Rapid charging and discharging electrolyte for lithium metal battery and preparation method of rapid charging and discharging electrolyte

By adding methoxycyclohexane and lithium hexafluorophosphate to the lithium metal battery electrolyte solution, a solid electrolyte interface with rich inorganic components is solved, and the problem of unstability of traditional electrolytes under high current is improved. The rapid charging and discharge of lithium metal batteries is improved Performance and cycle stability.

CN118919858APending Publication Date: 2024-11-08CHENGDU UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411299644.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The interface of the solid electrolyte formed by traditional carbonate electrolytes under high current is unstable, limiting the rapid charging and discharging capacity of lithium metal batteries. The existing improved methods are difficult to meet the demand for fast charging and discharging of lithium metal batteries.

Method used

An electrolyte containing methoxycyclohexane and lithium hexafluorophosphate is used to improve the solvation structure of Li+ to form a solid electrolyte interface rich inorganic components, improving the stability of the interface and ion transport performance.

Benefits of technology

It significantly improves the circulation performance and fast charging and discharging performance of lithium metal batteries, stabilizes the interface between the anode and the electrolyte, and enhances the fast charging capability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919858A_ABST
    Figure CN118919858A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electrolyte materials, in particular to a rapid charge-discharge electrolyte for a lithium metal battery and a preparation method of the rapid charge-discharge electrolyte. The rapid charge and discharge electrolyte comprises an organic solvent, lithium hexafluorophosphate and methoxycyclohexane. The preparation method comprises the following steps: adding methoxyl into a hexafluorophosphate-based electrolyte containing lithium hexafluorophosphate and an organic solvent, and stirring and mixing for more than 5 hours to prepare the rapid charge-discharge electrolyte for the lithium metal battery. According to the rapid charging and discharging electrolyte, on one hand, a solid electrolyte interface between an anode of the lithium metal battery and the electrolyte is stabilized, the cycle performance of the lithium metal battery is improved, on the other hand, ion transmission on the electrolyte and SE I is accelerated, and the rapid charging performance of the lithium metal battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrolyte materials, and in particular to a fast charging and discharging electrolyte for lithium metal batteries and a preparation method thereof. Background Art

[0002] The goals of “carbon peak” and “carbon neutrality” require lithium metal battery technology to have high energy density and fast charging and discharging capabilities, but the solid electrolyte interface (SEI) formed by traditional carbonate electrolytes under high current is unstable and has poor kinetics. It is easy to break and induce lithium dendrite growth, limiting the fast charging capability and application of lithium metal batteries.

[0003] At present, some studies have pointed out that: + The solvent structure determines the SEI characteristics; Li + Solvation intrasheath Li + A large number of organic solvent molecules are combined, and the derived SEI is mainly composed of organic components and cannot remain stable at high current density; The solvation sheath of the inorganic-rich SEI can often be derived, which has the advantages of stability and rapid kinetics.

[0004] In order to improve the SEI characteristics, there are two major strategies to improve the solvation structure of carbonate electrolytes: one is to increase the lithium salt concentration to increase the Li + The second is to introduce diluents into the high concentration electrolyte to create a unique Li + Solvated structure; however, both face the challenges of high viscosity and slow ion transport, making it difficult to meet fast charging requirements.

[0005] In the prior art, Chinese patent CN111755710A discloses a lithium primary battery electrolyte and its preparation method and application, which discloses that the organic solvent for preparing the lithium primary battery electrolyte includes tetraethylene glycol dimethyl ether, ethylene glycol dimethyl ether, ethylene carbonate, diethyl carbonate, cyclohexane, etc. However, this electrolyte is used for lithium primary batteries, focusing on the improvement of cathode performance and capacity, while the improvement of the anode side is not reflected.

[0006] Chinese patent CN116895841A discloses a lithium-ion battery fast-charge electrolyte, a preparation method and a lithium-ion battery, and specifically discloses that the lithium-ion battery fast-charge electrolyte includes an organic solvent, a lithium salt and an additive; the additive includes an ether compound and lithium nitrate; the ether compound includes at least one of diethylene glycol dimethyl ether, triethylene glycol dimethyl ether and tetraethylene glycol dimethyl ether; lithium nitrate is an excellent film-forming additive, and the Li3N-rich solid electrolyte interface film formed by it can effectively accelerate the migration of lithium ions and greatly improve the rate performance of the battery. However, the 2C charge and discharge rate cannot meet the requirements of lithium metal batteries for fast charge and discharge technology.

