Sodium-ion battery layered positive electrode material with low residual alkali content and preparation method of sodium-ion battery layered positive electrode material
By generating NaFePO4 and Na3FePO4C03 coatings on the surface of the positive electrode material of the sodium ion battery, the air stability and residual alkali problems of the O3 phase layered material of the sodium ion battery are solved, and its circulation performance and stability are significantly improved.
Patent Information
- Application Number
- CN202411411809.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-10-11
AI Technical Summary
The sodium ion battery O3-phase layered material has poor air chemical stability and high residual alkali content on the surface, which hinders its practical feasibility in the electrode preparation process. It is difficult for the prior art to effectively reduce the residual alkali content to improve the circulation performance of the material.
NaFePO4 and Na3FePO4C03 are used as surface coatings to prepare the quaternary precursor material through co-precipitation reaction. After high temperature sintering, the ball milling reaction is performed using FeC2O4·H2O and (NH4)2HPO4 to form a NaFePO4 cladding layer, and then it is black with acetylene. Mixed to form a Na3FePO4C03 coating layer, consumes residual alkali on the surface, and reduces the residual alkali content of the positive electrode material of the sodium ion battery.
It significantly reduces the residual alkali content of the positive electrode material of sodium ion battery, improves its stability and circulation performance in the air, reduces gas production during the circulation, enhances the thickness and conductivity of the material, and improves the battery. comprehensive performance.
Smart Images

Figure CN118919710A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sodium ion battery positive electrode materials, and specifically relates to a sodium ion battery layered positive electrode material with low residual alkali content and a preparation method thereof. Background Art
[0002] The urgency of developing clean energy technologies has led to extensive research on high-energy, low-cost electrical energy storage devices for large-scale grid storage. From the perspective of cost and sustainability, the use of sodium-ion batteries is more attractive than lithium-ion batteries because sodium-ion batteries are more abundant and less expensive than lithium-ion batteries.
[0003] The prospect of O3-phase layered materials for sodium-ion batteries is challenging due to their poor chemical stability to air and high residual alkali content on the surface. When preparing cathode sheets, the high residual alkali content triggers the defluorination of polyvinylidene fluoride (PVDF) binder, leading to particle agglomeration and slurry gelation during electrode preparation, which greatly hinders the practical feasibility of O3-phase layered cathode materials.
[0004] At present, there are related literature reports on related research on reducing the residual alkali content on the surface of materials. For example, the patent document CN 111370664A discloses that by introducing volatile acidic gas into an atmosphere rotary furnace for 1-5 hours, the surface residual alkali of the layered positive electrode material of the sodium ion battery is removed by the volatile acidic gas, and the layered positive electrode material with reduced surface residual alkali is obtained after cooling to room temperature. Although this method significantly reduces the residual alkali content of the layered positive electrode material and reduces the pH value, this method has high requirements for equipment and is not conducive to large-scale production.
[0005] For example, the patent document CN 116613294A discloses that an excellent crystal structure can be obtained by preparing two precursors with different particle sizes, sintering and mixing them separately, and controlling the sintering, coating and other conditions; the sodium ion battery obtained by the preparation method has a specific XRD crystal structure, which improves the surface stability of the positive electrode material of the sodium ion battery, prevents the side reaction with the electrolyte and the dissolution of metal ions, and the prepared sodium ion battery positive electrode material has a lower residual alkali content. Although the specific XRD crystal structure makes the prepared sodium ion battery positive electrode material have a lower residual alkali content, the specific XRD crystal structure is not easy to control.
