Negative pole piece, battery and electric device

By designing a negative electrode sheet with a double-layer film structure in a lithium-ion battery, using silicon-carbon composite materials with microporous and mesoporous structures, combined with carbon cladding, the density and stability of silicon-based negative electrode materials at high volume specific capacity are solved. The problem of sexuality achieves higher cycle stability and energy density.

CN118919642APending Publication Date: 2024-11-08JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411124248.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-08

Smart Images

  • Figure CN118919642A_ABST
    Figure CN118919642A_ABST
Patent Text Reader

Abstract

The embodiment of the invention discloses a negative pole piece, a battery and a power utilization device, the negative pole piece comprises a negative current collector and a film layer arranged on at least one surface of the negative current collector, the film layer comprises a first film layer and a second film layer, the first film layer is located between the negative current collector and the second film layer, the first film layer comprises a first negative active material, and the second film layer comprises a second negative active material. The first film layer comprises a first negative electrode active material, the second film layer comprises a second negative electrode active material, the first negative electrode active material comprises a first silicon-carbon composite material, the first silicon-carbon composite material comprises a first carbon matrix with a micropore structure and a first silicon-based material distributed in the pore structure of the first carbon matrix, and the second negative electrode active material comprises a second silicon-carbon composite material. The second silicon-carbon composite material comprises a second carbon matrix with a mesoporous structure and a second silicon-based material distributed in the pore structure of the second carbon matrix. According to the embodiment of the invention, the circulation and energy density requirements of the negative pole piece can be considered.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a negative electrode plate, a battery and an electrical device. Background Art

[0002] With the advent of the era of artificial intelligence, the increasing portability requirements of consumer electronic devices, and the limited space for electric vehicles, the development of lithium-ion batteries is facing "space anxiety", that is, volume energy density has become a top priority for the development of lithium-ion batteries. Silicon-based anodes with high (mass, volume) specific capacity are the most promising new generation of lithium-ion battery anode materials to partially replace commercial graphite, but huge volume expansion will occur during the lithium insertion process, leading to problems such as rupture of the solid electrolyte interface (SEI) and electrode pulverization, causing its capacity to decay rapidly. Although the development of nanotechnology has improved the mass specific capacity of silicon-based materials, the lower density has severely limited the advantages of its volume performance.

[0003] Therefore, promoting the commercialization of high-capacity silicon-based anodes requires researchers to fully utilize the high volumetric capacity advantage of silicon active materials and increase the density of electrode materials when designing materials, and to increase the loading amount of electrode materials and the volume proportion of active materials in the device to obtain lithium-ion batteries with high volumetric energy density. However, the excellent performance of silicon-based anodes is more in low electrode density (<0.5mg·cm –3 , basic research), low electrode loading (<1 mg cm –2 , basic research) and low silicon content (<15wt%, practical application), resulting in no significant improvement in the volume energy density of battery devices from both basic research and industrial development.

[0004] Carbon materials are widely used to buffer the volume expansion of silicon anodes and improve their electronic conductivity. However, the design of carbon structures for high volumetric capacity and high expansion silicon anode materials faces two major challenges:

[0005] 1) First, the use of a large amount of nano-silicon-carbon materials and the non-quantitative design of the carbon cage structure used to accommodate the volume change of silicon during the cycle (insufficient reserved space or too much unusable space) will greatly limit the increase in density or the stability of the cycle.

[0006] 2) Secondly, the huge stress generated by the volume expansion of silicon negative electrode materials, especially under the conditions of high density, high loading and high content of active materials, aggravates the structural instability of the entire electrode.

[0007] Therefore, a new negative electrode plate is urgently needed to solve the above problems. Summary of the invention

[0008] In order to solve the problems of the prior art, the present application provides a negative electrode plate, a battery and an electrical device, which can take into account the cycle and energy density requirements of the negative electrode plate.

[0009] In a first aspect, the present application provides a negative electrode plate, comprising a negative electrode current collector and a film layer provided on at least one surface of the negative electrode current collector, the film layer comprising a first film layer and a second film layer, the first film layer being located between the negative electrode current collector and the second film layer, the first film layer comprising a first negative electrode active substance, the second film layer comprising a second negative electrode active substance, the first negative electrode active substance comprising a first silicon-carbon composite material, the first silicon-carbon composite material comprising a first carbon matrix having a microporous structure, and a first silicon-based material distributed in the pore structure of the first carbon matrix, the second negative electrode active substance comprising a second silicon-carbon composite material, the second silicon-carbon composite material comprising a second carbon matrix having a mesoporous structure, and a second silicon-based material distributed in the pore structure of the second carbon matrix.

[0010] Furthermore, the surfaces of the first silicon-based material and the second silicon-based material both have a carbon coating layer, and the thickness of the carbon coating layer is 1 to 5 nm.

[0011] Furthermore, the median particle sizes of the first silicon-carbon composite material and the second silicon-carbon composite material are equal, and the median particle sizes of the first silicon-carbon composite material and the second silicon-carbon composite material are both 6-10 μm.

[0012] Furthermore, the first pore volume of the first carbon matrix is ​​0.5 to 0.8 cm 3 / g, the proportion of micropores in the pore size distribution is greater than 90%;

[0013] and / or,

[0014] The second pore volume of the second carbon matrix is ​​0.4 to 0.7 cm 3 / g, and the proportion of mesopores in the pore size distribution is greater than 40%.

[0015] Furthermore, the first negative electrode active material further includes a first graphite, the second negative electrode active material further includes a second graphite, and a first mass ratio of the first silicon-carbon composite material to the first graphite and a second mass ratio of the second silicon-carbon composite material to the second graphite are both (0.06-0.5):1.

[0016] Furthermore, the gram capacity of the first negative electrode active material and the gram capacity of the second negative electrode active material are equal.

[0017] Furthermore, the mass fraction of carbon element in the first silicon-carbon composite material and the second silicon-carbon composite material is both 50%±5%.