[0007] Therefore, it is still necessary to develop electrolytes that can achieve excellent anode stability and fast interfacial kinetics to meet the requirements of lithium metal batteries for fast charging and discharging technology. Summary of the invention

[0008] In order to solve the above technical problems, the present invention provides a fast charging and discharging electrolyte for lithium metal batteries and a preparation method thereof, which, on the one hand, stabilizes the SEI between the anode and the electrolyte of the lithium metal battery and improves the cycle performance of the lithium metal battery, and on the other hand, accelerates ion transmission between the electrolyte and SEI and improves the fast charging performance of the lithium metal battery.

[0009] The technical solution of the present invention is as follows:

[0010] The invention provides a fast charge and discharge electrolyte for a lithium metal battery. The fast charge and discharge electrolyte comprises an organic solvent, lithium hexafluorophosphate and methoxycyclohexane.

[0011] In a specific embodiment of the present invention, based on 100% of the mass of the fast charge and discharge electrolyte, the mass concentration of the methoxycyclohexane is 2-8%.

[0012] In a specific embodiment of the present invention, the mass concentration of methoxycyclohexane is 7.5-8%.

[0013] In a specific embodiment of the present invention, the mass concentration of methoxycyclohexane is 8%.

[0014] In a specific embodiment of the present invention, based on 100% of the mass of the fast charge and discharge electrolyte, the mass concentration of lithium hexafluorophosphate is 10-20%.

[0015] In a specific embodiment of the present invention, the mass concentration of lithium hexafluorophosphate is 13-13.5%.

[0016] In a specific embodiment of the present invention, the mass concentration of lithium hexafluorophosphate is 13.1%.

[0017] In a specific embodiment of the present invention, the organic solvent includes at least one of dimethyl carbonate, diethyl carbonate, propylene carbonate, ethylene carbonate and ethyl methyl carbonate.

[0018] In a specific embodiment of the present invention, the organic solvent is ethylene carbonate and diethyl carbonate.

[0019] In a specific embodiment of the present invention, the volume ratio of ethylene carbonate to diethyl carbonate is 1:1.

[0020] The invention discloses a method for preparing a fast charge and discharge electrolyte for a lithium metal battery. The method comprises the following steps: adding methoxycyclohexane to an electrolyte of an organic solvent and lithium hexafluorophosphate, stirring and mixing for more than 5 hours, and preparing the fast charge and discharge electrolyte.

[0021] In a specific embodiment of the present invention, based on 100% of the mass of the fast charge and discharge electrolyte, the mass concentration of methoxycyclohexane is 2-8%.

[0022] In a specific embodiment of the present invention, the mass concentration of methoxycyclohexane is 7.5-8%.

[0023] In a specific embodiment of the present invention, the mass concentration of methoxycyclohexane is 8%.

[0024] In a specific embodiment of the present invention, based on 100% of the mass of the fast charge and discharge electrolyte, the mass concentration of the lithium hexafluorophosphate is 10-20%.

[0025] In a specific embodiment of the present invention, the mass concentration of lithium hexafluorophosphate is 13-13.5%.

[0026] In a specific embodiment of the present invention, the mass concentration of lithium hexafluorophosphate is 13.1%.

[0027] In a specific embodiment of the present invention, the organic solvent includes at least one of dimethyl carbonate, diethyl carbonate, propylene carbonate, ethylene carbonate and ethyl methyl carbonate.

[0028] In a specific embodiment of the present invention, the organic solvent is ethylene carbonate and diethyl carbonate.

[0029] In a specific embodiment of the present invention, the volume ratio of the ethylene carbonate to the diethyl carbonate is 1:1.

[0030] In a specific embodiment of the present invention, the stirring and mixing time is 5 to 6 hours.

[0031] The fast charge and discharge electrolyte of the present invention can be used not only for lithium metal batteries but also for lithium ion batteries.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] 1. The present invention adds methoxycyclohexane to the electrolyte containing lithium hexafluorophosphate. The coordination effect of methoxycyclohexane containing ether bonds improves the Li + By improving the solvation structure of Li + The solvated structure of the derived inorganic-rich SEI contains more inorganic components such as LiF and LiCO3, which further improves the cycle stability and ion transport performance of SEI, thereby improving the rapid charge and discharge performance at a charge and discharge rate of 5C.