[0006] For example, the patent document CN 117466346A discloses a sodium ion battery positive electrode material and a preparation method thereof, and a sodium ion battery. The preparation method comprises the following steps: weighing a sodium electric precursor of nickel manganese iron hydroxide, a sodium source and an additive and mixing them at high speed; sintering the mixed material once at high temperature; adding a first coating material oxalic acid; mixing the powder at high speed; adding a second coating material and a third coating material to the powder after standing, wherein the second coating material is a metal salt additive including any one or a combination of nickel carbonate, nickel oxalate and ferrous oxalate, and the third coating material is a metal oxide additive including any one or a combination of titanium dioxide, tungsten trioxide and molybdenum trioxide; after mixing the materials at high speed, sintering them at high temperature twice to obtain the desired sodium ion battery positive electrode material. In the preparation method, during the primary sintering and secondary sintering processes, the first coating material is oxalic acid, which acid-dissolves the residual alkali in the mixing stage to improve the reaction activity and make it easier to combine with other coated metal elements, thereby reducing the residual alkali sodium ions in the system; the second coating material reacts quickly with the residual alkali in the reaction system to generate a corresponding sodium-rich structure sodium electric material, thereby increasing the capacity of the positive electrode material; the third coating material improves the conductivity of the surface of the positive electrode material and increases the thickness of the coating layer of the positive electrode material; the first coating material, the second coating material and the third coating material are coated by secondary sintering to achieve low residual alkali, reduced side reactions and thus reduced gas production, thereby improving the cycle performance and enhancing the comprehensive performance, thereby providing a sodium ion battery positive electrode material and a sodium ion battery with low residual alkali, increased coating layer thickness, good coating layer conductivity, less gas production, and better capacity and cycle performance. In the process of reducing the residual alkali on the surface of the positive electrode material of the sodium ion battery, the method sequentially adds oxalic acid and a metal additive step by step to reduce the residual alkali on the surface of the positive electrode material of the sodium ion battery while generating a corresponding sodium-rich structure of the sodium-electric material, so as to improve the capacity and cycle performance of the sodium ion battery. However, the best reduction in the residual alkali content in the embodiment is 4600ppm, i.e., 0.46%. Therefore, the effect of reducing the residual alkali on the surface of the positive electrode material of the sodium ion battery by reacting the metal salt additive with the residual alkali hydrolyzed by oxalic acid to form the corresponding sodium-rich structure still needs to be further improved. Summary of the invention
[0007] The technical problem solved by the present invention is to provide a sodium ion battery layered positive electrode material with low residual alkali content and a preparation method thereof. The sodium ion battery positive electrode material prepared by the method has excellent air stability, low residual alkali content, stable material processing performance, and the sodium ion battery prepared by the method has excellent cycle stability performance at high voltage.
[0008] The present invention adopts the following technical solutions to solve the above technical problems. A layered cathode material for a sodium-ion battery with a low residual alkali content is composed of a surface coating layer and an O3-type sodium-ion battery cathode material. The surface coating layer is NaFePO4 and Na3FePO4C03, and the O3-type sodium-ion battery cathode material is Na x Ni a Mn b Fe c Cu d M (1-a-b-c-d) O2, where 0.8 < x < 1.2, 0.1 < a < 0.7, 0.1 < b < 0.7, 0.1 < c < 0.7, 0.1 ≤ d ≤ 0.7, and M is one or more of Mg, Al, Ti, Co, Zn, Y, or Zr.
[0009] The preparation method of the layered cathode material for a sodium-ion battery with a low residual alkali content according to the present invention specifically comprises the following preparation steps: Step S1, mixing a solution containing a soluble nickel salt, a soluble ferrous salt, a soluble manganese salt, and a soluble copper salt to carry out a coprecipitation reaction to obtain a quaternary precursor material; Step S2, mixing the quaternary precursor material obtained in Step S1 with a sodium source and a compound containing M, and then subjecting the mixture to high-temperature sintering to obtain a sodium-ion battery cathode material; Step S3, mixing the sodium-ion battery cathode material obtained in Step S2 with FeC2O4·H2O and (NH4)2HPO4, and then using a wet planetary ball mill to mix them evenly. During the mixing process, FeC2O4·H2O and (NH4)2HPO4 react with the residual alkali on the surface of the sodium-ion battery cathode material to generate NaFePO4. Then, the mixture is dried and ground, and then the obtained mixture is subjected to high-temperature sintering and pulverization to obtain a sodium-ion battery cathode material coated with NaFePO4; Step S4, mixing the sodium-ion battery cathode material coated with NaFePO4 obtained in Step S3 with acetylene black, and then using a wet planetary ball mill to mix them evenly in an inert gas atmosphere. During the mixing process, NaFePO4 coated on the surface of the sodium-ion battery cathode material coated with NaFePO4 reacts with the residual alkali remaining on the surface to generate Na3FePO4CO3, thereby obtaining a layered cathode material for a sodium-ion battery with a low residual alkali content coated with NaFePO4 and Na3FePO4CO3 Further, in step S1, the soluble nickel salt is one or more of nickel sulfate, nickel chloride or nickel nitrate; the soluble ferrous salt is one or more of ferrous sulfate, ferrous chloride or ferrous nitrate; the soluble manganese salt is one or more of manganese sulfate, manganese chloride or manganese nitrate; the soluble copper salt is one or more of copper sulfate, copper chloride or copper nitrate; the ratio of the soluble nickel salt, the soluble ferrous salt, the soluble manganese salt and the soluble copper salt satisfies Na x Ni a Mn b Fe c Cu d M (1-a-b-c-d) O2 stoichiometric coefficient ratio.
