Modified polycrystalline positive electrode material and preparation method thereof, positive plate, sodium ion battery and electric equipment
Patent Information
- Application Number
- CN202410965356.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
[0002]多晶钠离子电池正极材料具有容量高、倍率性能好的优点,但是多晶材料颗粒强度小,滚压后或者循过后,材料颗粒开裂,造成容量衰减加剧的问题
[0039] (1) The modified polycrystalline cathode material provided by the present invention has high particle strength, is not easily broken, has excellent mechanical properties, can fundamentally suppress the cracking problem of polycrystalline materials, and takes into account both high capacity and high rate performance.
Smart Images

Figure CN118919711A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion battery positive electrode materials, and in particular to a modified polycrystalline positive electrode material and a preparation method thereof, a positive electrode sheet, a sodium ion battery and an electrical device. Background Art
[0002] Polycrystalline sodium-ion battery positive electrode materials have the advantages of high capacity and good rate performance, but the strength of polycrystalline material particles is low. After rolling or cycling, the material particles crack, causing the problem of increased capacity attenuation.
[0003] The main method to solve particle cracking is to replace the secondary balls with single crystal materials of suitable size. However, single crystal materials often cause loss of capacity and rate.
[0004] Therefore, in order to achieve both high capacity and high rate performance, it is necessary to fundamentally suppress the cracking problem of polycrystalline materials.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The first purpose of the present invention is to provide a modified polycrystalline positive electrode material, which has high particle strength, is not easy to break, has excellent mechanical properties, can fundamentally suppress the cracking problem of polycrystalline materials, and takes into account high capacity and high rate performance.
[0007] The second purpose of the present invention is to provide a method for preparing a modified polycrystalline positive electrode material, which method can make at least part of the element G located in the surface coating of the modified polycrystalline positive electrode material, and fill in the grain boundaries and gaps of the polycrystalline structure of the modified polycrystalline positive electrode material, so that the material has excellent mechanical properties, effectively inhibits cracking, and takes into account high capacity, high rate performance and excellent cycle performance.
[0008] The third object of the present invention is to provide a positive electrode sheet having the advantages of high capacity, high first coulombic efficiency, good rate performance and excellent cycle performance.
[0009] A fourth object of the present invention is to provide a sodium ion battery having high capacity and first coulombic efficiency, good rate performance and excellent cycle performance.
[0010] A fifth object of the present invention is to provide an electrical device.
[0011] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0012] The present invention first provides a modified polycrystalline positive electrode material, wherein the general formula of the modified polycrystalline positive electrode material is Na x Cu y Ni p Feq Mn m G n O2, wherein 0.7≤x≤1, 0≤y≤0.1, 0.2≤p≤0.4, 0≤q≤0.35, 0.3≤m≤0.5, 0.01≤n≤0.1, y+p+q+m+n=1, and G includes a metal element G2 with a valence of +2, a metal element G3 with a valence of +3, and a metal element G4 with a valence of +4;
[0013] Among them, at least part of the element G is located in the surface coating of the modified polycrystalline positive electrode material, and fills the grain boundaries and gaps of the polycrystalline structure of the modified polycrystalline positive electrode material.
[0014] Preferably, the G2 includes at least one of Mg and Zn.
[0015] Preferably, the G3 includes at least one of Co and Al.
[0016] Preferably, the G4 includes at least one of Ti and Zr.
[0017] Preferably, the first-cycle discharge capacity of a battery containing the modified polycrystalline positive electrode material at 0.1C is ≥121 mAh / g.
[0018] Preferably, the first coulombic efficiency of a battery containing the modified polycrystalline positive electrode material at 0.1C is ≥93.8%.
[0019] Preferably, the 1C / 0.1C rate of a battery containing the modified polycrystalline positive electrode material is ≥0.92.
[0020] Preferably, the capacity retention rate of a battery containing the modified polycrystalline positive electrode material after 100 cycles at 1C is ≥91%.
[0021] The present invention further provides a method for preparing a modified polycrystalline positive electrode material, comprising the following steps:
[0022] Performing a first sintering on the mixture of the precursor and the sodium source to obtain a sintered material;
[0023] The sintering material is mixed with a G-containing compound and subjected to a second sintering to obtain the modified polycrystalline positive electrode material;
[0024] Wherein, the precursor includes one of a quaternary precursor of copper-nickel-iron-manganese hydroxide, a ternary precursor of nickel-iron-manganese hydroxide, a ternary precursor of copper-nickel-manganese hydroxide, and a binary precursor of nickel-manganese hydroxide;
[0025] The molar ratio of Cu element, Ni element, Fe element and Mn element in the precursor is 0-0.1: 0.2-0.4: 0-0.35: 0.3-0.5;
[0026] The molar ratio of the precursor to the sodium element in the sodium source is 1:0.7-1;
[0027] The G in the G-containing compound includes a metal element G2 with a valence of +2, a metal element G3 with a valence of +3, and a metal element G4 with a valence of +4;
[0028] The molar ratio of the precursor to the G element in the G-containing compound is 1:0.01-0.1;
[0029] The second sintering temperature is 800-900°C.
[0030] Preferably, the second sintering heat preservation time is 10 to 30 hours.
