Copper-clad plate and preparation method thereof, circuit board and electronic equipment
By using a fluororesin layer and a thermosetting resin layer in the copper clad plate and combining fiber cloth reinforcement materials, the problems of mechanical strength difference and layer deviation in the existing technology are solved, and the effects of high mechanical strength and low dielectric loss are achieved. In the preparation of multi-layer circuit boards.
Patent Information
- Application Number
- CN202310504607.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-06
- Publication Date
- 2024-11-08
AI Technical Summary
The existing copper clad plates have poor mechanical strength, large shrinkage and large layer due to the use of thermoplastic polytetrafluoroethylene resin, which limits their application in printed circuit board multi-layer boards.
Using a fluororesin layer and a thermosetting resin layer, the thermosetting resin layer includes a thermosetting resin matrix and a first reinforcing material, such as a fiber cloth, the dielectric layer is located between the fluororesin layer and the copper foil layer to enhance mechanical properties and reduce dielectric loss.
It improves the mechanical strength and structural reliability of copper clad plates, reduces layer bias defects, and is suitable for the preparation of multi-layer circuit boards, significantly improves yield and reduces costs.
Smart Images

Figure CN118921841A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of electronic technology, and in particular to a copper clad laminate and a preparation method thereof, a circuit board, and an electronic device. Background Art
[0002] Copper Clad Laminate (CCL), also known as copper clad laminate, is a substrate material for printed circuit boards (PCBs). It plays the role of interconnection, insulation and support for printed circuit boards, and also has a great influence on the transmission effect of signals in circuits.
[0003] At present, in order to reduce the dielectric constant and dielectric loss of copper clad laminates, polytetrafluoroethylene (PTFE) is usually used as a resin matrix. However, since PTFE resin is a thermoplastic resin, the prepared copper clad laminate has defects such as poor mechanical strength, large expansion and contraction, and large layer deviation, which limits its application in the preparation of PCB multilayer boards.
[0004] Public Content
[0005] In view of this, the present disclosure provides a copper clad laminate and a preparation method thereof, a circuit board, and an electronic device, which can solve the above-mentioned technical problems.
[0006] Specifically, the following technical solutions are included:
[0007] In one aspect, a copper-clad laminate is provided, comprising: a fluororesin layer and a copper-clad structural layer located on at least one surface of the fluororesin layer;
[0008] The copper-clad structural layer comprises a dielectric layer and a copper foil layer bonded to each other, and the dielectric layer is bonded to the fluororesin layer;
[0009] The medium layer includes a thermosetting resin layer, and the thermosetting resin layer includes a thermosetting resin matrix and a first reinforcing material located inside the thermosetting resin matrix.
[0010] The copper clad laminate provided by the embodiment of the present disclosure has both excellent dielectric constant and low dielectric loss by using the fluororesin layer as the resin base layer. The mechanical properties of the copper clad laminate are improved by making its dielectric layer include a thermosetting resin layer, and the thermosetting resin layer includes a thermosetting resin matrix and a first reinforcing material located inside the thermosetting resin matrix, and the first reinforcing material is conducive to enhancing the dimensional stability of the thermosetting resin matrix, thereby making the mechanical properties of the thermosetting resin layer more excellent. It can be seen that the embodiment of the present disclosure uses the thermosetting resin layer containing the first reinforcing material as the dielectric layer and makes it located between the fluororesin layer and the copper foil layer. On the premise of ensuring that the copper clad laminate has both excellent dielectric constant and low dielectric loss, it is also conducive to enhancing the mechanical strength of the copper clad laminate, improving its structural reliability, and at the same time curbing the expansion and contraction of the copper clad laminate, thereby reducing its layer deviation defects during PCB processing.
[0011] In some possible implementations, the first reinforcing material includes fiber cloth, including but not limited to at least one of glass fiber cloth and quartz fiber cloth.
[0012] In some possible implementations, the weight percentage of the thermosetting resin matrix is 50%-80%;
[0013] The weight percentage of the first reinforcing material is 20%-50%.
[0014] In some possible implementations, the raw material for preparing the thermosetting resin matrix includes a thermosetting resin, and the thermosetting resin includes at least one of a polyolefin resin and a hydrocarbon resin.
[0015] In some possible implementations, the raw materials for preparing the thermosetting resin matrix further include a first inorganic filler for reinforcement.
[0016] In some possible implementations, the first inorganic filler for reinforcement includes a ceramic filler.
[0017] Some suitable ceramic fillers include, but are not limited to, at least one of silicon dioxide, titanium dioxide, aluminum oxide, aluminum nitride, boron nitride, barium titanate, strontium titanate, magnesium titanate, and calcium titanate.
[0018] In some possible implementations, the dielectric layer further includes a low dielectric resin layer, and the low dielectric resin layer is located between the thermosetting resin layer and the copper foil layer. By further adding a low dielectric resin layer to the dielectric layer, the electrical performance of the copper clad laminate can be further improved and its dielectric loss can be reduced.
[0019] In some possible implementations, the low dielectric resin layer includes at least one of polytetrafluoroethylene resin, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, and fluorinated ethylene propylene copolymer.
[0020] In some possible implementations, the fluororesin layer includes a fluororesin matrix, and a raw material for preparing the fluororesin matrix includes at least one of polytetrafluoroethylene resin and tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer.
[0021] In some possible implementations, the raw materials for preparing the fluororesin matrix further include a second inorganic filler for reinforcement.
[0022] In some possible implementations, the second inorganic filler for reinforcement includes a ceramic filler.
[0023] Some suitable ceramic fillers include, but are not limited to, at least one of silicon dioxide, titanium dioxide, aluminum oxide, aluminum nitride, boron nitride, barium titanate, strontium titanate, magnesium titanate, and calcium titanate.