[0010] Furthermore, the sodium source in step S2 is one or more of sodium carbonate, sodium formate, sodium hydroxide, sodium acetate, sodium chloride or sodium fluoride, and the molar ratio of the sodium source to the quaternary precursor material satisfies Na / (Ni+Fe+Cu+Mn)=1:1; the compound containing M is an oxide or hydroxide containing M, wherein the oxide containing M is MgO, TiO2, Al2O3, ZnO, CoO, ZrO or Y2O3; the mass ratio of the compound containing M to the quaternary precursor material satisfies that the compound containing M is 0.08wt%~0.12wt% of the mass of the quaternary precursor material.
[0011] Furthermore, the specific process of high temperature sintering in step S2 is: first heating the mixture to 400-600°C in an air atmosphere and sintering for 4-8 hours, then heating it to 950-1050°C and sintering for 10-15 hours, and the heating rate is 2-5°C / min.
[0012] Furthermore, the feeding ratio of the sodium ion battery positive electrode material to FeC2O4·H2O and (NH4)2HPO4 in step S3 satisfies that the molar ratio of the residual alkali content on the surface of the sodium ion battery positive electrode material to FeC2O4·H2O and (NH4)2HPO4 is 1:1~2:1~2.
[0013] Furthermore, the specific process of the ball milling mixing in step S3 is: ball milling at a rotation speed of 500-600 rpm for 1-2 hours.
[0014] Furthermore, the specific process of high temperature sintering in step S3 is: heating the mixture to 600-700° C. in an inert gas atmosphere and annealing for 8-10 hours, with a heating rate of 2-5° C. / min.
[0015] Furthermore, the specific process of the ball milling mixing in step S4 is: first, ball milling at a rotation speed of 500-600 rpm for 5-6 hours, during which the amount of acetylene black added is 20wt%-30wt% of the mass of the NaFePO4 coated sodium ion battery positive electrode material; and then ball milling at a rotation speed of 300-400 rpm for 3-4 hours, during which the amount of acetylene black added is 20wt%-30wt% of the mass of the NaFePO4 coated sodium ion battery positive electrode material.
[0016] Compared with the prior art, the present invention has the following advantages and beneficial effects: the sodium ion battery layered oxide positive electrode material provided by the present invention first reacts FeC2O4·H2O and (NH4)2HPO4 with the residual alkali sodium carbonate on the surface of the positive electrode material to generate a NaFePO4 coating layer, and then the generated NaFePO4 coating layer and the added acetylene black further react with the surface sodium carbonate to generate Na3FePO4C03, and the residual alkali sodium carbonate on the surface of the material is consumed twice, which can effectively reduce the residual alkali on the surface of the positive electrode material, and at the same time can effectively improve the stability of the material in the air; and can improve the slurry stability of the positive electrode material, and reduce the gas production during the cycle of the sodium ion battery. The coating layer formed by the positive electrode material of the sodium ion battery can be isolated from the electrolyte, reduce the direct contact between the positive electrode of the sodium ion battery and the electrolyte, and ensure the stability of the interface. In addition, the positive electrode material coating layer is a sodium-containing compound, which can provide a part of the sodium source during the charge and discharge process of the sodium ion battery, and further improve the cycle stability of the positive electrode material of the sodium ion battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The scanning electron microscope images of the positive electrode materials in Example 1 and Comparative Example 1 are shown.
[0018] Figure 2 This is the XRD diagram of the positive electrode material in Example 1.
[0019] Figure 3 This is the formation curve of the positive electrode material in Example 1.
[0020] Figure 4 These are the cycle test curves of the positive electrode materials in Examples 1-2 and Comparative Examples 1-2. DETAILED DESCRIPTION
[0021] The above contents of the present invention are further described in detail below through examples, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples, and all technologies implemented based on the above contents of the present invention belong to the scope of the present invention. Example 1
[0022] Step S1: Mix the salt solution containing Ni, Fe, Mn and Cu according to the stoichiometric coefficient ratio to perform a coprecipitation reaction to obtain the quaternary precursor material Ni 0.33 Mn 0.40 Fe 0.2 Cu 0.07 (OH)2.