[0031] Preferably, the temperature of the first sintering is 800-900° C., and / or the holding time of the first sintering is 10-30 hours.
[0032] Preferably, the G2 includes at least one of Mg and Zn.
[0033] Preferably, the G3 includes at least one of Co and Al.
[0034] Preferably, the G4 includes at least one of Ti and Zr.
[0035] The present invention further provides a positive electrode sheet, comprising the modified polycrystalline positive electrode material, or the modified polycrystalline positive electrode material prepared by the preparation method of the modified polycrystalline positive electrode material.
[0036] The present invention further provides a sodium ion battery, comprising the positive electrode sheet.
[0037] The present invention also provides an electrical device, comprising the sodium ion battery.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] (1) The modified polycrystalline positive electrode material provided by the present invention has high particle strength, is not easy to break, has excellent mechanical properties, can fundamentally suppress the cracking problem of polycrystalline materials, and takes into account both high capacity and high rate performance.
[0040] (2) The modified polycrystalline positive electrode material provided by the present invention has excellent cycle performance.
[0041] (3) After the modified polycrystalline positive electrode material provided by the present invention is made into a battery, there is no obvious cracking after 100 cycles at 1C.
[0042] (4) The preparation method of the modified polycrystalline positive electrode material provided by the present invention can make at least part of the element G located in the surface coating of the modified polycrystalline positive electrode material and fill in the grain boundaries and gaps of the polycrystalline structure of the modified polycrystalline positive electrode material, so that the material has excellent mechanical properties, effectively inhibits cracking, and takes into account high capacity, high rate performance and excellent cycle performance.
[0043] (5) The method for preparing the modified polycrystalline positive electrode material provided by the present invention does not require washing and drying steps after the second sintering, and has a simple process, a short flow and low cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0045] Figure 1 This is a SEM image of the modified polycrystalline positive electrode material obtained in Example 1 provided by the present invention;
[0046] Figure 2 This is a SEM image of the positive electrode material prepared in Comparative Example 5 provided by the present invention;
[0047] Figure 3 This is a SEM image of the positive electrode material particles of a battery made from the modified polycrystalline positive electrode material of Example 1 provided by the present invention after 100 cycles;
[0048] Figure 4 This is a SEM image of the positive electrode material particles of a battery made from the positive electrode material of Comparative Example 5 provided by the present invention after 100 cycles. DETAILED DESCRIPTION
[0049] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0050] If there is no special explanation, in the present invention, "the first aspect", "the second aspect", "the third aspect", "the fourth aspect", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "the first", "the second", "the third", "the fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0051] If there is no special explanation, the "include" and "comprising" mentioned in the present invention represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0052] If there is no special explanation, in the present invention, "one or more" or "at least one" refers to any one, any two or more of the listed items. Among them, "several" refers to any two or more of the listed items.
[0053] In a first aspect, the present invention provides a modified polycrystalline positive electrode material, wherein the general formula of the modified polycrystalline positive electrode material is Na x Cu y Ni p Fe q Mn m G n O2, wherein 0.7≤x≤1, 0≤y≤0.1, 0.2≤p≤0.4, 0≤q≤0.35, 0.3≤m≤0.5, 0.01≤n≤0.1, y+p+q+m+n=1, and the general formula as a whole satisfies the valence balance; G includes a metal element G2 with a valence of +2, a metal element G3 with a valence of +3 and a metal element G4 with a valence of +4.
[0054] Among them, at least part of the element G is located on the surface coating of the modified polycrystalline positive electrode material and fills the grain boundaries and gaps of the polycrystalline structure of the modified polycrystalline positive electrode material. It can be understood that part of the element G is embedded in the bulk of the modified polycrystalline positive electrode material to form doping modification.
[0055] The above general formula Na x Cu y Ni p Fe q Mn m G nIn O2, x includes but is not limited to any one of 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 1 or any range between two of them; y includes but is not limited to any one of 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1 or any range between two of them; p includes but is not limited to any one of 0.2, 0.23, 0.25, 0.28, 0.3, 0.32, 0.35, 0.38, 0.4 or any range between two of them; q includes but is not limited to any one of 0. The point value is any one of 0, 0.05, 0.1, 0.15, 0.2, 0.23, 0.25, 0.28, 0.3, 0.32, 0.35, or a range between any two of them; m includes but is not limited to the point value of any one of 0.3, 0.33, 0.35, 0.38, 0.4, 0.42, 0.45, 0.48, 0.5, or a range between any two of them; n includes but is not limited to the point value of any one of 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, or a range between any two of them.
[0056] The modified polycrystalline positive electrode material provided by the present invention has a part of the target element G embedded in the polycrystalline grain boundary, and a coating material formed by a part of the G-containing compound is located on the surface of the material and fills the polycrystalline structure gaps. The amount of G element used in the present invention is greater than the amount of conventional doping elements in the prior art. The modified polycrystalline positive electrode material of the present invention is a dense polycrystalline material formed by coating with the G-containing compound. The performance of the material can take into account the high capacity and high rate performance of the polycrystalline material, and improves the cracking problem of the material while maintaining the polycrystalline morphology.