[0018] Furthermore, the first film layer also includes a first negative electrode conductive agent and a first negative electrode binder, and the second film layer also includes a second negative electrode conductive agent and a second negative electrode binder. The mass fraction of the second negative electrode binder in the second film layer is greater than the mass fraction of the first negative electrode binder in the first film layer. The mass fraction of the first negative electrode binder in the first film layer is 2% to 4%, and the mass fraction of the second negative electrode binder in the second film layer is 2.8% to 5%.

[0019] Furthermore, the first negative electrode binder and the second negative electrode binder include an aqueous binder, and the aqueous binder includes at least one of styrene-butadiene rubber, nitrile rubber, butadiene rubber, modified styrene-butadiene rubber, sodium polyacrylate, water-based polyacrylonitrile copolymer and polyacrylate.

[0020] Furthermore, the mass fraction of the first negative electrode conductive agent in the first film layer is equal to the mass fraction of the second negative electrode conductive agent in the second film layer, and the mass fraction of the first negative electrode conductive agent in the first film layer and the mass fraction of the second negative electrode conductive agent in the second film layer are both 1.5% to 2%.

[0021] Furthermore, the first negative electrode conductive agent and the second negative electrode conductive agent include at least one of conductive carbon black, gas-generated carbon fiber, graphene, and carbon nanotubes.

[0022] Furthermore, the method for preparing the negative electrode sheet includes:

[0023] The first film layer is coated on the surface of at least one side of the negative electrode current collector, and the surface density of the first film layer is 55-105 g / m 2 ;

[0024] The second film layer is coated on the surface of the first film layer away from the negative electrode current collector, and the surface density of the second film layer is 55-105 g / m 2 ;

[0025] The first film layer and the second film layer are cold pressed to obtain the negative electrode plate.

[0026] In a second aspect, the present application also provides a battery, which includes a positive electrode plate, the above-mentioned negative electrode plate and an electrolyte.

[0027] Furthermore, the electrolyte includes an organic solvent and a lithium salt, and the concentration of the lithium salt is 0.1 mol / L to 2.0 mol / L.

[0028] In a third aspect, the present application further provides an electrical device, wherein the electrical device comprises the above-mentioned battery.

[0029] According to the specific embodiments provided in this application, this application discloses the following technical effects:

[0030] The present application provides a negative electrode plate, a battery and an electrical device, which can take into account the cycle and energy density requirements of the negative electrode plate. Specifically, the negative electrode plate includes a negative electrode current collector and a film layer provided on at least one surface of the negative electrode current collector, the film layer includes a first film layer and a second film layer, the first film layer is located between the negative electrode current collector and the second film layer, the first silicon-carbon composite material in the first film layer includes a first carbon matrix with a microporous structure, and a first silicon-based material distributed in the pore structure of the first carbon matrix, and the first carbon matrix with a microporous structure can be used to improve the cycle stability of the negative electrode plate, the second silicon-carbon composite material in the second film layer includes a second carbon matrix with a mesoporous structure, and a second silicon-based material distributed in the pore structure of the second carbon matrix, and the second carbon matrix with a mesoporous structure can be used to improve the gram capacity and energy density of the negative electrode plate.

[0031] Furthermore, in the present application, the median particle sizes of the first silicon-carbon composite material and the second silicon-carbon composite material are equal, and the median particle sizes of the first silicon-carbon composite material and the second silicon-carbon composite material are both 6-10 μm. This arrangement can prevent the stress generated by the volume expansion difference of particles of different particle sizes during the cycle from damaging the electrode structure, thereby improving the stability of the negative electrode structure during the cycle.

[0032] Furthermore, in the present application, the gram capacity of the first negative electrode active material and the second negative electrode active material is equal, and such a setting can prevent unsaturated deintercalation and uneven charge distribution of the electrode sheet caused by the difference in gram capacity between the two layers.

[0033] Furthermore, in the present application, the surfaces of the first silicon-based material and the second silicon-based material both have a carbon coating layer, and the carbon coating layer can be used to improve conductivity and prevent side reactions between exposed silicon and the electrolyte.

[0034] Furthermore, in the present application, since the volume expansion of the second carbon matrix with a mesoporous structure in the second film layer is larger than that of the first carbon matrix with a microporous structure in the first film layer, a greater adhesion force is required to maintain the charge connectivity between the active particles. Therefore, the mass fraction of the second negative electrode binder in the second film layer is set to be greater than the mass fraction of the first negative electrode binder in the first film layer, thereby ensuring that the gram capacity is fully utilized while reducing electrical insulation and lithium plating. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] The disclosure of the present invention will become more easily understood with reference to the accompanying drawings. It is easy for those skilled in the art to understand that these drawings are only for illustrative purposes and are not intended to limit the scope of protection of the present invention. In addition, similar numbers in the figures are used to represent similar components, among which:

[0036] Figure 1 This is one of the structural schematic diagrams of the negative electrode sheet provided in the embodiment of the present application;

[0037] Figure 2 This is the second structural schematic diagram of the negative electrode plate provided in the embodiment of the present application. DETAILED DESCRIPTION

[0038] Some embodiments of the present invention are described below with reference to the accompanying drawings. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the protection scope of the present invention.

[0039] As shown in the background technology, carbon materials are widely used to buffer the volume expansion of silicon negative electrodes and improve their electronic conductivity. However, the carbon structure design for high volumetric capacity and high expansion silicon negative electrode materials faces two major challenges: first, the use of a large amount of nano-silicon-carbon materials and the non-quantitative design of the carbon cage structure used to absorb the volume change of silicon during the cycle (insufficient reserved space or too large unusable space) will greatly limit the increase in density or the stability of the cycle; secondly, the huge stress generated by the volume expansion of silicon negative electrode materials, especially under the conditions of high density, high loading, and high content of active materials, aggravates the structural instability of the entire electrode. In this regard, the present invention creatively proposes a negative electrode plate, a battery, and an electrical device that can take into account the cycle and energy density requirements of the negative electrode plate.