[0024] In some possible implementations, the fluororesin layer further includes a second reinforcing material located inside the fluororesin.
[0025] In some possible implementations, the second reinforcing material includes fiber cloth, including but not limited to at least one of glass fiber cloth and quartz fiber cloth. Each of the above fiber cloths can effectively enhance the dimensional stability of the fluororesin layer.
[0026] On the other hand, a circuit board is provided, comprising at least one layer of the copper clad board as described above.
[0027] The copper clad laminate involved in the embodiment of the present disclosure has the advantages of low dielectric loss, high mechanical strength, low thermal expansion coefficient, etc. When it is used to prepare a circuit board, a multi-layer structure circuit board can be prepared, which significantly improves its yield and reduces costs.
[0028] On the other hand, an electronic device is provided, and the electronic device includes the above-mentioned circuit board.
[0029] The electronic device provided by the embodiment of the present disclosure has all the advantages of the copper clad laminate and circuit board of the embodiment of the present disclosure. Since the circuit board of the embodiment of the present disclosure has low dielectric loss, high structural reliability, and high electrical load-bearing density, the electrical performance of the electronic device is significantly improved.
[0030] In another aspect, a method for preparing a copper clad laminate is provided, wherein the copper clad laminate is as described above, and the method for preparing the copper clad laminate comprises:
[0031] Provide fluororesin film, dielectric film and copper foil with surface activation treatment respectively;
[0032] According to the structure of the copper-clad laminate, the fluororesin film, the dielectric film and the copper foil treated with surface activation are laminated to obtain a laminated intermediate;
[0033] The laminated intermediate is subjected to a pressing process, so that the fluororesin film is cured to form a fluororesin layer and the dielectric film is cured to form a dielectric layer, thereby obtaining the copper clad laminate.
[0034] In some possible implementations, the dielectric layer is a thermosetting resin layer;
[0035] Providing the dielectric film comprises:
[0036] Using the raw materials for preparing the thermosetting resin matrix, obtaining a thermosetting resin liquid composition;
[0037] The thermosetting resin liquid composition is combined with the first reinforcing material and dried to obtain a thermosetting resin semi-cured film as the dielectric film.
[0038] In some possible implementations, the dielectric layer includes a thermosetting resin layer and a low dielectric resin layer bonded to each other;
[0039] Providing the dielectric film includes: providing a thermosetting resin semi-cured film and a low dielectric resin film respectively and both of them serve as the dielectric film;
[0040] Providing the semi-cured film of thermosetting resin comprises:
[0041] Obtaining a thermosetting resin liquid composition according to the raw materials for preparing the thermosetting resin matrix;
[0042] The thermosetting resin liquid composition is combined with the first reinforcing material and dried to obtain the thermosetting resin semi-cured film.
[0043] In some possible implementations, the fluororesin layer includes a fluororesin matrix;
[0044] Providing the fluororesin film comprises:
[0045] Providing raw materials for preparing fluororesin matrix in dry powder form;
[0046] By means of a dry film-making process, a fluororesin green film is prepared using the fluororesin matrix preparation raw material in dry powder form;
[0047] The fluororesin raw film is subjected to a aging treatment under the protection of the protective plate, and the protective plate is removed to obtain the fluororesin film.
[0048] In some possible implementations, the fluororesin layer includes a fluororesin matrix and a second reinforcing material located inside the fluororesin matrix;
[0049] Providing the fluororesin film comprises:
[0050] Using the raw materials for preparing the fluororesin matrix, a fluororesin emulsion is obtained;
[0051] Combining the fluororesin emulsion with the second reinforcing material, and subjecting the mixture to drying treatment to obtain a fluororesin green film;
[0052] The fluororesin raw film is subjected to a aging treatment under the protection of the protective plate, and the protective plate is removed to obtain the fluororesin film. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] Figure 1 A schematic structural diagram of an exemplary copper clad laminate provided in an embodiment of the present disclosure;
[0054] Figure 2 A schematic structural diagram of another exemplary copper clad laminate provided in an embodiment of the present disclosure;
[0055] Figure 3 A schematic structural diagram of another exemplary copper clad laminate provided in an embodiment of the present disclosure;
[0056] Figure 4 A schematic structural diagram of another exemplary copper clad laminate provided in an embodiment of the present disclosure;
[0057] Figure 5 A schematic diagram of the structure of an exemplary three-layer circuit board provided in an embodiment of the present disclosure.
[0058] The reference numerals represent:
[0059] 1. Fluororesin layer; 2. Thermosetting resin layer; 3. Copper foil layer; 4. Low dielectric resin layer;
[0060] 1001, first core board layer; 1002, second core board layer; 200, bonding layer. DETAILED DESCRIPTION
[0061] In order to make the technical solutions and advantages of the present disclosure more clear, the embodiments of the present disclosure will be further described in detail below with reference to the accompanying drawings.
[0062] Today, with the rapid development of information technology, higher and higher requirements are placed on the information carrying, processing and transmission capabilities of electronic products. At the same time, higher requirements are also placed on the lightweight and small size of electronic products, which leads to a corresponding increase in the wiring density of printed circuit boards in electronic products.
[0063] As the substrate material of the printed circuit board, the copper clad laminate plays the role of interconnection, insulation and support for the printed circuit board, and also has a great influence on the transmission effect of the signal in the circuit. On the one hand, it is expected that the dielectric constant (Dielectronic Constant, Dk) of the copper clad laminate is low to improve its signal transmission capability. On the other hand, it is expected that the dielectric loss (Dielectronic Fonstant, Df) of the copper clad laminate is low to maintain the integrity of the signal and thus improve the transmission efficiency.