[0034] 2. The fast charge and discharge electrolyte of the present invention utilizes the large steric hindrance of the cyclohexane group in methoxycyclohexane. On the one hand, it stabilizes the SEI between the anode and the electrolyte of the lithium metal battery, thereby improving the battery cycle performance; on the other hand, it accelerates ion transmission between the electrolyte and SEI, thereby improving the fast charging performance of the lithium metal battery.

[0035] 3. The reagents used in the preparation of the fast charge and discharge electrolyte of the present invention are easy to obtain and simple to synthesize, and have the value of popularization and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 A photo of the fast charge and discharge electrolyte prepared in Example 1 provided by the present invention;

[0037] Figure 2 A comparison chart of the coulombic efficiency results of Example 1 and Comparative Example 1 provided by the present invention for Li||Cu batteries;

[0038] Figure 3 A comparison chart of the Raman spectra results of Example 1 and Comparative Examples 1-4 provided by the present invention;

[0039] Figure 4 The nuclear magnetic resonance spectrum (NMR) of the fast charge and discharge electrolyte of Example 1 and Comparative Example 1 provided by the present invention; wherein a is the NMR of Example 1 and Comparative Example 1 19 F spectrum, b is the NMR of Example 1 and Comparative Example 1 7 Li spectrum;

[0040] Figure 5 A statistical graph of the cycle performance results of the Li||NCM811 full battery at 1C of Example 1 and Comparative Example 1 provided by the present invention;

[0041] Figure 6 A statistical chart of the cycle performance results of the Li||NCM811 full battery at 5C of Example 1 and Comparative Example 1 provided by the present invention;

[0042] Figure 7 Scanning electron microscope images of the anodes of the Li||NCM811 full batteries of Example 1 and Comparative Example 1 provided by the present invention after 100 cycles at 1C: wherein a is the anode of Example 1, and b is the anode of Comparative Example 1;

[0043] Figure 8 X-ray photoelectron spectroscopy (XPS) graphs of the anode of the Li||NCM811 full battery of Example 1 and Comparative Example 1 provided in the present invention after 100 cycles at 1C; wherein a is the XPS Li1s spectrum, and b is the XPS F1s spectrum. DETAILED DESCRIPTION

[0044] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.

[0045] The invention adds methoxycyclohexane as an additive to an electrolyte containing an organic solvent and lithium hexafluorophosphate to obtain the fast charge and discharge electrolyte of the invention; the cyclohexane group contained in the methoxycyclohexane produces a steric hindrance, thereby improving the Li + The solvation structure stabilizes the SEI between the anode and the electrolyte, and improves the cycle performance and fast charging performance of the lithium metal battery.

[0046] The fast charge and discharge electrolyte of the present invention can be used in both lithium metal batteries and lithium ion batteries.

[0047] The invention discloses a fast charge and discharge electrolyte for lithium metal batteries, which comprises an organic solvent, lithium hexafluorophosphate and methoxycyclohexane.

[0048] In some fast charge and discharge electrolytes, based on 100% of the mass of the fast charge and discharge electrolyte, the mass concentration of methoxycyclohexane is 2-8%; preferably, the mass concentration of methoxycyclohexane is 7.5-8%; more preferably, the mass concentration of methoxycyclohexane is 8%.

[0049] In some fast charge and discharge electrolytes, the mass concentration of lithium hexafluorophosphate is 10-20% based on 100% mass of the fast charge and discharge electrolyte.

[0050] In some fast charge and discharge electrolytes, the mass concentration of lithium hexafluorophosphate can be selected as 10.1%, 10.5%, 11%, 12%, 13%, 13.1%, 13.2%, 13.3%, 13.4%, 13.5%, 14%, 15%, 16%, 17%, 18%, 19%, 20% and other specific values; preferably, the mass concentration of lithium hexafluorophosphate is 13-13.5%; more preferably, the mass concentration of lithium hexafluorophosphate is 13.1%.

[0051] In some fast charge and discharge electrolytes, the organic solvent includes at least one of dimethyl carbonate, diethyl carbonate, propylene carbonate, ethylene carbonate, and ethyl methyl carbonate.

