High-conductivity composite coating diaphragm as well as preparation method and application thereof

By coating the lithium-ion battery separator with a high-conductivity composite coating, the safety and performance deficiencies of the separator in high-energy-density batteries are solved, achieving higher ionic conductivity, temperature resistance and adhesion, thus improving the safety and stability of the battery.

CN118920022AActive Publication Date: 2024-11-08HEBEI GELLEC NEW ENERGY MATERIAL SCI&TECHNOLOY CO LTD

Patent Information

Application Number
CN202411152384.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-08
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

Existing lithium-ion battery separators cannot meet the safety performance requirements of high-energy-density batteries. Insufficient performance in areas such as heat resistance, strength, flame retardancy, porosity, and electrolyte wettability leads to the risk of spontaneous combustion and explosion of lithium-ion batteries.

Method used

A high-conductivity composite coating membrane is adopted. The coating consists of poly(p-phenylene terephthalamide) (PPTA), lithium aluminum titanium phosphate (LATP), aluminum nitride, and a first substance. These are mixed in a specific ratio and coated on a base membrane, followed by extraction and dehydration treatment to improve the ionic conductivity, temperature resistance, and adhesion of the membrane.

Benefits of technology

It improves the ionic conductivity, temperature resistance, and adhesion of lithium-ion battery separators, enhances battery safety and stability, and improves electrolyte wettability and permeability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118920022A_ABST
    Figure CN118920022A_ABST
Patent Text Reader

Abstract

The invention discloses a high-conductivity composite coating diaphragm and a preparation method and application thereof.The high-conductivity composite coating diaphragm comprises a base diaphragm and a coating coated on the base diaphragm, and the coating comprises poly-p-phenylene terephthamide, lithium titanium aluminum phosphate, aluminum nitride and a first substance, the first substance is one or a mixture of more of lithium nitrate, sodium dodecyl benzene sulfonate, organic nitrate and isosorbide dinitrate; by introducing aluminum nitride, the transmission of lithium ions in the coating diaphragm is improved, so that the ionic conductivity of the coating diaphragm is improved; due to the introduction of the PPTA, the temperature resistance and the binding power of the coating diaphragm are better improved; the introduction of LATP brings good porosity, thermal stability and liquid absorption rate to the coating diaphragm; the first substance is introduced as the dispersing agent of the LATP, so that the dispersity of the LATP is improved, and meanwhile, the lithium element is contained, so that the lithium supplementing effect on the diaphragm can be achieved, and the ionic conductivity of the diaphragm can be enhanced through the synergistic effect of the lithium element and the aluminum nitride.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of battery separators, and in particular relates to a high-conductivity composite coating separator and a preparation method and application thereof. Background Art

[0002] With the rapid development of high-power equipment such as new energy electric vehicles and large-scale energy storage systems, large-capacity, high-energy-density power and energy storage lithium-ion batteries have shown a blowout development in recent years.

[0003] However, in recent years, the frequent spontaneous combustion and explosion incidents of new energy electric vehicles have aroused great concern and doubts about the safety of power lithium-ion batteries. Among them, one of the core reasons is that the performance of existing lithium battery separators cannot meet the application requirements of high-energy-density batteries. Power lithium-ion batteries require higher safety performance, larger capacity, uniform performance of long-term stable output, and high-rate charge and discharge performance. As the "third electrode" of lithium-ion batteries, the separator is a key material to ensure the safety of the battery system and affect the battery performance. It needs to have high strength, heat resistance, flame retardancy, high porosity, uniformity and good wettability. The separator plays two main roles in lithium-ion batteries. First, the separator material needs to have good insulation and a certain strength to avoid direct contact between the positive and negative electrodes in the battery, and can effectively prevent short circuits caused by punctures such as burrs and dendrites, and ensure that there is no large-scale dimensional change under sudden high temperature conditions, thereby ensuring the safety of the battery. Second, the porous structure of the separator can provide a good migration channel for lithium ions to ensure stable and efficient operation of the battery. Therefore, it is of great significance to develop a separator with higher safety. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention aims to provide a high-conductivity composite coating diaphragm.