[0023] Step S2: Sodium carbonate and the quaternary precursor material are added to a ball mill according to a molar ratio of Na / (Ni+Fe+Cu+Mn)=1:1, and then MgO with a mass percentage of 0.1wt% of the quaternary precursor material is added to the ball mill for mixing. After mixing evenly, a mixture is obtained. The mixture is first heated to 500°C in an air atmosphere and sintered for 6h, and then heated to 980°C and sintered for 12h, with a heating rate of 3°C / min, to finally obtain Mg-doped NaNi 0.33 Mn 0.40 Fe 0.2 Cu 0.07 O2 positive electrode material.
[0024] Step S3: Measure Mg-doped NaNi 0.33 Mn 0.40 Fe 0.2 Cu 0.07 The Na2CO3 content on the surface of the O2 positive electrode material is 12740ppm. According to the content of sodium carbonate on the surface of the positive electrode material, it is mixed with FeC2O4·H2O and (NH4)2HPO4 at a fixed molar ratio of 1:2:2. The mixture is ball-milled at 600rpm for 1h by a wet planetary ball milling method, and then the mixture is dried and ground. Then, the mixture is heated to 600℃ at a heating rate of 5℃ / min in an argon atmosphere and annealed for 8h to obtain a NaFePO4-coated sodium ion battery positive electrode material.
[0025] Step S4: ball-milling the NaFePO4-coated sodium ion battery positive electrode material and acetylene black, the ball milling mixing process is divided into two steps: first, ball milling at a rotation speed of 500 rpm for 6 hours, during which the amount of acetylene black added is 25wt% of the mass of the NaFePO4-coated sodium ion battery positive electrode material coated with the NaFePO4; then ball milling at a rotation speed of 400 rpm for 4 hours, during which the amount of acetylene black added is 25wt% of the mass of the NaFePO4-coated sodium ion battery positive electrode material coated with the NaFePO4, the entire ball milling process is carried out in an argon-filled container, and finally a sodium ion battery layered positive electrode material coated with NaFePO4 and Na3FePO4CO3 is obtained.
[0026] The morphology of the cathode material was tested by field emission scanning electron microscopy. The test results are shown in Figure 1 The residual alkali of the positive electrode material was tested by titration method. The test results are shown in Table 1.
[0027] The prepared NaFePO4 and Na3FePO4CO3 coated sodium ion battery layered positive electrode materials were prepared into CR2032 button cells, which were conventionally formed with a formation voltage of 2.0-4.2V and a formation rate of 0.2C. The formation curve is shown in Figure 3 The rate performance test of the formed sodium ion battery was carried out, and the results are shown in Table 2. The cycle performance test of the formed battery was carried out under the conditions of constant temperature of 23°C, 0.5C charging and 1C discharging, and the process step was set to cycle 100 weeks to record the capacity retention rate. The results are shown in Figure 4 . Example 2
[0028] Step S1: Mix the salt solution containing Ni, Fe, Mn and Cu according to the stoichiometric coefficient ratio to perform a coprecipitation reaction to obtain the quaternary precursor material Ni 0.33 Mn 0.40 Fe 0.2 Cu 0.07 (OH)2.
[0029] Step S2: Sodium carbonate and the quaternary precursor material are added into a ball mill according to a molar ratio of Na / (Ni+Fe+Cu+Mn)=1:1, and then 0.1wt% of the mass of the quaternary precursor material TiO2 is added into the ball mill for mixing, and after uniform mixing, a mixture is obtained, and the mixture is first heated to 500°C in an air atmosphere and sintered for 6h, and then heated to 980°C and sintered for 12h, and the heating rate is 3°C / min, and finally Ti-doped NaNi 0.33 Mn 0.40 Fe 0.2 Cu 0.07 O2 positive electrode material.
[0030] Step S3: Measure Ti-doped NaNi 0.33 Mn 0.40 Fe 0.2 Cu 0.07 The Na2CO3 content on the surface of the O2 positive electrode material is 12603ppm. According to the content of sodium carbonate on the surface of the positive electrode material, it is mixed with FeC2O4·H2O and (NH4)2HPO4 at a fixed molar ratio of 1:2:2. The mixture is ball-milled at 600rpm for 1h by a wet planetary ball milling method, and then the mixture is dried and ground. Then, the mixture is heated to 600℃ at a heating rate of 5℃ / min in an argon atmosphere and annealed for 8h to obtain a NaFePO4-coated sodium ion battery positive electrode material.
