Multi-lamination coaxial through hole type fiber electrochemical device as well as preparation method and application thereof

By adopting a multi-layer coaxial through-hole structure and ribbon electrode design in fiber electrochemical devices, combined with hot melt adhesive packaging and vacuum drying technology, the problem of poor compaction of electrode active coating in fiber electrochemical devices is solved, and the problem of poor compaction of electrode active coating in fiber electrochemical devices is achieved. High energy density and strong scalability improve the electrochemical performance and structural adaptability of the device.

CN118919799APending Publication Date: 2024-11-08DONGHUA UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410997841.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In existing fiber electrochemical devices, the active coating of the fibrous electrode cannot be compacted, resulting in electron transport impedance and active material falling off, affecting device performance, and poor adaptability of the special-shaped structure.

Method used

Using a multi-layer coaxial through-hole fiber electrochemical device structure, a ribbon-shaped electrode and a separator are wound on a hollow flexible tube to form a stacked structure, and different active materials are loaded in the electrodes, combining hot melt adhesive packaging and vacuum Drying technology to achieve tight encapsulation and efficient electrochemical properties of electrodes.

Benefits of technology

It realizes high energy density, simple process and strong scalability fiber electrochemical devices, improves electrochemical performance and structural adaptability, and is suitable for structural enhancement and thermal management regulation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919799A_ABST
    Figure CN118919799A_ABST
Patent Text Reader

Abstract

The invention relates to a multi-lamination coaxial through hole type fiber electrochemical device and a preparation method and application thereof, a coaxial structure which is difficult to prepare in the field of fiber electrochemical devices is realized by adopting a simpler winding method, and the conventional dual-electrode coaxial mode is expanded into a multi-electrode lamination coaxial mode with high energy density. Different active materials are loaded in the electrode, so that a series of fiber devices with functional characteristics, such as electrochemical discoloration, energy storage, sensing and the like, can be constructed. Besides, other functional fibers and fluid materials, such as high-strength and high-modulus fibers, electric heating fibers, high-heat-conductivity fibers, heat-conducting fluid and heat storage fluid, can be further assembled or added in the through hole structure, so that the further expansion of the fiber energy storage device on the functions of structure enhancement, heat management adjustment and the like is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of fiber devices, and particularly relates to a multi-layer coaxial through-hole fiber electrochemical device and a preparation method and application thereof. Background Art

[0002] With the rapid popularization of smart wearable devices, more flexible and portable flexible electronic devices have become a need, and electronic devices have gradually begun to change from rigid to flexible. The current structures of flexible electronic devices are mainly two-dimensional planes and one-dimensional linear. In comparison, linear fiber devices that can be better integrated into woven structures have higher compatibility with wearable structures than conventional planar devices. At the same time, due to mass and volume limitations, more and more work tends to design functional devices as structures that integrate function and load-bearing. Research in this direction has previously focused on the rigidity of the outer packaging or additional support structure of the device, which has not completely solved the mechanical defects of the device itself and has poor adaptability to special-shaped structures. Here, inspired by the high mechanical properties of fiber-resin composites, the structure obtained by combining low-dimensional fiber devices with resins shows great application potential. Therefore, it is of great significance to develop electrochemical fiber devices with excellent performance.

[0003] In current fiber electrochemical devices, the electrode structure is mainly fiber-shaped. The active coating of the fiber-shaped electrode cannot be compacted, the loose structure will lead to the obstruction of electron transmission, and the active material is more likely to fall off, affecting the device performance. Summary of the invention

[0004] In view of the defects of the prior art, the technical problem to be solved by the present invention is to provide a multi-layer coaxial through-hole fiber electrochemical device and its preparation method and application, and in particular to a multi-layer coaxial through-hole fiber electrochemical device with high energy density, simple manufacturing process and strong scalability and its preparation method and application.

