A formation and capacitance process for a sodium-ion short blade battery

By optimizing the formation and capacity stabilization processes of sodium-ion short blade batteries, the problem of insufficient performance of sodium-ion batteries in existing technologies has been solved, achieving improvements in initial capacity and cycle life, and significantly improving battery performance.

CN118919892BActive Publication Date: 2026-11-17安徽吉厚智能科技有限公司
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411263293.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2026-11-17
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

Existing sodium-ion battery formation and capacitance methods refer to those for lithium-ion batteries, but they have failed to significantly improve the performance of sodium-ion batteries, especially in terms of energy density and cycle life.

Method used

The formation and capacitance steps of sodium-ion short blade batteries are optimized, including resting, constant current charging and charge-discharge treatment under specific temperature and negative pressure, to form a stable sodium-ion intercalation layer, exhaust gas, and optimize the intercalation and deintercalation behavior of positive and negative electrode materials.

Benefits of technology

It significantly improves the initial capacity, charge-discharge efficiency, and cycle life of sodium-ion batteries, enhances battery performance, and reduces gas production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention belongs to the field of sodium-ion battery technology, specifically disclosing a formation and capacity-setting process for a sodium-ion short blade battery. The process includes the following steps: S1: battery pretreatment; S2: battery formation; S3: battery resting; S4: battery capacity setting. This invention provides a formation and capacity-setting process for a sodium-ion short blade battery. By optimizing the formation and capacity-setting steps in sodium-ion battery production, and optimizing the relevant parameters in these steps, the initial capacity, charge-discharge efficiency, and cycle life of the sodium-ion battery can be significantly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of sodium-ion battery technology, and particularly relates to a formation and capacity-maintaining process for a sodium-ion short blade battery. Background Technology

[0002] Sodium-ion batteries are rechargeable batteries that primarily function by the movement of sodium ions between the positive and negative electrodes, similar in principle to lithium-ion batteries. The electrode materials used in sodium-ion batteries are mainly sodium salts, which are more abundant and cheaper than lithium salts; therefore, sodium-ion batteries have broad application prospects in new energy storage and power fields. However, the commercialization of sodium-ion batteries still faces significant challenges due to limitations in energy density and cycle life.

[0003] Formation and capacity stabilization are crucial steps in sodium-ion battery production, directly impacting battery performance. Battery formation involves activating the internal positive and negative electrode materials through specific charge-discharge methods to improve charge-discharge performance. During formation and capacity stabilization, venting is necessary to eliminate gases generated during the formation process. Currently, sodium-ion battery formation and capacity stabilization methods largely follow those for lithium-ion batteries. However, applying lithium-ion formation and capacity stabilization methods to sodium-ion production does not significantly improve sodium-ion battery performance. Summary of the Invention

[0004] The purpose of this invention is to overcome the above-mentioned problems in the prior art and provide a formation and capacity stabilization process for sodium-ion short blade batteries. By optimizing the formation and capacity stabilization steps in sodium-ion battery production and optimizing the relevant parameters in the formation and capacity stabilization steps, the initial capacity, charge-discharge efficiency and cycle life of sodium-ion batteries can be significantly improved.

[0005] To achieve the above-mentioned technical objectives and effects, the present invention is implemented through the following technical solution:

[0006] A formation and capacity-maintaining process for a sodium-ion short blade battery, comprising the following steps:

[0007] S1: Battery Pretreatment

[0008] The sodium-ion short blade battery is placed at a first temperature and left to stand for a first time to obtain the first battery after standing.

[0009] S2: Battery Formation

[0010] Under the conditions of first negative pressure and second temperature, the first static battery is subjected to constant current charging to obtain the formed battery.

[0011] S3: Battery idle

[0012] The formed battery was left to stand at a third temperature for a second time to obtain a second settling battery.

[0013] S4: Battery Capacitance Setting

[0014] Under a second negative pressure and a fourth temperature, the second static battery is charged and discharged to obtain a battery after being converted to a constant capacity.

[0015] Furthermore, in step S1, the first temperature is 40–60°C, and the first time is 20–30 hours.

[0016] Furthermore, in step S2, the first negative pressure is -60 to -100 Pa, and the second temperature is 40 to 60 °C.

[0017] Furthermore, in step S2, the specific process of constant current charging is as follows:

[0018] S201: First, charge the first static battery with a constant current rate at a first current rate to raise the voltage of the first static battery to the first voltage, thus obtaining a battery after one charge.