[0064] Polytetrafluoroethylene (PTFE) resin has excellent dielectric constant and low dielectric loss. Using polytetrafluoroethylene (PTFE) as a resin matrix to prepare a copper clad laminate is beneficial to reducing the dielectric constant and dielectric loss of the copper clad laminate.
[0065] However, since PTFE resin is a thermoplastic resin, the prepared copper clad laminate has defects such as poor mechanical strength, large expansion and contraction, and large layer deviation, which in turn affects the high-density development of printed circuit boards and also limits the application of copper clad laminates in the preparation of PCB multilayer boards.
[0066] On the one hand, an embodiment of the present disclosure provides a copper-clad laminate, which includes: a fluororesin layer and a copper-clad structural layer located on at least one surface of the fluororesin layer. The copper-clad structural layer includes a dielectric layer and a copper foil layer bonded to each other, and the dielectric layer is bonded to the fluororesin. Among them, the dielectric layer includes a thermosetting resin layer, and the thermosetting resin layer includes a thermosetting resin matrix and a first reinforcing material located inside the thermosetting resin matrix.
[0067] The copper clad laminate provided by the embodiment of the present disclosure has both excellent dielectric constant and low dielectric loss by using the fluororesin layer as the resin base layer. The mechanical properties of the copper clad laminate are improved by making its dielectric layer include a thermosetting resin layer, and the thermosetting resin layer includes a thermosetting resin matrix and a first reinforcing material located inside the thermosetting resin matrix, and the first reinforcing material is conducive to enhancing the dimensional stability of the thermosetting resin matrix, thereby making the mechanical properties of the thermosetting resin layer more excellent. It can be seen that the embodiment of the present disclosure uses the thermosetting resin layer containing the first reinforcing material as the dielectric layer and makes it located between the fluororesin layer and the copper foil layer. On the premise of ensuring that the copper clad laminate has both excellent dielectric constant and low dielectric loss, it is also conducive to enhancing the mechanical strength of the copper clad laminate, improving its structural reliability, and at the same time curbing the expansion and contraction of the copper clad laminate, thereby reducing its layer deviation defects during PCB processing.
[0068] In the disclosed embodiment, the first reinforcing material is embedded in the thermosetting resin matrix, that is, the first reinforcing material is not exposed on the surface of the thermosetting resin layer. The thermosetting resin layer is in contact with the fluororesin layer based on its thermosetting resin matrix, and the first reinforcing material does not directly contact the fluororesin layer.
[0069] In some examples, the first reinforcing material includes but is not limited to fiber cloth, wherein the fiber cloth can be embedded in the thermosetting resin matrix in a single layer or in multiple layers. For example, two, three, four or more layers of fiber cloth can be stacked in sequence and embedded as a whole in the thermosetting resin.
[0070] Some fiber cloths suitable for the first reinforcing material include but are not limited to at least one of glass fiber cloth and quartz fiber cloth, each of which can effectively enhance the dimensional stability of the thermosetting resin layer. Currently known types of glass fiber cloth and quartz fiber cloth can be applied to this application.
[0071] For the thermosetting resin layer, the weight percentage of the thermosetting resin matrix is 50%-80%, and the weight percentage of the first reinforcing material is the balance, which is 20%-50% accordingly. For example, the weight percentage of the first reinforcing material in the thermosetting resin layer includes but is not limited to 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 35%, 40%, 45%, 50%, etc.
[0072] The first reinforcing material is proportioned in the thermosetting resin layer as above, so as to achieve a good reinforcing effect without affecting the basic properties of the thermosetting resin matrix.
[0073] In the disclosed embodiments, it is desirable to use a thermosetting resin having a low dielectric constant and dielectric loss. For example, the dielectric loss factor Df of the thermosetting resin is less than 0.002. In this way, while effectively improving the mechanical strength of the copper clad laminate, the adverse effects on the dielectric properties of the copper clad laminate can be reduced.
[0074] In some examples, the raw materials for preparing the thermosetting resin matrix involved in the embodiments of the present disclosure include at least one of polyolefin resin and hydrocarbon resin.
[0075] Taking polyolefin resin as an example, the polymerizable monomers for synthesizing the polyolefin resin include but are not limited to at least one of butadiene, isoprene, styrene, divinylbenzene, benzocyclobutene and its derivatives, and pentadiene.
[0076] For example, some polyolefin resins include, but are not limited to, at least one of styrene-divinylbenzene copolymer, styrene-butadiene copolymer, unsaturated polybutadiene, and polyisoprene.
[0077] By using polyolefin resin and / or hydrocarbon resin to form a thermosetting resin layer, not only the thermosetting resin layer has good mechanical properties and low dielectric loss, but also the bonding force between the polyolefin resin and / or hydrocarbon resin and the copper foil layer is stronger than that of fluororesin, all of which are beneficial to improving the structural reliability of the copper clad laminate and reducing the dielectric loss of the copper clad laminate.
[0078] In some implementations, the raw material for preparing the thermosetting resin matrix further includes a first inorganic filler for reinforcement, that is, the raw material for preparing the thermosetting resin matrix includes a thermosetting resin and a first inorganic filler for reinforcement.
[0079] The first inorganic filler used for reinforcement is in the form of powder, and its size can be nanometer, micrometer or micro-nanometer. The first inorganic filler used for reinforcement further enhances the mechanical properties of the thermosetting resin matrix.
[0080] Exemplarily, the first inorganic filler for reinforcement includes but is not limited to ceramic fillers. Some suitable ceramic fillers include but are not limited to at least one of silicon dioxide, titanium dioxide, aluminum oxide, aluminum nitride, boron nitride, barium titanate, strontium titanate, magnesium titanate, and calcium titanate.
[0081] By using the above ceramic filler as a reinforcing filler for a thermosetting resin matrix, its mechanical properties and reliability can be further improved and its thermal expansion coefficient can be reduced.