[0005] Another object of the present invention is to provide a method for preparing the above-mentioned high-conductivity composite coating diaphragm.

[0006] Another object of the present invention is to provide a slurry.

[0007] Another object of the present invention is to provide a method for preparing the slurry.

[0008] The purpose of the present invention is achieved through the following technical solutions.

[0009] A high-conductivity composite coating diaphragm comprises: a base film and a coating coated on the base film, wherein the coating comprises: poly(p-phenylene terephthalamide) (PPTA), lithium aluminum titanium phosphate (LATP), aluminum nitride and a first substance, wherein the ratio of poly(p-phenylene terephthalamide) (PPTA), lithium aluminum titanium phosphate (LATP), aluminum nitride and the first substance is (7-12): (2-10): (0.15-1): (0.05-0.3) by mass, and the first substance is one or a mixture of several of lithium nitrate, sodium dodecylbenzene sulfonate, organic nitrate and isosorbide dinitrate.

[0010] The method for preparing the above-mentioned high-conductivity composite coating membrane comprises: coating the slurry on the base membrane, obtaining a coating on the base membrane, obtaining a high-conductivity composite coating membrane precursor, extracting the high-conductivity composite coating membrane precursor, dehydrating the high-conductivity composite coating membrane, and obtaining a high-conductivity composite coating membrane.

[0011] In the above technical solution, the extraction adopts an extraction liquid, and the high-conductivity composite coating membrane precursor passes through the extraction liquids with extractant concentrations from high to low in sequence, and the extractant is N-methylpyrrolidone (NMP).

[0012] In the above technical scheme, the extracting liquids with the highest to lowest extracting agent concentrations are the first extracting liquid, the second extracting liquid, the third extracting liquid and the fourth extracting liquid, respectively. The first extracting liquid, the second extracting liquid and the third extracting liquid are mixtures of extracting agent and water, and the fourth extracting liquid is water. The concentration of the extracting agent in the first extracting liquid is 65-80wt%, the concentration of the extracting agent in the second extracting liquid is 40-60wt%, and the concentration of the extracting agent in the third extracting liquid is 20-40wt%.

[0013] In the above technical solution, the dehydration treatment is drying at 50-60°C for 6-12 minutes.

[0014] A slurry includes poly (p-phenylene terephthalamide) (PPTA), lithium aluminum titanium phosphate (LATP), aluminum nitride and a first substance. In the slurry, the ratio of poly (p-phenylene terephthalamide) (PPTA), lithium aluminum titanium phosphate (LATP), aluminum nitride and the first substance is (7-12): (2-10): (0.15-1): (0.05-0.3) by mass. The first substance is one or a mixture of several selected from lithium nitrate, sodium dodecylbenzene sulfonate, organic nitrate and isosorbide dinitrate.

[0015] In the above technical solution, the slurry also includes: a solvent, the solvent is a single-component solvent and / or a multi-component solvent, the single-component solvent is N-methylpyrrolidone, the multi-component solvent includes: solvent 1 and solvent 2, solvent 1 includes: acetonitrile and / or dimethylformamide, solvent 2 includes: hexamethylphosphoramide, dimethylacetamide and tetramethylurea, one or a mixture of several thereof.

[0016] In the above technical solution, the slurry also includes: calcium chloride.

[0017] In the above technical solution, the ratio of the mass fraction of lithium aluminum titanium phosphate (LATP) to the volume fraction of the solvent is (2-10):(93-97), the unit of the mass fraction is g, and the unit of the volume fraction is mL.

[0018] In the above technical solution, the ratio of calcium chloride to lithium aluminum titanium phosphate (LATP) is (0.05-0.1): (2-8) by mass.

[0019] A method for preparing a slurry comprises: mixing a first slurry and a second slurry until they are uniform to obtain a slurry, wherein the first slurry comprises: lithium aluminum titanium phosphate (LATP), aluminum nitride, a first substance and a first solvent, and the second slurry comprises: poly(p-phenylene terephthalamide) (PPTA), calcium chloride and a second solvent; wherein, by weight, the ratio of poly(p-phenylene terephthalamide) (PPTA), lithium aluminum titanium phosphate (LATP), aluminum nitride and the first substance is (7-12): (2-10): (0.15-1): (0.05-0.3), and the first substance is one or a mixture of several of lithium nitrate, sodium dodecylbenzene sulfonate, organic nitrate and isosorbide dinitrate.

