Preparation method of convergent or divergent spherical light source

Through electrostatic spraying technology, luminescent materials are adsorbed on the spherical curved surface to form a uniform and stable spherical electroluminescent light source, which solves the problem of spherical light source preparation in the prior art and improves the equipment operation convenience and raw material utilization rate.

CN118921784APending Publication Date: 2024-11-08INNER MONGOLIA UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410220548.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-02-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art is difficult to prepare uniformly and stably converged or divergent spherical electroluminescent light sources on spherical curved surfaces, and electrostatic spraying methods have not yet been used in this field.

Method used

The electrostatic spraying technology uses negative charges to make the luminescent material bear a negative charge under the high-voltage DC electric field, and is uniformly adsorbed on the concave or convex substrate. Through DC driving, a uniform or stable convergence or divergent spherical light source is formed. The convex substrate is used to form a convex light source. The substrate forms a divergent light source.

Benefits of technology

The preparation of spherical light source uniformly and stably on the spherical curved surface is realized, which improves the utilization rate of raw materials and the convenience of equipment operation, and solves the problems of expensive equipment and high waste rate of raw materials in the prior art.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118921784A_ABST
    Figure CN118921784A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a convergent or divergent spherical light source. A luminescent material is adsorbed on the surface of a concave or convex substrate through an electrostatic spraying technology and is driven by direct current to form a uniform and stable convergent or divergent spherical light source. The concave substrate forms a convergent light source which is used for focusing an optical signal; the convex substrate forms a divergent light source which is used for diverging optical signals. By optimizing the preparation process of each layer of structure of the device and the luminescence performance of the device, a convergent or divergent spherical light source capable of stably and uniformly emitting light under the driving of direct-current voltage is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a converging or diverging spherical light source, and belongs to the field of light-emitting devices. Background Art

[0002] With the continuous development of science and technology, electroluminescent devices are constantly being improved and improved. Most of them are used in electronic screens, lighting, medical equipment, traffic lights and other fields, but there are no reports of using them as optical signal conversion devices. In 2003, Podkletnov of Russia discovered a kind of uncharged momentum beam particles formed by high-voltage discharge of rare earth superconductors. In order to explore the energy exchange relationship between rare earth superconducting momentum beams and photons, we designed an optical detection device, which is a spherical convergent or divergent light source and a stable surface light source. When the previous light source is prepared, most of the methods use sputtering, screen printing, scraping, spin coating, slit coating and other technologies, but these methods have many disadvantages, expensive equipment, inconvenient operation, high material waste rate, and cannot be realized on spherical curved substrates. With the continuous development of spraying technology, many researchers have found that the spraying method is not only convenient and simple, but also has a high utilization rate of raw materials during spraying. However, to date, no work has been found to use electrostatic spraying to prepare uniform and stable convergent or divergent spherical electroluminescent light sources.

[0003] The present invention proposes a method of using electrostatic spraying technology and the principle of corona discharge to make the luminescent material carry negative charge under the action of high voltage DC electric field and uniformly adsorb on the surface of the substrate with positive charge. Using a concave or convex substrate, a uniform and stable converging or diverging spherical light source driven by DC is prepared. The concave substrate forms a converging light source, which is used to uniformly focus the optical signal; the convex substrate forms a diverging light source, which is used to uniformly diverge the optical signal. Summary of the invention

[0004] The present invention is a preparation method for adsorbing luminescent materials on a concave or convex substrate surface by electrostatic spraying technology and driving with direct current to form a uniform and stable converging or diverging spherical light source.

[0005] Summary of the invention is as follows: Self-made concave or convex substrate. The concave or convex metal bottom electrode can be made of metal discs with good ductility and conductivity, such as silver, aluminum, iron, nickel, gold, copper, etc., and pressed with a self-made model to make metal concave or convex substrates of different sizes. You can also use materials such as glass, PET, ceramics, etc. with concave and convex spherical shapes, and plate the conductive material on the surface to make it conductive as a substrate.

[0006] The treatment method of the metal substrate can be physical grinding or electrochemical polishing. The specific method of physical grinding is to first use coarse yarn cloth or polishing powder to grind the oxide film on the metal surface, then use polishing agent or polishing paste and polishing cloth to polish along the surface texture of the oxide layer to make it smooth, and finally use fine sandpaper or polishing powder to remedy the surface state to prevent it from oxidizing again. The electrochemical polishing method first cleans the metal substrate, removes the oxide film on the metal surface with an acid solution (hydrochloric acid, nitric acid, etc.) or an alkaline solution (sodium hydroxide, potassium hydroxide, etc.), and then selects the polishing liquid. Different materials use different polishing liquids. The polishing liquid can be a polishing liquid composed of phosphoric acid and sulfuric acid; a polishing liquid composed of phosphoric acid and citric acid; a polishing liquid composed of perchloric acid and phosphoric acid, etc. After the polishing liquid is mixed evenly in a suitable proportion, it is placed in an electrolyte tank. The metal to be polished is used as the anode, and the corrosion-resistant material (graphite, stainless steel, etc.) is used as the cathode to form a closed circuit. The DC voltage range is (10~20V) and the current size is (15~50mA). The polishing time is generally 2~3min. After cleaning the treated substrate, blow it dry in time to prevent re-oxidation.