[0005] The present invention provides a fiber electrochemical device, which is a coaxial through-hole fiber electrochemical device with a stacked structure; wherein the stacked structure comprises electrode layers stacked in sequence; wherein a diaphragm is arranged between the electrode layers.

[0006] The present invention provides a method for preparing a fiber electrochemical device, comprising:

[0007] Winding electrodes and diaphragms on a hollow flexible tube, then inserting a heat shrink tube and injecting electrolyte at the same time, packaging, and obtaining a fiber electrochemical device; wherein winding electrodes and diaphragms on a hollow flexible tube includes: winding positive electrode, diaphragm, negative electrode, and diaphragm in sequence, repeating this step more than 0 times to form a laminated structure, or winding negative electrode, diaphragm, positive electrode, and diaphragm in sequence, repeating this step more than 0 times to form a laminated structure.

[0008] Furthermore, the electrode and the diaphragm are wound on the hollow flexible tube to form a multi-layer structure, which is then put into a heat shrink tube, the positive and negative electrode ears are led out from both ends and one end of the device is encapsulated with hot melt adhesive, vacuum dried, and then the electrolyte is poured and allowed to stand to allow the electrolyte to fully wet the positive and negative electrodes. Finally, the outer heat shrink tube is heated to shrink and the other end is encapsulated with hot melt adhesive to obtain a fiber electrochemical device.

[0009] Preferably, the diameter of the hollow flexible tube is 0.5-15 mm, the wall thickness is 0.05-5 mm, and the thermal stability temperature is above 300°C; the electrode is a strip electrode, wherein the width of the strip electrode is 1-10 mm, and the width of the strip positive and negative electrodes is adjusted according to the need to match the positive and negative electrode surface capacities; the diaphragm is a strip diaphragm, wherein the width of the strip diaphragm is 1-10 mm, and the width of the strip diaphragm should be greater than the width of the inner electrode; the diameter of the heat shrinkable tube is 1-20 mm, the wall thickness is 0.05-5 mm, and the heat shrinkage temperature is less than the starting shrinkage temperature of the diaphragm and the hollow flexible tube.

[0011] Preferably, the wound electrode and separator form a stacked structure, wherein when the stacked structure is repeatedly wound in the order of a strip-shaped positive electrode, a separator, a negative electrode, a separator, or a strip-shaped negative electrode, a separator, a positive electrode, a separator, adjacent strips are wound in the same or opposite spiral directions, and it is easy to spirally wind when the angle between the strip material and the axial direction of the hollow flexible tube is 10 to 80°.

[0012] Fiber devices with strip-shaped compacted electrodes have better electrochemical performance. At the same time, the strip-shaped electrodes are designed as more bendable coaxial spiral forms, which are compatible with the high degree of freedom of fiber devices.

[0013] Preferably, the electrode comprises a conductive substrate and a coating containing an active material; wherein the coating is loaded on one side or both sides of the conductive substrate;

[0014] Preferably, the wound electrode and the diaphragm form a stacked structure, wherein the innermost layer and the outermost layer of the stacked structure are both strip electrodes loaded with a coating containing an active material on one side, and when winding, the coating on the one side only contacts the diaphragm but not the hollow flexible tube and the outer heat shrink tube, and the electrodes not in the innermost layer and the outermost layer in the stacked structure are strip electrodes loaded with a coating containing an active material on both sides, and the number of electrode layers in the stacked structure is 2 to 10.

[0015] Preferably, the surface density of the coating in the electrode is 1 to 20 mg / cm 2 ; The active material is an electrochemically active material; wherein, by weight percentage, the coating components include: 20% to 100% electrochemically active material, 0% to 50% conductive filler, and 0% to 40% adhesive.

[0016] Furthermore, the preparation method of the electrode comprises: coating a slurry containing a coating component on one side or both sides of a conductive substrate, and compacting the slurry after drying; wherein the drying is air-blast drying, and the compacting is compacting by a roller press.