[0020] The ratio of the mass fraction of lithium aluminum titanium phosphate (LATP) to the volume fraction of the first solvent is (16-33): (60.8-82.5), the unit of mass fraction is g, and the unit of volume fraction is mL; by volume fraction, the ratio of the first solvent to the second solvent is (6.08-16.5): (70-90); by mass fraction, the ratio of calcium chloride to lithium aluminum titanium phosphate (LATP) is (0.05-0.1): (2-8).

[0021] In the above technical solution, the first slurry and the second slurry are mixed and stirred at 30-45° C. and 350-400 r / min for 3-5 hours until they are uniform.

[0022] In the above technical solution, the method for preparing the first slurry is: mixing LATP, aluminum nitride, the first substance and the first solvent until they are uniformly dispersed.

[0023] In the method for preparing the first slurry, LATP, aluminum nitride, the first substance and the first solvent are mixed, and the mixture is mixed and uniformly dispersed by wet ball milling for 3 to 5 hours.

[0024] In the above technical scheme, the method for preparing the second slurry is: mixing calcium chloride and a second solvent at 70-85°C, stirring until uniform, cooling to 0-3°C, and then adding p-phenylenediamine (PPDA), terephthaloyl chloride (TPC) and pyridine, stirring until uniform, to obtain a second slurry, wherein the ratio of the volume fraction of the second solvent, the mass fraction of p-phenylenediamine, the mass fraction of terephthaloyl chloride and the volume fraction of pyridine is (90-110): (4-5): (7-9): (4-5), wherein the unit of mass fraction is g, and the unit of volume fraction is mL (p-phenylenediamine and terephthaloyl chloride are used to synthesize poly (p-phenylenediamine) (PPTA), and pyridine is used to remove small molecular HCl produced in the process of synthesizing PPTA).

[0025] In the above technical solution, the first solvent is one or a mixture of several of N-methylpyrrolidone, acetonitrile and dimethylformamide.

[0026] In the above technical solution, the second solvent is one or a mixture of hexamethylphosphoramide, dimethylacetamide, N-methylpyrrolidone and tetramethylurea.

[0027] In the above technical solution, the first solvent and the second solvent may be the same or different.

[0028] In the above technical scheme, the method for obtaining lithium aluminum titanium phosphate (LATP) is: uniformly mixing a lithium source, an aluminum source, a titanium source and ammonium dihydrogen phosphate to obtain a first powder, keeping the first powder at 700-900° C. for 8 hours to obtain a LATP sintered block, grinding it into powder, and obtaining lithium aluminum titanium phosphate (LATP), wherein, in terms of the amount of substance, the ratio of lithium in the lithium source, aluminum in the aluminum source, titanium in the titanium source and phosphorus in the ammonium dihydrogen phosphate is (10-15): (1-5): (30-35): (55-65);

[0029] In the method for obtaining LATP, the lithium source is lithium carbonate or lithium nitrate; the aluminum source is boehmite or aluminum oxide; and the titanium source is one or a mixture of titanium dioxide, titanium hydroxide and tetrabutyl titanate.

[0030] In the method for obtaining LATP, a lithium source, an aluminum source, a titanium source and ammonium dihydrogen phosphate are uniformly mixed by wet ball milling for 2 to 3 hours.

[0031] In the method for obtaining LATP, wet ball milling is followed by drying, the drying temperature is 60 to 80° C., and the drying time is 16 to 24 hours.

[0032] In the method for obtaining LATP, the rate of heating to 700-900°C is 4-6°C / min.

[0033] In the above technical solution, the ball-to-material ratio of the wet ball mill is (0.8-1.2):(6-8), the wet ball mill uses grinding balls with a diameter of 5-10 mm, the orbital speed of the wet ball mill is 180-250 r / min, and the rotation speed is 550-650 r / min.

