfide, resulting in a low specific capacity. At the same time, due to the low ionic conductivity of sulfur and the discharge product lithium sulfide, the ionic conductivity of the traditional positive electrode is low, and when the load is high, some active substances cannot fully participate in the charge and discharge, resulting in a low specific capacity.
[0030] In view of this, it is necessary to provide a solid-state lithium-sulfur battery positive electrode material with high mass fraction, high loading capacity and improved specific capacity.
[0031] The first aspect of the present application provides a positive electrode material, comprising the following raw materials in parts by weight: 10 parts of porous carbon conductive agent, 7 to 14 parts of additives, 38 to 44 parts of active substances, and 32 to 40 parts of solid electrolytes; wherein the active substances include sulfur powder; and the additives include one or both of phosphorus pentasulfide and phosphorus trisulfide.
[0032] In the embodiments of the present application, lithium sulfide generated by elemental sulfur and lithium ions during battery discharge can generate lithium phosphorus sulfur (Li3PS4) solid electrolyte in situ with additives. The lithium phosphorus sulfur solid electrolyte can enable most of the active substances to participate in the charge and discharge cycle, improve the utilization rate of the active substances, form an ion conductive network, and lithium ions can be conducted faster. It can also improve the ionic conductivity of the positive electrode material, so that at a high area loading, the assembled all-solid-state battery can improve the specific capacity of the lithium-sulfur battery while ensuring the stability of the cycle.
[0033] The additive may be phosphorus pentasulfide, which can improve the specific capacity of the positive electrode material together with the porous carbon conductive agent, thereby further improving the specific capacity of the lithium-sulfur battery.
[0034] The weight of the additive is 7 to 14 parts, for example, 7, 8, 9, 10, 11, 12, 13, 14, or any range thereof. It can be 10-12 parts.
[0035] The weight of the active substance is 38 to 44 parts, for example, 38, 39, 40, 41, 42, 43, 44, or any range thereof. It can be 40-42 parts.
[0036] The weight of the solid electrolyte is 32 to 40 parts, for example, 32, 33, 34, 35, 36, 7, 8, 39, 40, or any range thereof. It can be 38-40 parts.
[0037] In some embodiments, the porous carbon conductive agent includes one or more of Ketjen black, acetylene black, DENKA BLACK, thermal black, channel black, graphite, carbon fiber and activated carbon. One or both of Ketjen black and activated carbon can be selected.
[0038] Using Ketjen Black and activated carbon as porous carbon conductive agents is conducive to better adhesion of additives to the surface of the porous carbon conductive agent, better penetration of active substances into the gaps, and better improvement of the conductivity of the battery.
[0039] In some embodiments, the solid electrolyte includes one or more of lithium phosphorus sulfur chlorine, lithium phosphorus sulfur, lithium germanium phosphorus sulfur and lithium lanthanum zirconium oxygen. Lithium phosphorus sulfur chlorine can be selected. Selecting lithium phosphorus sulfur chlorine as the solid electrolyte can better enable most of the active materials to participate in the charge and discharge cycle and improve the overall ionic conductivity of the positive electrode material.
[0040] The second aspect of the present application provides a method for preparing the above-mentioned positive electrode material, comprising:
[0041] S10, ball-milling the porous carbon conductive agent and the additive and then performing a first sintering treatment to obtain a first intermediate product;
[0042] S20, ball-milling the first intermediate product and the active material and then performing a second sintering treatment to obtain a second intermediate product;
[0043] S30, ball-milling the second intermediate product and the solid electrolyte to obtain a positive electrode material.
[0044] As can be understood by those skilled in the art, ball milling utilizes the impact of the falling grinding body and the grinding effect between the grinding body and the inner wall of the ball mill to crush and mix the materials. When the ball mill rotates, due to the friction between the grinding body and the inner wall of the ball mill. The raw materials are brought up in the direction of rotation and then fall down, and are crushed continuously. The operating conditions are good, and the crushing is carried out in a closed machine without flying dust; the operation is reliable, the grinding body is cheap and easy to replace; it can be operated intermittently or continuously. Choosing to perform ball milling three times can better mix the two substances during each ball milling process, and the mixing effect of the next ball milling will be better and more uniform; the additive can achieve the target effect during the first ball milling and be better adsorbed on the surface of the porous carbon conductive agent. Multiple sintering can effectively control the temperature. When the additive needs to reach a molten state, the temperature is increased, and the adsorption of the active material can control the low temperature, and the specific capacity of the obtained battery is higher.