[0017] Preferably, the conductive substrate comprises one or more of metal, carbon material, polymer, semiconductor, and MXene; the electrode is a positive electrode, wherein the active material in the positive electrode is one or more of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, ternary material, sodium nickel oxide, sodium manganese oxide, sodium iron oxide, tungsten trioxide, titanium dioxide, molybdenum trioxide, niobium pentoxide, tantalum pentoxide, vanadium pentoxide, polythiophene, and carbon nanotubes; the electrode is a negative electrode, wherein the active material in the negative electrode is one or more of graphite, lithium titanate, silicon carbon, silicon, manganese dioxide, cobalt tetraoxide, nickel oxide, iridium oxide, ruthenium oxide, Prussian blue, vanadium pentoxide, and polyaniline. The conductive filler is one or more of acetylene black, ketjen black, carbon nanotubes, carbon black, graphite, carbon fiber, and graphene; the binder is one or more of polytetrafluoroethylene, polyvinylidene fluoride, sodium carboxymethyl cellulose, styrene-butadiene rubber, polyacrylic acid, and polymethyl methacrylate.

[0018] Preferably, the hollow flexible tube is a hollow flexible tube that is resistant to packaging high temperature and electrolyte; the hollow flexible tube that is resistant to packaging high temperature and electrolyte includes one or more of polytetrafluoroethylene, polyethylene, polypropylene, perfluoroethylene propylene copolymer, polyurethane, and epoxy resin; the outer heat shrinkable tube includes one or more of polytetrafluoroethylene, polyethylene, polypropylene, perfluoroethylene propylene copolymer, polyurethane, and epoxy resin; the diaphragm includes one or more of polyethylene terephthalate, polyethylene, polypropylene, polyvinylidene fluoride copolymer, polyacrylonitrile, glass fiber, and ceramic fiber; the electrolyte includes one or more of lithium trifluoromethanesulfonate, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(fluorosulfonyl)imide, lithium perchlorate, ethylene carbonate, propylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, vinylene carbonate, and fluoroethylene carbonate.

[0019] Preferably, vacuum drying is performed before the electrolyte is poured, wherein the vacuum drying temperature is lower than the initial shrinkage temperature of the heat shrinkable tube, the diaphragm, and the hollow flexible tube; during the packaging, the heat shrinkage temperature is higher than the initial shrinkage temperature of the heat shrinkable tube but lower than the initial shrinkage temperature of the diaphragm and the hollow flexible tube.

[0020] The present invention provides an application of the fiber electrochemical device in the field of structural enhancement or thermal management regulation. For example, the fiber device has a through hole, and the through hole can additionally carry one or more of high-strength and high-modulus fibers, electric heating fibers, high thermal conductivity fibers, heat-conducting fluids, and heat storage fluids, so that the fiber device can perform structural enhancement or thermal management regulation, etc.

[0021] The multi-layer coaxial through-hole electrochemical fiber structure device of the present invention is a fiber-type electrochemical device that can be further structurally enhanced or thermally managed.

[0022] The present invention introduces a laminated structure with high space utilization into a fiber electrochemical device, combined with a winding process that is easy to mass-produce and continuous, and winds the electrodes and the diaphragm in sequence on a hollow flexible tube that is resistant to packaging high temperatures and electrolytes, in the order of a strip-shaped positive electrode, a diaphragm, a negative electrode, a diaphragm or a strip-shaped negative electrode, a diaphragm, a positive electrode, a diaphragm, and then inserts a heat shrink tube and injects electrolyte at the same time, and then prepares a through-hole fiber structure electrochemical device through heat shrink packaging, i.e., a multi-layer coaxial through-hole electrochemical fiber structure device.