[0052] In some fast charge and discharge electrolytes, the organic solvent is ethylene carbonate and diethyl carbonate; more preferably, the volume ratio of ethylene carbonate to diethyl carbonate is 1:1.

[0053] The present invention also provides a method for preparing a fast charge and discharge electrolyte for a lithium metal battery, wherein methoxycyclohexane is added to an electrolyte of an organic solvent and lithium hexafluorophosphate, and the mixture is stirred for more than 5 hours to prepare the fast charge and discharge electrolyte.

[0054] In some preparation methods, the stirring and mixing is carried out at room temperature.

[0055] In some preparation methods, based on 100% of the mass of the fast charge and discharge electrolyte, the mass concentration of methoxycyclohexane is 2-8%; preferably, the mass concentration of methoxycyclohexane is 7.5-8%; more preferably, the mass concentration of methoxycyclohexane is 8%.

[0056] In some preparation methods, based on 100% of the mass of the fast charge and discharge electrolyte, the mass concentration of the lithium hexafluorophosphate is 10-20%.

[0057] In some preparation methods, the mass concentration of lithium hexafluorophosphate can be selected from 10 to 20% as 10.1%, 10.5%, 11%, 12%, 13%, 13.1%, 13.2%, 13.3%, 13.4%, 13.5%, 14%, 15%, 16%, 17%, 18%, 19%, 20% and other specific values; it can also be selected as a range value. Preferably, the mass concentration of lithium hexafluorophosphate is 13 to 13.5%; among the aforementioned specific values, more preferably, the mass concentration of lithium hexafluorophosphate is 13.1%.

[0058] In some preparation methods, the organic solvent includes at least one of dimethyl carbonate, diethyl carbonate, propylene carbonate, ethylene carbonate, and ethyl methyl carbonate; preferably, the organic solvent is ethylene carbonate and diethyl carbonate; more preferably, the volume ratio of the ethylene carbonate to the diethyl carbonate is 1:1.

[0059] In some preparation methods, the stirring and mixing time is 5 to 6 hours.

[0060] In some preparation methods, the stirring and mixing time can be specifically selected as 5 h, 5.5 h, or 6 h.

[0061] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the following is a further detailed description in conjunction with the accompanying drawings and the accompanying drawings. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0062] Example 1

[0063] This embodiment provides a fast charge and discharge electrolyte for lithium metal batteries, and the preparation method thereof is as follows:

[0064] Methoxycyclohexane was added to a lithium hexafluorophosphate-based electrolyte containing lithium hexafluorophosphate, and the mixture was magnetically stirred for 6 hours to obtain a fast charge and discharge electrolyte.

[0065] Among them, the mass concentration of lithium hexafluorophosphate in the fast charge and discharge electrolyte is 13.1%, and the mass concentration of methoxycyclohexane is 8%; the organic solvents in the lithium hexafluorophosphate-based electrolyte are ethylene carbonate and diethyl carbonate, and the volume ratio of the two is 1:1.

[0066] The photo of the fast charge and discharge electrolyte prepared in this example is shown in Figure 1 shown.

[0067] Example 2

[0068] This embodiment provides a fast charge and discharge electrolyte for lithium metal batteries, and the preparation method thereof is as follows:

[0069] Methoxycyclohexane was added to a lithium hexafluorophosphate-based electrolyte containing lithium hexafluorophosphate, and the mixture was magnetically stirred for 5.5 hours to obtain a fast charge and discharge electrolyte.

[0070] Among them, the mass concentration of lithium hexafluorophosphate in the fast charge and discharge electrolyte is 13.1%, and the mass concentration of methoxycyclohexane is 8%; the organic solvents in the lithium hexafluorophosphate-based electrolyte are ethylene carbonate and diethyl carbonate, and the volume ratio of the two is 1:1.

[0071] Example 3

[0072] This embodiment provides a fast charge and discharge electrolyte for lithium metal batteries, and the preparation method thereof is as follows:

[0073] Methoxycyclohexane was added to a lithium hexafluorophosphate-based electrolyte containing lithium hexafluorophosphate, and the mixture was magnetically stirred for 5 hours to obtain a fast charge and discharge electrolyte.