[0057] The modified polycrystalline positive electrode material provided by the present invention has a specific chemical composition and a specific structure, has high particle strength, is not easy to break, and has excellent mechanical properties. It not only fundamentally suppresses the cracking problem of polycrystalline materials, but also takes into account high capacity and high rate performance.
[0058] Specifically, part of the element G is located in the surface layer of the modified polycrystalline positive electrode material, which can fill the gaps in the loose and porous polycrystalline structure and coat the surface. The coating material formed by the metal element G2 with a valence of +2, the metal element G3 with a valence of +3, and the metal element G4 with a valence of +4 can improve the surface structure of the polycrystalline material, improve the particle strength, enhance the mechanical and electrical properties of the material, effectively inhibit cracking, and improve the cycle performance. Moreover, the use of +2, +3, and +4 valence elements at the same time has the effect of synergistically optimizing electrical properties (including capacity, first efficiency, rate, and cycle retention rate). In addition, an appropriate amount of G can take into account both high capacity and high rate performance.
[0059] In some specific embodiments, the G2 includes at least one of Mg and Zn.
[0060] In some specific embodiments, the G3 includes at least one of Co and Al.
[0061] In some specific embodiments, the G4 includes at least one of Ti and Zr.
[0062] The modified polycrystalline positive electrode material has a high capacity. In some specific embodiments, the first-week discharge capacity of a battery containing the modified polycrystalline positive electrode material at 0.1C is ≥121 mAh / g; including but not limited to any point value of 121.5 mAh / g, 123 mAh / g, 125 mAh / g, 130 mAh / g, 132 mAh / g, 134 mAh / g, 136 mAh / g, 138 mAh / g, 140 mAh / g, 142 mAh / g, 145 mAh / g, 150 mAh / g or any range value between two of them.
[0063] The modified polycrystalline positive electrode material has a high first coulombic efficiency. In some specific embodiments, the first coulombic efficiency of a battery containing the modified polycrystalline positive electrode material at 0.1C is ≥93.8%; including but not limited to any point value of 93.8%, 94%, 94.4%, 94.7%, 95%, 95.3% or any range value between two of them.
[0064] The modified polycrystalline positive electrode material has high rate performance. In some specific embodiments, the 1C / 0.1C rate of a battery containing the modified polycrystalline positive electrode material is ≥ 0.92; including but not limited to any point value of 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, 0.99 or a range value between any two of them.
[0065] The modified polycrystalline positive electrode material has good cycle performance. In some specific embodiments, the capacity retention rate of a battery containing the modified polycrystalline positive electrode material after 100 cycles at 1C is ≥ 91%, including but not limited to any point value of 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98% or any range value between two of them.
[0066] The modified polycrystalline positive electrode material has excellent mechanical properties. In some specific embodiments, a battery containing the modified polycrystalline positive electrode material has no obvious cracking after cycling for 100 weeks at 1C.
[0067] In a second aspect, the present invention provides a method for preparing a modified polycrystalline positive electrode material, comprising the following steps:
[0068] The mixture of the precursor and the sodium source is first sintered, and then cooled to obtain a sintered material.
[0069] Wherein, the precursor includes one of a quaternary precursor of copper-nickel-iron-manganese hydroxide, a ternary precursor of nickel-iron-manganese hydroxide, a ternary precursor of copper-nickel-manganese hydroxide, and a binary precursor of nickel-manganese hydroxide;
[0070] The molar ratio of Cu, Ni, Fe and Mn in the precursor is 0-0.1 (including but not limited to any one of 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09 and 0.1 or any range between two of them): 0.2-0.4 (including but not limited to any one of 0.2, 0.23, 0.25, 0.28, 0.3, 0.32, 0.35, 0.38 and 0.4). point value or any range between two of them): 0~0.35 (including but not limited to any one of 0, 0.05, 0.1, 0.15, 0.2, 0.23, 0.25, 0.28, 0.3, 0.32, 0.35 or any range between two of them): 0.3~0.5 (including but not limited to any one of 0.3, 0.33, 0.35, 0.38, 0.4, 0.42, 0.45, 0.48, 0.5 or any range between two of them).
[0071] The molar ratio of the sodium element in the precursor and the sodium source is 1:0.7-1, including but not limited to any point value of 1:0.7, 1:0.75, 1:0.8, 1:0.85, 1:0.9, 1:0.95, 1:1 or a range value between any two of them. That is, in the target positive electrode material, the molar ratio of the sum of the molar amounts of metals other than Na to the molar amount of the sodium element is 1:0.7-1, that is, the molar content of the sodium element in the product is 0.7-1.
[0072] Afterwards, the sintering material is mixed with the G-containing compound and subjected to a second sintering, and the modified polycrystalline positive electrode material is obtained after cooling.
[0073] Wherein, G in the G-containing compound includes a metal element G2 with a valence of +2, a metal element G3 with a valence of +3, and a metal element G4 with a valence of +4.
[0074] The molar ratio of the G element in the precursor and the G-containing compound is 1:0.01-0.1, including but not limited to any one of 1:0.01, 1:0.02, 1:0.03, 1:0.04, 1:0.05, 1:0.06, 1:0.07, 1:0.08, 1:0.09, 1:0.1 or a range between any two of them.