[0031] Step S4: ball-milling the NaFePO4-coated sodium ion battery positive electrode material and acetylene black, the ball milling mixing process is divided into two steps: first, ball milling at a rotation speed of 500 rpm for 6 hours, during which the amount of acetylene black added is 25wt% of the mass of the NaFePO4 coated with the NaFePO4 positive electrode material; then ball milling at a rotation speed of 400 rpm for 4 hours, during which the amount of acetylene black added is 25wt% of the mass of the NaFePO4 coated with the NaFePO4 positive electrode material. The entire ball milling process is carried out in an argon-filled container to finally obtain a sodium ion battery layered positive electrode material coated with NaFePO4 and Na3FePO4CO3.
[0032] The prepared NaFePO4 and Na3FePO4CO3 coated sodium ion battery layered positive electrode materials were prepared into CR2032 button cells, which were subjected to conventional formation with a formation voltage of 2.0-4.2V and a formation rate of 0.2C. The formation results are shown in Figure 3 The rate performance test of the formed sodium ion battery was carried out, and the results are shown in Table 2. The cycle performance test of the formed battery was carried out under the conditions of constant temperature of 23°C, 0.5C charging and 1C discharging, and the process step was set to cycle 100 weeks to record the capacity retention rate. The results are shown in Figure 4 .
[0033] Comparative Example 1 Step S1: Mix the salt solution containing Ni, Fe, Mn and Cu according to the stoichiometric coefficient ratio to perform a coprecipitation reaction to obtain the quaternary precursor material Ni 0.33 Mn 0.40 Fe 0.2 Cu 0.07 (OH)2.
[0034] Step S2: Sodium carbonate and the quaternary precursor material are added to a ball mill according to a molar ratio of Na / (Ni+Fe+Cu+Mn)=1:1, and then MgO with a mass percentage of 0.1wt% of the quaternary precursor material is added to the ball mill for mixing. After mixing evenly, a mixture is obtained. The mixture is first heated to 500°C in an air atmosphere and sintered for 6h, and then heated to 980°C and sintered for 12h, with a heating rate of 3°C / min, to finally obtain Mg-doped NaNi 0.33 Mn 0.40 Fe 0.2 Cu 0.07 O2 positive electrode material.
[0035] The prepared Mg-doped NaNi 0.33 Mn 0.40 Fe 0.2 Cu 0.07The O2 positive electrode material was prepared into a CR2032 button cell, which was subjected to conventional formation with a formation voltage of 2.0-4.2 V and a formation rate of 0.2C. The formation results are shown in Figure 3 The rate performance test of the formed sodium ion battery was carried out, and the results are shown in Table 2. The cycle performance test of the formed sodium ion battery was carried out under the conditions of constant temperature of 23°C, 0.5C charging and 1C discharging, and the process step was set to cycle 100 weeks to record the capacity retention rate. The results are shown in Figure 4 .
[0036] Comparative Example 2 Step S1: Mix the salt solution containing Ni, Fe, Mn and Cu according to the stoichiometric coefficient ratio to perform a coprecipitation reaction to obtain the quaternary precursor material Ni 0.33 Mn 0.40 Fe 0.2 Cu 0.07 (OH)2.
[0037] Step S2: Sodium carbonate and the quaternary precursor material are added to a ball mill according to a molar ratio of Na / (Ni+Fe+Cu+Mn)=1:1, and then MgO with a mass percentage of 0.1wt% of the quaternary precursor material is added to the ball mill for mixing. After mixing evenly, a mixture is obtained. The mixture is first heated to 500°C in an air atmosphere and sintered for 6h, and then heated to 980°C and sintered for 12h, with a heating rate of 3°C / min, to finally obtain Mg-doped NaNi 0.33 Mn 0.40 Fe 0.2 Cu 0.07 O2 cathode material.