[0040] The following are optional technical solutions for this application, but are not intended to limit the technical solutions provided in this application. Through the following optional technical solutions, the technical objectives and beneficial effects of this application can be better achieved and realized.

[0041] In a first aspect, the present application provides a negative electrode sheet, such as Figures 1-2 As shown, the negative electrode plate includes a negative electrode collector 10 and a film layer arranged on at least one surface of the negative electrode collector 10, the film layer includes a first film layer 20 and a second film layer 30, the first film layer 20 is located between the negative electrode collector 10 and the second film layer 30, the first film layer 20 includes a first negative electrode active material, the second film layer 30 includes a second negative electrode active material, the first negative electrode active material includes a first silicon-carbon composite material, the first silicon-carbon composite material includes a first carbon matrix with a microporous structure, and a first silicon-based material distributed in the pore structure of the first carbon matrix, and the first carbon matrix with a microporous structure can be used to improve the cycle stability of the negative electrode plate; the second negative electrode active material includes a second silicon-carbon composite material, the second silicon-carbon composite material includes a second carbon matrix with a mesoporous structure, and a second silicon-based material distributed in the pore structure of the second carbon matrix, and the second carbon matrix with a mesoporous structure can be used to improve the gram capacity and energy density of the negative electrode plate.

[0042] In a specific embodiment, Figure 1 As shown, the negative electrode plate includes a negative electrode current collector 10 , a first film layer 20 and a second film layer 30 which are arranged in sequence, and the first film layer 20 is located between the negative electrode current collector 10 and the second film layer 30 .

[0043] In another specific embodiment, Figure 2 As shown, the negative electrode plate includes a second film layer 30, a first film layer 20, a negative electrode current collector 10, a first film layer 20 and a second film layer 30 which are arranged in sequence, that is, the first film layer 20 is arranged on the surfaces of both sides of the negative electrode current collector 10 facing away, and the second film layer 30 is arranged on the surfaces of the first film layer 20 on both sides.

[0044] Further, in the present application, the median particle size of the first silicon-carbon composite material and the second silicon-carbon composite material is equal, and the median particle size (D50) of the first silicon-carbon composite material and the second silicon-carbon composite material is 6-10 μm. Schematically, the median particle size (D50) of the first silicon-carbon composite material and the second silicon-carbon composite material can be 6, 7, 8, 9, 10 μm, and the specific point values ​​between the above point values. Due to the limited space and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range. This setting can prevent the stress generated by the volume expansion difference of particles of different particle sizes during the cycle from damaging the pole piece structure, thereby improving the stability of the negative pole piece structure during the cycle. It should be noted here that the median particle size (D50) described in the present application refers to particles smaller than this particle size accounting for 50% of the total. For the median particle size (D50) of each material, it can be measured and screened by methods known in the art, for example, it can be measured using a laser particle size analyzer and screened with sieves of different mesh sizes.

[0045] In the embodiment of the present application, the first pore volume of the first carbon matrix is ​​0.5-0.8 cm 3 / g, the proportion of micropores in the pore size distribution is greater than 90%. Schematically, the first pore volume of the first carbon matrix can be 0.5, 0.6, 0.7, 0.8 cm 3 / g, and specific values ​​between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer exhaustively list the specific values ​​included in the above range. The second pore volume of the second carbon matrix is ​​0.4-0.7cm 3 / g, the proportion of mesopores in the pore size distribution is greater than 40%. Schematically, the second pore volume of the second carbon matrix can be 0.4, 0.5, 0.6, 0.7 cm 3 / g, and specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range. The present application uses a first carbon matrix with a microporous structure to improve the cycle stability of the negative electrode plate, and uses a second carbon matrix with a mesoporous structure to improve the gram capacity and energy density of the negative electrode plate.

[0046] In a specific embodiment, the first carbon matrix with a microporous structure and the second carbon matrix with a mesoporous structure are prepared by sintering a precursor to form pores, and the precursor includes at least one of hard carbon, soft carbon or biomass carbon material.

[0047] Preferably, the surfaces of the first silicon-based material and the second silicon-based material are both provided with a carbon coating layer, and the provision of the carbon coating layer can increase the ion diffusion channel, thereby being used to improve the conductivity of the battery; at the same time, the provision of the carbon coating layer can also prevent the silicon from being exposed and reacting with the electrolyte, thereby making the battery have good cycle performance. Specifically, the thickness of the carbon coating layer is 1 to 5 nm. Schematically, the thickness of the carbon coating layer can be 1, 2, 3, 4, 5 nm, and specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0048] Further, in the present application, the gram capacity of the first negative electrode active material and the second negative electrode active material are equal, and such a setting can prevent the unsaturated deintercalation and uneven charge distribution of the pole piece caused by the difference in gram capacity in the two layers. The first negative electrode active material also includes a first graphite, and the second negative electrode active material also includes a second graphite. By adjusting the mixing ratio of the two active materials of graphite and silicon, the gram capacity of the first negative electrode active material and the second negative electrode active material can be equal. Specifically, the first mass ratio of the first silicon-carbon composite material and the first graphite and the second mass ratio of the second silicon-carbon composite material and the second graphite are both (0.06-0.5): 1. Schematically, the first mass ratio of the first silicon-carbon composite material and the first graphite and the second mass ratio of the second silicon-carbon composite material and the second graphite can be 0.06: 1, 0.1: 1, 0.2: 1, 0.3: 1, 0.4: 1, 0.5: 1, and the specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0049] Preferably, the mass fraction of carbon element in the first silicon-carbon composite material and the second silicon-carbon composite material is 50%±5%.