[0075] The second sintering temperature is 800-900°C, including but not limited to any one of 800°C, 820°C, 830°C, 850°C, 760°C, 880°C, 900°C or a range between any two of them.
[0076] The general formula of the modified polycrystalline positive electrode material prepared by the above method is Na x Cu y Ni p Fe q Mn m G n O2, where 0.7≤x≤1, 0≤y≤0.1, 0.2≤p≤0.4, 0≤q≤0.35, 0.3≤m≤0.5, 0.01≤n≤0.1, y+p+q+m+n=1.
[0077] The sintered material obtained after the first sintering is characterized in that the Na element is in excess, which is 0.007≤x×n≤0.1. The reason is that the active sodium content x in the final product corresponds to the metal content y+p+q+m+n=1. In comparison, the total metal content of the sintered material of the polycrystalline product sintered without G is y+p+q+m=1-n. The sodium x×n corresponding to the missing metal elements is the excess sodium in the first sintering, and the excess range is 0.007≤x≤0.1.
[0078] That is, the sintered material obtained after the first sintering is a polycrystalline oxide material with excessive sodium. After the second sintering, the excess sodium in the sintered material participates in the reaction to form a sodium multi-element coating layer including at least three elements of +2 valence, +3 valence, and +4 valence, and the sodium in the final product modified polycrystalline positive electrode material is not excessive.
[0079] Therefore, the preparation method of the modified polycrystalline positive electrode material provided by the present invention does not require washing and drying steps after the second sintering (while the excess sodium ratio is very high when preparing single crystal materials, about 30% to 50%, so washing and drying steps are required).
[0080] Further, the modified polycrystalline positive electrode material prepared by the above method, by using a precursor composed of specific elements and a suitable amount of sodium source for one sintering, adding a specific amount of G-containing compound for two sintering, and controlling a suitable second sintering temperature, can make at least part of the element G located in the surface coating of the modified polycrystalline positive electrode material, and fill in the grain boundaries and gaps of the polycrystalline structure of the modified polycrystalline positive electrode material, the coating material mainly exists in the form of oxides containing Na, G2, G3, and G4, and the coating material can effectively inhibit cracking and improve the cycle performance. At the same time, the combination of G2, G3, and G4 has the effect of synergistically optimizing the comprehensive electrical performance (including capacity, first efficiency, rate, and cycle retention rate). The specific amount of G can also take into account both high capacity and high rate performance.
[0081] Therefore, the modified polycrystalline positive electrode material prepared by the above method has excellent mechanical properties, can fundamentally suppress the cracking problem of polycrystalline materials, and takes into account high capacity, high initial efficiency, high rate performance and excellent cycle stability.
[0082] In some specific embodiments, the holding time of the second sintering is 10 to 30 hours, including but not limited to any one of 10 hours, 12 hours, 15 hours, 16 hours, 18 hours, 20 hours, 22 hours, 24 hours, 25 hours, 28 hours, and 30 hours, or a range between any two of them.
[0083] In some specific embodiments, the first sintering temperature is 800-900° C., including but not limited to any one of 800° C., 820° C., 830° C., 850° C., 760° C., 880° C., and 900° C., or a range between any two of them. At this temperature, a polycrystalline sintered material can be obtained.
[0084] In some specific embodiments, the holding time of the first sintering is 10 to 30 hours, including but not limited to any one of 10 hours, 12 hours, 15 hours, 16 hours, 18 hours, 20 hours, 22 hours, 24 hours, 25 hours, 28 hours, and 30 hours, or a range between any two of them.
[0085] In some specific embodiments, the G2 includes at least one of Mg and Zn.
[0086] In some specific embodiments, the G3 includes at least one of Co and Al.
[0087] In some specific embodiments, the G4 includes at least one of Ti and Zr.
[0088] In some specific embodiments, the sodium source includes a sodium-containing compound, such as sodium carbonate, but is not limited thereto.
[0089] In some specific embodiments, the first sintering is followed by crushing and screening, and the particle size of the obtained sintered material can be any conventional particle size, which is not limited in the present invention.
[0090] In some specific embodiments, the G-containing compound includes G-containing oxides, hydroxides, carbonates, etc., which are not limited in the present invention.
[0091] In some specific embodiments, in the process of mixing the sintering material with the G-containing compound, any method commonly used in the art, such as mixed grinding, may be adopted, and the present invention is not limited thereto.
[0092] In some specific embodiments, the second sintering is followed by pulverization and screening, and the particle size of the obtained modified polycrystalline positive electrode material can be any conventional particle size, which is not limited in the present invention.
[0093] In a third aspect, the present invention provides a positive electrode sheet, comprising the modified polycrystalline positive electrode material, or the modified polycrystalline positive electrode material prepared by the preparation method of the modified polycrystalline positive electrode material.
[0094] The positive electrode sheet has the advantages of high capacity, high first coulombic efficiency, good rate performance and excellent cycle performance.
[0095] Optionally, the positive electrode sheet further includes a conductive agent and / or a binder, which is not limited in the present invention.
[0096] In a fourth aspect, the present invention provides a sodium ion battery comprising the positive electrode sheet.
[0097] The sodium ion battery has high capacity and first coulombic efficiency, good rate performance and excellent cycle performance.
