Magnetic wedge and rotating electrical machine

By designing a magnetic wedge composed of flat magnetic metal particles and inclusion phases in a rotating electric motor, controlling its orientation angle, and arranging the stator radially or axially, the problems of high-order harmonic loss and insufficient mechanical properties of existing magnetic wedges are solved, and a rotating electric motor with low loss, high permeability, and high strength is realized.

CN118920741APending Publication Date: 2024-11-08KK TOSHIBA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311170980.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-08-24
Filing Date
2023-09-12
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing magnetic wedges in rotating motors suffer from problems such as large high-order harmonic losses, low magnetic saturation, low permeability, and insufficient mechanical properties, especially in terms of thermal stability and strength, which need to be improved.

Method used

A magnetic wedge is formed by multiple flat magnetic metal particles and inclusion phases. The flat surfaces of the flat magnetic metal particles are oriented in the width and length directions, and the orientation angles of the center and ends are controlled within a specific range. The stator is arranged radially or axially with the rotor at intervals to form a radially or axially spaced rotary motor.

Benefits of technology

It achieves low magnetic loss, high permeability and excellent mechanical properties, improves the efficiency and strength of rotating motors, and enhances thermal stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118920741A_ABST
    Figure CN118920741A_ABST
Patent Text Reader

Abstract

The invention provides a magnetic wedge and a rotating electrical machine. A magnetic wedge according to an embodiment of the present invention is a magnetic wedge for a rotating electrical machine, the magnetic wedge being provided with a plurality of flat magnetic metal particles and an inclusion phase, the flat surfaces of the plurality of flat magnetic metal particles being oriented along a contour line in the width direction in a center portion of the magnetic wedge in the width direction, and the flat surfaces of the plurality of flat magnetic metal particles being oriented along a contour line in the width direction in end portions in the width direction. The flat surface is oriented along the contour line in the thickness direction of the magnetic wedge, and the average orientation angle of the plurality of flat magnetic metal particles with respect to the contour line in the width direction in the center portion in the width direction is 20 degrees or less. The average of the orientation angles of the plurality of flat magnetic metal particles with respect to the contour line in the thickness direction at the ends in the width direction is 60 degrees or less.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Citation of Related Applications

[0002] This application is based on and claims priority from Japanese Patent Application No. 2022-148539 (filing date: September 16, 2022) and Japanese Patent Application No. 2023-136592 (filing date: August 24, 2023), and the entire contents of which are incorporated herein by reference. Technical Field

[0003] Embodiments of the present invention relate to a magnetic wedge and a rotating electric machine. Background Art

[0004] Generally, the coil winding of a rotating electric machine is accommodated in the core slot and supported and fixed by a wedge provided at the slot opening. The material of the wedge is usually a non-magnetic body, but since the magnetic resistance value in the gap between the stator core and the rotor core becomes discontinuous, the magnetic flux distribution of the core surface facing each other across the gap in the wedge pulsates, increasing the harmonic loss. In order to reduce the harmonic loss, a wedge with moderate magnetism (magnetic wedge) has been provided in the past. By using a magnetic wedge, the harmonic loss is reduced and the efficiency of the rotating electric machine is improved. Figure 1 It is a schematic diagram of the use state of the magnetic wedge and the effect of the magnetic wedge. Figure 1 In FIG. 1 , a radial gap type rotating electrical machine is shown as an example. Figure 1 , a magnetic wedge 100 , a coil 230 , a core T-iron 250 , and a core slot 260 are described.

[0005] In the case of magnetic wedges, of course, the higher the magnetic permeability of the magnetic wedge, the lower the high-order harmonic loss. Figure 1 As shown, since the magnetic wedge is arranged in a manner to bridge the adjacent core T-irons, there is a defect that the leakage flux flowing between the core T-irons through the magnetic wedge increases. In addition, the conventional magnetic wedge is prone to magnetic saturation due to its low saturation magnetization, and the efficiency improvement of the rotating electric machine is limited due to its low loss. In addition, the conventional magnetic wedge has a low magnetic permeability, which limits the efficiency improvement of the rotating electric machine and is insufficient in terms of thermal stability and mechanical properties (strength, toughness). Therefore, it is expected that the characteristics of the magnetic wedge will be improved in terms of saturation magnetization, magnetic permeability, loss, strength, toughness, etc. In particular, it is expected that the characteristics of the magnetic wedge will be improved in terms of magnetic permeability, loss, strength, etc. Summary of the invention

[0006] Problem that the invention aims to solve

[0007] An object of the present invention is to provide a magnetic wedge and a rotating electrical machine having excellent magnetic characteristics and mechanical characteristics.

[0008] Means used to solve problems

[0009] The magnetic wedge of the embodiment is a magnetic wedge of a rotating electrical machine, wherein the magnetic wedge includes a plurality of flat magnetic metal particles and an inclusion phase, wherein in a central portion in a width direction of the magnetic wedge, the flat surfaces of the plurality of flat magnetic metal particles are oriented along a contour line in the width direction, and in an end portion in the width direction, the flat surfaces are oriented along a contour line in a thickness direction of the magnetic wedge, an average of orientation angles of the plurality of flat magnetic metal particles in the central portion in the width direction relative to the contour line in the width direction is 20 degrees or less, and an average of orientation angles of the plurality of flat magnetic metal particles in the end portion in the width direction relative to the contour line in the thickness direction is 60 degrees or less.

[0010] In addition, the magnetic wedge of the embodiment is the magnetic wedge of the radial gap type rotating electric machine in which the stator is arranged to face the rotor at a predetermined interval in the radial direction, the length direction is the axial direction, the thickness direction is the radial direction, and the width direction is the rotation direction. In addition, the magnetic wedge is the magnetic wedge for the axial gap type rotating electric machine in which the stator is arranged to face the rotor at a predetermined interval in the axial direction, the length direction is the radial direction, the thickness direction is the axial direction, and the width direction is the rotation direction.

[0011] According to the above configuration, a magnetic wedge and a rotating electrical machine having excellent magnetic characteristics and mechanical characteristics can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 It is a schematic diagram of the use state of the magnetic wedge and the effect of the magnetic wedge.

[0013] Figure 2 This is a conceptual diagram showing an example of a method of determining the thickness of flat magnetic metal particles in the magnetic wedge according to the first embodiment.

[0014] Figure 3A -C is a conceptual diagram for explaining a method of obtaining the maximum length and the minimum length within the flat surface of the flat magnetic metal particle in the magnetic wedge of the first embodiment.

[0015] Figure 4 This is a conceptual diagram for explaining another example of how to determine the maximum length and the minimum length within the flat surface of a flat magnetic metal particle in the magnetic wedge of the first embodiment.

[0016] Figure 5 This is a schematic diagram showing the direction of measuring the coercive force by changing the direction every 22.5 degrees with respect to the 360-degree angle within the flat surface of the flat magnetic metal particle in the magnetic wedge of the first embodiment.

[0017] Fig. 6A-B is a schematic diagram of the flat magnetic metal particles in the magnetic wedge according to the first embodiment.

[0018] Figure 7 It is a schematic diagram of the magnetic wedge according to the first embodiment.

[0019] Figure 8 AD is a schematic diagram of a magnetic wedge according to the first embodiment.

[0020] Fig.9A -C is a schematic diagram of the magnetic wedge according to the first embodiment.

[0021] Fig.10 It is a schematic diagram of the magnetic wedge according to the first embodiment.

[0022] Fig.11 This is an example of the orientation angle of the flat magnetic metal particles in the magnetic wedge of the first embodiment.

[0023] Fig.12 This is an example of a cross-sectional photograph of the magnetic wedge according to the first embodiment.

[0024] Fig.13 This is an example of a cross-sectional photograph of the magnetic wedge according to the first embodiment.

[0025] Fig.14 It is a schematic diagram of the magnetic wedge of Example 1 of the first embodiment and the magnetic wedges of Comparative Examples 1, 2, 3, and 4.

[0026] Fig.15 It is a schematic diagram of the magnetic wedge according to the first embodiment.

[0027] Fig.16 This is a schematic diagram of the fifth step in the method for manufacturing the magnetic wedge according to the first embodiment.

[0028] Fig.17 It is a schematic diagram showing an example of a radial gap type rotating electrical machine according to the second embodiment.

[0029] Fig.18 It is a schematic diagram showing an example of an axial gap type rotating electrical machine according to the second embodiment.

[0030] Fig.19 This is a schematic diagram showing an example of a generator according to the second embodiment.

[0031] Fig. 20 This is a schematic diagram showing an example of a linear motor according to the second embodiment.

[0032] Explanation of symbols

[0033] 6: Flat surface

[0034] 9: Coating layer

[0035] 10: Flat magnetic metal particles

[0036] 20: Inclusion phase

[0037] 100: Magnetic wedge

[0038] 200: Rotating motor

[0039] 210: Rotor

[0040] 220: Stator

[0041] 222: Stator core

[0042] 230: Coil

[0043] 232: Excitation coil

[0044] 234: Armature coil

[0045] 240: Gap surface

[0046] 250: Iron core T-iron

[0047] 260: Core slot

[0048] 270: Stator

[0049] 280: Axis

[0050] 290: Movable components DETAILED DESCRIPTION

[0051] Hereinafter, the embodiments will be described with reference to the drawings. In the drawings, the same or similar parts are denoted by the same or similar reference numerals. In the present specification, unless otherwise specified, all measurements are performed at 25°C.

[0052] In this specification, the directions of "axial direction", "rotational direction" and "radial direction" are defined based on the rotor of the rotating electrical machine. That is, "axial direction" means the direction along the rotation axis of the rotor, and "rotational direction" means the direction of rotation of the rotor around the rotation axis (or its tangential direction). In addition, "radial direction" means the direction orthogonal to (perpendicularly intersecting) the rotation axis of the rotor.

[0053] (First embodiment)

[0054] The magnetic wedge of the embodiment is a magnetic wedge of a rotating electrical machine, wherein the magnetic wedge includes a plurality of flat magnetic metal particles and an inclusion phase, wherein in a central portion in a width direction of the magnetic wedge, the flat surfaces of the plurality of flat magnetic metal particles are oriented along a contour line in the width direction, and in an end portion in the width direction, the flat surfaces are oriented along a contour line in a thickness direction of the magnetic wedge, an average of orientation angles of the plurality of flat magnetic metal particles in the central portion in the width direction relative to the contour line in the width direction is 20 degrees or less, and an average of orientation angles of the plurality of flat magnetic metal particles in the end portion in the width direction relative to the contour line in the thickness direction is 60 degrees or less.

[0055] In addition, the magnetic wedge of the embodiment is a magnetic wedge of a rotating electrical machine, wherein the magnetic wedge includes a plurality of flat magnetic metal particles and an inclusion phase, in a central portion in a width direction of the magnetic wedge, the flat surfaces of the plurality of flat magnetic metal particles are oriented in the width direction and the length direction, in an end portion in the width direction of the magnetic wedge, the flat surfaces are oriented in the thickness direction and the length direction, the average of the orientation angles of the plurality of flat magnetic metal particles in the central portion in the width direction is 20 degrees or less, and the average of the orientation angles of the plurality of flat magnetic metal particles in the end portion in the width direction is 30 degrees or more and 90 degrees or less.

[0056] In addition, the magnetic wedge of the embodiment is the magnetic wedge of the radial gap type rotating electric machine in which the stator is arranged opposite to the rotor in the radial direction with a predetermined interval, the length direction is the axial direction, the thickness direction is the radial direction, and the width direction is the rotation direction. In addition, the magnetic wedge of the embodiment is the magnetic wedge used for the axial gap type rotating electric machine in which the stator is arranged opposite to the rotor in the axial direction with a predetermined interval, the length direction is the radial direction, the thickness direction is the axial direction, and the width direction is the rotation direction. The average thickness of the plurality of flat magnetic metal particles is 10 nm or more and 100 μm or less, and the plurality of flat magnetic metal particles have a flat surface and a magnetic metal phase containing at least one first element selected from Fe, Co and Ni, the average value of the ratio of the average length in the flat surface to the thickness is 5 or more and 10000 or less, and the inclusion phase exists between the plurality of flat magnetic metal particles and contains at least one second element selected from oxygen (O), carbon (C), nitrogen (N) and fluorine (F).