[0074] Among them, the mass concentration of lithium hexafluorophosphate in the fast charge and discharge electrolyte is 13.1%, and the mass concentration of methoxycyclohexane is 8%; the organic solvents in the lithium hexafluorophosphate-based electrolyte are ethylene carbonate and diethyl carbonate, and the volume ratio of the two is 1:1.

[0075] Comparative Example 1

[0076] This comparative example provides a lithium hexafluorophosphate-based electrolyte, which differs from Example 1 in that no methoxycyclohexane is added.

[0077] Comparative Example 2

[0078] This comparative example provides a lithium hexafluorophosphate-based electrolyte, which is different from Example 1 in that the mass concentration of methoxycyclohexane is replaced by 4% in 8%.

[0079] Comparative Example 3

[0080] This comparative example provides a lithium hexafluorophosphate-based electrolyte, which differs from Example 1 in that the mass concentration of methoxycyclohexane is replaced by 6% instead of 8%.

[0081] Comparative Example 4

[0082] This comparative example provides a lithium hexafluorophosphate-based electrolyte, which is different from Example 1 in that the mass concentration of methoxycyclohexane is replaced by 10% instead of 8%.

[0083] The fast charge and discharge electrolyte of Example 1 and the hexafluorophosphate-based electrolyte of Comparative Example 1 were used in Li||Cu half-cells at 1 mA / cm 2 、1mAh / cm 2 Under the conditions, the comparison results of the coulombic efficiency of the two half-cells are as follows Figure 2 shown.

[0084] Depend on Figure 2 It can be seen that the half-cell coulombic efficiency of the fast charge and discharge electrolyte of Example 1 can remain stable and cycle for more than 100 cycles; while the half-cell coulombic efficiency of the hexafluorophosphate-based electrolyte of Comparative Example 1 begins to show obvious decay after about 20 cycles; therefore, the fast charge and discharge electrolyte of the present invention can promote uniform electroplating and stripping of lithium ions.

[0085] Comparison of Raman spectra of the fast charge and discharge electrolyte of Example 1 and the lithium hexafluorophosphate-based electrolytes of Comparative Examples 1-4 Figure 3 shown.

[0086] Depend on Figure 3 It can be seen that the fast charge and discharge electrolyte of Example 1 Moved to high field, indicating that Li + The enhanced bonding forms more contact ion pairs and aggregated ion clusters, deriving a solvation structure rich in inorganic anions, which is more conducive to the formation of inorganic SEI.

[0087] The results of nuclear magnetic resonance spectroscopy (NMR) characterization of the fast charge and discharge electrolyte of Example 1 and the hexafluorophosphate-based electrolyte of Comparative Example 1 are shown in the following table: Figure 4 As shown; wherein a is the NMR of Example 1 and Comparative Example 1 19 F spectrum, b is the NMR of Example 1 and Comparative Example 1 7 Li spectrum.

[0088] By the attached Figure 4 NMR in 19 F spectrum shows that the characteristic peak of Example 1 moves to the low field compared with Comparative Example 1, indicating that the electron cloud density around the anion is reduced, indicating that the anion and Li + The binding is enhanced; Figure 4 NMR 7 The Li spectrum shows that Li + The electron cloud density around it is greatly reduced, which is attributed to the Li + The number of organic solvent molecules combined is greatly reduced.

[0089] The fast charge and discharge electrolyte of Example 1 and the hexafluorophosphate-based electrolyte of Comparative Example 1 were used in Li||NCM811 full cells at 1C / 1C and 4.0mg / cm 2 , 2.8-4.3V conditions, the cycle performance (specific capacity, coulombic efficiency) of the two full batteries are as follows Figure 5 As shown; at 5C / 5C, 4.0mg / cm 2 , 2.8-4.3V conditions, the cycle performance (specific capacity, coulombic efficiency) of the two full batteries are as follows Figure 6 shown.

[0090] Depend on Figure 5 It can be seen that the Li||NCM811 full battery of Example 1 has a cycle number of 500 times at a charge and discharge rate of 1C, and the capacity retention rate is still 80% at 462 cycles; in contrast, the capacity retention rate of the Li||NCM811 full battery of Comparative Example 1 drops to 80% after 171 cycles. The fast charge and discharge electrolyte of Comparative Example 1 has a significant improvement in the cycle performance of the full battery.