[0098] Optionally, the sodium ion battery further comprises a negative electrode sheet, an electrolyte and a separator, which is not limited in the present invention.
[0099] In a fifth aspect, the present invention provides an electrical device comprising the sodium ion battery.
[0100] Optionally, the electrical equipment includes equipment or devices of the above-mentioned sodium ion battery, such as electric vehicles, electric motorcycles, electric bicycles, electric tools, starting power supplies, energy storage devices, electronic products, and office equipment, etc., which are not limited to the present invention.
[0101] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.
[0102] Example 1
[0103] The method for preparing the modified polycrystalline positive electrode material provided in this embodiment comprises the following steps:
[0104] According to the general formula Na 0.7 Ni 0.2 Fe 0.29 Mn 0.5 G 0.01 O2 ratio to prepare the positive electrode material, where G 0.01 Mg 0.002 Al0.003 Zr 0.005 :
[0105] The nickel iron manganese hydroxide ternary precursor Ni 0.2 Fe 0.29 Mn 0.5 (OH) 1.98 After being fully mixed with the required sodium source sodium carbonate (i.e., the molar ratio of sodium element to precursor is 0.7:1), the first sintering is carried out at 900°C for 10 hours. After cooling, the sintering is crushed and sieved to obtain a sintered polycrystalline product Na 0.7 Ni 0.2 Fe 0.29 Mn 0.5 O 1.98 (It should be noted that the calcined products of all embodiments and comparative examples are process products relative to the final product. Since the ratio of the calcined product is set to reserve vacancies for the metal G element, the molecular formula given is an approximate molecular formula or a molecular formula under ideal conditions, that is, the calcined product does not strictly satisfy the molecular formula, and may be a pure product satisfying the molecular formula, or an approximate product with a small amount of unpredictable impurities).
[0106] According to the required amount of G element, the first sintered polycrystalline product and the corresponding Mg raw material (magnesium hydroxide), Al raw material (aluminum hydroxide) and Zr raw material (zirconium dioxide) are fully mixed and ball-milled, and then the second sintering is carried out at 900 ° C for 10 hours. After cooling, it is crushed and sieved to obtain the modified polycrystalline positive electrode material Na 0.7 Ni 0.2 Fe 0.29 Mn 0.5 Mg 0.002 Al 0.003 Zr 0.005 O2.
[0107] Example 2
[0108] The method for preparing the modified polycrystalline positive electrode material provided in this embodiment comprises the following steps:
[0109] According to the general formula Na 1.0 Cu 0.1 Ni 0.22 Fe 0.28 Mn 0.3 G 0.1 O2 ratio to prepare the positive electrode material, where G 0.1 Zn 0.03 Co 0.02 Ti 0.05 :
[0110] The copper-nickel-iron-manganese hydroxide quaternary precursor Cu 0.1 Ni0.22 Fe 0.28 Mn 0.3 (OH) 1.8 After being fully mixed with the required sodium source sodium carbonate, the first sintering is carried out at 800°C for 30 hours. After cooling, it is crushed and sieved to obtain a sintered polycrystalline product Na 1.0 Cu 0.1 Ni 0.22 Fe 0.28 Mn 0.3 O 1.9 ;
[0111] According to the required amount of G element, the first sintered polycrystalline product and the corresponding Zn raw material (zinc oxide), Co raw material (cobalt tetraoxide), and Ti (titanium dioxide) raw material are fully mixed and ball-milled, and then the second sintering is carried out at 800 ° C for 30 hours. After cooling, it is crushed and sieved to obtain the modified polycrystalline positive electrode material Na1Cu 0.1 Ni 0.22 Fe 0.28 Mn 0.3 Zn 0.03 Co 0.02 Ti 0.05 O2.
[0112] Example 3
[0113] The method for preparing the modified polycrystalline positive electrode material provided in this embodiment comprises the following steps:
[0114] According to the general formula Na 0.9 Cu 0.02 Ni 0.23 Fe 0.35 Mn 0.35 G 0.05 O2 ratio to prepare the positive electrode material, where G 0.05 Mg 0.01 Zn 0.01 Al 0.01 Zr 0.01 Ti 0.01 :
[0115] The copper-nickel-iron-manganese hydroxide quaternary precursor Cu 0.02 Ni 0.23 Fe 0.35 Mn 0.35 (OH) 1.9 After being fully mixed with the required sodium source sodium carbonate, the first sintering was carried out at 850°C for 20 hours. After cooling, it was crushed and sieved to obtain a sintered polycrystalline product Na 09 Cu 002 Ni 023 Fe 035 Mn035 O 19 ;
[0116] According to the required amount of G element, the first sintered polycrystalline product and the corresponding Mg raw material (magnesium oxide), Zn raw material (zinc oxide), Al raw material (aluminum oxide), Zr raw material (zirconium dioxide), and Ti (titanium dioxide) raw material are fully mixed and ball-milled, and then a second sintering is performed at a temperature of 800°C for 20 hours. After cooling, it is crushed and sieved to obtain the modified polycrystalline positive electrode material Na 0.9 Cu 0.02 Ni 0.23 Fe 0.35 Mn 0.35 Mg 0.01 Zn 0.01 Al 0.01 Zr 0.01 Ti 0.01 O2.