[0057] The flat magnetic metal particles are flat particles (flaky particles, flattened particles) formed into a flaky (flaky, flattened) shape (flaky shape, flattened shape).

[0058] The so-called thickness refers to the average thickness of a flat magnetic metal particle. As a method for calculating the thickness, the method is not limited as long as it is a method that can calculate the average thickness of a flat magnetic metal particle. For example, the following method can also be used, that is, using a transmission electron microscope (TEM: Transmission Electron Microscopy) or a scanning electron microscope (SEM: Scanning Electron Microscopy) or an optical microscope, etc., to observe the cross-section of the flat magnetic metal particle perpendicular to the flat surface, in the cross-section of the observed flat magnetic metal particle, select any 10 or more places in the direction within the flat surface, measure the thickness of each selected place, and use the average value. In addition, the following method can also be used, that is, in the cross-section of the observed flat magnetic metal particle, in the direction within the flat surface, select 10 or more places at equal intervals from the end to the other end (in this case, the end and the other end are special places, so it is preferably not selected), measure the thickness of each selected place, and use the average value.

[0059] Figure 2 This is a conceptual diagram showing an example of a method of determining the thickness of flat magnetic metal particles in the magnetic wedge according to the first embodiment. Figure 2 The method for calculating the thickness at this time is specifically shown in FIG. 10 locations (excluding the end) are selected at equal intervals from one end toward the other end in the direction within the flat surface, and the thickness of each location is set to t 1 ,t 2 ,…,t 10 When the thickness of the flat magnetic metal particle is (t 1 +t 2 +…+t 10 ) / 10. Furthermore, in order to obtain average information, it is preferred to measure as many places as possible during the measurement. Furthermore, when the contour line of the cross section has a strongly concave-convex or rough surface contour line, and it is difficult to obtain the average thickness in its original state, it is preferred to smooth the contour line according to the average straight line or curve as appropriate according to the situation, and then perform the above method.

[0060] In addition, the so-called average thickness refers to the average value of the thickness of multiple flat magnetic metal particles, which is different from the simple "thickness" mentioned above. When calculating the average thickness, it is preferred to use the value averaged for more than 20 flat magnetic metal particles. In addition, in order to obtain average information, it is preferred to obtain it with as many flat magnetic metal particles as possible. In addition, when it is not possible to observe more than 20 flat magnetic metal particles, it is preferred to observe as many flat magnetic metal particles as possible and use the value averaged from them. The average thickness of the flat magnetic metal particles is preferably greater than 10nm and less than 100μm, more preferably greater than 10nm and less than 1μm, and further preferably greater than 10nm and less than 100nm. In addition, it is preferred that the flat magnetic metal particles contain particles having a thickness of greater than 10nm and less than 100μm, more preferably greater than 10nm and less than 1μm, and further preferably greater than 10nm and less than 100nm. As a result, when a magnetic field is applied in a direction parallel to the flat surface, the eddy current loss can be sufficiently reduced, which is preferred. In addition, the thinner the thickness is, the magnetic moment is confined in a direction parallel to the flat surface, and magnetization is easy by rotational magnetization. When magnetization is carried out by rotational magnetization, magnetization is easy to be reversibly carried out, so the coercive force is reduced, thereby reducing the hysteresis loss, which is preferable.

[0061] The average length of the flat magnetic metal particles can be defined by (a+b) / 2 using the maximum length a and the minimum length b within the flat surface. The maximum length a and the minimum length b can be calculated as follows. For example, the rectangle with the smallest area can be considered among the rectangles circumscribed with the flat surface. The length of the long side of the rectangle is taken as the maximum length a, and the length of the short side is taken as the minimum length b. Figure 3A -C is a conceptual diagram for explaining a method of obtaining the maximum length and the minimum length within the flat surface of the flat magnetic metal particle in the magnetic wedge of the first embodiment. Figure 3A-C is a schematic diagram showing the maximum length a and the minimum length b obtained by the above method, taking several flat magnetic metal particles as examples. The maximum length a and the minimum length b, like the average thickness, can be obtained by observing the flat magnetic metal particles with a TEM, SEM, or an optical microscope. In addition, the maximum length a and the minimum length b can also be obtained by performing image analysis of microscope photos on a computer. In any method, it is preferred to obtain the results with more than 20 flat magnetic metal particles as the object. In addition, in order to obtain average information, it is preferred to obtain the results with as many flat magnetic metal particles as possible as the object. In addition, in the case where more than 20 flat magnetic metal particles cannot be observed, it is preferred to observe as many flat magnetic metal particles as possible and adopt the value obtained by averaging them. In addition, it is preferred to obtain the results with the average value as much as possible at this time, so it is preferred to observe or image analyze the state where the flat magnetic metal particles are uniformly dispersed (the state where a plurality of flat magnetic metal particles with different maximum lengths and minimum lengths are dispersed as randomly as possible). For example, it is preferred that a plurality of flat magnetic metal particles are affixed to a tape while being sufficiently stirred and mixed, or a plurality of flat magnetic metal particles are dropped from above and affixed to a tape by dropping, thereby performing observation or image analysis.

[0062] However, when the maximum length a and the minimum length b are calculated using the above method from flat magnetic metal particles, the method may not grasp the essence. Figure 4 This is a conceptual diagram for explaining another example of how to find the maximum length and the minimum length of a flat magnetic metal particle within a flat surface in the magnetic wedge of the first embodiment. Figure 4 In this case, the flat magnetic metal particles are in a state of being elongated and curved. However, in this case, the maximum length and the minimum length of the flat magnetic metal particles are essentially Figure 4 The lengths of a and b shown. Thus, the method for obtaining the maximum lengths a and b is not completely unambiguous. There is basically no problem in adopting the method of "considering the rectangle with the smallest area among the rectangles circumscribed to the flat surface, and taking the length of the long side of the rectangle as the maximum length a, and the length of the short side as the minimum length b". However, when this method does not capture the essence according to the particle shape, the maximum length a and the minimum length b that capture the essence are obtained as a matter of course. The thickness t can be defined as the length in the direction perpendicular to the flat surface. The ratio A of the average length in the flat surface to the thickness can be defined as A = ((a+b) / 2) / t, using the maximum length a, the minimum length b, and the thickness t.

[0063] The average value of the ratio of the average length in the flat surface of the flat magnetic metal particles to the thickness is preferably 5 or more and 10000 or less. This is because the magnetic permeability can be increased and the ferromagnetic resonance frequency can be increased, thereby reducing the ferromagnetic resonance loss.

[0064] The average value is used for the ratio of the average length in the flat surface to the thickness. It is preferred to use the value obtained by averaging more than 20 flat magnetic metal particles. In addition, in order to obtain average information, it is preferred to obtain it with as many flat magnetic metal particles as possible as the object. In addition, when it is not possible to observe more than 20 flat magnetic metal particles, it is preferred to observe as many flat magnetic metal particles as possible and use the value obtained by averaging them. Furthermore, for example, when there are particles Pa, particles Pb, and particles Pc, their thicknesses are called Ta, Tb, and Tc, and the average length in the flat surface is called La, Lb, and Lc, the average thickness can be calculated as (Ta+Tb+Tc) / 3, and the average value of the ratio of the average length in the flat surface to the thickness can be calculated as (La / Ta+Lb / Tb+Lc / Tc) / 3.

[0065] It is preferred that the flat magnetic metal particles have a coercive force difference based on direction within the flat surface. The larger the ratio of the coercive force difference based on direction, the more preferred it is, preferably 1% or more, more preferably the ratio of the coercive force difference is 10% or more, further preferably the ratio of the coercive force difference is 50% or more, and further preferably the ratio of the coercive force difference is 100% or more. The ratio of the coercive force difference mentioned here can be defined as the maximum coercive force Hc (max) and the minimum coercive force Hc (min) within the flat surface, as (Hc (max) - Hc (min)) / Hc (min) × 100 (%). Furthermore, the coercive force can be evaluated using a vibrating sample magnetometer (VSM: Vibrating Sample Magnetometer) or the like. When the coercive force is low, a coercive force of less than 0.1 Oe can be measured by using a low magnetic field unit. The direction within the flat surface is changed relative to the direction of the measuring magnetic field for measurement.

[0066] Furthermore, the term "having a coercive force difference" means that when the coercive force is measured by applying a magnetic field in the 360-degree direction within the flat surface, there is a direction in which the coercive force is the largest and a direction in which the coercive force is the smallest. For example, when the coercive force is measured by changing the direction every 22.5 degrees relative to the 360-degree angle within the flat surface, when there is an angle indicating a coercive force difference, that is, an angle with a larger coercive force and an angle with a smaller coercive force, it is considered that "there is a coercive force difference". Figure 5 This is a schematic diagram showing the direction of the coercive force when the direction is changed every 22.5 degrees relative to the 360-degree angle within the flat surface of the flat magnetic metal particle in the magnetic wedge of the first embodiment. Figure 5In the figure, the flat surface of the flat magnetic metal particle is viewed from above. By having a coercive force difference in the flat surface, the minimum coercive force value is reduced compared to the isotropic material with almost no coercive force difference, which is preferred. In the material with magnetic anisotropy in the flat surface, the coercive force has a difference depending on the direction in the flat surface, and the minimum coercive force value is reduced compared to the magnetic isotropic material. This can reduce hysteresis loss and improve magnetic permeability, which is preferred. Figure 5 In FIG. 1 , a flat magnetic metal particle 10 and a flat surface 6 are shown.

[0067] In addition, the flat magnetic metal particles have a magnetic metal phase, which contains at least one first element selected from Fe, Co and Ni. Furthermore, the flat magnetic metal particles contain Fe and Co, and the amount of Co relative to the total amount of Fe and Co is preferably more than 10 atomic % and less than 60 atomic %, and more preferably contains more than 10 atomic % and less than 40 atomic %. This makes it easy to impart moderately large magnetic anisotropy and improve the above-mentioned magnetic properties, so it is preferred. In addition, the Fe-Co system is easy to achieve high saturation magnetization, so it is preferred. In addition, by having the composition range of Fe and Co within the above-mentioned range, a higher saturation magnetization can be achieved, which is preferred. In addition, when the composition of the flat magnetic metal particles and the attached metal is the same, it is easy to improve thermal stability and mechanical properties such as strength and hardness, which is preferred.

[0068] Elements can be easily analyzed by EDX (Energy Dispersive X-ray spectroscopy) and ICP (Inductively Coupled Plasma) emission spectrometry.

[0069] The flat magnetic metal particles preferably contain at least one non-magnetic metal selected from Mg, Al, Si, Ca, Zr, Ti, Hf, Zn, Mn, Ba, Sr, Cr, Mo, Ag, Ga, Sc, V, Y, Nb, Pb, Cu, In, Sn, and rare earth elements. Thus, the thermal stability and oxidation resistance of the flat magnetic metal particles can be improved. Among them, Al and Si are particularly preferred because they are easy to solid-dissolve with Fe, Co, and Ni, which are the main components of the flat magnetic metal particles, and contribute to improving thermal stability and oxidation resistance.

