Low-temperature molten salt regeneration and recovery method of waste ternary positive electrode material

Through the low-temperature molten salt regeneration and recovery method, the high-temperature energy consumption and insufficient material structure repair of eutectic molten salt method are solved by using dimethyl carbonate and N-methylpyrrolidone solution treatment combined with lithium nitrate and potassium nitrate. It has achieved efficient regeneration and electrochemical performance improvement of ternary materials.

CN118919910APending Publication Date: 2024-11-08SHANGHAI JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411191112.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the existing lithium-ion battery positive electrode material recovery technology, the high-temperature regeneration step of the eutectic molten salt method leads to high energy consumption and limited effect on material structure repair, making it difficult to effectively reduce the recrystallization temperature of the ternary material.

Method used

Using the low-temperature molten salt regeneration and recycling method, the eutectics of waste ternary battery are significantly reduced by soaking the cathode material of the waste ternary battery in dimethyl carbonate and N-methylpyrrolidone solution, combined with the heating forging and remodeling of lithium nitrate and potassium nitrate. The molten salt temperature realizes direct regeneration of ternary materials.

Benefits of technology

It significantly reduces the energy consumption of the regeneration process, simplifies operation, improves the electrochemical performance repair effect of ternary materials, improves the long cycle and rate performance of the material, and improves the surface morphology, which is close to the performance of commercial materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919910A_ABST
    Figure CN118919910A_ABST
Patent Text Reader

Abstract

The invention relates to a low-temperature molten salt regeneration and recovery method of a waste ternary positive electrode material, which comprises the following steps of: disassembling a positive electrode from a discharged waste ternary battery, and sequentially soaking the positive electrode in a dimethyl carbonate solution and an N-methyl pyrrolidone solution, so that a ternary positive electrode active substance is separated from the surface of the positive electrode and is precipitated; and mixing the extracted ternary positive electrode active material with lithium nitrate and potassium nitrate, and sequentially carrying out heating forging and heating remodeling to realize recovery of the ternary positive electrode material. The method can obviously reduce the eutectic molten salt temperature and the energy consumption in the regeneration process, is simple and convenient to operate, is green and environment-friendly, and can quickly realize direct regeneration of the ternary material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a technology in the field of lithium battery manufacturing, specifically a low-temperature molten salt regeneration and recovery method for waste ternary positive electrode materials. Background Art

[0002] Existing lithium-ion battery cathode material recycling technologies include: pyrometallurgical recycling, wet recycling, direct regeneration and eutectic molten salt method. The eutectic molten salt method is to regenerate the waste lithium-ion cathode material in molten salt. The eutectic molten salt system has a crucial influence on the repair of the material structure. Since the recrystallization temperature of the ternary material cannot be changed, the temperature of the eutectic molten salt is the key to reducing the overall energy consumption of the regeneration step. Summary of the invention

[0003] In view of the above-mentioned deficiencies in the prior art, the present invention proposes a low-temperature molten salt regeneration and recovery method for waste ternary positive electrode materials. The low-temperature molten salt system significantly reduces the eutectic molten salt temperature and the energy consumption of the regeneration process. At the same time, the operation is simple, green and environmentally friendly, and can quickly realize the direct regeneration of ternary materials.

[0004] The present invention is achieved through the following technical solutions:

[0005] The invention relates to a low-temperature molten salt regeneration and recovery method for waste ternary positive electrode materials. The method comprises the following steps: the positive electrode is disassembled from the discharged waste ternary battery and then immersed in a dimethyl carbonate solution and an N-methylpyrrolidone solution in sequence, so that the ternary positive electrode active material is separated from the positive electrode surface and precipitated; the extracted ternary positive electrode active material is mixed with lithium nitrate and potassium nitrate and then subjected to heating forging and heating reshaping in sequence, so as to realize the recovery of the ternary positive electrode material.

[0006] The discharging is carried out by, but not limited to, immersing the waste ternary battery in a NaCl aqueous solution for discharging.

[0007] The immersion comprises: cutting the positive electrode of the battery into small pieces and then immersing the pieces in a dimethyl carbonate solution (DMC) for 3 to 24 hours, and then immersing the positive electrode pieces in an N-methylpyrrolidone solution (NMP) for 3 to 24 hours.

[0008] The precipitation refers to drying the precipitate obtained by centrifuging the N-methylpyrrolidone solution.

[0009] The molar ratio of lithium nitrate to potassium nitrate is 0.6-0.9.