[0117] Example 4
[0118] The method for preparing the modified polycrystalline positive electrode material provided in this embodiment comprises the following steps:
[0119] According to the general formula Na 0.99 Cu 0.05 Ni 0.4 Mn 0.45 G 0.1 O2 ratio to prepare the positive electrode material, where G 0.1 Mg 0.03 Zn 0.01 Al 0.01 Ti 0.05 :
[0120] The copper-nickel-iron-manganese hydroxide quaternary precursor Cu 0.05 Ni 0.4 Mn 0.45 (OH) 1.8 After being fully mixed with the required sodium source sodium carbonate, the first sintering was carried out at 850°C for 20 hours. After cooling, it was crushed and sieved to obtain a sintered polycrystalline product Na 0.99 Cu 0.05 Ni 0.4 Mn 0.45 O 1.9 ;
[0121] According to the required amount of G element, the first sintered polycrystalline product and the corresponding Mg raw material (magnesium oxide), Zn raw material (zinc oxide), Al raw material (aluminum hydroxide), and Ti (titanium dioxide) raw material are fully mixed and ball-milled, and then the second sintering is carried out at 800 ° C for 20 hours. After cooling, it is crushed and sieved to obtain the modified polycrystalline positive electrode material Na0.99 Cu 0.05 Ni 0.4 Mn 0.45 Mg 0.03 Zn 0.01 Al 0.01 Ti 0.05 O2.
[0122] Comparative Example 1
[0123] The preparation method of the positive electrode material provided in this comparative example is basically the same as that in Example 1, except that the general formula Na 0.68 Ni 0.2 Fe 0.28 Mn 0.51 G 0.01 O2 ratio to prepare the positive electrode material, the precursor used is replaced by Ni 0.2 Fe 0.28 Mn 0.51 (OH) 1.98 .
[0124] Comparative Example 2
[0125] The preparation method of the positive electrode material provided in this comparative example is basically the same as that in Example 2, except that the positive electrode material is prepared according to the general formula Na 1.02 Cu 0.11 Ni 0.22 Fe 0.28 Mn 0.29 G 0.1 O2 ratio to prepare the positive electrode material, the precursor used is replaced by Cu 0.11 Ni 0.22 Fe 0.28 Mn 0.29 (OH) 1.8 .
[0126] Comparative Example 3
[0127] The preparation method of the positive electrode material provided in this comparative example is basically the same as that in Example 3, except that the general formula Na 0.9 Cu 0.02 Ni 0.225 Fe 0.36 Mn 0.345 G 0.05 O2 ratio to prepare the positive electrode material, the precursor used is replaced by Cu 0.02 Ni 0.225 Fe 0.36 Mn 0.345 (OH) 1.9 .
[0128] Comparative Example 4
[0129] The preparation method of the positive electrode material provided in this comparative example is basically the same as that of Example 4, except that the general formula Na 0.99 Cu 0.04 Ni 0.41 Mn 0.45 G 0.1 O2 ratio to prepare the positive electrode material, the precursor used is replaced by Cu 0.04 Ni 0.41 Mn 0.45 (OH) 1.8 .
[0130] Comparative Example 5
[0131] The positive electrode material provided in this comparative example is the sintered polycrystalline product Na prepared in Example 1. 0.7 Ni 0.2 Fe 0.29 Mn 0.5 O 1.98 .
[0132] Comparative Example 6
[0133] The preparation method of the positive electrode material provided in this comparative example is basically the same as that in Example 2, except that the positive electrode material is prepared according to the general formula Na 1.0 Cu 0.1 Ni 0.217 Fe 0.277 Mn 0.297 G 0.109 O2 ratio to prepare the positive electrode material, where G 0.109 Zn 0.033 Co 0.023 Ti 0.053 , the precursor used was replaced by Cu 0.1 Ni 0.217 Fe 0.277 Mn 0.297 (OH) 1.782 .
[0134] Comparative Example 7
[0135] The preparation method of the positive electrode material provided in this comparative example is basically the same as that in Example 3, except that the general formula Na 0.86 Cu 0.02 Ni 0.23 Fe 0.35 Mn 0.35 G 0.05 O2 ratio to prepare the positive electrode material, where G 0.05 For Al 0.01 Zr 0.02 Ti 0.02 .
[0136] Comparative Example 8
[0137] The preparation method of the positive electrode material provided in this comparative example is basically the same as that in Example 3, except that the general formula Na 0.91 Cu 0.02 Ni 0.23 Fe 0.35 Mn 0.35 G 0.05 O2 ratio to prepare the positive electrode material, where G 0.05 Mg 0.02 Zn 0.01 Zr 0.01 Ti 0.01 .
[0138] Comparative Example 9
[0139] The preparation method of the positive electrode material provided in this comparative example is basically the same as that in Example 3, except that the general formula Na 0.91 Cu 0.02 Ni 0.23 Fe 0.35 Mn 0.35 G 0.05 O2 ratio to prepare the positive electrode material, where G 0.05 Mg 0.01 Zn 0.02 Al 0.02 .