[0082] In some examples, the raw materials for preparing the thermosetting resin matrix include the following components in percentage by mass: 50%-79% thermosetting resin, 20%-48% first inorganic filler for reinforcement, and 0.2%-2% first additive.
[0083] The mass percentage of thermosetting resin therein includes but is not limited to: 50%, 52%, 55%, 58%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79% and the like.
[0084] The mass percentage of the first inorganic filler for reinforcement includes but is not limited to: 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, etc.
[0085] The mass percentage of the first additive therein includes but is not limited to: 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, etc.
[0086] The first additive may include at least one of an initiator, a coupling agent, and a dispersant, which may be arbitrarily selected according to actual performance requirements of the thermosetting resin layer.
[0087] For example, the initiator includes but is not limited to at least one of α,α'-di(tert-butylperoxym-isopropyl)benzene, diisopropylbenzene peroxide, tert-butylperoxyisopropylbenzene, 1,1-bis(tert-hexylperoxide)-3,3,5-trimethylcyclohexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)-3-hexyne, tert-butyl peroxyoctanoate, and tert-butyl peroxybenzoate. The coupling agent includes but is not limited to at least one of a silane coupling agent, a borate coupling agent, and a titanate coupling agent. The dispersant can be used to uniformly disperse the first inorganic filler used for reinforcement in the thermosetting resin.
[0088] In some implementations, the dielectric layer of the copper clad laminate provided by the embodiments of the present disclosure further includes a low dielectric resin layer, and the low dielectric resin layer is located between the thermosetting resin layer and the copper foil layer. That is, one side surface of the thermosetting resin layer is bonded to the fluororesin layer, and the other side surface is bonded to one side surface of the low dielectric resin layer, and the other side surface of the low dielectric resin layer is bonded to the copper foil layer.
[0089] In the embodiment of the present disclosure, the dielectric constant Dk of the low dielectric resin used in the low dielectric resin layer may be less than 3, and the low dielectric resin may be a thermosetting resin or a thermoplastic resin.
[0090] Since the resin used in the low dielectric resin layer has better dielectric properties than the resin used in the thermosetting resin layer, by further adding a low dielectric resin layer to the dielectric layer, the electrical properties of the copper clad laminate can be further improved and its dielectric loss can be reduced.
[0091] In some examples, some suitable raw materials for preparing the low dielectric resin layer include at least one of polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), and fluorinated ethylene propylene (FEP).
[0092] The fluororesin layer may be a single-layer structure or a multi-layer structure. For example, a multi-layer structure of the fluororesin layer may be obtained by stacking layers formed by different types of fluororesins.
[0093] In some implementations, the fluororesin layer involved in the embodiments of the present disclosure includes a fluororesin matrix, the raw materials for preparing the fluororesin matrix include fluororesin, and the fluororesin includes at least one of polytetrafluoroethylene resin (PTFE) and tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer.
[0094] For example, the material of the fluororesin layer is polytetrafluoroethylene resin, and the material of the low dielectric resin layer is tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer or fluorinated ethylene propylene copolymer.
[0095] In some examples, the raw materials for preparing the fluororesin matrix also include a second inorganic filler for reinforcement, and the second inorganic filler for reinforcement is in the form of powder, and its size can be nanometer, micrometer or micro-nanometer. The second inorganic filler for reinforcement further enhances the dimensional stability of the fluororesin layer, thereby improving the structural reliability of the copper clad laminate.
[0096] Exemplarily, the second inorganic filler used for reinforcement includes but is not limited to ceramic fillers. Some suitable ceramic fillers include but are not limited to at least one of silicon dioxide, titanium dioxide, aluminum oxide, aluminum nitride, boron nitride, barium titanate, strontium titanate, magnesium titanate, and calcium titanate.
[0097] By using the above-mentioned ceramic filler as a reinforcing filler for the fluororesin layer, its mechanical properties and reliability can be further improved and its thermal expansion coefficient can be reduced.
[0098] In some examples, the raw material for preparing the fluororesin matrix is in the form of dry powder, which includes the following components in percentage by mass: 30%-50% fluororesin, 50%-70% second inorganic filler for reinforcement. By the above proportions, the fluororesin layer prepared by the dry method is ensured to have excellent mechanical strength.
[0099] For example, the mass percentage of the second inorganic filler used for reinforcement includes but is not limited to: 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, etc.
[0100] The mass percentage of fluororesin therein includes but is not limited to: 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, etc.
[0101] In some examples, the raw material for preparing the fluororesin matrix is in the form of an emulsion, which includes the following components in percentage by mass: 45%-70% fluororesin, 25%-45% second inorganic filler for reinforcement, and 5%-20% second additive, wherein the second additive includes at least an emulsifier, and further, the second additive may also include a surfactant, a dispersion stabilizer, and the like.
[0102] For example, the mass percentage of fluororesin therein includes but is not limited to: 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, etc.
[0103] The mass percentage of the second inorganic filler used for reinforcement includes but is not limited to: 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, etc.
[0104] The mass percentage of the second additive therein includes but is not limited to: 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, etc.
[0105] The second additive includes at least an emulsifier, which is used to form a stable emulsion of the fluororesin in the aqueous solution to facilitate stable film formation. Exemplarily, the emulsifier can be a fluorine-containing surfactant, which includes but is not limited to ammonium perfluorooctanoate, w-hydroperfluoroheptanoic acid or w-hydroperfluorononanoic acid potassium, etc. The dispersion stabilizer can be liquid paraffin, fluorochloro oil, etc.
[0106] In some implementations, the fluororesin layer according to the embodiments of the present disclosure includes a fluororesin matrix and a second reinforcing material located inside the fluororesin.