[0010] The molar ratio of the ternary positive electrode active material to lithium nitrate and potassium nitrate is 10:1.

[0011] The heating forging means: heating to 100-190°C at 3-10°C / min and then maintaining for 3-12h.

[0012] The heating reshaping refers to: heating to 600-1000°C at 3-10°C / min and maintaining for 3-12h. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 The XRD patterns of the commercial ternary 111 material (Pristine), the scrapped ternary material (D-111), and the recycled material (R-111) in Example 1;

[0014] Figure 2 for Figure 1 A partial enlarged view of

[0015] Figure 3 The long cycle curves of the commercial ternary 111 material (P), the scrapped ternary material (D), and the recycled material (R) in Example 1;

[0016] Figure 4 It is a magnification diagram of the commercial ternary 111 material (P), the scrapped ternary material (D), and the recycled material (R) in Example 1;

[0017] Figure 5 This is the SEM image of the recycled material in Example 1. DETAILED DESCRIPTION Example 1

[0018] This embodiment relates to a low-temperature molten salt regeneration and recovery method for waste ternary positive electrode materials, comprising:

[0019] Step 1: Keep the used batteries in a NaCl aqueous solution for 3 hours.

[0020] Step 2: Disassemble the used batteries, cut the positive electrode into small pieces, and soak them in DMC for 3 hours.

[0021] Step 3: Take out the positive electrode sheet and continue to soak it in NMP for 3 hours. At this time, the positive electrode active material is separated from the aluminum foil. Take out the aluminum foil and centrifuge the obtained solution. Centrifuge it three times to obtain a precipitate and dry it.

[0022] Step 4: Mix the dried material with a certain proportion of lithium nitrate and potassium nitrate (molar ratio of 0.72), keep warm at 130° C. for 5 hours, and heat up at a rate of 3° C. / min.

[0023] Step 5: Continue heating the material to 800°C at a heating rate of 10°C / min and keep it at that temperature for 5 hours.

[0024] Step 6: Allow the material to cool naturally, wash with water, separate, and dry to obtain the regenerated positive electrode material.

[0025] like Figure 1 and Figure 2 As shown in the figure, there are XRD patterns of the commercial ternary 111 material (Pristine), the scrapped ternary material (D-111), and the recycled material (R-111) in this embodiment. As can be seen from the figure, the 006 / 102 and 110 / 108 peak spacings of the recycled material (R-111) are obviously repaired, and the 101 peak impurity peak is reduced, indicating that the lattice structure of the material has been well repaired.

[0026] like Figure 3 As shown in the figure, the long cycle curves of the commercial ternary 111 material (P), the scrapped ternary material (D), and the recycled material (R) in this embodiment. It can be seen that the long cycle performance of the recycled material is greatly improved and returns to the same level as the commercial material.

[0027] like Figure 4 As shown, the rate diagrams of the commercial ternary 111 material (P), scrapped ternary material (D), and recycled material (R) in this embodiment. It can be seen from the figure that the long rate performance of the recycled material is well improved, and the rate performance is even slightly better than that of the commercial material.

[0028] like Figure 5 As shown in FIG. 1 , the SEM image of the recycled material in this embodiment shows that the surface morphology of the recycled material is repaired, and the microcracks and holes on the surface of the primary particles are obviously repaired.

[0029] The experimental results of this embodiment are as follows: N-methylpyrrolidone (NMP) is used as a solvent, and the above-mentioned recycled materials are mixed with conductive carbon black and polyvinylidene fluoride (PVDF) in a mass ratio of 8:1:1 as this embodiment, stirred evenly into a slurry and coated on the surface of aluminum foil, and then vacuum dried for 12 hours, and pressed into a positive electrode sheet with a diameter of 10 mm; metallic lithium is used as a reference electrode, a microporous polypropylene membrane is used as a diaphragm, and 1 mol / L lithium hexafluorophosphate / ethylene carbonate, diethyl carbonate, methyl ethyl carbonate (volume ratio of 1:1:1) is used as the electrolyte. In a glove box filled with high-purity argon, 2025 button batteries are assembled. After standing for 12 hours, the electrochemical performance test is carried out.