[0070] Furthermore, in order to induce magnetic anisotropy, there is also a method of making the crystallinity of flat magnetic metal particles amorphous as much as possible, and inducing magnetic anisotropy in one direction in the plane through magnetic field and strain. In this case, it is best to form a composition that easily makes the flat magnetic metal particles amorphous as much as possible. Based on this viewpoint, the magnetic metal contained in the flat magnetic metal particles preferably contains at least one additive element selected from B (boron), Si (silicon), Al (aluminum), C (carbon), Ti (titanium), Zr (zirconium), Hf (hafnium), Nb (niobium), Ta (tantalum), Mo (molybdenum), Cr (chromium), Cu (copper), W (tungsten), P (phosphorus), N (nitrogen), Ga (gallium), and Y (yttrium). An additive element with a large difference in atomic radius with at least one first element selected from Fe, Co, and Ni is preferred. In addition, an additive element that increases the negative value of the mixing enthalpy of at least one first element selected from Fe, Co, and Ni and the additive element is preferred. In addition, it is preferred to be a multi-element system containing more than three elements in total by containing the first element and the additive element. In addition, semi-metallic additive elements such as B and Si are easy to be amorphized due to their slow crystallization rate, so they are advantageously mixed in the system. From the above viewpoints, B, Si, P, Ti, Zr, Hf, Nb, Y, Cu, etc. are preferred, and among them, it is more preferred that the additive element contains any one of B, Si, Zr, Hf, and Y. As an example, it is preferred that the first element as the magnetic metal phase contains Fe and Co, and the additive element contains Si and B. In addition, the total amount of the above additive elements is preferably 0.001at% or more and 80at% or less, more preferably 5at% or more and 80at% or less, and further preferably 10at% or more and 40at% or less relative to the total amount of the above first element and the above additive elements. Furthermore, the greater the total amount of the above additive elements, the easier it is to be amorphized and impart magnetic anisotropy, so it is preferred (that is, it is preferred from the viewpoint of low loss and high magnetic permeability), but on the other hand, the saturation magnetization decreases due to the decrease in the proportion of the magnetic metal phase, which is not preferred in this respect. From the above, it is important to comprehensively consider high saturation magnetization, low loss, high magnetic permeability, etc., and select the composition and the amount of added elements.

[0071] The flat magnetic metal particles preferably have at least a portion of their surfaces covered with a coating layer having a thickness of 0.1 nm to 1 μm inclusive and containing at least one second element selected from oxygen (O), carbon (C), nitrogen (N) and fluorine (F).

[0072] Fig. 6A - B is a schematic diagram of the flat magnetic metal particles in the magnetic wedge according to the first embodiment. The coating layer 9 and the flat magnetic metal particles 10 are shown.

[0073] The coating layer more preferably contains at least one non-magnetic metal selected from Mg, Al, Si, Ca, Zr, Ti, Hf, Zn, Mn, Ba, Sr, Cr, Mo, Ag, Ga, Sc, V, Y, Nb, Pb, Cu, In, Sn, and rare earth elements, and contains at least one second element selected from oxygen (O), carbon (C), nitrogen (N), and fluorine (F). As the non-magnetic metal, Al and Si are particularly preferred from the viewpoint of thermal stability. When the flat magnetic metal particles contain at least one non-magnetic metal selected from Mg, Al, Si, Ca, Zr, Ti, Hf, Zn, Mn, Ba, Sr, Cr, Mo, Ag, Ga, Sc, V, Y, Nb, Pb, Cu, In, Sn, and rare earth elements, it is more preferred that the coating layer contains at least one non-magnetic metal that is the same as one of the constituent components of the flat magnetic metal particles, i.e., the non-magnetic metal. Among oxygen (O), carbon (C), nitrogen (N) and fluorine (F), oxygen (O) is preferably contained, preferably an oxide or a composite oxide. The above is based on the viewpoints of the ease of formation, oxidation resistance and thermal stability of the coating. By adopting the above materials, the close adhesion between the flat magnetic metal particles and the coating can be improved, and the thermal stability and oxidation resistance of the magnetic wedge described later can be improved. The coating can not only improve the thermal stability and oxidation resistance of the flat magnetic metal particles, but also improve the electrical resistance of the flat magnetic metal particles. By increasing the resistance, eddy current losses can be suppressed and the frequency characteristics of the magnetic permeability can be improved. Therefore, it is preferred that the coating has a high electrical resistance, for example, it is preferred to have a resistance value of 1 mΩ·cm or more.

[0074] In addition, the presence of a coating layer is also preferred from a magnetic point of view. Flat magnetic metal particles can be regarded as quasi-thin films because their thickness dimensions are relatively small relative to the dimensions of the flat surface. At this time, a coating layer is formed on the surface of the flat magnetic metal particles and integrated, which can be regarded as a quasi-stacked thin film structure, which can stabilize the magnetic domain structure in energy. In this way, the coercive force can be reduced (thereby reducing the hysteresis loss), which is preferred. At this time, the magnetic permeability is also increased, which is preferred. Based on this viewpoint, it is more preferred that the coating layer is non-magnetic (the magnetic domain structure becomes easier to stabilize).

[0075] Regarding the thickness of the coating layer, the thicker the better from the viewpoints of thermal stability, oxidation resistance and electrical resistance. However, if the coating layer becomes too thick, the magnetic permeability will also decrease due to the decrease in saturation magnetization, which is not preferred. In addition, from the magnetic point of view, if the thickness becomes too thick, the "effect of low coercivity, low loss and high magnetic permeability through stabilization of the magnetic domain structure" will be reduced. Considering the above, the thickness of the coating layer is preferably greater than 0.1nm and less than 1μm, and more preferably greater than 0.1nm and less than 100nm.

[0076] Figure 7FIG. 1 is a schematic diagram of a magnetic wedge according to the present embodiment. Figure 7 As shown, not only a simple rectangular parallelepiped shape (rectangular cross section), but also various shapes such as trapezoidal, hexagonal and convex cross sections can be considered. Here, no matter what the shape is, three mutually orthogonal or perpendicular axes are defined as width direction, thickness direction and length direction. The so-called length direction of the magnetic wedge is the direction in which the length of the magnetic wedge is long. The so-called thickness direction and width direction of the magnetic wedge are directions orthogonal to the length direction of the magnetic wedge. In addition, the thickness direction and width direction of the magnetic wedge can be distinguished from the orientation state of the flat magnetic metal particles described later.

[0077] The closer the magnetic wedge is to the gap surface between the rotor and the stator, the more effective it is (the effect of improving the efficiency of the rotating electrical machine). Therefore, from this point of view, trapezoidal, convex, and hexagonal shapes are preferred over rectangular shapes. In addition, from the point of view of "a shape that easily introduces magnetic flux to the magnetic wedge side (thereby easily improving the efficiency of the rotating electrical machine)", trapezoidal and convex shapes are preferred over hexagonal shapes. On the other hand, from the point of view of ease of manufacturing and high reliability as a material (mechanical properties, thermal properties), the rectangular type is most preferred, followed by the trapezoidal and hexagonal types. This means that the trapezoidal type is easy to be arranged close to the gap surface between the rotor and the stator, and it is easy to introduce magnetic flux to the magnetic wedge side according to the shape of the trapezoidal type. It is also easy to manufacture and easy to improve the reliability as a material (mechanical properties, thermal properties), so it is very preferred.

[0078] Figure 8 AD is a schematic diagram of a magnetic wedge according to the present embodiment. Figure 8 A shows the cross section is rectangular, Figure 8 B shows the case where the cross section is trapezoidal. Figure 8 C indicates the case where the cross section is hexagonal. Figure 8D shows an example of the orientation of a plurality of flat magnetic metal particles when the cross section is convex. In the center portion in the width direction, the flat surfaces of the plurality of flat magnetic metal particles are oriented along the contour line in the width direction. At this time, the average of the orientation angles of the flat magnetic metal particles in the center portion in the rotation direction relative to the rotation direction (width direction) is preferably 20 degrees or less, more preferably 1 degree or more and 20 degrees or less, and further preferably 1 degree or more and 10 degrees or less. In addition, the flat surfaces are oriented along the contour line in the thickness direction at the end portion in the width direction. At this time, the average of the orientation angles of the plurality of flat magnetic metal particles in the end portion in the width direction relative to the contour line in the thickness direction is preferably 60 degrees or less, more preferably 1 degree or more and 60 degrees or less, further preferably 1 degree or more and 45 degrees or less, further preferably 1 degree or more and 30 degrees or less, further preferably 1 degree or more and 20 degrees or less, and further preferably 1 degree or more and 10 degrees or less. In addition, the so-called center portion refers to the region including the range of the "average length of the flat magnetic metal particles" of the center line of the cross section having the width direction and the thickness direction in the center line in the width direction of the magnetic wedge. In addition, the end portion refers to an area within the range of "the average length of the flat magnetic metal particles" from one end in the width direction of the magnetic wedge, that is, from the contour line in the thickness direction. Furthermore, the definition of the center portion and the end portion as more preferred is as follows. The center portion refers to an area within the range of "half the length of the average length of the flat magnetic metal particles" including the center line of the cross section having the width direction and the thickness direction in the center line in the width direction of the magnetic wedge. In addition, the end portion refers to an area within the range of "half the length of the average length of the flat magnetic metal particles" from one end in the width direction of the magnetic wedge, that is, from the contour line in the thickness direction.

[0079] Fig.9A -C is a schematic diagram of a magnetic wedge according to this embodiment. Fig.9A When the cross section is trapezoidal, Fig. 9B When the cross section is hexagonal, Fig. 9C An example of the orientation of a plurality of flat magnetic metal particles when the cross section is convex is shown. Fig.9A -C shows the Figure 8 AD are different orientation examples, but all are preferred. Fig.9A -C, the orientation in the center of the width direction is Figure 8 AD is the same, but the orientation in the end portion in the width direction is Figure 8 Different. Fig.9A In the embodiment shown in -C, at the end in the width direction, the orientation angle of the flat magnetic metal particles relative to the width direction is preferably 30 degrees or more and 90 degrees or less, more preferably 45 degrees or more and 90 degrees or less, and further preferably 60 degrees or more and 90 degrees or less. Figure 8 AD and Fig.9A -C orientation, the magnetic properties such as high magnetic permeability and low loss are improved, the efficiency of the rotating electric machine is greatly improved, and excellent mechanical properties such as improved magnetic wedge strength can be achieved. In addition, by orienting the flat surface of the flat magnetic metal particles in the center along the outline of the width direction and orienting the flat surface along the outline of the thickness direction at the end, the magnetic properties and mechanical properties are averaged three-dimensionally, and excellent magnetic properties and mechanical properties can be achieved in all directions of the x direction, y direction, and z direction.

[0080] Fig.10 Schematic diagram of a magnetic wedge according to this embodiment. Fig.10 Shown in Figure 8 A's magnetic wedge is a schematic diagram of an example configuration, but it is always an example and can also be Figure 8 B-D, Fig.9A -C-like form. Fig.10The magnetic wedge shown is a magnetic wedge used in a radial gap type rotating electric machine in which a stator is arranged opposite to a rotor in a manner with a predetermined interval in the radial direction. In the case of a magnetic wedge of a radial gap type rotating electric machine, the length direction of the magnetic wedge is the axial direction of the rotating electric machine, the width direction of the magnetic wedge is the rotating direction of the rotating electric machine, and the thickness direction of the magnetic wedge is the radial direction of the rotating electric machine. In the center portion of the magnetic wedge in the rotating direction, the flat surface of the flat magnetic metal particles is oriented in the rotating direction and the axial direction. At this time, the orientation angle of the flat magnetic metal particles in the center portion in the rotating direction with respect to the rotating direction (width direction) is preferably 20 degrees or less, more preferably 1 degree or more and 20 degrees or less, and further preferably 1 degree or more and 10 degrees or less. In addition, at the end portion in the rotating direction, the flat surface is oriented in the radial direction and the axial direction. At this time, the orientation angle of the flat magnetic metal particles in the end portion in the rotating direction with respect to the rotating direction (width direction) is preferably 30 degrees or more and 90 degrees or less, more preferably 45 degrees or more and 90 degrees or less, and further preferably 60 degrees or more and 90 degrees or less. Furthermore, the so-called center portion refers to the area within the range of "the average length of flat magnetic metal particles" including the center line of the cross section having the width direction and the thickness direction or the cross section perpendicular to the length direction in the center line of the magnetic wedge in the rotation direction. In addition, the so-called end portion refers to the area within the range of "the average length of flat magnetic metal particles" from one end in the rotation direction of the magnetic wedge. The area between the center portion and the end portion is the "middle portion". Furthermore, the definition of the center portion and the end portion as a more preferred embodiment is as follows. The so-called center portion refers to the area within the range of "half the length of the average length of flat magnetic metal particles" including the center line of the cross section having the width direction and the thickness direction in the center line of the magnetic wedge in the width direction. In addition, the so-called end portion refers to the area within the range of "half the length of the average length of flat magnetic metal particles" from one end in the width direction of the magnetic wedge, that is, from the contour line in the thickness direction.