[0034] Application of high conductivity composite coating separator in lithium-ion batteries.

[0035] The invention discloses a method for synergistically improving the heat resistance, breakdown voltage and / or adhesion of a diaphragm by using four substances. The four substances are poly(p-phenylene terephthalamide) (PPTA), lithium aluminum titanium phosphate (LATP), aluminum nitride and a first substance. The first substance is a mixture of one or more of lithium nitrate, sodium dodecylbenzene sulfonate, organic nitrate and isosorbide nitrate. The ratio of poly(p-phenylene terephthalamide) (PPTA), lithium aluminum titanium phosphate (LATP), aluminum nitride and the first substance is (7-12): (2-10): (0.15-1): (0.05-0.3) by mass.

[0036] The application of a first substance, lithium aluminum titanium phosphate (LATP) and aluminum nitride to synergistically improve the ionic conductivity of the diaphragm, wherein the first substance is one or a mixture of several of lithium nitrate, sodium dodecylbenzene sulfonate, organic nitrate and isosorbide dinitrate.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] 1. The present invention improves the transmission of lithium ions in the coating diaphragm by introducing aluminum nitride, thereby improving the ionic conductivity of the coating diaphragm; the introduction of PPTA better improves the temperature resistance and adhesion of the coating diaphragm; the introduction of LATP brings good porosity (good air permeability), thermal stability and liquid absorption rate to the coating diaphragm; the first substance is introduced as a dispersant for LATP, which improves the dispersibility of LATP. At the same time, due to the presence of lithium element, it can play the role of replenishing lithium for the diaphragm, and can synergize with aluminum nitride to enhance the ionic conductivity of the diaphragm.

[0039] 2. The first slurry and the second slurry of the present invention have good compatibility.

[0040] 3. The preparation method of the present invention has high repeatability. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 This is the SEM of the coated diaphragm prepared in Example 5;

[0042] Figure 2 This is the appearance of the slurry prepared in Example 1 after standing for 24 hours;

[0043] Figure 3This is the appearance of the slurry prepared in Comparative Example 2 after standing for 24 hours. DETAILED DESCRIPTION

[0044] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0045] The purchase sources of the drugs involved in the following embodiments and comparative examples are as follows:

[0046] Lithium carbonate, purity 99.5%;

[0047] Boehmite, purity 99%;

[0048] Titanium dioxide, 99% pure;

[0049] Ammonium dihydrogen phosphate, analytical grade;

[0050] Lithium nitrate, analytical grade;

[0051] Aluminum nitride, purity 99.9%;

[0052] Calcium chloride, purity 94%;

[0053] p-phenylenediamine, purity 99.5%;

[0054] Terephthaloyl chloride, purity 99.5%;

[0055] Pyridine, purity 99.8%;

[0056] N-methylpyrrolidone (NMP), purity 99.5%;

[0057] Electrolyte: The electrolyte includes an electrolyte and a solvent. The electrolyte is LiPF6. The concentration of the electrolyte in the electrolyte is 1.0M. The solvents are ethyl carbonate, methyl carbonate and dimethyl carbonate. The volume ratio of ethyl carbonate, methyl carbonate and dimethyl carbonate is 1:1:1.

[0058] The models and manufacturers of the equipment involved in the following embodiments and comparative examples are as follows:

[0059] High-speed planetary ball mill, MSK-SFM-15, Hefei Kejing Material Technology Co., Ltd.;

[0060] Scanning electron microscope, Sigma 300, Carl Zeiss, Germany;

[0061] Japan AsahiSeiko Asahi Seiko air permeability meter, model EH01-551MR;

[0062] Japan Shimadzu stretching machine, model, AGS-X (100N);

[0063] Electrochemical workstation, CHI660E, Shanghai Chenhua Instrument Co., Ltd.

[0064] In the following examples and comparative examples, the ball-to-material ratio of the wet ball mill is 1:7, the wet ball mill uses zirconia balls with a diameter of 5 mm, the orbital speed of the wet ball mill is 200 r / min, and the rotation speed is 600 r / min.