[0050] Furthermore, the first film layer also includes a first negative electrode binder, and the second film layer also includes a second negative electrode binder. Since the volume expansion of the second carbon matrix with a mesoporous structure in the second film layer is larger than that of the first carbon matrix with a microporous structure in the first film layer, a greater adhesion force is required to maintain the charge connectivity between the active particles. Therefore, the mass fraction of the second negative electrode binder in the second film layer is set to be greater than the mass fraction of the first negative electrode binder in the first film layer, thereby ensuring that the gram capacity is fully utilized while reducing electrical insulation and lithium precipitation. Specifically, the mass fraction of the first negative electrode binder in the first film layer is 2% to 4%. Schematically, the mass fraction of the first negative electrode binder in the first film layer can be 2%, 2.5%, 3%, 3.5%, 4%, and specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range. The mass fraction of the second negative electrode binder in the second film layer is 2.8% to 5%. Schematically, the mass fraction of the second negative electrode binder in the second film layer can be 2.8%, 3%, 3.5%, 4%, 4.5%, 5%, and specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the said range.

[0051] Furthermore, the first negative electrode binder and the second negative electrode binder include an aqueous binder, and the aqueous binder includes at least one of styrene-butadiene rubber, nitrile rubber, butadiene rubber, modified styrene-butadiene rubber, sodium polyacrylate, aqueous polyacrylonitrile copolymer and polyacrylate.

[0052] In a specific embodiment, the first film layer further includes a first thickener, and the second film layer further includes a second thickener. The first thickener and the second thickener include at least one of sodium carboxymethyl cellulose and polyether-modified silicone polymer.

[0053] Furthermore, the first film layer also includes a first negative electrode conductive agent, and the second film layer also includes a second negative electrode conductive agent, and the mass fraction of the first negative electrode conductive agent in the first film layer is equal to the mass fraction of the second negative electrode conductive agent in the second film layer. The design is based on the fact that the active material in the second film layer located on the surface of the pole piece is a mesoporous silicon-carbon material, whose kinetic performance is inferior to that of the microporous type, and the transmission distance of lithium ions in the particle phase is long, but the second film layer is close to the electrolyte, and the lithium ion concentration around its active particles is high, and the charge exchange rate is fast; while the microporous silicon-carbon material of the first film layer is the opposite, the transmission distance of lithium ions in the active particle phase is short, but the transmission distance of lithium ions from the electrolyte to the surface of the active particles is long, and the overall pole piece potential difference is small, so there is no need to use the difference in conductive agents to evenly distribute the charge.

[0054] Specifically, the mass fraction of the first negative electrode conductive agent in the first film layer and the mass fraction of the second negative electrode conductive agent in the second film layer are both 1.5% to 2%. Schematically, the mass fraction of the first negative electrode conductive agent in the first film layer and the mass fraction of the second negative electrode conductive agent in the second film layer can be 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, and specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the said range.

[0055] In the embodiment of the present application, the first negative electrode conductive agent and the second negative electrode conductive agent include at least one of conductive carbon black, gas-generated carbon fiber, graphene, and carbon nanotubes.

[0056] The present application has no particular limitation on the negative electrode current collector, as long as it has conductivity and does not cause chemical changes in the battery without violating the inventive concept of the present application. Optionally, the negative electrode current collector can be one of homogeneous copper foil, porous copper foil and copper foil with a carbon coating layer.

[0057] As a preferred embodiment, in the first film layer, the mass fractions of the first negative electrode active material, the first negative electrode conductor, and the first negative electrode binder are 94-96.5%, 1.5%-2%, and 2%-4%, respectively; in the second film layer, the mass fractions of the second negative electrode active material, the second negative electrode conductor, and the second negative electrode binder are 93-95.7%, 1.5%-2%, and 2.8%-5%, respectively.

[0058] The method for preparing the negative electrode sheet comprises:

[0059] S1: Coating the first film layer 20 to the surface of at least one side of the negative electrode current collector 10, wherein the surface density of the first film layer 20 is 55-105 g / m 2 The coating can be at least one of extrusion coating, transfer coating, and spray coating.

[0060] S2: Coat the second film layer 30 on the surface of the first film layer 20 away from the negative electrode current collector 10, and the surface density of the second film layer 30 is 55-105 g / m 2 .

[0061] S3: cold pressing the first film layer 20 and the second film layer 30 to obtain the negative electrode sheet.

[0062] In a second aspect, the present application also provides a battery, which includes a positive electrode plate, the above-mentioned negative electrode plate and an electrolyte.

[0063] The positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer coated on at least one surface of the positive electrode current collector, wherein the positive electrode active material layer comprises a positive electrode active material, a positive electrode conductive agent and a positive electrode binder.

[0064] There is no particular restriction on the positive electrode current collector in the embodiments of the present application, as long as it has conductivity and does not cause chemical changes in the battery. Specifically, the positive electrode current collector includes but is not limited to any one of aluminum, nickel or stainless steel, such as the positive electrode current collector is aluminum foil, etc. The shape of the positive electrode current collector includes but is not limited to metal foil, metal grid, metal mesh, etc., and the user can choose according to actual needs, and no specific limitation is made here.

[0065] The positive electrode active material is a compound that can reversibly embed and deintercalate lithium. The positive electrode active material in the present application can be any positive electrode active material known in the art. For example, the positive electrode active material includes but is not limited to a chemical formula such as Li c Ni h Co y M z O 2-b N b (wherein 0.95≤c≤1.2, h>0, y≥0, z≥0, and h+y+z=1, 0≤b≤1, M is selected from a combination of one or more of Mn and Al, and N is selected from a combination of one or more of F, P, and S) The positive electrode active material may also be, but is not limited to, LiCoO 2 、LiNiO 2 , LiV O 2 、LiCrO 2 、LiMn 2 O 4 、LiCoMnO 4 , Li 2 NiMn 3 O 8 、LiNi 0.5 Mn 1.5 O 4 、LiCoPO 4 、LiMnPO 4 、LiFePO 4 、LiNiPO 4 、LiCoFSO 4 , CuS 2 , FeS 2 、MoS 2 、NiS、TiS 2 The positive electrode active material may also be subjected to a modification treatment. The method for modifying the positive electrode active material should be known to those skilled in the art. For example, the positive electrode active material may be modified by coating, doping, etc. The material used for the modification treatment may include but is not limited to a combination of one or more of Al, B, P, Zr, Si, Ti, Ge, Sn, Mg, Ce, W, etc.