[0023] Beneficial Effects

[0024] The present invention uses a simpler winding method to achieve a coaxial structure that is difficult to prepare in the field of fiber electrochemical devices, and expands the conventional dual-electrode coaxial structure into a multi-electrode stacked coaxial structure with high energy density. By loading different active materials in the electrodes, a series of fiber devices with functional characteristics can be constructed, such as electrochemical color change, energy storage, sensing, etc. In addition, other functional fibers and fluid materials can be further assembled or attached in the through-hole structure, such as high-strength and high-modulus fibers, electric heating fibers, high thermal conductivity fibers, thermal conductive fluids, thermal storage fluids, etc., to achieve further expansion of fiber energy storage devices in terms of structural enhancement and thermal management regulation. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic diagram of the structure of a multi-layer coaxial through-hole fiber electrochemical device;

[0026] Figure 2 This is the specific capacity-voltage curve obtained in Example 1;

[0027] Figure 3 The curve of cycle number-Coulomb efficiency-capacity retention rate obtained in Example 1;

[0028] Figure 4 This is the specific capacity-voltage curve obtained in Example 2;

[0029] Figure 5 The curve diagram of cycle number-Coulomb efficiency-capacity retention rate obtained in Example 2;

[0030] Figure 6 This is the specific capacity-voltage curve obtained in Example 3;

[0031] Figure 7 This is a curve diagram of cycle number-Coulomb efficiency-capacity retention rate obtained in Example 3. DETAILED DESCRIPTION

[0032] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0033] Example 1

[0034] (1) Preparation of strip pole pieces and diaphragms

[0035] Weigh the ternary positive electrode, polyvinylidene fluoride and acetylene black in a mass ratio of 8:1:1, then add an appropriate amount of N-methyl-2-pyrrolidone, first stir vigorously with a homogenizer for 15 minutes, and then stir magnetically for 12 hours. The obtained positive electrode slurry is scraped on one side of the aluminum foil, and air-dried at 100°C for 1 hour, and then compacted with a roller press. Weigh graphite, polyvinylidene fluoride and acetylene black in a mass ratio of 8:1:1, then add an appropriate amount of N-methyl-2-pyrrolidone, first stir vigorously with a homogenizer for 15 minutes, and then stir magnetically for 12 hours. The obtained negative electrode slurry is first scraped on one side of the copper foil, and air-dried at 100°C for 1 hour, then the negative electrode slurry is scraped on the other side of the copper foil, and air-dried at 100°C for 1 hour, and finally compacted with a roller press. The positive electrode sheet, negative electrode sheet and separator were cut into equal-length strips of 2.5 mm, 2.9 mm and 2.5 mm in width respectively using a paper cutter.

[0036] (2) Preparation of multi-layer coaxial through-hole fiber electrochemical devices

[0037] Take a high-temperature resistant hollow flexible tube with an inner diameter of 0.5mm, and insert a copper wire with a diameter of 0.5mm into the hollow position to facilitate the subsequent winding of the strip material. Wrap the prepared strip positive electrode, diaphragm, negative electrode, diaphragm, and positive electrode on the hollow flexible tube in sequence. During the winding process, adjacent strips are wound in opposite spiral directions, and the axial angle between the strip and the hollow flexible tube is 30°. During the winding process, a small amount of acetone solution of polyvinylidene fluoride-hexafluoropropylene copolymer can be dripped at both ends, and the winding structure can be stabilized after the acetone evaporates. Lead out the positive and negative pole ears from both ends and use hot melt adhesive to encapsulate one end of the fiber device, then vacuum dry it in a vacuum oven at 60-80℃ for 10-12h, then fill the electrolyte in the glove box and let it stand for 4h to allow the electrolyte to fully wet the positive and negative electrodes. Finally, heat and shrink the outer layer of heat shrinkable tube and encapsulate the other end with hot melt adhesive to obtain Figure 1 The multi-layer coaxial through-hole fiber electrochemical device shown.

[0038] The charge and discharge performance of the multi-layer coaxial through-hole fiber electrochemical device was tested. The test steps were set as follows: first stand for 10 hours, then cycle three times at 0.1C, then cycle the fourth cycle at 0.2C, and finally continue the charge and discharge cycle at 0.5C. The third cycle reflects the performance at 0.1C rate, and the fifth cycle is used as the capacity retention rate benchmark.