[0107] The second reinforcing material is embedded in the fluororesin matrix. The fluororesin layer is in contact with the thermosetting resin layer based on the fluororesin matrix, and the second reinforcing material does not directly contact the thermosetting resin layer.
[0108] In some examples, the second reinforcing material includes but is not limited to fiber cloth, wherein the fiber cloth can be embedded in the fluororesin matrix in a single layer or in multiple layers. For example, two, three, four or more layers of fiber cloth can be stacked in sequence and embedded as a whole in the fluororesin.
[0109] Some fiber cloths suitable for the second reinforcing material include but are not limited to at least one of glass fiber cloth and quartz fiber cloth. Each of the above fiber cloths can effectively enhance the dimensional stability of the fluororesin layer.
[0110] For the fluororesin layer, the weight percentage of the fluororesin matrix is 50%-80%, and the weight percentage of the second reinforcing material is the balance, which is 20%-50% accordingly. For example, the weight percentage of the second reinforcing material in the fluororesin layer includes but is not limited to 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 35%, 40%, 45%, 50%, etc.
[0111] The second reinforcing material is proportioned in the fluororesin layer as above, so as to achieve a good reinforcing effect without affecting the dielectric properties of the fluororesin matrix.
[0112] The copper clad laminate provided in the embodiment of the present disclosure may be a double-sided copper clad laminate, wherein the copper clad structural layer is two layers, and the two copper clad structural layers are symmetrically attached to two opposite surfaces of the fluororesin layer.
[0113] In combination with the above description of the structure and composition of the copper clad laminate, the structures of various types of copper clad laminates provided in the embodiments of the present disclosure are described exemplarily:
[0114] As an example, the attached Figure 1 As shown, the copper clad laminate provided by the embodiment of the present disclosure includes a fluororesin layer 1, a copper clad structural layer symmetrically adhered to two opposite surfaces of the fluororesin layer 1, the copper clad structural layer includes a thermosetting resin layer 2 and a copper foil layer 3, the thermosetting resin layer 2 is adhered to the surface of the fluororesin layer 1, and the copper foil layer 3 is adhered to the surface of the thermosetting resin layer 2 facing away from the fluororesin layer 1.
[0115] Among them, the fluororesin layer 1 includes a fluororesin matrix, the raw materials for preparing the fluororesin matrix include fluororesin and a second inorganic filler for reinforcement, and the thermosetting resin layer 2 includes a thermosetting resin matrix and a first reinforcing material located inside the thermosetting resin matrix, and the raw materials for preparing the thermosetting resin matrix include a thermosetting resin and a first inorganic filler for reinforcement.
[0116] As another example, Figure 2As shown, the copper clad laminate provided by the embodiment of the present disclosure includes a fluororesin layer 1, a copper clad structural layer symmetrically adhered to two opposite surfaces of the fluororesin layer 1, the copper clad structural layer includes a thermosetting resin layer 2 and a copper foil layer 3, the thermosetting resin layer 2 is adhered to the surface of the fluororesin layer 1, and the copper foil layer 3 is adhered to the surface of the thermosetting resin layer 2 facing away from the fluororesin layer 1.
[0117] The fluororesin layer 1 includes a fluororesin matrix and a second reinforcing material located inside the fluororesin matrix, and the raw materials for preparing the fluororesin matrix include fluororesin and a second inorganic filler for reinforcement. And the thermosetting resin layer 2 includes a thermosetting resin matrix and a first reinforcing material located inside the thermosetting resin matrix, and the raw materials for preparing the thermosetting resin matrix include a thermosetting resin and a first inorganic filler for reinforcement.
[0118] As another example, Figure 3 As shown, the copper clad laminate provided by the embodiment of the present disclosure includes a fluororesin layer 1, a copper clad structural layer symmetrically attached to two opposite surfaces of the fluororesin layer 1, the copper clad structural layer includes a thermosetting resin layer 2, a low dielectric resin layer 4 and a copper foil layer 3, the thermosetting resin layer 2 is attached to the surface of the fluororesin layer 1, the low dielectric resin layer 4 is attached to the surface of the thermosetting resin layer 2 facing away from the fluororesin layer 1, and the copper foil layer 3 is attached to the surface of the low dielectric resin layer 4 facing away from the thermosetting resin layer 2.
[0119] Among them, the fluororesin layer 1 includes a fluororesin matrix, the raw materials for preparing the fluororesin matrix include fluororesin and a second inorganic filler for reinforcement, and the thermosetting resin layer 2 includes a thermosetting resin matrix and a first reinforcing material located inside the thermosetting resin matrix, and the raw materials for preparing the thermosetting resin matrix include a thermosetting resin and a first inorganic filler for reinforcement.
[0120] As another example, Figure 4 As shown, the copper clad laminate provided by the embodiment of the present disclosure includes a fluororesin layer 1, a copper clad structural layer symmetrically attached to two opposite surfaces of the fluororesin layer 1, the copper clad structural layer includes a thermosetting resin layer 2, a low dielectric resin layer 4 and a copper foil layer 3, the thermosetting resin layer 2 is attached to the surface of the fluororesin layer 1, the low dielectric resin layer 4 is attached to the surface of the thermosetting resin layer 2 facing away from the fluororesin layer 1, and the copper foil layer 3 is attached to the surface of the low dielectric resin layer 4 facing away from the thermosetting resin layer 2.
[0121] The fluororesin layer 1 includes a fluororesin matrix and a second reinforcing material located inside the fluororesin matrix, and the raw materials for preparing the fluororesin matrix include fluororesin and a second inorganic filler for reinforcement. And the thermosetting resin layer 2 includes a thermosetting resin matrix and a first reinforcing material located inside the thermosetting resin matrix, and the raw materials for preparing the thermosetting resin matrix include a thermosetting resin and a first inorganic filler for reinforcement.