[0007] Preparation of luminescent materials. Select ZnS, CaS, SrAl2O4, CaAl2O4, BaAl2O4, etc. as the matrix of the luminescent material, use rare earth elements (such as Eu, Tb, Er, etc.), transition metals (such as Mn, Cu, Pb, etc.) and other activators to dope the above materials in a certain proportion, and then use a high-temperature solid-phase method to obtain the luminescent powder. The proportion of activator doping is generally 2~5%, and the powder mixing must be very uniform. Generally, deionized water or anhydrous ethanol is added for wet grinding. The grinding time is 8~24h, and the size of the luminescent powder particles is less than 5μm. In a nitrogen or hydrogen sulfide gas atmosphere, the reaction temperature of the luminescent powder in a high-temperature tube furnace is 800~1100℃. The surface conductivity of the luminescent powder obtained by the reaction is not strong. In order to make its luminescent performance better, a layer of Cu must be coated on the surface of the luminescent particles. x S, the copper coating solution can be a solution of cupric acetate or cuprous chloride, the solution concentration is 0.001~0.1g / L, the solution temperature is 20~80℃, and the copper coating time is 1~3h. The luminescent powder after copper coating is dried and stored.

[0008] The device preparation process. Figure 1Schematic diagram of the structure of a converging or diverging spherical light source, in which 1 represents a concave or convex conductive substrate, and above the substrate are 2 light-emitting layers and 3 transparent top electrodes. The light-emitting layer can be electrostatically sprayed to adsorb the light-emitting powder directly on the conductive metal substrate, spray 1 to 9 layers, and then spray the binder on it. The binder concentration is diluted 5 to 10 times, the spraying speed is low to medium, the number of spray layers is 1 to 5, the thickness of the light-emitting layer is about 10 to 100 μm, and it is annealed and dried at 80 to 150 ° C for 1 to 2 hours to make it firmly bonded to the substrate. The top electrode can be transparent conductive electrodes such as polyacetylene, graphene, and AgNMs. The top electrode is prepared by solution spraying or solution spin coating. In the spraying method, a transparent conductive solution is first prepared. Generally, the standard solution is diluted 5 to 10 times. Then the solution is placed in a 5 to 30 mL spray pot and sprayed at a certain speed. The number of spray layers is 1 to 9, and the thickness is about 5 to 10 μm. After the completion, it is annealed and dried at 80 to 120 ° C for 0.5 to 1 h. The conductive solution is prepared by spin coating. Generally, the standard solution is diluted 2 to 3 times. The spin coater speed is 1500 to 2500 rpm / min, the spin coating time is 10 to 20 seconds, and the thickness is about 3 to 5 μm. After the completion, it is annealed at 80 to 120 ° C for 0.5 to 1 h. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] Figure 1 Structural diagram of converging and diverging spherical light sources Figure 2 Actual working diagram of concave electroluminescent device at different voltages Figure 3 Luminescent properties of concave electroluminescent devices DETAILED DESCRIPTION

[0010] The present invention will be described in more detail by the following examples, but the present invention is not limited to these examples.

[0011] Use 99.999% aluminum sheets purchased from the market to cut circular sheets of appropriate diameter, place the cut circular sheets in a homemade concave mold, and press them into a curved surface with the help of a hydraulic tablet press.

[0012] The concave aluminum sheet was cleaned with detergent, acetone, and ethanol for 10 minutes respectively, and then dried. The cleaned aluminum sheet model was immersed in 0.1M NaOH solution. A large number of bubbles were generated after about 1 minute. Finally, it was cleaned with anhydrous ethanol and the aluminum sheet model was stored in anhydrous ethanol for polishing. The polishing liquid was prepared with a volume ratio of perchloric acid to anhydrous ethanol of 1:4, and the polishing liquid was placed on a magnetic stirrer to keep the temperature at 0°C.

[0013] The graphite electrode is used as the cathode, and the aluminum sheet model is used as the anode in the polishing liquid. A DC voltage of 16V is applied, and the current is about 0.35A. A large number of bubbles are generated on the surface of the aluminum sheet, and the polishing time is 2~3min. The treated aluminum sheet is bright and shiny. After cleaning with anhydrous ethanol, dry and store.

[0014] Zinc sulfide doped manganese luminescent powder is widely used in DC electroluminescent devices and has stable luminescent performance. Mix 99.5% zinc sulfide and 0.5% manganese chloride by weight and calcine at 900℃ for 60min in nitrogen atmosphere. Soak the prepared luminescent powder in 70℃ copper acetate aqueous solution (0.1g / L) for 180min, wash and dry.