[0081] The orientation angle of the flat magnetic metal particles can be calculated as follows. First, when the target magnetic wedge is placed in a rotating motor, the target magnetic wedge is taken out from the interior of the rotating motor. Here, the rotation direction of the rotating motor is the width direction of the target magnetic wedge. Next, the external dimensions of the target magnetic wedge are measured. Thus, the length direction of the magnetic wedge (the direction in which the length of the magnetic wedge is the longest) is determined. For example, in the case where the shape of the target magnetic wedge is a roughly rectangular parallelepiped shape, the direction along the longest side of the roughly rectangular parallelepiped shape is determined as the length direction of the target magnetic wedge. Next, a cross section perpendicular to the length direction of the target magnetic wedge is determined. With respect to this cross section, the end face of the target magnetic wedge is avoided. With respect to this cross section, the target magnetic wedge is cut perpendicularly to the length direction of the target magnetic wedge in a manner having a length of more than 1 / 10 of the length of the target magnetic wedge in the length direction.

[0082] The cross section formed by cutting is a cross section including the width direction and the thickness direction or a cross section perpendicular to the length direction. Next, the center line of the cross section formed by cutting is calculated. As the center line of the cross section formed by cutting, for example, a straight line including the geometric center of the cross section can be used. Next, in the target magnetic wedge, the cross section formed by cutting is observed using an optical microscope, SEM, or TEM. Next, for each flat magnetic metal particle observed in the cross section formed by cutting, the rectangle with the smallest area among the rectangles circumscribed to each flat magnetic metal particle is considered, and the angle formed by the long side direction of the rectangle with respect to the rotation direction of the rotating motor in which the target magnetic wedge is provided is defined as the orientation angle of the flat magnetic metal particle. Furthermore, the orientation angle does not distinguish between positive and negative in the angle formed by the rotation direction and the flat surface of the flat magnetic metal particle. Fig.11 In the figure, two or three examples of the orientation angles of flat magnetic metal particles obtained by this method are shown. Even if there is not even a single complete flat magnetic metal particle in the area of ​​the observation range (even if a part protrudes from the area and enters the middle part), the orientation angle of the particle is evaluated. However, the flat magnetic metal particles sometimes contain particles that are difficult to evaluate because the particle outline is unclear during observation. In other words, sometimes the outline of a specific particle cannot be clearly determined by image analysis, and in such a case it is removed from the observation object. In this way, the orientation angles of all the flat magnetic metal particles contained in the area of ​​the observation range are calculated, and the average value is used as the orientation angle of the flat magnetic metal particles in the center and the flat magnetic metal particles contained in the ends. In addition, the observed cross section is evaluated using multiple cross sections, for example, more than 3 cross sections, and the average value is used. The center and the ends are shown in Fig.10 middle. Fig.10 FIG. 1 shows a flat magnetic metal particle 10, an inclusion phase 20, and a magnetic wedge 100. In addition, regarding the orientation angle, Fig.11 0 degrees, 45 degrees, and 90 degrees are shown as examples.

[0083] Furthermore, when the target magnetic wedge is not set in the rotating electrical machine, the center portion with the smallest average orientation angle is found in the cross section perpendicular to the length direction, and the direction perpendicular to the center line of the center portion is taken as the width direction (rotation direction). Specifically, the width direction (rotation direction) is temporarily determined once in the plane perpendicular to the length direction. Next, the center portion is obtained relative to the temporarily determined width direction (rotation direction), and the orientation angle of the flat magnetic metal particle in the center portion is obtained. At this time, regarding the orientation angle, the rectangle with the smallest area among the rectangles circumscribed with the magnetic metal particle is considered, and it is defined as the angle formed by the long side direction of the rectangle and the "temporarily determined width direction (rotation direction)". Next, in the cross section perpendicular to the length direction, the width direction (rotation direction) is changed, and the orientation angle of the center portion is obtained by the same procedure. At this time, it is assumed that it is set in the rotating electrical machine and changed in a way to form an actual configuration. Then, the "temporarily determined width direction (rotation direction)" when the orientation angle of the center portion is the smallest is determined as the "formal width direction (rotation direction)".

[0084] The orientation angle is represented by the average value of the orientation angles of a plurality of flat magnetic metal particles contained in each region of the center portion and the end portions. Fig.12 An example of a cross-sectional photograph of a magnetic wedge according to this embodiment is shown in FIG. Fig.12 In the magnetic wedge, it is found that the cross section is trapezoidal, the orientation angle of the center is about 4 degrees, and the orientation angle of the end is about 37 degrees relative to the contour line in the thickness direction. In addition, Fig.13 An example of a cross-sectional photograph of a magnetic wedge according to this embodiment is shown in FIG. Fig.13 The cross section of the magnetic wedge is rectangular, the orientation angle in the center is about 5 degrees, and the orientation angle in the end is about 33 degrees. The flat magnetic metal particles have such orientation, which improves the magnetic properties such as high magnetic permeability and low loss, greatly improves the efficiency of the rotating electrical machine, and can also achieve excellent mechanical properties such as increased strength of the magnetic wedge.

[0085] Furthermore, the orientation of the flat magnetic metal particles can also be discussed in terms of the ratio of the number. In this case, the number of oriented flat magnetic metal particles is preferably 10% or more, more preferably 50% or more, and even more preferably 80% or more relative to the total number of flat magnetic metal particles contained in the central portion and the end portions. By having such an orientation of the flat magnetic metal particles, magnetic properties such as high magnetic permeability and low loss are improved, the efficiency of the rotating electrical machine is greatly improved, and excellent mechanical properties such as increased strength of the magnetic wedge can be achieved.

[0086] Fig.14Schematic diagrams comparing the magnetic wedge of the present embodiment (Example 1) and the conventional magnetic wedges (Comparative Examples 1 to 4) are shown in FIG. Comparative Example 1 is a magnetic wedge in which spherical magnetic metal particles are dispersed, Comparative Example 2 is a magnetic wedge in which flat magnetic metal particles are stacked and oriented in the y direction, Comparative Example 3 is a magnetic wedge in which flat magnetic metal particles are stacked and oriented in the z direction, and Comparative Example 4 is a magnetic wedge in which flat magnetic metal particles are stacked and oriented in the x direction. A detailed comparison will be described later, but in Example 1, by stacking and oriented the flat magnetic metal particles in the z direction at the center and stacking and oriented the flat magnetic metal particles in the x direction at the ends, the magnetic properties and mechanical properties are averaged three-dimensionally, and excellent properties can be achieved in all directions of the x direction, the y direction, and the z direction. This is a property that cannot be achieved in any of Comparative Examples 1 to 4. Furthermore, in Comparative Examples 2 to 4, since magnetic particles are stacked in only one direction, the magnetic properties and mechanical properties are characterized in a manner that is excellent in a specific direction, and therefore, it is not possible to have excellent properties in all directions of the x-direction, y-direction, and z-direction as in Example 1. Furthermore, Fig.17 Schematic diagram of an example of a radial gap type rotating electrical machine is shown in FIG.

[0087] In this specification, the term "flat magnetic metal particles are stacked and oriented in the y direction" means that a plurality of flat magnetic metal particles are stacked in the y direction and the flat surfaces of the flat magnetic metal particles are oriented in the x and z directions. The term "flat magnetic metal particles are stacked and oriented in the x direction" means that a plurality of flat magnetic metal particles are stacked in the x direction and the flat surfaces of the flat magnetic metal particles are oriented in the y and z directions. The term "flat magnetic metal particles are stacked and oriented in the z direction" means that a plurality of flat magnetic metal particles are stacked in the z direction and the flat surfaces of each flat magnetic metal particle are oriented in the x and y directions.

[0088] Fig.15 This is a schematic diagram of a magnetic wedge in the case of an axial gap type rotating electrical machine. Fig.15The magnetic wedge shown is a magnetic wedge used in an axial gap type rotating electric machine in which a stator is arranged opposite to a rotor in a manner with a predetermined interval in the axial direction. In the case of a magnetic wedge used in an axial gap type rotating electric machine, the length direction of the magnetic wedge is the radial direction of the rotating electric machine, the width direction of the magnetic wedge is the rotating direction of the rotating electric machine, and the thickness direction of the magnetic wedge is the axial direction of the rotating electric machine. In the center portion in the rotating direction, the flat surface is oriented in the rotating direction and the radial direction, and in the end portion in the rotating direction, the flat surface is oriented in the axial direction and the radial direction. At this time, the orientation angle of the flat magnetic metal particles in the center portion in the rotating direction relative to the rotating direction (width direction) is preferably 20 degrees or less, more preferably 1 degree or more and 20 degrees or less, and further preferably 1 degree or more and 10 degrees or less. In addition, in the end portion in the rotating direction, the flat surface is oriented in the axial direction and the radial direction. At this time, the orientation angle of the flat magnetic metal particles in the end portion in the rotating direction relative to the rotating direction (width direction) is preferably 30 degrees or more and 90 degrees or less, more preferably 45 degrees or more and 90 degrees or less, and further preferably 60 degrees or more and 90 degrees or less. Since the excellent magnetic properties, excellent mechanical properties, and improved efficiency of the rotating machine obtained are the same as those of the radial gap type rotating machine described above, they are omitted here. Fig.18 Schematic diagram of an example of an axial gap type rotating electrical machine is shown in FIG.

[0089] A method for manufacturing a magnetic wedge according to the present embodiment will be described. Note that the manufacturing method is not particularly limited, and will be described as an example.

[0090] The first step is a step of manufacturing a magnetic metal belt containing at least one first element selected from Fe, Co, and Ni. This step is a step of manufacturing a belt or a film using a film forming device such as a roller quenching device and a sputtering device. At this time, in the film forming method using the film forming device, it is preferred to form a film with uniaxial anisotropy in the film surface by film forming in a magnetic field and rotary film forming. Furthermore, when using the film forming device, the thickness can be reduced, and a film with a refined structure can be easily formed, and rotational magnetization can be easily generated. Therefore, it is best to use the film forming method when manufacturing a rotational magnetization type film. The roller quenching device is suitable for mass synthesis, so it is preferred when synthesizing a large amount of materials. When using the roller quenching device, a single roller quenching device is simple and preferred.

[0091] The second step is a step of heat treating the magnetic metal strip at a temperature of 50°C to 800°C. In this step, the strip may be cut into appropriate sizes for easy placement in an electric furnace for heat treatment. For example, a stirring device or the like may be used to cut the strip into appropriate sizes. By performing this step, it is easy to improve the crushing property in the following third step, i.e., the crushing step, which is preferred. Furthermore, the heat treatment atmosphere is preferably a vacuum atmosphere with a low oxygen concentration, an inert atmosphere, or a reducing atmosphere, and more preferably H 2 (hydrogen), CO (carbon monoxide), CH 4 (methane) and other reducing atmospheres. The reason for this is that even if the magnetic metal strip is oxidized, the oxidized metal can be reduced and returned to metal by performing a heat treatment in a reducing atmosphere. Thus, by reducing the magnetic metal strip whose saturation magnetization has been reduced due to oxidation, the saturation magnetization can be restored. Furthermore, if the crystallization of the magnetic metal strip progresses significantly by heat treatment, an increase in coercive force and a decrease in magnetic permeability occur, so conditions are preferably selected to suppress excessive crystallization. In addition, it is more preferred to perform the heat treatment in a magnetic field. The larger the applied magnetic field, the better, but it is preferably applied with 1 kOe or more, and more preferably with 10 kOe or more. Thus, magnetic anisotropy can be exhibited within the plane of the magnetic metal strip, and excellent magnetic properties can be achieved, so it is preferred.