[0065] In the following examples and comparative examples, the base film is a polyethylene film with a thickness of 9 um.

[0066] In the following examples and comparative examples, water is deionized water.

[0067] Air permeability value: Place the coated membrane on the Japanese AsahiSeiko air permeability tester, test 10 points evenly, and take the average value of the 10 points, which is the air permeability value;

[0068] Breakdown voltage: Lay the coated diaphragm flat on the test conductive plate, test 50 breakdown points, and the average value of the 50 breakdown points is the breakdown voltage;

[0069] Thermal shrinkage: Cut the coated membrane into 4 cm × 6 cm, measure the area change of the 4 cm × 6 cm coated membrane in an oven at 180°C for 1 hour, and obtain the thermal shrinkage rate;

[0070] Ionic conductivity: At room temperature and 100% RH, the coated membrane is immersed in an electrolyte and the ionic conductivity is measured by the AC impedance method at room temperature;

[0071] Diaphragm adhesion: Cut the coated diaphragm into a shape of 25mm×60mm, then stick the tape on the coated diaphragm, and use a Japanese Shimadzu stretching machine to tear the tape and the coated diaphragm apart. The force used is the diaphragm adhesion.

[0072] In the tests of air permeability, breakdown voltage, thermal shrinkage, ionic conductivity and membrane adhesion, the coated membrane is one of the coated membranes prepared in Examples 5 to 8 and Comparative Examples 4 to 5.

[0073] Embodiments 1 to 4

[0074] A method for preparing a slurry comprises: mixing a first slurry and a second slurry, stirring at 35° C. and 380 r / min for 4 hours until the mixture is uniform, to obtain the slurry, wherein the first slurry is a mixture of LATP, aluminum nitride, a first substance and a first solvent, the second slurry comprises: poly(p-phenylene terephthalamide) (PPTA), calcium chloride and a second solvent, the ratio of poly(p-phenylene terephthalamide) (PPTA), LATP, aluminum nitride and the first substance is X by weight, the first substance is lithium nitrate, the first solvent is N-methylpyrrolidone (NMP), and the second solvent is N-methylpyrrolidone (NMP).

[0075] The ratio of the mass fraction of LATP to the volume fraction of the first solvent is Y, the unit of mass fraction is g, and the unit of volume fraction is mL; the ratio of the first solvent to the second solvent is Z by volume; the ratio of calcium chloride to lithium aluminum titanium phosphate (LATP) is W by mass.

[0076] The method for preparing the first slurry is: mixing LATP, aluminum nitride, the first substance and the first solvent, and wet-milling for 4 hours until the mixture is uniformly dispersed.

[0077] The method for obtaining LATP is as follows: a lithium source, an aluminum source, a titanium source and ammonium dihydrogen phosphate are mixed, wet ball milled for 2.5 hours until uniform, dried in an oven at 70°C for 18 hours to obtain a first powder, the first powder is placed in a muffle furnace, heated from room temperature to 850°C at a heating rate of 5°C / min and kept at 850°C for 8 hours to obtain a LATP sintered block, ground to obtain LATP (powder), wherein, by amount of substance, the ratio of lithium in the lithium source, aluminum in the aluminum source, titanium in the titanium source and phosphorus in the ammonium dihydrogen phosphate is 13:3:34:60, the lithium source is lithium carbonate, the aluminum source is boehmite, and the titanium source is titanium dioxide.

[0078] The method for preparing the second slurry is: mixing calcium chloride and a second solvent at 80° C., stirring until uniform, cooling to 0° C., adding p-phenylenediamine (PPDA), and then adding terephthaloyl chloride (TPC) and pyridine, stirring for 30 minutes until uniform, to obtain a second slurry, wherein the ratio of the volume fraction of the second solvent, the mass fraction of p-phenylenediamine, the mass fraction of terephthaloyl chloride and the volume fraction of pyridine is 100:4.54:8.12:4.5, the unit of mass fraction is g, and the unit of volume fraction is mL, p-phenylenediamine and terephthaloyl chloride are used to synthesize poly(p-phenylene terephthalamide) (PPTA), and pyridine is used to remove small molecular HCl generated in the process of synthesizing PPTA.