[0066] The positive electrode conductor is a material that provides conductivity without causing adverse chemical reactions in the battery. In the embodiment of the present application, the positive electrode conductor may include a carbon-based material, powdered nickel or other metal particles or a conductive polymer. The carbon-based material may include particles such as carbon black, graphite, super-P, acetylene black (such as KETCHENTM black or DENKATM black), carbon fibers and nanotubes, graphene, etc. Examples of conductive polymers include polyaniline, polythiophene, polyacetylene, polypyrrole, poly (3,4-ethylenedioxythiophene) polystyrene sulfonate, etc. Preferably, the positive electrode conductor includes one or more of conductive carbon black (Super-P), acetylene black, Ketjen black, carbon nanotubes (CNTs), graphene (rGO), activated carbon, and carbon nanofibers (CNFs).

[0067] The positive electrode binder is a component that helps the positive electrode active material and the positive electrode conductor to bond with each other and with the positive electrode current collector. In the embodiment of the present application, the positive electrode binder includes but is not limited to polytetrafluoroethylene (PTFE), sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), polyvinylidene fluoride (PVDF), nitrile rubber (NBR), styrene ethylene butylene styrene copolymer (SEBS), styrene butadiene styrene copolymer (SBS), lithium polyacrylate (LiPAA), sodium polyacrylate (NaPAA), sodium alginate, lithium alginate. One or more. Users can choose according to actual needs, and no specific limitation is made here.

[0068] In the embodiment of the present application, the electrolyte includes an organic solvent and a lithium salt, wherein the organic solvent may use any organic solvent without particular limitation, as long as it can serve as a medium through which ions participating in the electrochemical reaction of the battery can move. Specifically, as organic solvents, there can be used: ester solvents, such as methyl acetate, ethyl acetate, γ-butyrolactone or ε-caprolactone; ether solvents, such as dibutyl ether or tetrahydrofuran; ketone solvents, such as cyclohexanone; aromatic hydrocarbon solvents, such as benzene or fluorobenzene; carbonate solvents, such as dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC) or propylene carbonate (PC); alcohol solvents, such as ethanol or isopropanol; nitriles, such as R-CN (wherein R is a linear, branched or cyclic C2-C20 hydrocarbon group, and may include a double bond aromatic ring or an ether bond); amides, such as dimethylformamide; dioxolanes, such as 1,3-dioxolane; or cyclopentane sulfones.

[0069] Any compound can be used as the lithium salt without particular limitation as long as it can provide lithium ions in the battery. Specifically, as the lithium salt, LiPF 6 、LiClO4 、LiAsF 6 , LiBF 4 、LiSbF 6 、LiAlO 4 、LiAlCl 4 、LiCF 3 SO 3 ,LiC 4 F 9 SO 3 、LiN(C 2 F 5 SO 3 ) 2 、LiN(C 2 F 5 SO 2 ) 2 、LiN(CF 3 SO 2 ) 2 , LiCl, LiI or LiB(C 2 O 4 ) 2 As a preferred embodiment, the concentration of the lithium salt is 0.1 mol / L to 2.0 mol / L. When the concentration of the lithium salt is within the above range, the electrolyte can have appropriate conductivity and viscosity, thereby exhibiting excellent functions, and lithium ions can move effectively.

[0070] In the embodiment of the present application, the battery also includes a separator, and the main function of the separator is to separate the negative electrode plate from the positive electrode plate and provide a path for the movement of lithium ions. Any separator can be used without particular limitation, as long as it is a separator commonly used in batteries. In particular, a separator having excellent wettability to the electrolyte and low resistance to the movement of ions in the electrolyte is preferred. Specifically, a porous polymer film can be used, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure having two or more layers thereof. In addition, a typical porous non-woven fabric can be used, for example, a non-woven fabric formed of glass fiber, polyethylene terephthalate fiber, etc. having a high melting point. In addition, a coated separator containing a ceramic component or a polymer material can be used to ensure heat resistance or mechanical strength, and can be selectively used in a single-layer or multi-layer structure.

[0071] In a third aspect, the present application further provides an electrical device, which includes the above-mentioned battery. The electrical device includes, but is not limited to, mobile devices, electric vehicles, spacecraft, electric toys, and electric tools. Mobile devices can be mobile phones, laptops, etc.; electric vehicles can be pure electric vehicles, hybrid electric vehicles, electric bicycles, etc.; spacecraft can be airplanes, rockets, spacecrafts, etc.; electric toys can be game consoles, electric car toys, electric ship toys, electric airplane toys, etc.; electric tools can be metal cutting electric tools, grinding electric tools, assembly electric tools, etc.

[0072] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents and instruments are not specified, they are all conventional products that can be purchased commercially.

[0073] Hereinafter, the embodiments of the present invention will be described in more detail by way of examples. However, the embodiments of the present invention are not limited only to these examples.

[0074] Example 1

[0075] 1) Preparation of negative electrode sheet

[0076] The components of the first film layer were mixed, deionized water was added and stirred into a uniform slurry, and the slurry was evenly coated on the surface of at least one side of the negative electrode current collector (8um copper foil was used for the negative electrode current collector). The coating surface density of the first film layer was 84.5g / m 2 .

[0077] Among them, the first film layer includes the first negative electrode active material (the design gram capacity of the first negative electrode active material is 450mAh / g), the first negative electrode conductive agent (the first negative electrode conductive agent is selected from SP and water-based SWCNT) and the first negative electrode binder (the first negative electrode binder is selected from water-based PAA and SBR, and the mass ratio of water-based PAA to SBR is 2:1), the first negative electrode active material includes the first silicon-carbon composite material (the D50 of the first silicon-carbon composite material is 8μm) and artificial graphite (the D50 of artificial graphite is 11μm), and the mass ratio of artificial graphite to the first silicon-carbon composite material in the first negative electrode active material is 2:8. The first silicon-carbon composite material includes a microporous biomass hard carbon substrate and nano-silicon deposited on the biomass hard carbon substrate, and the surface of the nano-silicon has a carbon coating layer, wherein the micropores in the microporous biomass hard carbon substrate account for 92%. The mass ratio of each component in the first film layer is: first negative electrode active material: SP: SWCNT: PAA: SBR = 95.8%: 1.42%: 0.08%: 1.8%: 0.9%.