[0122] For the copper clad laminate involved in the embodiment of the present disclosure, the thickness of the fluororesin layer can be greater than the thickness of the thermosetting resin layer to ensure that the copper clad laminate always maintains a low dielectric loss. The thickness of each layer involved in the copper clad laminate includes but is not limited to the following:
[0123] For the fluororesin layer, its thickness can be at least half of the total thickness of the copper clad laminate. For example, the thickness of the fluororesin layer can be 20μm-100μm, and further can be 55μm-95μm, which includes but is not limited to: 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, 55μm, 60μm, 62μm, 65μm, 68μm, 70μm, 73μm, 75μm, 77μm, 80μm, 82μm, 85μm, 87μm, 90μm, 93μm, 95μm, 100μm, etc.
[0124] For the copper foil layer, the thickness thereof may be 10 μm-40 μm, including but not limited to: 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm and the like.
[0125] For the thermosetting resin layer, its thickness can be 5μm-50μm, and further can be 25um-50um, which includes but is not limited to: 5μm, 10μm, 15μm, 20μm, 25μm, 26μm, 27μm, 28μm, 29μm, 30μm, 33μm, 35μm, 38μm, 40μm, 42μm, 44μm, 45μm, 46μm, 48μm, 50μm, etc.
[0126] For the low dielectric resin layer, its thickness can be 5μm-20μm, and further can be 8um-15um, which includes but is not limited to: 8um, 9um, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 17μm, 20μm, etc.
[0127] In summary, the copper clad laminate involved in the embodiment of the present disclosure has the advantages of low dielectric loss, high mechanical strength, low thermal expansion coefficient, etc. After testing, the copper clad laminate provided by the embodiment of the present disclosure can achieve a thermal expansion coefficient substantially equivalent to that of the conventional copper clad laminate on sale. This type of copper clad laminate can be used to prepare a multilayer circuit board using a process similar to the preparation process of the FR4 copper clad laminate, which can not only prepare a multilayer structure circuit board with a smaller layer deviation, but also significantly improve its yield, reducing the difficulty and cost of preparation.
[0128] On the other hand, an embodiment of the present disclosure further provides a circuit board, which includes at least one layer of any copper-clad board as described above.
[0129] The circuit board provided by the embodiment of the present disclosure has all the advantages of the copper-clad laminate of the embodiment of the present disclosure. The copper-clad laminate involved in the embodiment of the present disclosure has the advantages of low dielectric loss, high mechanical strength, low thermal expansion coefficient, etc. When it is used to prepare a circuit board, a multi-layer structure circuit board can be prepared, which significantly improves its yield and reduces costs.
[0130] The circuit board provided in the embodiment of the present disclosure can be prepared as a flexible circuit board (for example, the thickness of the thermosetting resin layer or the thickness of the fluororesin layer is reduced to a set value), or it can be prepared as a rigid circuit board.
[0131] When a circuit board is prepared using any of the copper clad laminates provided in the embodiments of the present disclosure, the circuit board can be in the form of a printed circuit board, wherein the copper clad laminate needs to undergo etching, hole opening and other processes to form wiring lines.
[0132] The circuit board provided in the embodiment of the present disclosure may be a single-layer circuit board formed by a single copper-clad laminate, or may be a multi-layer board formed by stacking a plurality of copper-clad laminates in sequence. For example, the number of layers of the circuit board may be three, four, five, six or more layers.
[0133] Figure 5 An example of a three-layer circuit board is provided, which includes a first core board layer 1001, an adhesive layer 200, and a second core board layer 1002 that are bonded in sequence, wherein the first core board layer 1001 and the second core board layer 1002 are both prepared using the copper clad laminate provided by the embodiment of the present disclosure. The adhesive layer 200 is used to bond the first core board layer 1001 and the second core board layer 1002, one side surface of the adhesive layer 200 is bonded to the copper foil layer of the first core board layer 1001, and the other side surface of the adhesive layer 200 is bonded to the copper foil layer of the second core board layer 1002.
[0134] When preparing a multi-layer circuit board, a bonding layer 200 can be laminated on the copper foil layer of the first core board layer 1001 , and another bonding layer 200 can be laminated on the copper foil layer of the second core board layer 1002 , and then the two bonding layers 200 are bonded to form an integral bonding layer 200 .
[0135] Figure 5 In the three-layer circuit board shown, the dielectric layers of the first core layer 1001 and the second core layer 1002 may be thermosetting resin layers, or the dielectric layers may include thermosetting resin layers and low dielectric resin layers.
[0136] In some examples, the bonding layer 200 may be prepared by using a thermosetting resin. In some examples, the thermosetting resin used in the bonding layer may be the above-mentioned polyolefin resin.
[0137] On the other hand, an embodiment of the present disclosure further provides an electronic device, which includes the above-mentioned circuit board.
[0138] Circuit boards are used to realize electrical interconnection and transmission of electronic components in electronic devices to meet the electrical characteristics required by electronic devices. The electronic device provided by the embodiment of the present disclosure has all the advantages of the copper clad laminate and circuit board of the embodiment of the present disclosure. Since the circuit board of the embodiment of the present disclosure has low dielectric loss, high structural reliability, and high electrical load density, the electrical performance of the electronic device can be significantly improved.
[0139] Illustratively, the electronic devices involved in the embodiments of the present disclosure include, but are not limited to: mobile phones, computers, tablet computers, laptop computers, servers, routers, switches, etc.
[0140] In another aspect, the present disclosure also provides a method for preparing a copper clad laminate, the copper clad laminate being as described above. The method for preparing the copper clad laminate comprises:
[0141] Step S1, respectively providing a fluororesin film, a dielectric film and a copper foil subjected to surface activation treatment.