[0079] Table 1

[0080] Example X Y Z W Example 1 9.6:6:0.6:0.16 30:66.2 13.24:80 0.06:6 Example 2 9.6:6:0.2:0.16 30:68.2 13.64:80 0.06:6 Example 3 10.8:3:0.3:0.08 30:66.2 6.62:90 0.08:3 Example 4 9.6:3.2:0.6:0.16 16:80.2 16.04:80 0.06:3.2

[0081] Comparative Example 1

[0082] A method for preparing a slurry comprises: mixing a third slurry and a second slurry prepared in Example 1, stirring at 35° C. and 380 r / min for 4 hours until uniform, wherein the third slurry is a mixture of LATP, a first substance and a first solvent, wherein, by mass, the ratio of poly(p-phenylene terephthalamide) (PPTA), LATP and the first substance is 9.6:6:0.16, by volume, the ratio of the first solvent in the third slurry to the second solvent in the second slurry is 13.84:80, the first substance is lithium nitrate, the first solvent is N-methylpyrrolidone (NMP), the second solvent is N-methylpyrrolidone (NMP), the ratio of the mass fraction of LATP to the volume fraction of the first solvent in the third slurry is 30:69.2, the unit of mass fraction is g, and the unit of volume fraction is mL,

[0083] The method for preparing the third slurry is: mixing the LATP prepared in Example 1, the first substance and the first solvent, and wet-milling for 4 hours until the mixture is uniformly dispersed.

[0084] Comparative Example 2

[0085] A method for preparing a slurry comprises: mixing LATP, NMP and aluminum nitride prepared in Example 1, wet ball milling for 4 hours, and dispersing LATP and aluminum nitride in NMP, wherein the ratio of the mass fraction of LATP, the mass fraction of aluminum nitride and the volume fraction of NMP is 30:3:67, the unit of mass fraction is g, and the unit of volume fraction is mL. The slurry is obviously stratified after being stationary for 3 hours and cannot be used.

[0086] Comparative Example 3

[0087] A slurry, which is the first slurry in Example 1.

[0088] Examples 5 to 8 and Comparative Examples 4 to 5

[0089] A method for preparing a coating membrane, comprising: coating a slurry on a base film, obtaining a coating on the base film, obtaining a coating membrane precursor, extracting the coating membrane precursor, drying it in an oven at 55° C. for 8 minutes for dehydration treatment, and obtaining a coating membrane, wherein the slurry is one of the slurries prepared in Examples 1 to 4, Comparative Example 1 and Comparative Example 3, as shown in Table 2 (the coating membranes prepared in Examples 5 to 8 are named high-conductivity composite coating membranes), wherein the extraction adopts an extraction liquid, and the extraction process is: the coating membrane precursor is obtained according to The extractants are passed through the extraction liquids with extractant concentrations from high to low, the extractant is N-methylpyrrolidone (NMP), the extractants with extractant concentrations from high to low are the first extractant, the second extractant, the third extractant and the fourth extractant, the first extractant, the second extractant and the third extractant are each a mixture of the extractant and water, the fourth extractant is water, wherein the concentration of the extractant in the first extract is 80wt%, the concentration of the extractant in the second extract is 50wt%, and the concentration of the extractant in the third extract is 30wt%.

[0090] Table 2

[0091] Coated diaphragm Slurry for preparing coated diaphragms Example 5 Example 1 Example 6 Example 2 Example 7 Example 3 Example 8 Example 4 Comparative Example 4 Comparative Example 1 Comparative Example 5 Comparative Example 3

[0092] Example 5 SEM of the coating membrane prepared Figure 1 shown.

[0093] During the process of preparing the coated membrane, the coated membrane prepared in Comparative Example 5 showed slight material shedding.

[0094] The coated membranes prepared in the embodiments and comparative examples were subjected to air permeability test, breakdown voltage test, thermal shrinkage test, ion conductivity test and adhesion test, and the air permeability value, breakdown voltage, thermal shrinkage rate, ion conductivity and membrane adhesion were obtained in turn. The results are shown in Table 3.