[0091] Depend on Figure 6It can be seen that the Li||NCM811 full battery of Example 1 still maintains a low capacity decay rate within 200 cycles at a high current density of 5C; while the capacity retention rate of the Li||NCM811 full battery of Comparative Example 1 has dropped to 80% after 27 cycles at a high current density of 5C.

[0092] The two Li||NCM811 full cells of Example 1 and Comparative Example 1 were heated at 1C / 1C and 4.0 mg / cm 2 After 100 cycles at 2.8-4.3V, the SEM results of the anode are as follows: Figure 7 As shown, a is the anode of Example 1, and b is the anode of Comparative Example 1; the X-ray photoelectron spectroscopy results are shown as Figure 8 As shown, a is the XPS Li1s spectrum and b is the XPS F1s spectrum.

[0093] By the attached Figure 7 As can be seen from Figure a, after the Li||NCM811 full battery of Example 1 has been cycled for 100 cycles, the lithium deposition morphology on the anode surface is smooth and crack-free; and as can be seen from Figure b, after the Li||NCM811 full battery of Comparative Example 1 has been cycled for 100 cycles, there are many holes on the anode surface and the lithium deposition is uneven; this proves that the fast charge and discharge electrolyte prepared by the present invention can form a stable inorganic-rich SEI on the anode surface of the lithium metal battery, thereby making Li + Deposited evenly on the anode surface.

[0094] According to the attached Figure 8 From the X-ray photoelectron energy spectrum, the inorganic-rich SEI derived from the fast charge and discharge electrolyte of Example 1 contains more inorganic components such as LiF, LiCO3, etc., which effectively improves the performance of the inorganic-rich SEI.

Claims

1. A fast charge and discharge electrolyte for lithium metal batteries, Features: The fast charge and discharge electrolyte comprises an organic solvent, lithium hexafluorophosphate and methoxycyclohexane.

2. The fast charge and discharge electrolyte according to claim 1, Features: Based on 100% of the mass of the fast charge and discharge electrolyte, the mass concentration of methoxycyclohexane is 2-8%; preferably, the mass concentration of methoxycyclohexane is 7.5-8%; more preferably, the mass concentration of methoxycyclohexane is 8%.

3. The fast charge and discharge electrolyte according to claim 1, Features: Based on 100% of the mass of the fast charge and discharge electrolyte, the mass concentration of lithium hexafluorophosphate is 10-20%; preferably, the mass concentration of lithium hexafluorophosphate is 13-13.5%; more preferably, the mass concentration of lithium hexafluorophosphate is 13.1%.

4. The fast charge and discharge electrolyte according to claim 1, Features: The organic solvent includes at least one of dimethyl carbonate, diethyl carbonate, propylene carbonate, ethylene carbonate, and ethyl methyl carbonate.

5. The fast charge and discharge electrolyte according to claim 1, Features: The organic solvent is ethylene carbonate and diethyl carbonate; more preferably, the volume ratio of ethylene carbonate to diethyl carbonate is 1:

1.

6. A method for preparing a fast charge and discharge electrolyte for a lithium metal battery, Features: Methoxycyclohexane is added to an organic solvent and an electrolyte solution of lithium hexafluorophosphate, and the mixture is stirred for more than 5 hours to prepare a fast charge and discharge electrolyte solution.

7. The preparation method according to claim 6, Features: Based on 100% of the mass of the fast charge and discharge electrolyte, the mass concentration of methoxycyclohexane is 2-8%; preferably, the mass concentration of methoxycyclohexane is 7.5-8%; more preferably, the mass concentration of methoxycyclohexane is 8%.

8. The preparation method according to claim 6, Features: Based on 100% of the mass of the fast charge and discharge electrolyte, the mass concentration of the lithium hexafluorophosphate is 10-20%; preferably, the mass concentration of the lithium hexafluorophosphate is 13-13.5%; more preferably, the mass concentration of the lithium hexafluorophosphate is 13.1%.

9. The preparation method according to claim 6, Features: The organic solvent includes at least one of dimethyl carbonate, diethyl carbonate, propylene carbonate, ethylene carbonate and ethyl methyl carbonate; preferably, the organic solvent is ethylene carbonate and diethyl carbonate; more preferably, the volume ratio of the ethylene carbonate to the diethyl carbonate is 1:

1.

10. The preparation method according to claim 6, Features: The stirring and mixing time is 5 to 6 hours.