[0092] The third step is a step of manufacturing flat magnetic metal particles by crushing the heat-treated magnetic metal belt. Furthermore, in this step, before the crushing, a stirring device or the like can also be used to cut the magnetic metal belt or film into appropriate sizes. In this step, the crushing is performed, for example, by a crushing device such as a bead mill and a planetary crusher. Furthermore, the type of the crushing device is not particularly selected. For example, planetary mills, bead mills, rotary ball mills, vibrating ball mills, stirring ball mills (mills), jet mills, centrifuges, or combined mills and centrifugal separation methods can be listed. When crushing, it is easy to crush while cooling at a temperature below 0°C, which is preferred. In particular, it is preferred to cool at a temperature such as liquid nitrogen temperature (77K) and dry ice temperature (194K), and it is particularly preferred to cool to liquid nitrogen temperature. As a result, the magnetic metal belt is prone to low-temperature brittleness and is easy to crush. In other words, it is preferred that the magnetic metal belt can be crushed efficiently without applying excessive stress and strain to the magnetic metal belt. However, even without cooling, sufficient pulverization can be achieved in many cases, and in such cases, cooling may not be performed.

[0093] Furthermore, in the third step, not only simple crushing, but also the thickness of the flat magnetic metal particles can be reduced by combined rolling. Furthermore, when the specified thickness is reached in the second step, the treatment for rolling can be omitted. Here, rolling can be carried out simultaneously, or it can be carried out after crushing, or it can be crushed after rolling. At this time, it is preferred to use a device that can add a strong gravitational acceleration, such as a planetary mill, a bead mill, a rotary ball mill, a vibrating ball mill, a stirring ball mill (mill), a jet mill, a centrifuge, or a method of combining a mill and a centrifugal separation. For example, when a high-power planetary milling device is used, it is possible to simply add a gravitational acceleration of tens of G, so it is preferred. When a high-power planetary milling device is used, it is more preferred to use an inclined planetary milling device in which the direction of the rotational gravitational acceleration and the direction of the revolution gravitational acceleration are not on the same straight line, but in a direction with an angle. In a conventional planetary milling device, the direction of the gravity acceleration due to rotation and the direction of the gravity acceleration due to revolution are on the same straight line, but in an inclined planetary milling device, since the container is rotated in an inclined state, the direction of the gravity acceleration due to rotation and the direction of the gravity acceleration due to revolution are not on the same straight line, but are in an angled direction. Thus, power can be efficiently transmitted to the sample, and crushing and rolling can be efficiently performed, so it is preferred. In addition, considering mass production, a bead mill device that is easy to process in large quantities is preferred.

[0094] It is preferred to carry out the above cutting, crushing and rolling (rolling is carried out as needed. Rolling is not carried out when not needed), and the cutting, crushing and rolling are repeated according to the situation to form flat magnetic metal particles with a specified thickness and aspect ratio. At this time, if the crushing and rolling are carried out in a manner of reaching a thickness of 10 nm or more and 100 μm or less, more preferably 10 nm or more and 1 μm or less, and further preferably 10 nm or more and 100 nm or less, particles that are easy to produce rotational magnetization are formed, which is preferred.

[0095] In order to achieve the degree of orientation of the flat magnetic metal particles as in the present embodiment, it is effective to improve the fluidity by making the flat magnetic metal particles smooth. Therefore, the average thickness of the flat magnetic metal particles is preferably 10 μm to 30 μm, more preferably 10 μm to 20 μm, and the average value of the ratio of the average length to the thickness of the flat magnetic metal particles is preferably 10 to 100, more preferably 10 to 50.

[0096] In addition, it is preferred that the obtained flat magnetic metal particles be subjected to heat treatment to appropriately remove lattice distortion. The heat treatment at this time is the same as the second step, preferably performed at a temperature of 50°C or higher and 800°C or lower, and the heat treatment atmosphere is preferably a vacuum atmosphere with a low oxygen concentration, an inert atmosphere, or a reducing atmosphere, and more preferably H 2 , CO, CH 4 In a reducing atmosphere such as above. In addition, it is more preferable to perform the heat treatment in a magnetic field. The reasons and details thereof are the same as those in the second step and thus the description is omitted.

[0097] Next, as the fourth step, the above-mentioned inclusion phase and magnetic metal particles are mixed to form a mixed powder of the inclusion phase and flat magnetic metal particles. Next, as the fifth step, the mixed powder of the inclusion phase and magnetic metal particles is molded. In addition, heat treatment may be appropriately performed before or after the above-mentioned steps. In other words, heat treatment may be performed before or after molding or simultaneously with molding. In addition, heat treatment may be performed before or after processing. The heat treatment conditions are as described above. In addition, it is more preferred to perform heat treatment in a magnetic field. The reasons and details thereof are the same as those in the second step and will be omitted here.

[0098] In order to obtain the magnetic wedge of the present embodiment, the fifth step is very important. In the fifth step, it is preferable to adopt a method of applying a pressing force in a uniaxial direction, such as uniaxial press forming or hot press forming. Fig.16Schematic diagram of the fifth step in the method for manufacturing a magnetic wedge of the present embodiment is shown in FIG. If a punching force is applied in a uniaxial direction, the flat magnetic metal particles are easily oriented in a stacked manner in the direction of the applied punching force. Therefore, if a simple uniaxial punching molding is used, the flat magnetic metal particles are oriented in a stacked manner in one direction in the direction of the applied punching force, and the magnetic wedge of the present embodiment cannot be obtained. Therefore, when a punching force is applied in a uniaxial direction, a mold magnetized in a direction parallel to the direction of the applied punching force is used as a molding mold. Furthermore, generally speaking, the distance (gap) between the mold punch and the mold punch is in a very narrow state of, for example, about 5 μm. In this case, the flat magnetic metal particles are not easy to move inside the mold, and the structure of the present embodiment cannot be obtained. Therefore, the distance between the mold punch and the mold punch is appropriately adjusted. For example, in the case of flat magnetic metal particles having an average thickness of 10 to 20 μm and an average value of the ratio of the average length in the flat surface to the thickness of about 10 to 50, a gap of about 50 μm is set. By setting such a gap, the fluidity of the inclusion phase is improved, and it can flow out of the gap appropriately and be discharged along the voids contained in the magnetic material. In addition, at this time, the flat magnetic metal particles are oriented while moving inside the mold, and the flat magnetic metal particles are attracted to the magnetized mold punch, resulting in local segregation. On the other hand, if the gap between the hot pressing mold punch and the mold punch is too large, the outflow of the inclusion phase becomes too much, and the amount of the inclusion phase contained in the magnetic material is reduced, which is not preferred. Therefore, it is important to appropriately set the distance (gap) between the mold punch and the mold punch. In the case of flat magnetic metal particles with an average thickness of 10 to 20 μm and an average value of the ratio of the average length in the flat surface to the thickness of about 10 to 50, it is preferred to make the gap greater than 5 μm and less than 100 μm, more preferably greater than 10 μm and less than 80 μm (more preferably about 50 μm). However, if the size of the flat magnetic metal particles (average thickness, average length within the flat surface relative to the average value of the thickness) changes, the optimal gap range may change. In addition, the optimal gap range may also change due to the type of included phases and molding conditions such as temperature, pressure, and time. Therefore, it is always just a target and can be appropriately set according to the actual size of the flat magnetic metal particles, the type of included phases, temperature, pressure, time, and other molding conditions.

[0099] In addition, a magnetic field is applied in a direction parallel to the direction of the external punching force. As a result, in the center of the formed magnetic wedge, the flat magnetic metal particles are easily stacked and oriented in the direction of the external punching force, and in the end, the flat magnetic metal particles are easily stacked and oriented in a direction perpendicular to the direction of the external punching force. Furthermore, in order to easily achieve such orientation, hot stamping is performed while applying a magnetic field. That is, the molding is performed while applying heat, magnetic field, and punching force at the same time. It is preferably performed at a hot pressing temperature of 50°C or more and 1000°C or less, and more preferably at a temperature of 50°C or more and 800°C or less. The larger the external magnetic field, the better, but it is preferably applied at 1kOe or more, and more preferably at 10kOe or more. The punching force is preferably 1MPa or more and 100MPa or less, and more preferably 1MPa or more and 10MPa or less. In addition, after molding, heat treatment is performed while applying a magnetic field in a direction perpendicular to the direction of the external punching force. As a result, the above-mentioned orientation is more easily achieved.

[0100] When the coercive force based on direction is measured in a plane parallel to the flat surface of the flat magnetic metal particle of the magnetic wedge, for example, the coercive force is measured by changing the direction every 22.5 degrees with respect to the 360 ​​degrees angle in the plane.

[0101] By having a coercive force difference in the above-mentioned plane of the magnetic wedge, the minimum coercive force value is reduced compared to the isotropic case where there is almost no coercive force difference, which is preferable. In a material having magnetic anisotropy in a plane, there is a coercive force difference depending on the direction in the plane, and the minimum coercive force value is reduced compared to a magnetic isotropic material. This can reduce hysteresis loss and improve magnetic permeability, which is preferable.

[0102] The ratio of the coercive force difference based on the direction in the plane parallel to the flat surface of the flat magnetic metal particle possessed by the magnetic wedge is as large as possible, and is preferably 1% or more. The ratio of the coercive force difference is more preferably 10% or more, further preferably 50% or more, and further preferably 100% or more. The ratio of the coercive force difference mentioned here can be defined by (Hc(max)-Hc(min)) / Hc(min)×100(%) using the maximum coercive force Hc(max) and the minimum coercive force Hc(min) in the flat surface.

[0103] Furthermore, the coercive force can be easily evaluated by using a vibrating sample magnetometer (VSM). When the coercive force is low, a coercive force of 0.1 Oe or less can be measured by using a low magnetic field unit. The direction of the magnetic field is changed within the above-mentioned plane of the magnetic wedge (within a plane parallel to the flat surface of the flat magnetic metal particle) for measurement.

[0104] When calculating the coercive force, the value obtained by dividing the difference in magnetic fields at two points intersecting the horizontal axis (magnetic fields H1 and H2 where magnetization is zero) by 2 can be used (that is, it can be calculated as coercive force = |H2-H1| / 2).

[0105] The inclusion phase contains at least one second element selected from oxygen (O), carbon (C), nitrogen (N) and fluorine (F). This is because the electrical resistance can be increased. Preferably, the resistivity of the inclusion phase is higher than the resistivity of the flat magnetic metal particles. This is because the eddy current loss of the flat magnetic metal particles can be reduced. Since the inclusion phase exists in a manner surrounding the flat magnetic metal particles, it is preferred to improve the oxidation resistance and thermal stability of the flat magnetic metal particles. Among them, from the viewpoint of high oxidation resistance and high thermal stability, it is more preferred to contain oxygen. Since the inclusion phase plays the role of mechanically bonding the flat magnetic metal particles to each other, it is also preferred from the viewpoint of high strength.