[0045] In some embodiments, the temperature of the first sintering process is 300°C to 420°C, for example, 300°C, 310°C, 320°C, 340°C, 350°C, 360°C, 380°C, 400°C, 420°C or any range thereof, and can be 380°C to 400°C.
[0046] In some embodiments, the first sintering treatment time is 4 hours to 5.2 hours, for example, 4 hours, 4.1 hours, 4.2 hours, 4.5 hours, 4.6 hours, 4.8 hours, 5 hours, or any range thereof, and can be 4.5 hours to 5 hours.
[0047] The first sintering treatment makes the additive reach a molten state in the above temperature environment, so as to better adsorb on the surface of the porous carbon conductive agent.
[0048] In some embodiments, the temperature of the first sintering process is 380°C to 400°C.
[0049] In some embodiments, the rotation speed of the ball milling is 400 rpm to 500 rpm.
[0050] In some embodiments, the temperature of the second sintering process is 150°C to 160°C, for example, 150°C, 151°C, 152°C, 155°C, 156°C, 158°C, 160°C, or any range thereof, and can be 152°C to 155°C.
[0051] In some embodiments, the second sintering treatment time is 10 hours to 14 hours, for example, 10 hours, 10.5 hours, 11 hours, 11.5 hours, 12 hours, or any range thereof, and can be 11 hours to 12 hours.
[0052] The temperature of the second sintering treatment is selected to be 152° C. to 155° C., and the time is selected to be 11 h to 12 h, so that the active material can enter the voids of the porous carbon conductive agent with the additive to better form an ion conductive network and increase the specific capacity of the battery.
[0053] In some embodiments, the ball milling mixing time is 3 hours to 8 hours, for example, 6 hours, 6.2 hours, 6.4 hours, 6.5 hours, 6.6 hours, 6.8 hours, 7 hours, 8 hours, or any range of the above values. 6.5 hours to 7 hours can be selected, which can make the mixing more uniform, and the particle size can reach the target range, which is conducive to the subsequent sintering.
[0054] A third aspect of the present application provides a positive electrode plate, comprising a positive electrode current collector and the positive electrode material of the first aspect or the positive electrode material prepared by the method of the second aspect coated on the positive electrode current collector.
[0055] A fourth aspect of the present application provides a lithium-sulfur battery, comprising a battery casing and a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte according to the third aspect located in the battery casing.
[0056] The present application will be further described below in conjunction with the examples. It should be understood that these examples are only for illustrative purposes, as it will be apparent to those skilled in the art that various modifications and variations are made within the scope of the present disclosure. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are based on mass, and all reagents used in the examples are commercially available or synthesized according to conventional methods, and can be used directly without further processing, and the instruments used in the examples are commercially available.
[0057] Comparative Example 1
[0058] S10, adding 10 parts of Ketjen Black EC600-JD into a ball mill, ball milling and mixing at a rotation speed of 500 rpm for 4 hours, and then transferring to a stainless steel reactor, and first sintering treatment at 400° C. for 5 hours to obtain a first intermediate product.
[0059] S20, adding the first intermediate product and 40 parts of sulfur powder into a ball mill, ball milling and mixing at a rotation speed of 500 rpm for 5 hours, and then transferring it to a stainless steel reactor, and performing a second sintering treatment at 155° C. for 12 hours to obtain a second intermediate product.
[0060] S30, adding the second intermediate product and 40 parts of lithium phosphorus sulfur chloride into a ball mill, and ball milling and mixing at a rotation speed of 500 rpm for 7 hours to obtain a positive electrode material.
[0061] Comparative Example 2
[0062] S10, adding 10 parts of Ketjen Black EC600-JD and 10 parts of potassium iodide into a ball mill, ball milling and mixing at a rotation speed of 500 rpm for 4 hours, and then transferring to a stainless steel reactor, and first sintering treatment at 400° C. for 5 hours to obtain a first intermediate product.