[0078] The components of the second film layer were mixed, deionized water was added and stirred into a uniform slurry, and the slurry was evenly coated on the surface of the first film layer away from the negative electrode current collector. The coating surface density of the second film layer was 84.4 g / m 2 .

[0079] Among them, the second film layer includes a second negative electrode active material (the design gram capacity of the second negative electrode active material is 450mAh / g), a second negative electrode conductive agent (the second negative electrode conductive agent is selected from SP and water-based SWCNT) and a second negative electrode binder (the second negative electrode binder is selected from water-based PAA and SBR, and the mass ratio of water-based PAA to SBR is 2:1), the second negative electrode active material includes a second silicon-carbon composite material (the D50 of the second silicon-carbon composite material is 8μm) and artificial graphite (the D50 of artificial graphite is 11μm), and the mass ratio of artificial graphite to the second silicon-carbon composite material in the second negative electrode active material is 2:8. The second silicon-carbon composite material includes a mesoporous biomass hard carbon substrate and nano-silicon deposited on the mesoporous biomass hard carbon substrate, and the surface of the nano-silicon has a carbon coating layer, wherein the mesopores in the mesoporous biomass hard carbon substrate account for 50%. The mass ratio of each component in the second film layer is: second negative electrode active material: SP: SWCNT: PAA: SBR = 95.5%: 1.42%: 0.08%: 2%: 1%.

[0080] The first film layer and the second film layer are dried and cold pressed to obtain the negative electrode sheet, and the compaction density is 1.55g / cm 3 .

[0081] 2) Preparation of positive electrode

[0082] The positive electrode active material is ternary nickel cobalt lithium manganese oxide LiNi 0.8 Co 0.1 Mn 0.11 O 2 The positive electrode conductive agent is SP and oily carbon nanotubes, the positive electrode adhesive is PVDF5130, and the positive electrode current collector is 13μm aluminum foil. The positive electrode active material, positive electrode conductive agent, and positive electrode adhesive are mixed in a mass ratio of 97:2:1, and NMP is added and stirred to form a uniform and stable positive electrode slurry. The positive electrode slurry is evenly coated on the positive electrode current collector, and the coating surface density is 172g / m 2 After drying and cold pressing, the positive electrode sheet is obtained, and the compaction density is 3.4g / cm 3 .

[0083] 3) Isolation film

[0084] The isolation film uses a polypropylene film as the isolation film base film with a thickness of 12 μm.

[0085] 4) Preparation of electrolyte

[0086] Ethylene carbonate, ethyl methyl carbonate and diethyl carbonate are mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and then a solute LiPF is added to the organic solvent. 6 Dissolve and mix evenly to obtain an electrolyte solution, in which LiPF 6 The concentration is 1.2 mol / L.

[0087] 5) Preparation of batteries

[0088] The positive electrode sheet, separator, and negative electrode sheet are arranged in order and assembled by winding; the electrolyte is injected into the dry battery cell, soaked for 24 hours, and then formed at 45°C. The formation process is: charge to 3.4V at 0.05C, and then charge to 3.75V at 0.2C; the battery is prepared after aging at room temperature for 24 hours.

[0089] 6) Testing of negative electrode and battery

[0090] The negative electrode sheet prepared in step 1) was subjected to membrane resistance and full charge rebound tests, and the battery prepared in step 5) was subjected to first efficiency, 1C cycle, and DCR tests.

[0091] Example 2

[0092] The difference between Example 2 and Example 1 is that the mass ratios of the components in the first film layer and the second film layer are different. In Example 2, the mass ratios of the components in the first film layer are: first negative electrode active material: SP: SWCNT: PAA: SBR = 96.2%: 1.42%: 0.08%: 1.6%: 0.7%; the mass ratios of the components in the second film layer are: second negative electrode active material: SP: SWCNT: PAA: SBR = 95.8%: 1.42%: 0.08%: 1.8%: 0.9%.

[0093] Example 3

[0094] The difference between Example 3 and Example 1 is that the mass ratios of the components in the first film layer and the second film layer are different. In Example 3, the mass ratios of the components in the first film layer are: first negative electrode active material: SP: SWCNT: PAA: SBR = 95%: 1.45%: 0.12%: 2.1%: 1.15%; the mass ratios of the components in the second film layer are: second negative electrode active material: SP: SWCNT: PAA: SBR = 94%: 1.45%: 0.12%: 2.8%: 1.63%.

[0095] Example 4

[0096] The difference between Example 4 and Example 1 is that the first silicon-carbon composite material is different from the second silicon-carbon composite material. In Example 4, the D50 of the first silicon-carbon composite material is 9.3 μm, and the first silicon-carbon composite material includes a microporous hard carbon substrate and nano-silicon deposited on the hard carbon substrate, and the surface of the nano-silicon has a carbon coating layer, wherein the micropores in the microporous hard carbon substrate account for 90%; the D50 of the second silicon-carbon composite material is 9.3 μm, and the second silicon-carbon composite material includes a mesoporous hard carbon substrate and nano-silicon deposited on the hard carbon substrate, and the surface of the nano-silicon has a carbon coating layer, wherein the mesopores in the mesoporous hard carbon substrate account for 44%.

[0097] Comparative Example 1

[0098] The difference between Comparative Example 1 and Example 1 is that the preparation of the negative electrode plate is different.