[0015] Silver nanowires (AgNMs) are widely used as electrodes due to their low resistance, high conductivity, high transmittance, good stability and low price. The polyol method is used to prepare AgNMs. 75 mg of polyvinyl pyrrolidone (PVP) was dissolved in 10 mL of ethylene glycol, heated in an oil bath at 160 ° C for 60 min, and magnetically stirred at 550 r / min. Then 40 μL of NaCl (3.5 mM) solution and 20 μL of KBr (1.8 mM) solution were transferred into the bottle, and 5.2 mL of AgNO3 (30.5 mM) was added at an injection rate of 0.2 mL / min. The solution was stirred again at 160 ° C for 3 h, and the color of the solution changed from white to gray. After the reaction, the AgNMs were diluted and centrifuged with acetone, and the supernatant was removed. After three times, the high-purity AgNMs were obtained and dispersed in an ethanol solution for storage.

[0016] Figure 1 In the figure, 1 is a prepared concave or convex aluminum sheet substrate, and above the substrate are a light-emitting layer 2 and a transparent top electrode 3 in sequence.

[0017] Luminescent layer. The luminescent powder ZnS:Mn is fully dried in an oven and filtered with a 300-mesh sieve. Take 50g of dry and uniform luminescent powder ZnS:Mn and put it into the fluidizing cup of the electrostatic sprayer. The voltage of the sprayer is set to 40V, and the spray rate is about 10mg / s. Take a concave substrate with a diameter of 4cm and spray it evenly for 1~2s. At this time, the luminescent powder is not firmly adhered to the aluminum substrate. Dilute the PB glue 10 times with a diluent and load it into the solution sprayer spray pot. Spray a layer of PB glue evenly on the surface of the luminescent powder, anneal and dry it at 120℃ for 1h to make the luminescent powder fully adhere to the aluminum substrate.

[0018] Spray the AgNMs top electrode on the light-emitting layer. Take 1 mL of AgNMs dispersion and add 10 mL of anhydrous ethanol to mix evenly. Put it into a 20 mL sprayer spray pot and spray it 4 to 5 times at medium speed. After each spraying, anneal and dry it at 120℃ for 30 minutes.

[0019] With the aluminum base as the positive electrode and the AgNMs layer as the negative electrode, a regulated DC current of 100V was applied, and the current instantly dropped from 35mA to 2mA. The concave electroluminescent device completed the formation process, the device lit up, the luminous color was yellow, and the luminous surface was uniform and stable. Figure 2 The following is a working diagram of the concave electroluminescent device when different voltages are applied. Figure 3 As shown in (A): the emission peak of the electroluminescence intensity (EL) of the light-emitting device is 580nm, and the EL intensity gradually increases with the increase of voltage. Figure 3 (B) The color of the EL light source indicated by the CIE chromaticity diagram.

Claims

1. The present invention proposes a preparation method for adsorbing a luminescent material on a concave or convex substrate surface by electrostatic spraying technology, and forming a uniform and stable converging or diverging spherical light source by direct current driving. The light-emitting device first prepares a concave or convex substrate and presses the substrate with a mold. After the substrate is processed, a luminescent layer and a top electrode layer are sprayed on the concave or convex substrate.

2. The converging or diverging spherical light source according to claim 1, characterized in that: The material of the concave or convex substrate can be selected from metals such as aluminum, copper, gold, nickel, silver or iron with good conductivity and ductility as the concave or convex bottom electrode. Glass, PET, ceramics and other materials with concave and convex shapes can also be used. Conductive materials are plated on the surface to make it conductive as a substrate. The processing method of the concave or convex substrate is to remove the surface oxide film by electrochemical polishing or physical grinding.

3. The converging or diverging spherical light source according to claim 1 or 2, characterized in that: The concave base forms a converging light source, which focuses the optical signal; the convex base forms a diverging light source, which diverges the optical signal.

4. The converging or diverging spherical light source according to claim 1 or 2, characterized in that: The concave or convex base can be prepared into concave or convex bottom electrodes of different sizes, and the light-emitting area of ​​the device will be of different sizes accordingly.

5. According to the converging or diverging spherical light source described in claims 1, 2, and 3, the light-emitting layer can use rare earth activators (Eu, Tb, Er) doped zinc sulfide luminescent powder, transition metals (Zn, Cu, Pb) doped zinc sulfide luminescent powder, and the top electrode uses transparent conductive electrodes such as polyacetylene, graphene, and AgNMs.

6. The converging or diverging spherical light source according to claim 1 or 4, characterized in that: The preparation process can adopt a variety of feasible methods. The light-emitting layer adopts a powder electrostatic spraying method, and the top electrode layer adopts a solution spin coating method or a solution spraying method.

7. The converging or diverging spherical light source according to claims 1, 4, and 5, characterized in that: The optimal number of spray layers for the light-emitting layer preparation method is 1 to 2 layers, and the optimal thickness is 20 μm to 30 μm. The optimal number of spray layers for the top electrode layer using the solution spraying method is 3 to 4 layers, and the optimal thickness is 5 to 7 μm.