[0063] S20, adding the first intermediate product and 40 parts of sulfur powder into a ball mill, ball milling and mixing at a rotation speed of 500 rpm for 5 hours, and then transferring it to a stainless steel reactor, and performing a second sintering treatment at 155° C. for 12 hours to obtain a second intermediate product.
[0064] S30, adding the second intermediate product and 40 parts of lithium phosphorus sulfur chloride into a ball mill, and ball milling and mixing at a rotation speed of 500 rpm for 7 hours to obtain a positive electrode material.
[0065] Example 1
[0066] S10, adding 10 parts of Ketjen Black EC600-JD and 10 parts of phosphorus pentasulfide into a ball mill, ball milling and mixing at a rotation speed of 500 rpm for 4 hours, and then transferring to a stainless steel reactor, and first sintering treatment at 400° C. for 5 hours to obtain a first intermediate product.
[0067] S20, adding the first intermediate product and 40 parts of sulfur powder into a ball mill, ball milling and mixing at a rotation speed of 500 rpm for 5 hours, and then transferring it to a stainless steel reactor, and performing a second sintering treatment at 155° C. for 12 hours to obtain a second intermediate product.
[0068] S30, adding the second intermediate product and 40 parts of lithium phosphorus sulfur chloride into a ball mill, and ball milling and mixing at a rotation speed of 500 rpm for 7 hours to obtain a positive electrode material.
[0069] The first intermediate product prepared in Example 1 was tested and the X-ray photoelectron spectroscopy (XPS) analysis chart was as follows: Figure 1 As shown, it can be seen that the first intermediate product has two characteristic peaks and split double peaks, the characteristic peaks are 163.9eV and 162.3eV, which are consistent with the two characteristic peaks of phosphorus pentasulfide.
[0070] The XPS graph of the second intermediate product prepared in Example 1 is as follows: Figure 2 As shown, it can be seen that the second intermediate product contains both the characteristic peak of phosphorus pentasulfide mentioned above and the characteristic peak of sulfur element 164.0 eV and its split double peak, and the intensity of the characteristic peak of sulfur is significantly higher than that of phosphorus pentasulfide.
[0071] The positive electrode material prepared in Example 1 was tested and the XPS graph obtained was as follows: Figure 3 As shown, it can be seen that the positive electrode material contains all the above peaks, as well as the characteristic peak of lithium phosphorus sulfur chlorine at 161.1 eV, indicating that the positive electrode material is a composite of the second intermediate product and lithium phosphorus sulfur chlorine.
[0072] Assembly of lithium-sulfur batteries:
[0073] In a peek mold with an outer diameter of 40 mm and an inner diameter of 10 mm, 100 mg of lithium phosphorus sulfur chlorine (solid electrolyte) was pressed into a tablet at a pressure of 300 MPa, and then 7.85 mg of the positive electrode material powder provided in Example 1 (the area loading of sulfur was 4 mg / cm 2 ), and the other side was equipped with a lithium-indium alloy negative electrode according to a molar ratio of 0.5:1. After the overall battery was assembled, an external frame was used to give the battery a pressure of 60 MPa, and an electrochemical test was carried out at 30°C.
[0074] The lithium-sulfur battery prepared in Example 1 and the lithium-sulfur battery prepared using the materials of Comparative Example 1 showed good performance at 0.1C rate and 4 mg / cm active material area loading. 2 The specific capacity comparison chart below is as follows Figure 4 shown.
[0075] The lithium-sulfur battery prepared in Example 1 and the lithium-sulfur battery prepared using the materials of Comparative Example 1 were compared at different rates and at an active material area loading of 4 mg / cm 2 The specific capacity comparison chart below is as follows Figure 5 As shown, 1C is 1675mA / g.
[0076] Example 2
[0077] The only difference between this embodiment and embodiment 1 is that the weight parts of phosphorus pentasulfide are 7 parts.
[0078] Example 3
[0079] The only difference between this embodiment and embodiment 1 is that the weight parts of phosphorus pentasulfide are 14 parts.
[0080] Example 4
[0081] The only difference between this embodiment and embodiment 1 is that the weight portion of sulfur powder is 50 parts.