[0142] Step S2: According to the structure of the copper-clad laminate, the fluororesin film, the dielectric film and the copper foil with surface activation treatment are laminated to obtain a laminated intermediate.
[0143] Step S3, pressing the laminated intermediate so that the fluororesin film is solidified to form a fluororesin layer and the dielectric film is solidified to form a dielectric layer, thereby obtaining a copper clad laminate.
[0144] The method for preparing a copper clad laminate provided in an embodiment of the present disclosure first provides a fluororesin film, a dielectric film and a copper foil treated with surface activation, then overlaps the fluororesin film, the dielectric film and the copper foil treated with surface activation in a certain order, and then performs a pressing process to solidify the resin, thereby preparing a copper clad laminate.
[0145] The disclosed embodiment activates the surface of the copper foil to enhance the bonding force between the copper foil layer and the dielectric layer. In some examples, the surface activation treatment of the copper foil includes: using a coupling agent to perform surface treatment on the low-roughness copper foil to obtain a surface-activated copper foil.
[0146] Some applicable coupling agents include but are not limited to: methoxysilane coupling agent, phenoxysilane coupling agent, divinylsilane coupling agent, etc. The above coupling agents can be used to modify the surface of the copper foil and improve the interface performance between the copper foil and the resin layer in contact.
[0147] For the low-roughness copper foil mentioned above, the surface roughness Rz of the copper foil may be less than or equal to 1.5 um, including but not limited to less than or equal to 1.4 um, 1.3 um, 1.2 um, 1.1 um, 1.0 um, etc.
[0148] According to the specific structure of the copper clad laminate, some implementation methods of the above-mentioned preparation steps are described exemplarily:
[0149] (1) Regarding providing a fluororesin film, this includes but is not limited to the following two implementations:
[0150] (1.1) The fluororesin layer includes a fluororesin matrix, and providing the fluororesin film includes the following steps:
[0151] Step 1.1.1, providing raw materials for preparing a fluororesin matrix in dry powder form.
[0152] Step 1.1.2: Prepare a fluororesin green film by dry film-making process using fluororesin as a raw material for preparing a fluororesin matrix in dry powder form.
[0153] Step 1.1.3: Under the protection of the protective plate, the fluororesin raw film is aged, and the protective plate is removed to obtain the fluororesin film.
[0154] Related technology When preparing copper clad laminates based on PTFE material, a fluororesin emulsion impregnation process is usually used to integrally form a fluororesin layer on the copper clad laminate. Small molecule additives such as emulsifiers and surfactants need to be added during the impregnation process. They are difficult to remove during the curing process of the fluororesin, which leads to high dielectric loss of the copper clad laminate.
[0155] The disclosed embodiment utilizes a dry film-making process to prepare a fluororesin raw film (for example, by casting and extruding the fluororesin raw film), and further matures it to obtain a fluororesin film, without adding additional small molecule additives thereto, so that the raw materials of the fluororesin layer are pure, thereby controlling the dielectric loss of the copper clad laminate to a low level.
[0156] In some examples, for step 1.1.1, the raw materials for preparing the fluororesin matrix in dry powder form include the following components in percentage by mass: 30%-50% fluororesin, 50%-70% second inorganic filler for reinforcement. The composition of the fluororesin and the second inorganic filler for reinforcement is as described above and will not be repeated here.
[0157] In some examples, for step 1.1.2, a fluororesin raw film is prepared by a dry film-making process using a fluororesin matrix preparation raw material in dry powder form, including: performing cast extrusion on the fluororesin matrix preparation raw material in dry powder form through calendering rolling and uniaxial / biaxial stretching process to obtain a fluororesin raw film.
[0158] In some examples, for step 1.1.3, the fluororesin raw film is cured under the protection of the protective sheet, and then the protective sheet is removed to obtain the fluororesin film, including: using two sets of protective sheets to attach to both sides of the fluororesin raw film respectively, and then placing the whole in a curing device for hot pressing and curing. The protective sheet is removed, and the obtained fluororesin film is cleaned and set aside.
[0159] The protective sheet is used to protect the fluororesin green film during the curing process, thereby preventing the fluororesin from adhering to the curing equipment during the high-temperature curing process.
[0160] Some suitable protective plates include, but are not limited to, metal plates such as copper plates, silver plates, aluminum plates or aluminum alloy plates.
[0161] The protective plate can be removed in a variety of ways, as long as the removal method does not adversely affect the cured fluororesin film. For example, the protective plate can be etched away using an etching solution, so that the fluororesin layer can be completely retained.
[0162] In some examples, the protective sheet is subjected to surface activation treatment to have organic activation groups on its surface. Thus, the protective sheet with organic activation groups is attached to both sides of the fluororesin green film, the fluororesin green film is aged and the protective sheet is removed to obtain a fluororesin film with organic activation groups on its surface.
[0163] Through the above arrangement, the organic activated groups on the protective plate are transferred to the cured fluororesin film. The fluororesin film is based on the organic activated groups, thereby effectively improving the bonding force between the fluororesin film and the thermosetting resin layer to obtain a stable bonding interface.
[0164] For example, performing surface activation treatment on the protective plate includes performing fluorination treatment on the protective plate, that is, the organic activation group is a fluorine-containing group.
[0165] After removing the protective plate, the aged fluororesin film may be cleaned, for example, by using deionized water to ensure that the surface of the fluororesin film is clean and free of impurities.
[0166] (1.2) The fluororesin layer includes a fluororesin matrix and a second reinforcing material located inside the fluororesin matrix. Then, providing the fluororesin film includes the following steps:
[0167] Step 1.2.1, using the raw materials for preparing the fluororesin matrix, obtain the fluororesin emulsion.