[0140] Comparative Example 10
[0141] The preparation method of the positive electrode material provided in this comparative example is basically the same as that of Example 4, except that the Mg raw material (magnesium oxide), the Zn raw material (zinc oxide), the Al raw material (aluminum hydroxide) and the Ti (titanium dioxide) raw material are not added during the second sintering, but are mixed evenly with sodium carbonate during the first sintering and then subjected to the first sintering together.
[0142] Comparative Example 11
[0143] The preparation method of the positive electrode material provided in this comparative example is basically the same as that of Example 4, except that the temperature of the second sintering is replaced with 920°C.
[0144] Comparative Example 12
[0145] The preparation method of the positive electrode material provided in this comparative example is basically the same as that of Example 4, except that the temperature of the second sintering is replaced with 780°C.
[0146] Experimental example
[0147] The positive electrode materials prepared in each embodiment and each comparative example were respectively used as active materials, and the active materials, SP and PVDF were mixed in a mass ratio of 90:5:5, and NMP was added thereto to make a viscous glue, which was coated on aluminum foil and baked in a vacuum drying oven at 120°C for 12 hours to obtain a positive electrode sheet. Then, a metal sodium sheet was used as a counter electrode, glass fiber (Waterman) was used as a diaphragm, 1 mol / L NaPF6, EC:DMC (volume ratio) = 1:1 were configured as an electrolyte, and a 2032 button cell was assembled in an Ar protective glove box. The electrochemical performance test was carried out according to the following method, and the results are shown in Table 1.
[0148] The first discharge capacity and first coulombic efficiency test: According to the voltage range of 2.2 ~ 4.0V, charging is carried out with a small current of 0.1C and discharging is carried out with a small current of 0.1C (unit: mAh / g).
[0149] First coulombic efficiency (abbreviated as first efficiency): the first week 0.1C discharge capacity / 0.1C charging capacity of the button battery, voltage range 2.2 ~ 4.0V, calculate the first efficiency (unit: %).
[0150] Particle cracking test: The positive electrode sheet prepared in the normal button battery assembly process is assembled into a button battery and cycled for 100 cycles. After that, it is taken out and dried and directly subjected to SEM testing.
[0151] Cycle retention rate test: Using 1C charge and discharge system, a 100-cycle performance test was performed (100-cycle capacity retention rate unit: %).
[0152] Rate test: In the voltage range of 2.2 to 4.0 V, charge with 1C current and discharge with 1C current to obtain 1C discharge capacity. Combined with the above 0.1C discharge capacity value, calculate the 1C / 0.1C rate value.
[0153] Characterization of coating effect: judged by SEM comparison.
[0154] Table 1 Physical and chemical data results
[0155]
[0156] It can be seen from Table 1 that each embodiment has good first effect, rate, cycle performance, and ability to resist cracking after cycling, thanks to the coating process (gap filling + surface coating).
[0157] When the element ratios of Comparative Examples 1 to 4 deviate from the specified range, they show different degrees of capacity reduction, rate reduction, first efficiency reduction, and cycle retention rate reduction, but the particle cracking is consistent with the embodiment, indicating that the ratio between Na, Cu, Ni, Fe, and Mn will affect the comprehensive electrochemical properties of the material, while the particle cracking has little to do with the ratio between Na, Cu, Ni, Fe, and Mn.
[0158] Comparative Example 5 is not doped with G and not coated with G, and mainly exhibits cracking and poor cycle retention rate.
[0159] In Comparative Example 6, G is excessively doped / coated. Although there is no cracking and the cycle retention rate is high, compared with Example 2, excessive doping / coating leads to a significant decrease in capacity and rate.
[0160] Comparative Examples 7 to 9 do not contain +2, +3, and +4 valence G elements, respectively, and show varying degrees of reduction in capacity, first efficiency, rate, and cycle retention rate, indicating that the simultaneous use of +2, +3, and +4 valence elements has the effect of synergistically optimizing electrical performance.
[0161] In comparative example 10, all elements (including G element) are added during the first calcination, which leads to cracking of particles, manifested as poor cycle retention rate, and SEM shows no gap filling and no surface coating effect, indicating that conventional first calcination addition cannot effectively form a coating effect and cannot prevent the cracking of polycrystalline materials.
[0162] Comparative Example 11 is a second sintering comparative example at a higher temperature. The high-temperature surface is seamlessly filled, but there is a surface coating effect, which is manifested as particle cracking and a slightly low cycle retention rate. This shows that the excessively high temperature causes the elements filled on the surface to further melt into the interior of the particles, leaving only a partial coating layer on the surface.
[0163] Comparative Example 12 is a comparative example in which the second sintering is carried out at a lower temperature. It only has a gap filling effect but no surface coating effect. It can be reasonably inferred that the coating elements cannot be melted into the bulk phase of the material due to the too low temperature, and only exist in the form of gap filling, which also shows relatively poor electrochemical performance.