[0039] like Figure 2 and Figure 3 As shown, the energy density of the fiber device is 57.1Wh / kg (0.1C), 54.3Wh / kg (0.2C); the specific capacity is 162mAh / g (0.1C), 155mAh / g (0.2C). After 113 cycles at 0.5C, the capacity retention rate is 70.2%.

[0040] Example 2

[0041] (1) Preparation of strip pole pieces and diaphragms

[0042] Weigh the ternary positive electrode, polyvinylidene fluoride and acetylene black in a mass ratio of 18:1:1, then add an appropriate amount of N-methyl-2-pyrrolidone, first stir vigorously with a homogenizer for 15 minutes, and then stir magnetically for 12 hours. The obtained positive electrode slurry is scraped on one side of the aluminum foil, and air-dried at 100°C for 1 hour, and then compacted with a roller press. Weigh graphite, polyvinylidene fluoride and acetylene black in a mass ratio of 18:1:1, then add an appropriate amount of N-methyl-2-pyrrolidone, first stir vigorously with a homogenizer for 15 minutes, and then stir magnetically for 12 hours. The obtained negative electrode slurry is first scraped on one side of the copper foil, and air-dried at 100°C for 1 hour, then scraped on the other side of the copper foil, and air-dried at 100°C for 1 hour, and finally compacted with a roller press. The positive electrode sheet, negative electrode sheet and separator were cut into equal-length strips of 3 mm, 3.5 mm and 3 mm in width respectively using a paper cutter.

[0043] (2) Preparation of multi-layer coaxial through-hole fiber electrochemical devices

[0044] Take a high-temperature resistant hollow flexible tube with an inner diameter of 2mm, and insert a copper wire with a diameter of 2mm in the hollow position to facilitate the subsequent winding of the strip material. The prepared strip positive electrode, diaphragm, negative electrode, diaphragm, and positive electrode are wound on the hollow flexible tube in sequence. During the winding process, the adjacent strips are wound in opposite spiral directions, and the axial angle between the strip and the hollow flexible tube is 60°. During the winding process, a small amount of acetone solution of polyvinylidene fluoride-hexafluoropropylene copolymer can be dripped at both ends, and the winding structure can be stabilized after the acetone evaporates. The positive and negative pole ears are drawn out from both ends and one end of the fiber device is encapsulated with hot melt adhesive, and then vacuum dried in a vacuum oven at 60-80℃ for 10-12h, and then the electrolyte is poured into the glove box and left to stand for 4h to allow the electrolyte to fully wet the positive and negative electrodes. Finally, the outer layer of the heat shrink tube is heated and shrunk and the other end is encapsulated with hot melt adhesive to obtain a multi-layer coaxial through-hole fiber electrochemical device.

[0045] The charge and discharge performance of the multi-layer coaxial through-hole fiber electrochemical device was tested. The test steps were set as follows: first stand for 10 hours, then cycle three times at 0.1C, then cycle the fourth cycle at 0.2C, and finally continue the charge and discharge cycle at 0.5C. The third cycle reflects the performance at 0.1C rate, and the fifth cycle is used as the capacity retention rate benchmark.

[0046] like Figure 4 and Figure 5 As shown, the energy density of the fiber device is 64.7Wh / kg (0.1C), 62.1Wh / kg (0.2C); the specific capacity is 171mAh / g (0.1C), 165mAh / g (0.2C). After 114 cycles at 0.5C, the capacity retention rate is 70.4%.