[0106] It is preferred that the inclusion phase contains resin. As resin, thermoplastic resin, thermosetting resin, polyester resin, vinyl ester resin, polyethylene resin, polystyrene resin, polyvinyl chloride resin, polyvinyl butyral resin, polyvinyl alcohol resin, polybutadiene resin, Teflon (registered trademark) resin, polyurethane resin, cellulose resin, ABS resin, nitrile rubber, styrene-butadiene rubber, silicone resin, other synthetic rubber, natural rubber, epoxy resin, phenolic resin, acrylic resin, polybenzimidazole resin, amide resin, polyimide resin, polyamide-imide resin, bismaleimide resin or their copolymers can be used. In particular, in order to achieve high thermal stability, it is preferred to contain silicone resin, polyimide resin, imide resin, bismaleimide resin with high heat resistance. Epoxy resin, phenolic resin, polyester resin are general-purpose resins with relatively high heat resistance and high strength, and are preferred. In addition, in order to improve the strength, materials such as FRP (Fiber-Reinforced Plastics) mixed with fibers such as glass fiber, aromatic polyamide fiber (Kevlar (registered trademark) fiber), carbon fiber, Zylon fiber, polyethylene fiber (Dyneema), and boron fiber are also preferred. Through the above, the bonding between the flat magnetic metal particles and the inclusion phase becomes strong, and the mechanical properties such as thermal stability, strength, and toughness are easily improved. In addition, by surrounding the flat magnetic particles with the inclusion phase, the oxidation resistance is excellent, and the magnetic property degradation caused by oxidation of the flat magnetic metal particles is not easily produced, which is preferred. Furthermore, the type of the resin can be identified by IR (Infrared Spectroscopy), NMR (Nuclear Magnetic Resonance), etc.

[0107] Bismaleimide resins can make the temperature during molding relatively low (for example, below 180°C), so they can be molded using general low-temperature hot stamping equipment, etc., so they are preferred. In addition, as the characteristics after molding, higher thermal stability and excellent mechanical properties can also be achieved, so they are preferred. In addition, it is easy to compound (bond) with flat magnetic metal particles, and it is easy to achieve excellent mechanical properties such as thermal stability, strength and toughness as a composite material, so it is preferred. In addition, the inclusion phase easily surrounds the flat magnetic particles, and it is not easy to cause deterioration of the magnetic properties caused by oxidation of the flat magnetic metal particles, so it is preferred.

[0108] The bismaleimide resin preferably has a glass transition temperature of 250° C. or higher. This is preferred because thermal stability, strength, and the like can be improved.

[0109] Specifically, the bismaleimide resin preferably contains 4,4′-diphenylmethane bismaleimide, phenylmethane maleimide, m-phenylene bismaleimide, bisphenol A diphenyl ether bismaleimide, 3,3′-dimethyl-5,5′-diethyl-4,4′-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, 1,6′-bismaleimide-(2,2,4-trimethyl)hexane, 2,2′-diallyl bisphenol A, 4,4′-diphenyl ether bismaleimide, 4,4′-diphenyl sulfone bismaleimide, 1,3-bis(3-maleimide phenoxy)benzene, 1,3-bis(4-maleimide phenoxy)benzene, bis(3-ethyl-5-methyl-4-maleimide phenyl)methane, 2,2′-bis[4-(4-maleimide phenoxy)phenyl]propane, etc. (The resin is prepared by polymerizing the monomers, but it is preferable to contain the above materials as monomers). This can improve thermal stability and strength, which is preferred.

[0110] In addition, as a curing agent for curing the monomer, it is preferred to contain 4,4'-diaminodiphenylmethane, diaminodiphenyl ether, diaminodiphenyl sulfone, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, o,o'-diallylbisphenol A, etc. However, the curing agent may be a curing agent other than the above as long as it can properly cure the monomer.

[0111] As a preferred combination of a monomer and a curing agent, for example, 4,4'-diphenylmethane bismaleimide and 4,4'-diaminodiphenylmethane can be mentioned. In addition, when 4,4'-diphenylmethane bismaleimide and 4,4'-diaminodiphenylmethane are contained, the ratio of 4,4'-diphenylmethane bismaleimide to 4,4'-diaminodiphenylmethane is preferably 1 to 3, and more preferably about 2. It is preferred to adopt the above ratio because thermal stability and strength can be improved.

[0112] The molecular weight of the inclusion phase (resin) is preferably 100 to 1000. This is preferred because thermal stability, strength, and the like are improved.

[0113] The polyimide resin preferably contains a repeating unit represented by the following chemical formula (1).

[0114] [Chemical formula 1]

[0115]

[0116] In the chemical formula (1), R preferably includes any of biphenyl, triphenyl and tetraphenyl structures. R' preferably represents a structure having at least one aromatic ring in the structure.

[0117] Furthermore, as the polyimide resin, it is more preferable to have the structural formula (2) or (3) below.

[0118] [Chemical formula 2]

[0119]

[0120] [Chemical formula 3]

[0121]

[0122] As described above, according to the present embodiment, the magnetic wedge is a magnetic wedge of a rotary electric machine, the magnetic wedge includes a plurality of flat magnetic metal particles and an inclusion phase, in the central portion in the width direction of the magnetic wedge, the flat surfaces of the plurality of flat magnetic metal particles are oriented in the width direction and the length direction, in the end portion in the width direction, the flat surfaces are oriented in the thickness direction and the length direction, the average of the orientation angles of the plurality of flat magnetic metal particles in the central portion in the width direction is 20 degrees or less, and the average of the orientation angles of the plurality of flat magnetic metal particles in the end portion in the width direction is 30 degrees or more and 90 degrees or less. In addition, the magnetic wedge is the magnetic wedge of a radial gap type rotary electric machine in which a stator is arranged in a manner of facing a rotor with a predetermined interval in the radial direction, the length direction is the axial direction, the thickness direction is the radial direction, and the width direction is the rotation direction. In addition, the magnetic wedge is the magnetic wedge used for an axial gap type rotary electric machine in which a stator is arranged in a manner of facing a rotor with a predetermined interval in the axial direction, the length direction is the radial direction, the thickness direction is the axial direction, and the width direction is the rotation direction. When the orientation angle in the center portion is 20 degrees or less and the orientation angle in the end portion is 30 degrees or more and 90 degrees or less, a magnetic wedge having excellent magnetic properties such as low magnetic loss and excellent mechanical properties such as high strength can be provided.

[0123] (Second embodiment)

[0124] The rotating electrical machine of this embodiment has the magnetic wedge of the first embodiment. Therefore, the contents overlapped with those of the first embodiment are omitted. In this specification, the rotating electrical machine means a concept including any one of an electric motor (motor), a generator (generator), and an electric generator that functions as both an electric motor and a generator as required.

[0125] Fig.17 This is an example of a radial gap type motor according to the present embodiment. The radial gap type motor includes a rotor and a stator which is arranged to face the rotor with a predetermined gap in the radial direction. Fig.17 In the embodiment, the rotor is arranged inside the stator, but it may be arranged outside. The rotor includes a rotor core and a shaft, and is supported in a rotatable manner. On the other hand, the stator includes a stator core, an exciting coil inserted in a slot of the stator core, and a magnetic wedge held in a wedge groove at an opening of the slot.

[0126] Fig.17 , an example of a magnetic wedge according to the first embodiment is shown, but the present invention is not limited thereto. In the case of a radial gap type rotating electrical machine, since the stator is arranged opposite to the rotor at a predetermined interval in the radial direction, the "gap surface" is a surface parallel to a cylindrical surface centered on the rotating axis of the rotor. Therefore, the radial direction is a direction perpendicular to the gap surface, and the axial direction and the rotation direction are directions parallel to the gap surface. Fig.17 1 , flat magnetic metal particles 10 , inclusion phases 20 , magnetic wedges 100 , a rotating electrical machine 200 , a rotor 210 , a stator 220 , a coil 230 , a gap surface 240 , and a core tee 250 are shown.

[0127] By disposing the magnetic wedge of the first embodiment, it is possible to suppress the leakage flux while reducing the harmonic loss generated on the rotor surface. In addition, the torque of the radial gap type motor is increased due to the increase in the magnetic flux passing through the gap. By either or both of the above-mentioned loss reduction effect and torque increase effect, high efficiency can be achieved.

[0128] The radial gap motor may be any of a motor having a conductor in the rotor (induction motor), a motor having a permanent magnet (permanent magnet motor), and a motor having a magnetic body (reluctance motor).

[0129] Fig.18This is an example of an axial gap type motor of the present embodiment. The axial gap type motor has a rotor and a stator arranged opposite to the rotor in the axial direction with a predetermined gap therebetween, the stator having a stator core, an excitation coil inserted in a slot of the stator core, and a magnetic wedge held in a wedge groove at the slot opening. By configuring the magnetic wedge of the present embodiment, it is possible to reduce the harmonic loss generated on the surface of the rotor while suppressing the increase in leakage flux. In addition, the torque of the axial gap type motor increases due to the increase in magnetic flux passing through the gap. With the above configuration, high efficiency can be achieved.

[0130] Fig.18 In the embodiment, the rotor is arranged between two stators, but it can also be arranged on one side or both sides of a stator. In the case of an axial gap type rotating electric machine, since the stator is arranged opposite to the rotor at a predetermined interval in the axial direction, the "gap surface" is a surface orthogonal to the rotation axis of the rotor. Therefore, the axial direction is a direction perpendicular to the gap surface, and the rotation direction and radial direction are directions parallel to the gap surface. Fig.18 , flat magnetic metal particles 10 , inclusion phases 20 , magnetic wedges 100 , a rotating electrical machine 200 , a rotor 210 , a coil 230 , a gap surface 240 , a core tee 250 , a stator 270 , and a shaft 280 are shown.

[0131] Fig.19 : is a schematic diagram showing an example of a generator according to the present embodiment. The generator generally comprises a rotor in which an excitation coil is housed in a slot of a rotor core (in addition, a rotor using a permanent magnet as an excitation source may also be used), and a stator in which an armature coil is housed in a slot of a stator core. By rotating the rotor and passing an excitation current through the excitation coil, electric power is generated in the armature coil. The rotor comprises a rotor core, an excitation coil inserted in a slot of the rotor core, and a magnetic wedge held in a wedge groove at an opening of the slot, and is supported rotatably by a bearing. By configuring the magnetic wedge according to the present embodiment, it is possible to reduce the harmonic loss generated on the surface of the stator while suppressing the increase in leakage flux. In addition, the generated voltage induced by the armature coil increases due to the increase in magnetic flux linked to the armature coil through the gap. By the above method, high efficiency can be achieved.

[0132] Fig.19 In the embodiment, the magnetic wedges are arranged at the slot openings of the rotor core, but they may be arranged at the slot openings of the stator core. In addition, the figure shows a winding type generator in which the rotor has an excitation coil, but it may be a permanent magnet type generator in which the rotor has a permanent magnet. In this case, the magnetic wedges may be arranged at the slot openings of the stator core. Fig.19, flat magnetic metal particles 10 , inclusion phases 20 , magnetic wedges 100 , a rotating electrical machine 200 , a rotor 210 , a stator core 222 , an excitation coil 232 , an armature coil 234 , a gap surface 240 , and a core tee 250 are shown.

[0133] Since the linear motor is a flat plate structure formed by unfolding the radial gap type motor, the magnetic wedge of the present invention can also be used in the linear motor. That is, the stator has a stator core and an exciting coil inserted in the slot of the stator core, and the magnetic wedge can also be set at the slot opening. Fig. 20 : is a schematic diagram showing an example of a linear motor of the present embodiment. In the linear motor, the moving direction of the movable element, the direction at right angles to the moving direction of the movable element, and the direction perpendicular to the stator correspond to the rotation direction, axial direction, and radial direction of the radial gap type motor, respectively. By configuring the magnetic wedge of the present embodiment, it is possible to reduce the harmonic loss generated by the surface of the movable element while suppressing the increase in leakage flux. In addition, the thrust of the linear motor is increased due to the increase in magnetic flux passing through the gap. As a result, high efficiency can be achieved. Fig. 20 1 , flat magnetic metal particles 10 , inclusion phases 20 , magnetic wedges 100 , stators 220 , coils 230 , gap surfaces 240 , core tees 250 , and movable elements 290 are shown.