[0038] Step S3: Measure Mg-doped NaNi 0.33 Mn 0.40 Fe 0.2 Cu 0.07 The Na2CO3 content on the surface of the O2 positive electrode material is 12740ppm. According to the content of sodium carbonate on the surface of the positive electrode material, it is mixed with FeC2O4·H2O and (NH4)2HPO4 at a fixed molar ratio of 1:2:2. The mixture is ball-milled at 600rpm for 1h by a wet planetary ball milling method, and then the mixture is dried and ground. Then, the mixture is heated to 600℃ at a heating rate of 5℃ / min in an argon atmosphere and annealed for 8h to obtain a NaFePO4-coated sodium ion battery positive electrode material.
[0039] The prepared NaFePO4-coated sodium ion battery positive electrode material was prepared into a CR2032 button cell, which was subjected to conventional formation with a formation voltage of 2.0-4.2V and a formation rate of 0.2C. The formation results are shown in Figure 3The rate performance test of the formed battery was carried out, and the results are shown in Table 2. The cycle performance test of the formed battery was carried out under the conditions of constant temperature of 23°C, 0.5C charging and 1C discharging, and the process step was set to cycle 100 cycles to record the capacity retention rate. The results are shown in Figure 4 .
[0040] Table 1
[0041] Table 2
[0042] From Table 1, by comparing the residual alkali content of the positive electrode materials of Examples 1-2 and Comparative Examples 1-2, it can be found that after two consumptions of sodium carbonate, the sodium carbonate content on the surface of the positive electrode material is significantly reduced, and at the same time, the sodium hydroxide content on the surface of the positive electrode material is also significantly reduced, indicating that this method can effectively reduce the residual alkali on the surface of the positive electrode material of the sodium ion battery and thus improve the processing performance of the positive electrode material.
[0043] From Table 2, by comparing the capacity and rate performance of the positive electrode materials prepared in Examples 1 to 2 and Comparative Examples 1 to 2, it can be found that coating NaFePO4 and Na3FePO4C03 on the sodium ion battery positive electrode material does not affect the capacity and rate performance of the sodium ion battery positive electrode material.
[0044] from Figure 1 It can be clearly seen from the scanning electron microscope (SEM) image provided in that the surface of the sample prepared in Example 1 is coated with a layer of material, while the surface of Comparative Example 1 is relatively smooth.
[0045] from Figure 2 The X-ray diffraction pattern provided in can confirm that the sodium ion battery positive electrode material prepared by this embodiment still retains the O3 phase layered transition metal oxide.
[0046] Figure 4 It is the cycle capacity retention rate of the sodium ion battery assembled with the sodium ion ground pool positive electrode materials prepared in Examples 1~2 and Comparative Examples 1~2. It can be seen from the figure that compared with Comparative Examples 1~2, the sodium ion battery positive electrode material prepared in Examples 1~2 has excellent cycle stability performance.
[0047] The above embodiments describe the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for illustrating the principles of the present invention. Without departing from the scope of the principles of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of protection of the present invention.
Claims
1. A layered positive electrode material for sodium ion batteries with low residual alkali content, characterized in that: The positive electrode material consists of a surface coating layer and an O3-type sodium-ion battery positive electrode material. The surface coating layer is NaFePO4 and Na3FePO4C03, and the O3-type sodium-ion battery positive electrode material is Na x Ni a Mn b Fe c Cu d M (1-a-b-c-d) O2, where 0.8 < x < 1.2, 0.1 < a < 0.7, 0.1 < b < 0.7, 0.1 < c < 0.7, 0.1 ≤ d ≤ 0.7, and M is one or more of Mg, Al, Ti, Co, Zn, Y, or Zr.
2. A method for preparing a sodium ion battery layered positive electrode material with low residual alkali content according to claim 1, characterized in that The specific preparation steps are: Step S1, mixing solutions containing a soluble nickel salt, a soluble ferrous salt, a soluble manganese salt and a soluble copper salt for coprecipitation reaction to obtain a quaternary precursor material; Step S2, mixing the quaternary precursor material obtained in step S1 with a sodium source and a compound containing M, and then sintering the mixture at a high temperature to obtain a positive electrode material for a sodium ion battery; Step S3, mixing the sodium ion battery positive electrode material obtained in step S2 with FeC2O4·H2O and (NH4)2HPO4, and then mixing them evenly by wet planetary ball milling. During the mixing process, FeC2O4·H2O and (NH4)2HPO4 react with the residual alkali on the surface of the sodium ion battery positive electrode material to generate NaFePO4, and then drying and grinding the mixture, and then sintering and crushing the obtained mixture at high temperature to obtain the NaFePO4-coated sodium ion battery positive electrode material; Step S4, mixing the NaFePO4-coated sodium ion battery positive electrode material obtained in step S3 with acetylene black and mixing them evenly by wet planetary ball milling under an inert gas atmosphere. During the mixing process, the NaFePO4 coated on the surface of the sodium ion battery positive electrode material coated with NaFePO4 reacts with the residual alkali remaining on the surface to generate Na3FePO4CO3, thereby obtaining a sodium ion battery layered positive electrode material with a low residual alkali content coated with NaFePO4 and Na3FePO4CO3.