[0082] Example 5
[0083] The only difference between this embodiment and embodiment 1 is that the weight parts of lithium phosphorus sulfur chlorine is 30 parts.
[0084] Example 6
[0085] The only difference between this embodiment and embodiment 1 is that the temperature of the first sintering treatment is 320° C. and the time of the first sintering treatment is 4 hours.
[0086] Example 7
[0087] The only difference between this embodiment and embodiment 1 is that the temperature of the first sintering treatment is 400° C. and the time of the first sintering treatment is 2 hours.
[0088] The performance of the lithium-sulfur batteries provided in Examples 1-9 and Comparative Examples 1-2 was tested, and the results are shown in Table 1:
[0089] Table 1
[0090]
[0091]
[0092] After conducting experiments with different experimental parameters, it can be found that after changing the material, sintering temperature, and sintering time, the performance of the positive electrode material has decreased to varying degrees, so in summary, the current treatment method can obtain the positive electrode with the best performance. The above is only a specific implementation of the present application, but the protection scope of the present application is not limited to this. Any technician familiar with the technical field can easily think of various equivalent modifications or replacements within the technical scope disclosed in this application, and these modifications or replacements should be included in the protection scope of this application. Therefore, the protection scope of this application shall be based on the protection scope of the claims.
Claims
1. A positive electrode material, It is characterized in that The raw materials include the following parts by weight: 10 parts of porous carbon conductive agent, 7 to 14 parts of additives, 38 to 44 parts of active materials, and 32 to 40 parts of solid electrolytes; wherein, The active substance includes sulfur powder; The additive includes one or both of phosphorus pentasulfide and phosphorus trisulfide.
2. The positive electrode material according to claim 1, It is characterized in that The porous carbon conductive agent includes one or more of Ketjen black, acetylene black, carbon black, graphite, carbon fiber and activated carbon.
3. The positive electrode material according to claim 1, It is characterized in that The solid electrolyte includes one or more of lithium phosphorus sulfur chlorine, lithium phosphorus sulfur, lithium germanium phosphorus sulfur and lithium lanthanum zirconium oxygen.
4. A method for preparing the positive electrode material according to any one of claims 1 to 3, It is characterized in that The steps include: The porous carbon conductive agent and the additive are ball-milled and mixed, and then subjected to a first sintering treatment to obtain a first intermediate product; The first intermediate product and the active material are ball-milled and mixed, and then subjected to a second sintering treatment to obtain a second intermediate product; The second intermediate product and the solid electrolyte are ball-milled and mixed to obtain the positive electrode material.
5. The method according to claim 4, It is characterized in that The temperature of the first sintering treatment is 300° C. to 420° C.; and / or The first sintering treatment takes 4 hours to 5.2 hours.
6. The method according to claim 5, It is characterized in that The temperature of the first sintering process is 380°C to 400°C.
7. The method according to claim 4, It is characterized in that The temperature of the second sintering treatment is 150° C. to 160° C.; and / or The second sintering treatment time is 10 hours to 14 hours.
8. The method according to claim 4, It is characterized in that The ball milling mixing time is 3h to 8h.
9. A positive electrode sheet, It is characterized in that The invention comprises the positive electrode material according to any one of claims 1 to 3 or the positive electrode material prepared by the method according to any one of claims 4 to 8.
10. A lithium-sulfur battery, It is characterized in that Comprising the positive electrode sheet according to claim 9.
Citation Information
Patent Citations
Positive electrode mixture and all-solid-state lithium sulfur cell
CN105308774A
Preparation method of sulfur composite positive electrode material and all-solid-state lithium-sulfur battery
CN111799459A
Solid-state lithium-sulfur battery, battery positive electrode and preparation method of battery positive electrode
CN113903882A
Solid-state battery and preparation method and application thereof
CN115360407A
Positive electrode mixture for composite all-solid-state lithium-sulfur battery
CN116018699A
Cited By
Positive electrode with high carrier mobility and application
CN119581482A
Positive electrode material and preparation method therefor, positive electrode sheet, and lithium-sulfur battery
EP4708373A1
Positive electrode material and preparation method therefor, positive electrode sheet, and lithium-sulfur battery
WO2026016953A1