[0047] Example 3

[0048] (1) Preparation of strip pole piece and diaphragm

[0049] Weigh lithium cobalt oxide, polyvinylidene fluoride and acetylene black in a mass ratio of 3:1:1, then add an appropriate amount of N-methyl-2-pyrrolidone, stir vigorously for 15 minutes with a homogenizer, and then stir magnetically for 12 hours. The obtained positive electrode slurry is scraped on one side of the aluminum foil, dried with air at 100°C for 1 hour, and then compacted with a roller press. Weigh graphite, polyvinylidene fluoride and acetylene black in a mass ratio of 3:1:1, then add an appropriate amount of N-methyl-2-pyrrolidone, stir vigorously for 15 minutes with a homogenizer, and then stir magnetically for 12 hours. Scrape the obtained negative electrode slurry on one side of the copper foil, dry vigorously at 100°C for 1 hour, and compact it with a roller press. Cut the positive electrode sheet, negative electrode sheet and diaphragm into equal-length strips of 4.3mm, 4.8mm and 4.5mm widths with a paper cutter.

[0050] (2) Preparation of multi-layer coaxial through-hole fiber electrochemical devices

[0051] Take a high-temperature resistant hollow flexible tube with an inner diameter of 4mm, and insert a copper wire with a diameter of 4mm in the hollow position to facilitate the subsequent winding of the strip material. The prepared strip negative electrode, separator, and positive electrode are wound on the hollow flexible tube in sequence. During the winding process, adjacent strips are wound in the same spiral direction, and the axial angle between the strip and the hollow flexible tube is 50°. During the winding process, a small amount of acetone solution of polyvinylidene fluoride-hexafluoropropylene copolymer can be dripped at both ends, and the winding structure can be stabilized after the acetone evaporates. The positive and negative pole ears are drawn out from both ends and one end of the fiber device is encapsulated with hot melt adhesive, and then vacuum dried in a vacuum oven at 60-80℃ for 10-12h, and then the electrolyte is poured in the glove box and left to stand for 4h to allow the electrolyte to fully wet the positive and negative electrodes. Finally, the outer layer of the heat shrink tube is heated and shrunk and the other end is encapsulated with hot melt adhesive to obtain a multi-layer coaxial through-hole fiber electrochemical device.

[0052] The charge and discharge performance of the multi-layer coaxial through-hole fiber electrochemical device was tested. The test steps were set as follows: first stand for 10 hours, then cycle three times at 0.1C, then cycle the fourth cycle at 0.2C, and finally continue the charge and discharge cycle at 0.5C. The third cycle reflects the performance at 0.1C rate, and the fifth cycle is used as the capacity retention rate benchmark.

[0053] like Figure 6 and Figure 7 As shown, the energy density of the fiber device is 14.9Wh / kg (0.1C), 11.6Wh / kg (0.2C); the specific capacity is 64.2mAh / g (0.1C), 51.0mAh / g (0.2C). After 37 cycles at 0.5C, the capacity retention rate is 70.5%.

Claims

1. A fiber electrochemical device, characterized in that: The fiber electrochemical device is a coaxial through-hole fiber electrochemical device with a stacked structure; wherein the stacked structure comprises electrode layers stacked in sequence; wherein a diaphragm is provided between the electrode layers.

2. A method for preparing a fiber electrochemical device, comprising: Winding the electrode and the diaphragm on the hollow flexible tube, then inserting the heat shrink tube and injecting the electrolyte, and packaging to obtain the fiber electrochemical device; The step of winding the electrodes and the separator on the hollow flexible tube includes: winding the positive electrode, the separator, the negative electrode, and the separator in sequence, or winding the negative electrode, the separator, the positive electrode, and the separator in sequence.

3. The preparation method according to claim 2, characterized in that: The diameter of the hollow flexible tube is 0.5 to 15 mm, the wall thickness is 0.05 to 5 mm, and the thermal stability temperature is above 300°C; the electrode is a strip electrode, wherein the width of the strip electrode is 1 to 10 mm; the diaphragm is a strip diaphragm, wherein the width of the strip diaphragm is 1 to 10 mm; the diameter of the heat shrinkable tube is 1 to 20 mm, the wall thickness is 0.05 to 5 mm, and the heat shrinkage temperature is less than the starting shrinkage temperature of the diaphragm and the hollow flexible tube.