[0099] In Comparative Example 1, the preparation method of the negative electrode sheet is:

[0100] Mix the components in the film layer, add deionized water and stir to form a uniform slurry, and evenly apply the slurry to the surface of at least one side of the negative electrode current collector (8um copper foil is used for the negative electrode current collector). The coating surface density of the film layer is 84.5g / m 2 .

[0101] Among them, the membrane layer includes the first negative electrode active material (the design gram capacity of the first negative electrode active material is 450mAh / g), the first negative electrode conductive agent (the first negative electrode conductive agent is selected from SP and water-based SWCNT) and the first negative electrode binder (the first negative electrode binder is selected from water-based PAA and SBR, and the mass ratio of water-based PAA to SBR is 2:1), the first negative electrode active material includes the first silicon-carbon composite material (the D50 of the first silicon-carbon composite material is 8μm) and artificial graphite (the D50 of artificial graphite is 11μm), and the mass ratio of artificial graphite to the first silicon-carbon composite material in the first negative electrode active material is 2:8. The first silicon-carbon composite material includes a microporous biomass hard carbon substrate and nano-silicon deposited on the biomass hard carbon substrate, and the surface of the nano-silicon has a carbon coating layer, wherein the micropores in the microporous biomass hard carbon substrate account for 92%. The mass ratio of each component in the film layer is: first negative electrode active material: SP: SWCNT: PAA: SBR = 95.8%: 1.42%: 0.08%: 1.8%: 0.9%.

[0102] The film layer is dried and cold pressed to obtain the negative electrode sheet, and the compaction density is 1.55g / cm 3 .

[0103] Comparative Example 2

[0104] The difference between Comparative Example 2 and Example 1 is that the preparation of the negative electrode plate is different.

[0105] In Comparative Example 2, the preparation method of the negative electrode sheet is:

[0106] Mix the components in the film layer, add deionized water and stir to form a uniform slurry, and evenly apply the slurry to the surface of at least one side of the negative electrode current collector (8um copper foil is used for the negative electrode current collector). The coating surface density of the film layer is 84.5g / m 2 .

[0107] Among them, the membrane layer includes a second negative electrode active material (the design gram capacity of the second negative electrode active material is 450mAh / g), a second negative electrode conductive agent (the second negative electrode conductive agent is selected from SP and water-based SWCNT) and a second negative electrode binder (the second negative electrode binder is selected from water-based PAA and SBR, and the mass ratio of water-based PAA to SBR is 2:1), the second negative electrode active material includes a second silicon-carbon composite material (the D50 of the second silicon-carbon composite material is 8μm) and artificial graphite (the D50 of artificial graphite is 11μm), and the mass ratio of artificial graphite to the second silicon-carbon composite material in the second negative electrode active material is 2:8. The second silicon-carbon composite material includes a mesoporous biomass hard carbon substrate and nano-silicon deposited on the mesoporous biomass hard carbon substrate, and the surface of the nano-silicon has a carbon coating layer, wherein the mesopores in the mesoporous biomass hard carbon substrate account for 50%. The mass ratio of each component in the film layer is: second negative electrode active material: SP: SWCNT: PAA: SBR = 95.5%: 1.42%: 0.08%: 2%: 1%.

[0108] The film layer is dried and cold pressed to obtain the negative electrode sheet, and the compaction density is 1.55g / cm 3 .

[0109] Comparative Example 3

[0110] The difference between Comparative Example 3 and Example 1 is that the preparation of the negative electrode plate is different.

[0111] In Comparative Example 3, the first silicon-carbon composite material in the first film layer includes a mesoporous biomass hard carbon substrate and nano-silicon deposited on the mesoporous biomass hard carbon substrate, the surface of the nano-silicon has a carbon coating layer, wherein the mesopores in the mesoporous biomass hard carbon substrate account for 50%; the second silicon-carbon composite material in the second film layer includes a microporous biomass hard carbon substrate and nano-silicon deposited on the biomass hard carbon substrate, the surface of the nano-silicon has a carbon coating layer, wherein the micropores in the microporous biomass hard carbon substrate account for 92%.

[0112] Test methods and conditions

[0113] 1. Membrane resistance test

[0114] Experimental equipment: Sheet resistor meter, model BER1300 (IEST Yuanneng Technology), electrode diameter is 14 mm.

[0115] The membrane resistance test was performed on the negative electrode sheets prepared in the embodiment and the comparative example, and the test method was as follows:

[0116] 1) Do not place the negative electrode on the membrane resistor meter, set the test pressure on the MRMS software, apply a pressure of 25MPa, hold the pressure for 25s, click to start the test, and return the electrode to zero after the result appears.

[0117] 2) Cut the rolled negative electrode sheet into a rectangular size of about 5cm×10cm, place it between the two electrodes of the membrane resistance meter, set the test parameters on the MRMS software, and start the test. The software automatically reads the thickness, resistance, resistivity, conductivity and other data of the negative electrode sheet. Six positions are randomly selected for testing on each negative electrode sheet, and the average value is the membrane resistance value of the negative electrode sheet.

[0118] 2. Full charge rebound test

[0119] 1) Use a micrometer to measure the negative electrode sheet after rolling, and record the thickness of the negative electrode sheet as C1;

[0120] 2) Charge the divided battery to 100% SOC at a charging current of 1C according to the standard test process, disassemble the fully charged battery, measure the fully charged negative electrode sheet with a micrometer, and record the electrode sheet thickness as C2;

[0121] 3) Full charge rebound rate = (C2-C1) / C1.

[0122] 3. Battery initial performance test

[0123] 1) In a 25°C constant temperature box, charge the battery to 4.25V at 1C current, let it stand for 30 minutes, then charge it to 4.25V at 0.2C current, and record the total charge capacity A;

[0124] 2) After standing for 30 minutes, discharge at 1C current to 2.5V and record the discharge capacity B;

[0125] 3) First effect = B / A.