[0134] As described above, according to the rotary electric machine of this embodiment, the increase of leakage flux caused by the use of magnetic wedges can be suppressed, and the pulsation of magnetic flux distribution in the surface portion of the core can be effectively alleviated, thereby achieving high efficiency. Furthermore, the slot shape of the rotary electric machine of this embodiment can also be a semi-closed slot (or semi-closed slot), but is preferably an open slot (or open slot, open slot). In this case, the harmonic loss can be greatly reduced, which is preferred.

[0135] The rotating electric machine of this embodiment can be used in transportation systems such as railways, electric vehicles, and hybrid vehicles, civil systems such as elevators and air conditioners, industrial systems such as robots, pumps, compressors, and blowers, energy systems such as thermal generators, hydroelectric generators, wind generators, nuclear power generators, and geothermal generators, and home appliances such as washing machines, and can seek to improve the efficiency of the system. In particular, in large-capacity machines for industrial use, since the slot shape generally adopts an open slot, it is preferable to have the magnetic wedge of the first embodiment. In addition, in the main motor for railways, since a mold-wound coil is used from the necessity of high voltage resistance and vibration resistance, and the slot shape adopts an open slot, it is preferable to have the magnetic wedge of the first embodiment.

[0136] In railways, the loss of rotating electric machines accounts for about half of the power consumed when traveling on the railway, so reducing the loss of rotating electric machines can greatly improve efficiency. In addition, in electric vehicles and hybrid vehicles, the efficiency of the main motor can be improved by adopting the magnetic wedge of the first embodiment, thereby extending the cruising distance.

[0137] Among power generators, a large effect can be expected for a hydroelectric generator, especially a variable speed water pumping generator. In addition, a large effect can also be expected for a wind power generator.

[0138] (Example)

[0139] Hereinafter, Examples 1 to 7 will be described in detail by comparison with Comparative Examples 1 to 6. The schematic diagram of the arrangement of the flat magnetic metal particles in the magnetic wedges of Example 1 and Comparative Examples 1 to 4 is shown in FIG. Fig.14 shown.

[0140] (Example 1)

[0141] First, a single-roll quenching device was used to produce a Fe-Co-Si-B (Fe70Co30B25(at%)-4wt%Si) strip. 2 The obtained tape was heat treated at 300°C in an atmosphere. Then, the tape was crushed using a stirring device to obtain flat magnetic metal particles (average thickness of about 15 μm, average length of the flat surface relative to the thickness ratio of about 30). Then, the obtained flat magnetic metal particles were mixed with an imide resin (polyimide resin) and molded. Molding was performed according to Fig.13Implementation. That is, the mold used for molding is a mold that is magnetized in a direction parallel to the direction of the applied punching pressure. The gap between the mold die and the mold punch is about 50μm. In addition, when the punching pressure is applied in a uniaxial direction, a magnetic field is applied in a direction parallel to the direction of the applied punching pressure. Then, hot stamping molding is performed, and after molding, a magnetic wedge is produced while applying a magnetic field in a direction perpendicular to the direction of the applied punching pressure. In addition, the magnetic wedge is produced in a manner that the cross-sectional shape of the magnetic wedge is rectangular. The width direction of the magnetic wedge is the x direction, the length direction is the y direction, and the thickness direction is the z direction. In the produced magnetic wedge, the orientation angle of the above-mentioned flat magnetic metal particles is measured. In the measurement, the orientation angles of all flat magnetic metal particles contained in the center, end, and each area of ​​the observation range are calculated, and the average value is used. In addition, the observed cross section is evaluated as 3 cross sections, and the average value is used. As a result, it was confirmed that the orientation angle in the center was 5 degrees (satisfying 20 degrees or less), and the orientation angle in the end was 33 degrees (satisfying 30 degrees or more and 90 degrees or less). By the way, regarding the orientation angle in the end, it was confirmed that the orientation angle relative to the contour line in the thickness direction was also 33 degrees.

[0142] (Example 2)

[0143] The process is substantially the same as Example 1 except that the resin used in molding is specified as a bismaleimide resin. Furthermore, the ratio of 4,4′-diphenylmethane bismaleimide to 4,4′-diaminodiphenylmethane is 2. It is confirmed that the orientation angle in the center is 5 degrees (satisfying 20 degrees or less), and the orientation angle in the end is 34 degrees (satisfying 30 degrees or more and 90 degrees or less). By the way, regarding the orientation angle in the end, it is confirmed that the orientation angle relative to the contour line in the thickness direction is also 34 degrees.

[0144] (Example 3)

[0145] Except that the cross-sectional shape of the magnetic wedge (cross-section on the xz plane) was set to a trapezoidal shape, it was substantially the same as Example 2. Furthermore, it was confirmed that the orientation angle in the center portion was approximately 4 degrees (satisfying 20 degrees or less), and the orientation degree in the end portion was approximately 37 degrees (satisfying 60 degrees or less) relative to the contour line in the thickness direction.

[0146] (Example 4)

[0147] Except that the cross-sectional shape of the magnetic wedge (cross-section on the xz plane) is set to a convex shape, it is substantially the same as Example 2. Furthermore, it was confirmed that the orientation angle in the center portion was approximately 5 degrees (satisfying 20 degrees or less), and the orientation degree in the end portion was approximately 38 degrees (satisfying 60 degrees or less) relative to the contour line in the thickness direction.

[0148] (Example 5)

[0149] Except that the cross-sectional shape of the magnetic wedge (cross-section on the xz plane) is set to a hexagon, it is substantially the same as Example 2. Furthermore, it was confirmed that the orientation angle in the center portion was approximately 4 degrees (satisfying 20 degrees or less), and the orientation degree in the end portion was approximately 30 degrees (satisfying 60 degrees or less) relative to the contour line in the thickness direction.

[0150] (Example 6)

[0151] The same method as in Example 2 was used except that the ratio of 4,4′-diphenylmethane bismaleimide to 4,4′-diaminodiphenylmethane was set to 1. The orientation angle in the center was confirmed to be 5 degrees (satisfying 20 degrees or less), and the orientation angle in the end was confirmed to be 34 degrees (satisfying 30 degrees or more and 90 degrees or less). Incidentally, regarding the orientation angle in the end, the orientation angle relative to the contour line in the thickness direction was also confirmed to be 34 degrees.

[0152] (Example 7)

[0153] The method is substantially the same as Example 2 except that the ratio of 4,4′-diphenylmethane bismaleimide to 4,4′-diaminodiphenylmethane is set to 3. It was confirmed that the orientation angle in the center portion was 5 degrees (satisfying 20 degrees or less), and the orientation angle in the end portion was 34 degrees (satisfying 30 degrees or more and 90 degrees or less). Incidentally, regarding the orientation angle in the end portion, it was confirmed that the orientation angle relative to the contour line in the thickness direction was also 34 degrees.

[0154] (Comparative Example 1)

[0155] As the magnetic wedges in which spherical magnetic metal particles are dispersed, a commercially available magnetic wedge is used. This material is a material in which Fe powder is dispersed three-dimensionally isotropically.

[0156] (Comparative Example 2)

[0157] The process is the same as in Example 1 except that the molding method is simple hot stamping (using a non-magnetized mold and without applying a magnetic field) and the magnetic wedges are formed by cutting to form flat magnetic metal particles stacked and oriented in the y direction.

[0158] (Comparative Example 3)

[0159] The process is the same as in Example 1 except that the molding method is simple hot stamping (using a non-magnetized mold and without applying a magnetic field) and the magnetic wedges are formed by cutting to form flat magnetic metal particles stacked and oriented in the z direction.

[0160] (Comparative Example 4)

[0161] The same procedure as in Example 1 was followed except that the molding method was simple hot stamping (using an unmagnetized mold and without applying a magnetic field) and that a magnetic wedge was formed by cutting to form flat magnetic metal particles stacked and oriented in the x direction.

[0162] (Comparative Example 5)

[0163] The method is substantially the same as Example 2 except that the ratio of 4,4′-diphenylmethane bismaleimide to 4,4′-diaminodiphenylmethane is set to 0.7. It was confirmed that the orientation angle in the center portion was 5 degrees (satisfying 20 degrees or less), and the orientation angle in the end portion was 34 degrees (satisfying 30 degrees or more and 90 degrees or less). Incidentally, regarding the orientation angle in the end portion, it was confirmed that the orientation angle relative to the contour line in the thickness direction was also 34 degrees.

[0164] (Comparative Example 6)

[0165] The method is substantially the same as Example 2 except that the ratio of 4,4′-diphenylmethane bismaleimide to 4,4′-diaminodiphenylmethane is set to 3.3. The orientation angle in the center portion is confirmed to be 5 degrees (satisfying 20 degrees or less), and the orientation angle in the end portion is confirmed to be 34 degrees (satisfying 30 degrees or more and 90 degrees or less). Incidentally, regarding the orientation angle in the end portion, the orientation angle relative to the contour line in the thickness direction is also confirmed to be 34 degrees.

[0166] Table 1 shows the cross-sectional shape of the magnetic wedge according to the present embodiment, the type of resin, and the ratio of 4,4′-diphenylmethane bismaleimide to 4,4′-diaminodiphenylmethane together with Comparative Examples 1 to 6.

[0167] Table 2 shows the magnetic properties of the magnetic wedge according to the present embodiment, the bending strength as a mechanical property, the bending strength after a heat resistance test as a thermomechanical property, and the degree of improvement in efficiency as a rotating electrical machine together with Comparative Examples 1 to 6.

[0168] (1) Iron loss: The iron loss under the operating conditions of 100 Hz and 1 T was measured using a BH analyzer. Furthermore, when the iron loss could not be directly measured under the conditions of 100 Hz and 1 T, the frequency dependence and magnetic flux density dependence of the iron loss were measured, and the iron loss at 100 Hz and 1 T was estimated from the data (and the estimated value was used). The iron loss was expressed as a ratio based on the iron loss of Comparative Example 1.

[0169] (2) Magnetic permeability: The magnetic permeability at 100 Hz was measured. The magnetic permeability was expressed as a ratio based on the iron loss of Comparative Example 1.

[0170] (3) Efficiency improvement of rotating electrical machine: A standard radial gap motor was moved, and the efficiency improvement was calculated based on the efficiency when a non-magnetic wedge was used. The efficiency improvement was expressed as a ratio based on the efficiency improvement in Comparative Example 1.

[0171] (4) Strength: The flexural strength of the evaluation sample at 25°C was measured and expressed as a ratio to the flexural strength of the sample of Comparative Example 1 at 25°C (= flexural strength of the evaluation sample at 25°C / flexural strength of the sample of Comparative Example 1 at 25°C).

[0172] (5) Strength after heat resistance test: After the evaluation sample is heated at 220°C in the atmosphere for 100 hours (heat resistance test), the flexural strength is measured at 25°C and expressed as the ratio of the flexural strength at 25°C to the flexural strength of the sample of Comparative Example 1 at 25°C after being heated at 220°C in the atmosphere for 100 hours (= flexural strength of the evaluation sample at 25°C after being heated at 220°C in the atmosphere for 100 hours / flexural strength of Comparative Example 1 at 25°C after being heated at 220°C in the atmosphere for 100 hours).