4. The preparation method according to claim 2, characterized in that: The wound electrodes and separators form a stacked structure, wherein when the stacked structure is repeatedly wound in the order of a strip-shaped positive electrode, a separator, a negative electrode, a separator, or a strip-shaped negative electrode, a separator, a positive electrode, a separator, adjacent strips are wound in the same or opposite spiral directions, and the angle between the strip material and the axial direction of the hollow flexible tube is 10 to 80 degrees.

5. The preparation method according to claim 2, characterized in that: The electrode comprises a conductive substrate and a coating containing an active material; wherein the coating is loaded on one or both sides of the conductive substrate; The wound electrodes and the diaphragm form a stacked structure, wherein the innermost and outermost layers of the stacked structure are both strip electrodes loaded with active material coatings on one side, and when winding, the single-sided coating only contacts the diaphragm but not the hollow flexible tube and the outer heat shrink tube, and the electrodes not in the innermost and outermost layers of the stacked structure are strip electrodes loaded with active material coatings on both sides, and the number of electrode layers in the stacked structure is 2 to 10.

6. The preparation method according to claim 5, characterized in that: The surface density of the coating in the electrode is 1 to 20 mg / cm 2 ; The active material is an electrochemically active material; The coating components include, by weight percentage, 20% to 100% of electrochemical active material, 0% to 50% of conductive filler, and 0% to 40% of adhesive.

7. The preparation method according to claim 5, characterized in that: The conductive substrate includes one or more of metal, carbon material, polymer, semiconductor, and MXene; the electrode is a positive electrode, wherein the active material in the positive electrode is one or more of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, ternary material, sodium nickel oxide, sodium manganese oxide, sodium iron oxide, tungsten trioxide, titanium dioxide, molybdenum trioxide, niobium pentoxide, tantalum pentoxide, vanadium pentoxide, polythiophene, and carbon nanotubes; the electrode is a negative electrode, wherein the active material in the negative electrode is one or more of graphite, lithium titanate, silicon carbon, silicon, manganese dioxide, cobalt tetraoxide, nickel oxide, iridium oxide, ruthenium oxide, Prussian blue, vanadium pentoxide, and polyaniline; the conductive filler is one or more of acetylene black, Ketjen black, carbon nanotubes, carbon black, graphite, carbon fiber, and graphene; the binder is one or more of polytetrafluoroethylene, polyvinylidene fluoride, sodium carboxymethyl cellulose, styrene-butadiene rubber, polyacrylic acid, and polymethyl methacrylate.

8. The preparation method according to claim 2, characterized in that: The hollow flexible tube is resistant to high packaging temperatures and electrolytes; the hollow flexible tube resistant to high packaging temperatures and electrolytes includes one or more of polytetrafluoroethylene, polyethylene, polypropylene, perfluoroethylene propylene copolymer, polyurethane, and epoxy resin; the heat shrinkable tube includes one or more of polytetrafluoroethylene, polyethylene, polypropylene, perfluoroethylene propylene copolymer, polyurethane, and epoxy resin; the diaphragm includes one or more of polyethylene terephthalate, polyethylene, polypropylene, polyvinylidene fluoride copolymer, polyacrylonitrile, glass fiber, and ceramic fiber; the electrolyte includes one or more of lithium trifluoromethanesulfonate, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(fluorosulfonyl)imide, lithium perchlorate, ethylene carbonate, propylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, vinylene carbonate, and fluoroethylene carbonate.

9. The preparation method according to claim 2, characterized in that: Before the electrolyte is poured, vacuum drying is performed, wherein the vacuum drying temperature is lower than the initial shrinkage temperature of the heat shrinkable tube, the diaphragm, and the hollow flexible tube; during the packaging, the heat shrinkage temperature is higher than the initial shrinkage temperature of the heat shrinkable tube but lower than the initial shrinkage temperature of the diaphragm and the hollow flexible tube.

10. Use of the fiber electrochemical device according to claim 1 in the field of structural reinforcement or thermal management regulation.