[0126] 4. 25℃ battery standard 1C / 1C cycle test

[0127] 1) Place the battery in a 25°C constant temperature box for 30 minutes and charge it to 4.25V at 1C current;

[0128] 2) After standing for 30 minutes, discharge to 2.5V at 1C current;

[0129] 3) Cycle 1) to 2) and record the discharge capacity Cn, where n is the number of cycles;

[0130] The capacity retention rate at a certain cycle number n is the ratio of the capacity Cn at that cycle number to the first cycle capacity C1. The test is stopped when the discharge capacity of the battery is lower than 80% of the initial capacity.

[0131] 5. Battery DCR test

[0132] 1) At 25°C, charge the fresh battery to 4.25V at 1C.

[0133] 2) After standing for 30 minutes, discharge at 1C for 30 minutes (adjust to 50% SOC);

[0134] 3) Let stand for 60 minutes;

[0135] 4) Discharge at a rate of 2C for 30s, record the open circuit voltage U1, U2 and discharge current I before and after discharge, battery DCR = (U1-U2) / I, and the fresh battery DCR is D1;

[0136] After the 1C cycle test, the battery is subjected to a DCR test according to the process of 1) to 4), and the DCR after the cycle is obtained as D2;

[0137] DCR growth rate = (D2-D1) / D1.

[0138] The test results of the negative electrode sheets and batteries prepared in Examples 1-4 and Comparative Examples 1-3 are shown in Table 1.

[0139] Table 1

[0140]

[0141] From the test results in Table 1, we can see that:

[0142] 1) Compared with Comparative Examples 1 to 3, Examples 1 to 4 have excellent cycle performance, especially after the content of the first negative electrode binder and the second negative electrode binder in Example 2 is reduced compared with that in Example 1, the cycle performance of the battery is still better than that of Comparative Examples 1 to 3, proving that the layered negative electrode sheet has excellent structural stability.

[0143] 2) The membrane resistance and DCR growth after cycling of Examples 1 to 4 are smaller than those of Comparative Examples 1 to 3, which proves that the layered design can effectively improve the integrity of the charge transfer network of the electrode and reduce the electrochemical polarization of the electrode caused by the difference in charge distribution.

[0144] 3) Compared with Comparative Examples 1 to 3, the full charge rebound ratio of the negative electrode sheets of Examples 1 to 4 is also greatly reduced, which proves that the layered negative electrode sheets of the present invention can effectively reduce the volume expansion and contraction caused by silicon deintercalation and lithium on the structural degradation of the electrode layer, and can prevent the stress caused by the volume expansion difference of particles of different particle sizes during the cycle from damaging the electrode structure. Therefore, the structural stability of the negative electrode sheet during the cycle can be improved.

Claims

1. A negative electrode plate, characterized in that: The negative electrode plate includes a negative electrode current collector and a film layer arranged on at least one surface of the negative electrode current collector, the film layer includes a first film layer and a second film layer, the first film layer is located between the negative electrode current collector and the second film layer, the first film layer includes a first negative electrode active material, the second film layer includes a second negative electrode active material, the first negative electrode active material includes a first silicon-carbon composite material, the first silicon-carbon composite material includes a first carbon matrix with a microporous structure, and a first silicon-based material distributed in the pore structure of the first carbon matrix, the second negative electrode active material includes a second silicon-carbon composite material, the second silicon-carbon composite material includes a second carbon matrix with a mesoporous structure, and a second silicon-based material distributed in the pore structure of the second carbon matrix.

2. The negative electrode sheet according to claim 1, characterized in that: The surfaces of the first silicon-based material and the second silicon-based material both have a carbon coating layer, and the thickness of the carbon coating layer is 1-5 nm.

3. The negative electrode sheet according to claim 1, characterized in that: The median particle sizes of the first silicon-carbon composite material and the second silicon-carbon composite material are equal, and the median particle sizes of the first silicon-carbon composite material and the second silicon-carbon composite material are both 6-10 μm.

4. The negative electrode sheet according to claim 1, characterized in that: The first pore volume of the first carbon matrix is ​​0.5 to 0.8 cm 3 / g, the proportion of micropores in the pore size distribution is greater than 90%; and / or, The second pore volume of the second carbon matrix is ​​0.4 to 0.7 cm 3 / g, and the proportion of mesopores in the pore size distribution is greater than 40%.

5. The negative electrode sheet according to claim 1, characterized in that: The first negative electrode active material further includes a first graphite, the second negative electrode active material further includes a second graphite, and a first mass ratio of the first silicon-carbon composite material to the first graphite and a second mass ratio of the second silicon-carbon composite material to the second graphite are both (0.06-0.5):

1.

6. The negative electrode sheet according to claim 1, characterized in that: The mass fraction of carbon element in the first silicon-carbon composite material and the second silicon-carbon composite material is 50%±5%.

7. The negative electrode sheet according to any one of claims 1 to 6, characterized in that: The first film layer also includes a first negative electrode conductor and a first negative electrode binder, and the second film layer also includes a second negative electrode conductor and a second negative electrode binder. The mass fraction of the second negative electrode binder in the second film layer is greater than the mass fraction of the first negative electrode binder in the first film layer. The mass fraction of the first negative electrode binder in the first film layer is 2% to 4%, and the mass fraction of the second negative electrode binder in the second film layer is 2.8% to 5%.

8. The negative electrode sheet according to claim 7, characterized in that: The mass fraction of the first negative electrode conductive agent in the first film layer is equal to the mass fraction of the second negative electrode conductive agent in the second film layer, and the mass fraction of the first negative electrode conductive agent in the first film layer and the mass fraction of the second negative electrode conductive agent in the second film layer are both 1.5% to 2%.

9. A battery, characterized in that: It comprises a positive electrode sheet, a negative electrode sheet as claimed in any one of claims 1 to 8 and an electrolyte.

10. An electrical device, characterized in that: A battery comprising the battery of claim 9.

Citation Information

Cited By

  • Negative plate and battery

    CN119764337A

  • Battery cell, battery apparatus and electrical apparatus

    WO2026118564A1

  • Battery cell and manufacturing method therefor, battery, and electric device

    WO2026200176A1