[0173] Table 1

[0174]

[0175] Table 2

[0176]

[0177] As can be seen from Table 2, compared with Comparative Example 1, in Comparative Examples 2, 3, and 4, the loss in all directions of x, y, and z is reduced, the magnetic permeability is improved, and there is some improvement, but there are directions where the improvement is small due to the direction. The improvement is small in the y direction in Comparative Example 2, in the z direction in Comparative Example 3, and in the x direction in Comparative Example 4. In addition, the efficiency improvement of the rotating electric machine is large in Comparative Example 2, but small in Comparative Examples 3 and 4. This is mainly because the magnetic flux leakage between the T-irons is increased in Comparative Example 3, and the magnetic flux leakage in the axial direction is increased in Comparative Example 4. In addition, regarding strength, there are defects such as low strength in the y direction in Comparative Example 2, low strength in the z direction in Comparative Example 3, and low strength in the x direction in Comparative Example 4. In addition, the strength after the heat resistance test also has roughly the same tendency. Correspondingly, it is known that in Example 1, by changing the orientation angle of the flat magnetic metal particles at the center and the end, excellent magnetic properties (low loss, high magnetic permeability) and excellent mechanical properties (high strength, etc.) can be achieved regardless of the direction. That is, by stacking and orienting the flat magnetic metal particles in the z direction at the center and stacking and orienting the flat magnetic metal particles in the x direction at the ends, the magnetic properties and mechanical properties are averaged three-dimensionally, and excellent properties are achieved in all directions of the x direction, y direction, and z direction. Similarly, it is known that in Example 2, although the strength and the strength after the heat resistance test are slightly inferior to those of Example 1, it also has roughly the same excellent properties. In addition, in Examples 3 to 5, it is known that the cross-sectional shape of the magnetic wedge (the cross section on the xz plane) is changed to a trapezoidal type, a convex type, or a hexagonal type, but compared with the rectangular type of Example 2, it has roughly the same excellent properties. Examples 6 and 7 are examples in which the ratio of 4,4′-diphenylmethane bismaleimide to 4,4′-diaminodiphenylmethane is changed to 1 and 3, but compared with the ratio of 2 in Example 2, although the strength and the strength after the heat resistance test are slightly inferior, it has roughly the same excellent properties. In contrast, in Comparative Examples 5 and 6, the ratio of 4,4′-diphenylmethane bismaleimide to 4,4′-diaminodiphenylmethane was changed to 0.7 and 3.3, respectively, and it was found that the strength and the strength after the heat resistance test were greatly deteriorated. In other words, it was found that the ratio of 4,4′-diphenylmethane bismaleimide to 4,4′-diaminodiphenylmethane is preferably 1 to 3, and most preferably 2.

[0178] Several embodiments and examples of the present invention have been described, but these embodiments and examples are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other ways, and various omissions, substitutions, and changes can be made without departing from the scope of the subject matter of the invention. These embodiments and their variations are included in the scope and subject matter of the invention, and are also included in the invention described in the claims and their equivalents.

[0179] In addition, the above-mentioned embodiments can be summarized as the following technical solutions.

[0180] (Technical Solution 1)

[0181] A magnetic wedge is a magnetic wedge of a rotating electric machine, wherein:

[0182] The magnetic wedge comprises a plurality of flat magnetic metal particles and an inclusion phase.

[0183] In the central portion of the magnetic wedge in the width direction, the flat surfaces of the plurality of flat magnetic metal particles are oriented along the contour line in the width direction, and in the end portions in the width direction, the flat surfaces are oriented along the contour line in the thickness direction of the magnetic wedge, an average of orientation angles of the plurality of flat magnetic metal particles in the central portion in the width direction relative to the contour line in the width direction is 20 degrees or less, and an average of orientation angles of the plurality of flat magnetic metal particles in the end portions in the width direction relative to the contour line in the thickness direction is 60 degrees or less.

[0184] (Technical Solution 2)

[0185] A magnetic wedge is a magnetic wedge of a rotating electric machine, wherein:

[0186] The magnetic wedge comprises a plurality of flat magnetic metal particles and an inclusion phase.

[0187] In the central portion of the magnetic wedge in the width direction, the flat surfaces of the plurality of flat magnetic metal particles are oriented in the width direction and the length direction, and in the end portions of the magnetic wedge in the width direction, the flat surfaces are oriented in the thickness direction and the length direction, an average of the orientation angles of the plurality of flat magnetic metal particles in the central portion in the width direction is less than 20 degrees, and an average of the orientation angles of the plurality of flat magnetic metal particles in the end portions in the width direction is greater than or equal to 30 degrees and less than or equal to 90 degrees.

[0188] (Technical Solution 3)

[0189] The magnetic wedge according to claim 1 or 2, wherein the cross section of the magnetic wedge perpendicular to the longitudinal direction is at least one selected from a trapezoidal shape, a convex shape, a hexagonal shape, and a rectangular shape.

[0190] (Technical Solution 4)

[0191] The magnetic wedge according to any one of claims 1 to 3 is a magnetic wedge of a radial gap type rotating electric machine in which a stator is arranged opposite to a rotor at a predetermined interval in the radial direction, wherein:

[0192] The length direction is axial,

[0193] The thickness direction is the radial direction,

[0194] The width direction is the rotation direction.

[0195] (Technical Solution 5)

[0196] The magnetic wedge according to any one of claims 1 to 3 is used in an axial gap type rotating electrical machine in which a stator is disposed opposite to a rotor at a predetermined interval in the axial direction, wherein:

[0197] The length direction is radial,

[0198] The thickness direction is the axial direction,

[0199] The width direction is the rotation direction.

[0200] (Technical Solution 6)

[0201] A magnetic wedge according to any one of technical solutions 1 to 5, wherein:

[0202] The plurality of flat magnetic metal particles have an average thickness of 10 nm or more and 100 μm or less, and have the flat surface and a magnetic metal phase containing at least one first element selected from Fe, Co and Ni, and an average value of a ratio of an average length in the flat surface to the thickness is 5 or more and 10000 or less,

[0203] The inclusion phase exists between the plurality of flat magnetic metal particles and contains at least one second element selected from the group consisting of oxygen (O), carbon (C), nitrogen (N), and fluorine (F).

[0204] (Technical Solution 7)

[0205] The magnetic wedge according to claim 6 , wherein the average thickness of the plurality of flat magnetic metal particles is 10 μm to 30 μm, and the average value of the ratio of the average length to the thickness of the flat magnetic metal particles is 10 to 100.

[0206] (Technical Solution 8)

[0207] The magnetic wedge according to claim 1 or 2, wherein the inclusion phase contains resin.

[0208] (Technical Solution 9)

[0209] According to the magnetic wedge described in Technical Solution 8, the resin is bismaleimide resin.

[0210] (Technical Solution 10)

[0211] The magnetic wedge according to technical solution 9, wherein the bismaleimide resin contains 4,4′-diphenylmethane bismaleimide.

[0212] (Technical Solution 11)

[0213] The magnetic wedge according to claim 10 , wherein the bismaleimide resin contains 4,4′-diphenylmethane bismaleimide and 4,4′-diaminodiphenylmethane, and the ratio of 4,4′-diphenylmethane bismaleimide to 4,4′-diaminodiphenylmethane is 1 to 3.

[0214] (Technical Solution 12)

[0215] The magnetic wedge according to any one of claims 9 to 11, wherein the bismaleimide resin has a glass transition temperature of 250° C. or higher.

[0216] (Technical Solution 13)

[0217] The magnetic wedge according to any one of technical solutions 8 to 12, wherein the molecular weight of the resin is 100 or more and 1000 or less.

[0218] (Technical Solution 14)

[0219] A magnetic wedge according to any one of technical solutions 1 to 13, wherein at least a portion of the surface of the flat magnetic metal particle is covered with a coating layer, the coating layer has a thickness of not less than 0.1 nm and not more than 1 μm, and contains at least one second element selected from oxygen (O), carbon (C), nitrogen (N) and fluorine (F).

[0220] (Technical Solution 15)

[0221] The magnetic wedge according to any one of claims 1 to 14, wherein the magnetic wedge has a coercive force difference depending on a direction in a plane parallel to the flat surface.

[0222] (Technical Solution 16)

[0223] A rotating electrical machine includes the magnetic wedge according to any one of claims 1 to 15.

Claims

1. A magnetic wedge, which is a magnetic wedge of a rotating electrical machine, wherein: The magnetic wedge comprises a plurality of flat magnetic metal particles and an inclusion phase. In the central portion of the magnetic wedge in the width direction, the flat surfaces of the plurality of flat magnetic metal particles are oriented along the contour line in the width direction, and in the end portions in the width direction, the flat surfaces are oriented along the contour line in the thickness direction of the magnetic wedge, an average of orientation angles of the plurality of flat magnetic metal particles in the central portion in the width direction relative to the contour line in the width direction is 20 degrees or less, and an average of orientation angles of the plurality of flat magnetic metal particles in the end portions in the width direction relative to the contour line in the thickness direction is 60 degrees or less.

2. A magnetic wedge, which is a magnetic wedge of a rotating electrical machine, wherein: The magnetic wedge comprises a plurality of flat magnetic metal particles and an inclusion phase. In the central portion of the magnetic wedge in the width direction, the flat surfaces of the plurality of flat magnetic metal particles are oriented in the width direction and the length direction, and in the end portions of the magnetic wedge in the width direction, the flat surfaces are oriented in the thickness direction and the length direction, an average of the orientation angles of the plurality of flat magnetic metal particles in the central portion in the width direction is less than 20 degrees, and an average of the orientation angles of the plurality of flat magnetic metal particles in the end portions in the width direction is greater than or equal to 30 degrees and less than or equal to 90 degrees.

3. The magnetic wedge according to claim 1 or 2, wherein: The cross section of the magnetic wedge perpendicular to the longitudinal direction is at least one selected from a trapezoidal shape, a convex shape, a hexagonal shape, and a rectangular shape.

4. The magnetic wedge according to claim 1 or 2, which is a magnetic wedge of a radial gap type rotating electric machine in which a stator is arranged to face a rotor at a predetermined interval in the radial direction, wherein: The length direction is axial, The thickness direction is the radial direction, The width direction is the rotation direction.

5. The magnetic wedge according to claim 1 or 2, which is used for an axial gap type rotating electric machine in which a stator is arranged to face a rotor at a predetermined interval in the axial direction, wherein: The length direction is radial, The thickness direction is the axial direction, The width direction is the rotation direction.

6. The magnetic wedge according to claim 1 or 2, wherein: The plurality of flat magnetic metal particles have an average thickness of 10 nm or more and 100 μm or less, and have the flat surface and a magnetic metal phase containing at least one first element selected from Fe, Co and Ni, and an average value of a ratio of an average length in the flat surface to the thickness is 5 or more and 10000 or less, The inclusion phase exists between the plurality of flat magnetic metal particles and contains at least one second element selected from the group consisting of oxygen (O), carbon (C), nitrogen (N), and fluorine (F).

7. The magnetic wedge according to claim 6, wherein: The average thickness of the plurality of flat magnetic metal particles is 10 μm or more and 30 μm or less, and the average value of the ratio of the average length to the thickness of the flat magnetic metal particles is 10 or more and 100 or less.

8. The magnetic wedge according to claim 1 or 2, wherein: The inclusion phase contains resin.

9. The magnetic wedge according to claim 8, wherein: The resin is bismaleimide resin.

10. The magnetic wedge according to claim 9, wherein: The bismaleimide resin contains 4,4′-diphenylmethane bismaleimide.

11. The magnetic wedge according to claim 10, wherein: The bismaleimide resin contains 4,4′-diphenylmethane bismaleimide and 4,4′-diaminodiphenylmethane, and the ratio of 4,4′-diphenylmethane bismaleimide to 4,4′-diaminodiphenylmethane is 1 to 3.

12. The magnetic wedge according to claim 9, wherein: The bismaleimide resin has a glass transition temperature of 250° C. or higher.

13. The magnetic wedge according to claim 8, wherein: The molecular weight of the resin is 100 or more and 1000 or less.

14. The magnetic wedge according to claim 1 or 2, wherein: At least a portion of the surface of the flat magnetic metal particle is covered with a coating layer, the coating layer has a thickness of 0.1 nm to 1 μm, and contains at least one second element selected from oxygen (O), carbon (C), nitrogen (N), and fluorine (F).

15. The magnetic wedge according to claim 1 or 2, wherein: In a plane parallel to the flat surface, there is a coercive force difference depending on the direction. 16 . A rotating electrical machine comprising the magnetic wedge according to claim 1 .