[0164] Furthermore, if Figure 1 The SEM image of the modified polycrystalline positive electrode material prepared in Example 1 is shown. Figure 2 The SEM image of the positive electrode material prepared in Comparative Example 5 is shown. Figure 2 , Comparative Example 5 Polycrystalline Uncoated Process Characteristics: It has obvious grain boundaries, a loose and porous polycrystalline structure composed of primary grains, and the primary particles are small, with a thickness and length of less than 1 μm. Figure 1, Example 1 polycrystalline coating characteristics: grain boundaries are blurred and cannot be clearly distinguished, but it can be clearly observed that the structure after coating is gap filling and surface coating coexist. Figure 2 The comparison clearly shows that Figure 1 There are no grain boundary gaps (i.e. there is a gap filling effect), and Figure 1 There is obviously a coating layer (i.e., there is a surface coating effect). It can be seen that in the modified polycrystalline positive electrode material provided by the present invention, at least part of the element G is located in the surface coating of the modified polycrystalline positive electrode material and filled in the grain boundaries and gaps of the polycrystalline structure of the modified polycrystalline positive electrode material. And part of the element G is embedded in the bulk phase of the modified polycrystalline positive electrode material to form doping.
[0165] like Figure 3 The figure shows the SEM image of the positive electrode material particles of the battery made of the modified polycrystalline positive electrode material of Example 1 after 100 cycles. It can be seen that after being corroded by the electrolyte, the morphology of the positive electrode material particles is still relatively intact, only part of the coating layer is corroded, and there is no cracking or slight cracking. Figure 4 The figure shows the SEM image of the positive electrode material particles of the battery made of the positive electrode material of Comparative Example 5 after 100 cycles. It can be seen that after being corroded by the electrolyte, the positive electrode material particles are obviously cracked.
[0166] In addition, by Figure 1-Figure 4 It can be seen that the morphology of the positive electrode material is a polycrystalline oxide material.
[0167] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.
Claims
1. A modified polycrystalline positive electrode material, characterized in that: The general formula of the modified polycrystalline positive electrode material is Na x Cu y Ni p Fe q Mn m G n O2, wherein 0.7≤x≤1, 0≤y≤0.1, 0.2≤p≤0.4, 0≤q≤0.35, 0.3≤m≤0.5, 0.01≤n≤0.1, y+p+q+m+n=1, and G includes a metal element G2 with a valence of +2, a metal element G3 with a valence of +3, and a metal element G4 with a valence of +4; Among them, at least part of the element G is located in the surface coating of the modified polycrystalline positive electrode material, and fills the grain boundaries and gaps of the polycrystalline structure of the modified polycrystalline positive electrode material.
2. The modified polycrystalline positive electrode material according to claim 1, characterized in that: At least one of the following conditions is met: (1) G2 includes at least one of Mg and Zn; (2) G3 includes at least one of Co and Al; (3) The G4 includes at least one of Ti and Zr.
3. The modified polycrystalline positive electrode material according to claim 1, characterized in that: At least one of the following conditions is met: (1) The first-week discharge capacity of a battery containing the modified polycrystalline positive electrode material at 0.1C is ≥121 mAh / g; (2) The first coulombic efficiency of a battery containing the modified polycrystalline positive electrode material at 0.1C is ≥93.8%; (3) The 1C / 0.1C ratio of the battery containing the modified polycrystalline positive electrode material is ≥ 0.92; (4) The capacity retention rate of a battery containing the modified polycrystalline positive electrode material after 100 cycles at 1C is ≥91%.
4. A method for preparing a modified polycrystalline positive electrode material, characterized in that: The steps include: Performing a first sintering on the mixture of the precursor and the sodium source to obtain a sintered material; The sintering material is mixed with a G-containing compound and subjected to a second sintering to obtain the modified polycrystalline positive electrode material; Wherein, the precursor includes one of a quaternary precursor of copper-nickel-iron-manganese hydroxide, a ternary precursor of nickel-iron-manganese hydroxide, a ternary precursor of copper-nickel-manganese hydroxide, and a binary precursor of nickel-manganese hydroxide; The molar ratio of Cu element, Ni element, Fe element and Mn element in the precursor is 0-0.1: 0.2-0.4: 0-0.35: 0.3-0.5; The molar ratio of the precursor to the sodium element in the sodium source is 1:0.7-1; The G in the G-containing compound includes a metal element G2 with a valence of +2, a metal element G3 with a valence of +3, and a metal element G4 with a valence of +4; The molar ratio of the precursor to the G element in the G-containing compound is 1:0.01-0.1; The second sintering temperature is 800-900°C.
5. The method for preparing the modified polycrystalline positive electrode material according to claim 4, characterized in that: The second sintering heat preservation time is 10 to 30 hours.
6. The method for preparing the modified polycrystalline positive electrode material according to claim 4, characterized in that: The temperature of the first sintering is 800-900° C., and / or the holding time of the first sintering is 10-30 hours.
7. The method for preparing the modified polycrystalline positive electrode material according to claim 4, characterized in that: At least one of the following conditions is met: (1) G2 includes at least one of Mg and Zn; (2) G3 includes at least one of Co and Al; (3) The G4 includes at least one of Ti and Zr.
8. A positive electrode sheet, characterized in that: It comprises the modified polycrystalline positive electrode material as claimed in any one of claims 1 to 3, or the modified polycrystalline positive electrode material prepared by the preparation method of the modified polycrystalline positive electrode material as claimed in any one of claims 4 to 7.
9. A sodium ion battery, characterized in that: Comprising the positive electrode sheet as claimed in claim 8.
10. An electrical device, characterized in that: Comprising the sodium ion battery as claimed in claim 9.