[0019] S202: Charge the battery after the first charge at a constant current rate of the second current rate to raise the voltage of the battery after the first charge to the second voltage, thus obtaining the battery after the second charge.

[0020] S203: Finally, the battery after the second charge is charged with constant current at the third current rate to raise the voltage of the battery after the second charge to the third voltage, thus obtaining the formed battery.

[0021] Furthermore, the first current multiplier is less than the second current multiplier, and the second current multiplier is less than the third current multiplier.

[0022] Furthermore, the first current multiplier is 0.01–0.05C, the second current multiplier is 0.09–0.15C, and the third current multiplier is 0.19–0.25C;

[0023] The first voltage is 2.8–3.2V, the second voltage is 3.4–3.8V, and the third voltage is 3.9–4.2V.

[0024] Furthermore, in step S3, the third temperature is room temperature, and the second time is 40–60 hours;

[0025] In step S4, the second negative pressure is -60 to -100 Pa, and the fourth temperature is room temperature.

[0026] Furthermore, in step S4, the specific process of charging and discharging is as follows:

[0027] S401: Charge the second static battery to the fourth voltage at a constant current and constant voltage rate at the fourth current rate to obtain the battery after three charges.

[0028] S402: Discharge the battery after three charges at a constant current rate of the fifth current to the fifth voltage to obtain the battery after one discharge.

[0029] S403: Repeat steps S401 to S4021 twice to obtain the processed battery;

[0030] S404: Charge the processed battery to the sixth voltage at a constant current and constant voltage rate of the sixth current to obtain a battery after constant capacity.

[0031] Furthermore, the fourth current factor is less than the fifth current factor;

[0032] The fourth current multiplier is less than the sixth current multiplier.

[0033] Furthermore, the fourth current multiplier is 0.20–0.40C, the fifth current multiplier is 0.45–0.60C, and the sixth current multiplier is 0.45–0.60C;

[0034] The fourth voltage is 4.0-4.4V, the fifth voltage is 1.8-3.0V, and the sixth voltage is 3.7-3.9V.

[0035] Compared with the prior art, the beneficial effects of the present invention are:

[0036] 1. This invention provides a formation and capacity-stabilizing process for sodium-ion short blade batteries. By optimizing the formation and capacity-stabilizing steps and parameters, the initial capacity, charge-discharge efficiency, and cycle life of sodium-ion batteries are significantly improved.

[0037] 2. In this invention, the pretreatment step involves allowing the battery to stand at a specific temperature for a period of time to achieve a stable internal state. In the formation step, sodium ions gradually embed into the negative electrode material from the positive electrode material, and the waste gas generated during this process is extracted by negative pressure, ultimately forming a stable sodium ion embedding layer. In the standing step, allowing the battery to stand at room temperature helps to further optimize the embedding and de-embedding behavior of sodium ions in the positive and negative electrode materials, improving the battery's charge and discharge efficiency and cycle life. In the final capacity setting step, the process is carried out under negative pressure and room temperature conditions to allow the battery to reach a new stable internal state, and the waste gas is discharged by negative pressure, which can further improve battery performance.

[0038] 3. By optimizing the sodium-ion battery formation process, this invention can significantly improve the initial capacity of sodium-ion short blade batteries, and also significantly improve cycle life and gas generation. Detailed Implementation

[0039] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0040] A formation and capacity-maintaining process for a sodium-ion short blade battery, comprising the following steps:

[0041] S1: Battery Pretreatment

[0042] The sodium-ion short blade battery is placed at a first temperature and left to stand for a first time to obtain the first battery after standing.

[0043] In step S1, the first temperature is 40-60°C, preferably 45°C;

[0044] The optimal timeframe is 20–30 hours, with 24 hours being the preferred time.

[0045] S2: Battery Formation

[0046] Under the conditions of first negative pressure and second temperature, the first static battery is subjected to constant current charging to obtain the formed battery.

[0047] In step S2, the first negative pressure is -60 to -100 Pa, preferably -75 Pa;

[0048] The second temperature is 40–60°C, preferably 45°C;

[0049] In step S2, the specific process of constant current charging is as follows:

[0050] S201: First, charge the first static battery with a constant current rate at a first current rate to raise the voltage of the first static battery to the first voltage, thus obtaining a battery after one charge.

[0051] S202: Charge the battery after the first charge at a constant current rate of the second current rate to raise the voltage of the battery after the first charge to the second voltage, thus obtaining the battery after the second charge.