[0030] The electrochemical performance test results show that the discharge capacity of the long-cycle scrapped material (D) is 72.7 mAh / g after 50 cycles, the discharge capacity of the scrapped material (D) at a rate of 10C is 18.8 mAh / g, and the discharge capacity of the scrapped material (D) after the rate is over is 102.6 mAh / g; the discharge capacity of the recycled material (R) is 152.2 mAh / g, the discharge capacity of the recycled material (R) at a rate of 10C is 39.4 mAh / g, and the discharge capacity of the recycled material (R) after the rate is over is 152.6 mAh / g (0.2C) Example 2

[0031] This embodiment includes the following steps:

[0032] Step 1: Keep the used batteries in a NaCl aqueous solution for 12 hours of discharge treatment.

[0033] Step 2: Disassemble the used batteries, cut the positive electrode into small pieces, and soak them in DMC for 12 hours.

[0034] Step 3: Take out the positive electrode sheet and continue to soak it in NMP for 12 hours. At this time, the positive electrode active material is separated from the aluminum foil. Take out the aluminum foil and centrifuge the obtained solution. Centrifuge it three times to obtain a precipitate and dry it.

[0035] Step 4: Mix the dried material with a certain proportion of lithium nitrate and potassium nitrate (molar ratio of 0.8), keep the mixture at 180° C. for 8 h, and heat at a rate of 5° C. / min.

[0036] Step 5: Continue heating the material to 900°C at a heating rate of 5°C / min and keep it at that temperature for 8h.

[0037] Step 6: Allow the material to cool naturally, wash with water, separate, and dry to obtain the regenerated positive electrode material.

[0038] The experimental results of this embodiment are as follows: N-methylpyrrolidone (NMP) is used as a solvent, and the above-mentioned recycled materials are mixed with conductive carbon black and polyvinylidene fluoride (PVDF) in a mass ratio of 8:1:1 as this embodiment, stirred evenly into a slurry and coated on the surface of aluminum foil, and then vacuum dried for 12 hours, and pressed into a positive electrode sheet with a diameter of 10 mm; metallic lithium is used as a reference electrode, a microporous polypropylene membrane is used as a diaphragm, and 1 mol / L lithium hexafluorophosphate / ethylene carbonate, diethyl carbonate, methyl ethyl carbonate (volume ratio of 1:1:1) is used as the electrolyte. In a glove box filled with high-purity argon, 2025 button batteries are assembled. After standing for 12 hours, the electrochemical performance test is carried out.

[0039] The results of electrochemical performance tests show that the discharge capacity of the long-cycle recycled material (R) is 151.8 mAh / g after 50 cycles, the discharge capacity of the recycled material (R) is 40.6 mAh / g at a rate of 10C, and the discharge capacity of the recycled material (R) is 153.1 mAh / g (0.2C) after the rate is completed. Example 3

[0040] This embodiment includes the following steps:

[0041] Step 1: Keep the used batteries in a NaCl aqueous solution for 24 hours.

[0042] Step 2: Disassemble the used batteries, cut the positive electrode into small pieces, and soak them in DMC for 24 hours.

[0043] Step 3: Take out the positive electrode sheet and continue to soak it in NMP for 24 hours. At this time, the positive electrode active material is separated from the aluminum foil. Take out the aluminum foil and centrifuge the obtained solution. Centrifuge it three times to obtain a precipitate and dry it.

[0044] Step 4: Mix the dried material with a certain proportion of lithium nitrate and potassium nitrate (molar ratio of 0.88), keep warm at 150° C. for 10 h, and heat up at a rate of 5° C. / min.

[0045] Step 5: Continue heating the material to 750°C at a heating rate of 5°C / min and keep the temperature for 12 hours.

[0046] Step 6: Allow the material to cool naturally, wash with water, separate, and dry to obtain the regenerated positive electrode material.

[0047] The experimental results of this embodiment are as follows: N-methylpyrrolidone (NMP) is used as a solvent, and the above-mentioned recycled materials are mixed with conductive carbon black and polyvinylidene fluoride (PVDF) in a mass ratio of 8:1:1 as this embodiment, stirred evenly into a slurry and coated on the surface of aluminum foil, and then vacuum dried for 12 hours, and pressed into a positive electrode sheet with a diameter of 10 mm; metallic lithium is used as a reference electrode, a microporous polypropylene membrane is used as a diaphragm, and 1 mol / L lithium hexafluorophosphate / ethylene carbonate, diethyl carbonate, methyl ethyl carbonate (volume ratio of 1:1:1) is used as the electrolyte. In a glove box filled with high-purity argon, 2025 button batteries are assembled. After standing for 12 hours, the electrochemical performance test is carried out.