[0095] Table 3

[0096]

[0097]

[0098] Through the air permeability test, it can be known that the introduction of LATP can reduce the air permeability of the coating membrane. At the same time, the introduction of LATP can effectively improve the breakdown voltage of the membrane and to a certain extent cooperate with PPTA to increase the temperature resistance of the membrane, so that the membrane has a more stable performance. At the same time, the coating membrane has good ionic conductivity due to the introduction of aluminum nitride. No PPTA was added to the slurry prepared in Comparative Example 3, so that the membrane adhesion of the coating membrane prepared by the slurry of Comparative Example 3 was very low, and even a slight drop of material occurred. However, it also proved from the side that the introduction of PPTA greatly improved the adhesion of the membrane. No PPTA was added to the slurry prepared in Comparative Example 3, so that the thermal shrinkage rate of the coating membrane prepared by the slurry of Comparative Example 3 was very large, indicating that PPTA can improve the high temperature resistance of the coating membrane.

[0099] The coating membrane prepared in Example 5 was microscopically scanned. From the SEM image, it can be seen that the LATP is distributed relatively evenly and the PPTA fibers are evenly distributed on the surface of the base membrane.

[0100] Depend on Figure 2 and Figure 3 It can be seen that the slurry prepared in Example 1 has no obvious stratification after standing for 24 hours, and the slurry prepared in Comparative Example 2 has obvious stratification after standing for 24 hours. By comparing the two, it can be seen that after the introduction of the first substance (lithium nitrate), LATP has good dispersibility.

[0101] The coating membranes prepared in the examples and comparative examples were subjected to liquid absorption test, liquid climbing test and liquid retention test, and the liquid absorption rate, liquid climbing value and liquid retention rate were obtained in turn, wherein:

[0102] The liquid absorption rate is obtained by weighing a 5cm×5cm diaphragm m0, soaking it in electrolyte, taking out the electrolyte on the surface and wiping it with a non-woven cloth and weighing it m1. The liquid absorption rate of the diaphragm is calculated by (m1-m0) / m0*100%.

[0103] Liquid retention rate: The liquid absorption rate is calculated by soaking a 5cm×5cm diaphragm in electrolyte, then taking out the electrolyte on the surface and wiping it with a non-woven cloth, weighing m2. After wiping the surface electrolyte, place it in the air for 1 hour and weigh m3. The liquid retention rate of the diaphragm is calculated by (m2-m3) / m2*100%.

[0104] Liquid creepage value: Cut the coated diaphragm into 4cm×15cm, place it vertically and immerse the bottom (length 1cm) in the electrolyte for 20min / 40min / 60min. The length of the diaphragm soaked in the electrolyte after soaking for different time periods is the liquid creepage value of the coated diaphragm.

[0105] The coated diaphragm is one of the coated diaphragms prepared in Examples 5 to 8.

[0106] Table 4

[0107]

[0108]

[0109] The results of the liquid absorption, liquid retention and liquid climbing tests show that the slurry of the present invention provides the diaphragm with better electrolyte wettability and can better preserve the electrolyte in the battery.

[0110] The present invention is described above by way of example. It should be noted that, without departing from the core of the present invention, any simple deformation, modification or other equivalent replacement that can be made by those skilled in the art without inventive effort falls within the protection scope of the present invention.

Claims

1. A high conductivity composite coating diaphragm, characterized in that: include: A base film and a coating applied on the base film, wherein the coating comprises: poly(p-phenylene terephthalamide), lithium aluminum titanium phosphate, aluminum nitride and a first substance, wherein the ratio of poly(p-phenylene terephthalamide), lithium aluminum titanium phosphate, aluminum nitride and the first substance is (7-12):(2-10):(0.15-1):(0.05-0.3) by mass, and the first substance is one or a mixture of several of lithium nitrate, sodium dodecylbenzene sulfonate, organic nitrate and isosorbide dinitrate.