[0052] S203: Finally, the battery after the second charge is charged with constant current at the third current rate to raise the voltage of the battery after the second charge to the third voltage, thus obtaining the battery after formation.

[0053] Among them, the first current multiplier is less than the second current multiplier, and the second current multiplier is less than the third current multiplier;

[0054] The first current multiplier is 0.01 to 0.05C, preferably 0.05C;

[0055] The second current multiplier is 0.09 to 0.15C, preferably 0.1C;

[0056] The third current multiplier is 0.19 to 0.25C, preferably 0.2C;

[0057] The first voltage is 2.8–3.2V, preferably 3.0V;

[0058] The second voltage is 3.4–3.8V, preferably 3.5V;

[0059] The third voltage is 3.9–4.2V, preferably 3.95V;

[0060] S3: Battery idle

[0061] The formed battery was left to stand at a third temperature for a second time to obtain a second settling battery.

[0062] In step S3, the third temperature is room temperature;

[0063] The second time is 40-60 hours, preferably 45 hours;

[0064] S4: Battery Capacitance Setting

[0065] Under the second negative pressure and the fourth temperature, the second static battery is charged and discharged to obtain a battery after being converted to a constant capacity.

[0066] In step S4, the second negative pressure is -60 to -100 Pa, preferably -75 Pa;

[0067] The fourth temperature is room temperature;

[0068] In step S4, the specific process of charging and discharging is as follows:

[0069] S401: Charge the second static battery to the fourth voltage at a constant current and constant voltage rate at the fourth current rate to obtain the battery after three charges.

[0070] S402: Discharge the battery after three charges at a constant current rate of the fifth current to the fifth voltage to obtain the battery after one discharge.

[0071] S403: Repeat steps S401 to S4021 twice to obtain the processed battery;

[0072] S404: Charge the processed battery to the sixth voltage at a constant current and constant voltage rate at the sixth current rate to obtain a battery after constant capacity.

[0073] In the specific process of charging and discharging, the fourth current factor is less than the fifth current factor, and the fourth current factor is less than the sixth current factor.

[0074] Specifically, the fourth current factor is 0.20 to 0.40C, preferably 0.33C;

[0075] The fifth current multiplier is 0.45-0.60C, preferably 0.5C;

[0076] The sixth current multiplier is 0.45-0.60C, preferably 0.5C;

[0077] The fourth voltage is 4.0-4.4V, preferably 4.2V;

[0078] The fifth voltage is 1.8-3.0V, preferably 2.0V;

[0079] The sixth voltage is 3.7-3.9V, preferably 3.85V.

[0080] The following are specific examples.

[0081] Example

[0082] The sodium-ion short blade battery was pretreated by standing in an environment of 45°C for 24 hours. Then, under negative pressure of -75Pa and temperature of 45°C, it was first charged at a constant current of 0.05C to 3.0V, then at a constant current of 0.1C to 3.5V, and finally at a constant current of 0.2C to 3.95V. Afterward, it was left to stand at room temperature for 48 hours. Finally, under negative pressure of -75Pa and room temperature, the battery was subjected to constant-capacity determination, charged at a constant current and constant voltage of 0.33C to 4.2V, then discharged at a constant current of 0.5C to 2.0V, and cycled twice. Finally, it was charged at a constant current and constant voltage of 0.5C to 3.85V, completing the formation and capacity determination process.

[0083] Comparative Example

[0084] The sodium-ion short blade battery was pretreated by standing in an environment of 45°C for 24 hours. Then, under negative pressure of -75Pa and temperature of 45°C, it was first charged at a constant current of 0.05C to 3.0V, then at a constant current of 0.1C to 3.5V, and finally at a constant current of 0.2C to 3.95V. After that, it was left to stand at room temperature for 48 hours. Finally, the battery was subjected to constant capacity determination at room temperature, charged at a constant current and constant voltage of 0.33C to 4.2V, then discharged at a constant current of 0.5C to 2.0V, and cycled twice. Finally, it was charged at a constant current and constant voltage of 0.5C to 3.85V, completing the formation and capacity determination process.

[0085] Experimental Example

[0086] The sodium-ion short blade batteries in the examples and comparative examples were subjected to performance tests after the formation and capacitance process was completed. The test results are shown in Table 1.