[0048] The electrochemical performance test results show that the discharge capacity of the long-cycle regenerated material (R) is 152.6 mAh / g after 50 cycles, the discharge capacity of the regenerated material (R) is 40.9 mAh / g at a rate of 10C, and the discharge capacity of the regenerated material (R) is 151.9 mAh / g (0.2C) after the rate is completed. Example 4

[0049] This embodiment includes the following steps:

[0050] Step 1: Keep the used batteries in a NaCl aqueous solution for 30 hours.

[0051] Step 2: Disassemble the used batteries, cut the positive electrode into small pieces, and soak them in DMC for 10 hours.

[0052] Step 3: Take out the positive electrode sheet and continue to soak it in NMP for 10 hours. At this time, the positive electrode active material is separated from the aluminum foil. Take out the aluminum foil and centrifuge the obtained solution. Centrifuge it three times to obtain a precipitate and dry it.

[0053] Step 4: Mix the dried material with a certain proportion of lithium nitrate and potassium nitrate (molar ratio of 0.63), keep warm for 10 hours at 110°C, and heat up at a rate of 10°C / min.

[0054] Step 5: Continue heating the material to 1000°C at a heating rate of 3°C / min and keep it at that temperature for 3h.

[0055] Step 6: Allow the material to cool naturally, wash with water, separate, and dry to obtain the regenerated positive electrode material.

[0056] The experimental results of this embodiment are as follows: N-methylpyrrolidone (NMP) is used as a solvent, and the above-mentioned recycled materials are mixed with conductive carbon black and polyvinylidene fluoride (PVDF) in a mass ratio of 8:1:1 as this embodiment, stirred evenly into a slurry and coated on the surface of aluminum foil, and then vacuum dried for 12 hours, and pressed into a positive electrode sheet with a diameter of 10 mm; metallic lithium is used as a reference electrode, a microporous polypropylene membrane is used as a diaphragm, and 1 mol / L lithium hexafluorophosphate / ethylene carbonate, diethyl carbonate, methyl ethyl carbonate (volume ratio of 1:1:1) is used as the electrolyte. In a glove box filled with high-purity argon, 2025 button batteries are assembled. After standing for 12 hours, the electrochemical performance test is carried out.

[0057] The results of electrochemical performance tests show that the discharge capacity of the long-cycle regenerated material (R) is 153.4 mAh / g after 50 cycles, the discharge capacity of the regenerated material (R) is 40.3 mAh / g at a rate of 10C, and the discharge capacity of the regenerated material (R) is 153.3 mAh / g (0.2C) after the rate is completed.

[0058] Compared with the prior art, the present invention can significantly improve the repair effect of the electrochemical performance of the recycled material, and the discharge specific capacity under high-rate charge and discharge conditions is improved to a certain extent compared with commercial materials.

[0059] The above-mentioned specific implementation can be partially adjusted in different ways by those skilled in the art without departing from the principle and purpose of the present invention. The protection scope of the present invention shall be based on the claims and shall not be limited by the above-mentioned specific implementation. Each implementation scheme within its scope shall be subject to the constraints of the present invention.

Claims

1. A low-temperature molten salt regeneration and recovery method for waste ternary positive electrode materials, characterized in that: The positive electrode is disassembled from the discharged waste ternary battery and then immersed in dimethyl carbonate solution and N-methylpyrrolidone solution in turn, so that the ternary positive electrode active material is separated from the positive electrode surface and precipitated; the extracted ternary positive electrode active material is mixed with lithium nitrate and potassium nitrate and then subjected to heat forging and heat reshaping in turn to achieve the recovery of the ternary positive electrode material.

2. The low-temperature molten salt regeneration and recovery method of waste ternary positive electrode materials according to claim 1 is characterized in that: The immersion comprises: cutting the positive electrode of the battery into small pieces and then immersing the pieces in a dimethyl carbonate solution (DMC) for 3 to 24 hours, and then immersing the positive electrode pieces in an N-methylpyrrolidone solution (NMP) for 3 to 24 hours.

3. The low-temperature molten salt regeneration and recovery method of waste ternary positive electrode materials according to claim 1 is characterized in that: The molar ratio of lithium nitrate to potassium nitrate is 0.6-0.

9.

4. The low-temperature molten salt regeneration and recovery method of waste ternary positive electrode materials according to claim 1 is characterized in that: The heating forging means: heating to 100-190°C at 3-10°C / min and then maintaining for 3-12h.