2. The method for preparing the high-conductivity composite coating diaphragm according to claim 1, characterized in that: include: The slurry is coated on the base film to obtain a coating on the base film to obtain a high-conductivity composite coating membrane precursor, and the high-conductivity composite coating membrane precursor is extracted and dehydrated to obtain a high-conductivity composite coating membrane.

3. A slurry, characterized in that: include: Poly(p-phenylene terephthalamide), lithium aluminum titanium phosphate, aluminum nitride and the first substance are present in a slurry in a ratio of (7-12):(2-10):(0.15-1):(0.05-0.3) by mass. The first substance is a mixture of one or more of lithium nitrate, sodium dodecylbenzene sulfonate, organic nitrate and isosorbide dinitrate.

4. The slurry according to claim 3, characterized in that The slurry also includes: a solvent, which is a single-component solvent and / or a multi-component solvent. The single-component solvent is N-methylpyrrolidone, and the multi-component solvent includes: solvent 1 and solvent 2. Solvent 1 includes: acetonitrile and / or dimethylformamide, and solvent 2 includes: one or a mixture of hexamethylphosphoramide, dimethylacetamide and tetramethylurea.

5. A method for preparing a slurry, characterized in that: include: The first slurry and the second slurry are mixed until uniform to obtain a slurry, wherein the first slurry comprises: lithium aluminum titanium phosphate, aluminum nitride, a first substance and a first solvent, and the second slurry comprises: poly(p-phenylene terephthalamide), calcium chloride and a second solvent; wherein, by weight, the ratio of poly(p-phenylene terephthalamide), lithium aluminum titanium phosphate, aluminum nitride and the first substance is (7-12): (2-10): (0.15-1): (0.05-0.3), and the first substance is one or a mixture of several selected from lithium nitrate, sodium dodecylbenzene sulfonate, organic nitrate and isosorbide dinitrate, The ratio of the mass fraction of lithium aluminum titanium phosphate to the volume fraction of the first solvent is (16-33): (60.8-82.5), the unit of mass fraction is g, and the unit of volume fraction is mL; by volume, the ratio of the first solvent to the second solvent is (6.08-16.5): (70-90); by mass, the ratio of calcium chloride to lithium aluminum titanium phosphate is (0.05-0.1): (2-8).

6. The preparation method according to claim 5, characterized in that: The first solvent is one or a mixture of N-methylpyrrolidone, acetonitrile and dimethylformamide.

7. The preparation method according to claim 5, characterized in that: The second solvent is one or a mixture of hexamethylphosphoramide, dimethylacetamide, N-methylpyrrolidone and tetramethylurea.

8. Use of the high-conductivity composite coating separator as claimed in claim 1 in lithium-ion batteries.

9. Use of four substances in synergistically improving the temperature resistance, breakdown voltage and / or adhesion of a diaphragm, characterized in that: The four substances are poly (p-phenylene terephthalamide), lithium aluminum titanium phosphate, aluminum nitride and a first substance. The first substance is a mixture of one or more of lithium nitrate, sodium dodecylbenzene sulfonate, organic nitrate and isosorbide dinitrate. Calculated by mass, the ratio of poly (p-phenylene terephthalamide), lithium aluminum titanium phosphate, aluminum nitride and the first substance is (7-12): (2-10): (0.15-1): (0.05-0.3).

10. Application of the first substance, lithium aluminum titanium phosphate and aluminum nitride to synergistically improve the ionic conductivity of the diaphragm, characterized in that: The first substance is one or a mixture of lithium nitrate, sodium dodecylbenzene sulfonate, organic nitrate and isosorbide dinitrate.

Citation Information

Patent Citations

  • Polymer composite film, preparation method thereof and lithium ion battery comprising same

    CN108242522A

  • Lithium ion battery diaphragm, preparation method thereof and lithium ion battery

    CN115548576A

  • Ethylenediamine tetraacetic acid-based multiphase composite electrolyte diaphragm and preparation method thereof

    CN115911751A

  • Slurry composition, method for manufacturing the same, and coated body formed by use thereof

    JP2016103439A

Cited By

  • Battery diaphragm containing pyridyl heterocyclic aramid as well as preparation method and application of battery diaphragm

    CN120565996A