[0087] Table 1

[0088] Performance parameters Example Comparative Example Battery thickness after calibration 20.4mm 22.5mm Constant capacity 69Ah 65Ah Cycle life 80% of 1000 laps 200 laps 80%

[0089] As can be seen from the data in Table 1, after the capacity is set, the thickness of the battery in the example is smaller than that in the comparative example, and its capacity and cycle life are also improved, indicating that the performance of the sodium-ion short blade battery prepared by this process has been improved.

[0090] Furthermore, the sodium-ion short blade battery prepared in the examples has a smooth and normal outer surface; while the sodium-ion short blade battery prepared in the comparative examples has obvious sodium precipitation on its outer surface; indicating that the sodium-ion short blade battery prepared by the formation and capacity setting process of the present invention has excellent appearance.

[0091] This invention provides a formation and capacity stabilization process for sodium-ion short blade batteries. By optimizing the formation and capacity stabilization steps in sodium-ion battery production and optimizing the relevant parameters in the formation and capacity stabilization steps, the initial capacity, charge-discharge efficiency and cycle life of sodium-ion batteries can be significantly improved, and it can be widely used in the production and manufacturing of sodium-ion batteries.

[0092] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0093] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the claimed invention.

Claims

1. A formation and capacity-maintaining process for a sodium-ion short blade battery, characterized in that, The process includes the following steps: S1: Battery Pretreatment The sodium-ion short blade battery is placed at a first temperature and left to stand for a first time to obtain the battery after the first standing period. S2: Battery Formation Under the conditions of a first negative pressure and a second temperature, the first statically rested battery is subjected to constant current charging to obtain a formed battery. The specific process of constant current charging is as follows: S201: First, charge the first static battery with a constant current rate at a first current rate to raise the voltage of the first static battery to the first voltage, thus obtaining a battery after one charge. S202: Charge the battery after the first charge at a constant current rate of the second current rate to raise the voltage of the battery after the first charge to the second voltage, thus obtaining the battery after the second charge. S203: Finally, the battery after the second charge is charged with constant current at the third current rate to raise the voltage of the battery after the second charge to the third voltage, thus obtaining the battery after formation. Furthermore, the first current multiplier is less than the second current multiplier, and the second current multiplier is less than the third current multiplier; The first current multiplier is 0.01–0.05C, the second current multiplier is 0.09–0.15C, and the third current multiplier is 0.19–0.25C; The first voltage is 2.8–3.2V, the second voltage is 3.4–3.8V, and the third voltage is 3.9–4.2V; S3: Battery idle The formed battery was left to stand at a third temperature for a second time to obtain a second settling battery, wherein the third temperature was room temperature and the second time was 40-60 hours. S4: Battery Capacitance Setting Under a second negative pressure and a fourth temperature, the second statically settled battery is subjected to charge-discharge treatment to obtain a battery after being formed and capacitated. The second negative pressure is -60 to -100 Pa, and the fourth temperature is room temperature. The specific process of charge-discharge treatment is as follows: S401: Charge the second static battery to the fourth voltage at a constant current and constant voltage rate at the fourth current rate to obtain the battery after three charges. S402: Discharge the battery after three charges at a constant current rate of the fifth current to the fifth voltage to obtain the battery after one discharge. S403: Repeat steps S401 to S402 1 to 2 times to obtain the processed battery; S404: Charge the processed battery to the sixth voltage at a constant current and constant voltage rate of the sixth current to obtain a battery after constant capacity.

2. The formation and capacity-maintaining process for a sodium-ion short blade battery according to claim 1, characterized in that, In step S1, the first temperature is 40-60℃ and the first time is 20-30h.

3. The formation and capacity-maintaining process for a sodium-ion short blade battery according to claim 1, characterized in that, In step S2, the first negative pressure is -60 to -100 Pa, and the second temperature is 40 to 60 °C.

4. The formation and capacity-maintaining process for a sodium-ion short blade battery according to claim 1, characterized in that, The fourth current factor is less than the fifth current factor; The fourth current multiplier is less than the sixth current multiplier.

5. The formation and capacity-maintaining process for a sodium-ion short blade battery according to claim 1, characterized in that, The fourth current multiplier is 0.20–0.40C, the fifth current multiplier is 0.45–0.60C, and the sixth current multiplier is 0.45–0.60C. The fourth voltage is 4.0-4.4V, the fifth voltage is 1.8-3.0V, and the sixth voltage is 3.7-3.9V.

Citation Information

Patent Citations

  • Preparation method of sodium ion battery

    CN117199502A

  • Formation method of sodium ion battery

    CN118099572A

  • Formation method of sodium ion battery

    CN118554046A