3. The method for preparing a sodium ion battery layered positive electrode material with low residual alkali content according to claim 2, characterized in that: In step S1, the soluble nickel salt is one or more of nickel sulfate, nickel chloride or nickel nitrate; the soluble ferrous salt is one or more of ferrous sulfate, ferrous chloride or ferrous nitrate; the soluble manganese salt is one or more of manganese sulfate, manganese chloride or manganese nitrate; the soluble copper salt is one or more of copper sulfate, copper chloride or copper nitrate; the ratio of the soluble nickel salt, the soluble ferrous salt, the soluble manganese salt and the soluble copper salt satisfies Na x Ni a Mn b Fe c Cu d M (1-a-b-c-d) O2 stoichiometric coefficient ratio.
4. The method for preparing a sodium ion battery layered positive electrode material with low residual alkali content according to claim 2, characterized in that: The sodium source in step S2 is one or more of sodium carbonate, sodium formate, sodium hydroxide, sodium acetate, sodium chloride or sodium fluoride, and the molar ratio of the sodium source to the quaternary precursor material satisfies Na / (Ni+Fe+Cu+Mn)=1:1; the compound containing M is an oxide or hydroxide containing M, and the feeding mass ratio of the compound containing M to the quaternary precursor material satisfies that the compound containing M is 0.08wt%~0.12wt% of the mass of the quaternary precursor material.
5. The method for preparing a sodium ion battery layered positive electrode material with low residual alkali content according to claim 2, characterized in that: The specific process of high temperature sintering in step S2 is: first heating the mixture to 400-600°C in air atmosphere and sintering for 4-8 hours, then heating it to 950-1050°C and sintering for 10-15 hours, and the heating rate is 2-5°C / min.
6. The method for preparing a sodium ion battery layered positive electrode material with low residual alkali content according to claim 2, characterized in that: The feeding ratio of the sodium ion battery positive electrode material to FeC2O4·H2O and (NH4)2HPO4 in step S3 satisfies that the molar ratio of the residual alkali content on the surface of the sodium ion battery positive electrode material to FeC2O4·H2O and (NH4)2HPO4 is 1:1~2:1~2.
7. The method for preparing a sodium ion battery layered positive electrode material with low residual alkali content according to claim 2, characterized in that: The specific process of the ball milling mixing in step S3 is: ball milling at a rotation speed of 500-600 rpm for 1-2 hours.
8. The method for preparing a sodium ion battery layered positive electrode material with low residual alkali content according to claim 2, characterized in that: The specific process of high temperature sintering in step S3 is: heating the mixture to 600-700° C. in an inert gas atmosphere and annealing for 8-10 hours, with a heating rate of 2-5° C. / min.
9. The method for preparing a sodium ion battery layered positive electrode material with low residual alkali content according to claim 2, characterized in that: The specific process of ball milling mixing in step S4 is: first, ball milling at a rotation speed of 500-600 rpm for 5-6 hours, during which the amount of acetylene black added is 20wt%-30wt% of the mass of the NaFePO4 coated sodium ion battery positive electrode material; and then ball milling at a rotation speed of 300-400 rpm for 3-4 hours, during which the amount of acetylene black added is 20wt%-30wt% of the mass of the NaFePO4 coated sodium ion battery positive electrode material.
Citation Information
Patent Citations
Aqueous sodium ion secondary battery
CN113939931A
Sodium-ion battery positive electrode material as well as preparation method and application thereof
CN115411258A
Sodium-ion battery positive electrode material as well as preparation method and application thereof
CN115763768A
Positive electrode material, preparation method thereof and lithium ion battery
CN116404109A
Sodium-ion battery positive electrode material and preparation method thereof, positive electrode and sodium-ion battery
CN116759570A
Cited By
Sodium-ion battery positive electrode material, preparation method thereof and sodium-ion battery
CN119581540A