[0168] Step 1.2.2, combining the fluororesin emulsion with the second reinforcing material, and drying the mixture to obtain a fluororesin raw film.
[0169] Step 1.2.3: Under the protection of the protective plate, the fluororesin raw film is aged, and then the protective plate is removed to obtain the fluororesin film.
[0170] For step 1.2.1, the raw material for preparing the fluororesin matrix is in the form of an emulsion, which includes the following components in percentage by mass: 45%-70% fluororesin, 25%-45% second inorganic filler for reinforcement, and 5%-20% second additive, wherein the second additive includes at least an emulsifier, and further, the second additive may also include a surfactant, a dispersion stabilizer, and the like.
[0171] When the above components are used to obtain the fluororesin emulsion, water is also needed as a solvent to dissolve and disperse the raw materials for preparing the fluororesin matrix to form an emulsion. Of course, water will be effectively removed from the resin system during the subsequent drying process.
[0172] The raw materials for preparing the fluororesin matrix and water are stirred (for example, stirred in a high-speed stirrer) until they are uniform, thereby obtaining a fluororesin emulsion with a uniform texture.
[0173] For step 1.2.2, the fluororesin emulsion can be impregnated and filled with the second reinforcing material in the form of fiber cloth through an impregnation process, thereby combining the fluororesin emulsion with the second reinforcing material.
[0174] The process of impregnating fiber cloth with resin is common in the art, and the embodiments of the present disclosure are not described in detail here. For example, in the embodiments of the present disclosure, a fluororesin emulsion is placed in a dipping tank of a gluing machine, and the second reinforcing material is passed through the dipping tank of the gluing machine for resin impregnation, and the thickness of the fluororesin liquid film is controlled by a scraping roller to obtain a fluororesin liquid film of a certain thickness, and after drying, a fluororesin raw film is obtained.
[0175] The fluororesin liquid film can be baked, and the baking treatment includes a drying section and a sintering section performed in sequence. The drying temperature corresponding to the drying section can volatilize and remove volatile additives such as water contained therein. For example, the drying temperature can be 100°C-150°C, including but not limited to: 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, etc. The sintering temperature corresponding to the sintering section can meet the sintering molding of the PTFE emulsion. For example, the sintering temperature can be 300°C-380°C, including but not limited to: 300°C, 310°C, 320°C, 330°C, 340°C, 350°C, 360°C, 370°C, 380°C, etc.
[0176] For step 1.2.3, the fluororesin raw film is cured under the protection of the protective sheet, and then the protective sheet is removed to obtain the fluororesin film, which may include: using two sets of protective sheets to attach to both sides of the fluororesin raw film respectively, and then placing the whole in a curing device for hot pressing and curing. The protective sheet is removed, and the obtained fluororesin film is cleaned and set aside.
[0177] The protective sheet is used to protect the fluororesin raw film during the curing process, thereby preventing the fluororesin from adhering to the curing equipment during the high-temperature curing process. Some suitable protective sheets include but are not limited to metal sheets such as copper sheets, silver sheets, aluminum sheets or aluminum alloy sheets.
[0178] The protective plate can be removed in a variety of ways, as long as the removal method does not adversely affect the cured fluororesin film. For example, the protective plate can be etched away using an etching solution, so that the fluororesin layer can be completely retained.
[0179] In some examples, the protective sheet is subjected to surface activation treatment to have organic activation groups on its surface. Thus, the protective sheet with organic activation groups is attached to both sides of the fluororesin green film, the fluororesin green film is aged and the protective sheet is removed to obtain a fluororesin film with organic activation groups on its surface.
[0180] Through the above arrangement, the organic activated groups on the protective plate are transferred to the cured fluororesin film. The fluororesin film is based on the organic activated groups, thereby effectively improving the bonding force between the fluororesin film and the thermosetting resin layer to obtain a stable bonding interface.
[0181] For example, performing surface activation treatment on the protective plate includes performing fluorination treatment on the protective plate, that is, the organic activation group is a fluorine-containing group.
[0182] (2) Regarding providing a dielectric film, this includes but is not limited to the following two implementation methods:
[0183] (2.1) The dielectric layer of the copper clad laminate is a thermosetting resin layer. Accordingly, the dielectric film includes a semi-cured film of a thermosetting resin. Then, providing the dielectric film includes the following steps:
[0184] Step 2.1.1, using the raw materials for preparing the thermosetting resin matrix, obtain a thermosetting resin liquid composition.
[0185] Step 2.1.2: Combine the thermosetting resin liquid composition with the first reinforcing material, and dry it to obtain a thermosetting resin semi-cured film as a dielectric film.
[0186] For step 2.1.1, the raw materials for preparing the thermosetting resin matrix include the following components in percentage by mass: 50%-79% of thermosetting resin, 20%-48% of the first inorganic filler for reinforcement, and 0.2%-2% of the first additive.
[0187] When obtaining a thermosetting resin liquid composition, an organic solvent is required to dissolve the resin so that the thermosetting resin liquid composition has a desired viscosity. Of course, the organic solvent can be removed from the resin system in the subsequent drying process.
[0188] Some suitable organic solvents include, but are not limited to, at least one of cyclohexane, toluene, xylene, methyl ethyl ketone, ethyl acetate, and ethylene dichloride.
[0189] The raw materials for preparing the thermosetting resin matrix and the organic solvent are stirred (for example, in a high-speed stirrer) until they are uniform, thereby obtaining a thermosetting resin liquid composition with uniform texture.
[0190] For step 2.1.2, the thermosetting resin liquid composition may be impregnated and filled with the first reinforcing material in the form of fiber cloth through an impregnation process, so that the thermosetting resin liquid composition is combined with the first reinforcing material.
[0191] For example, in the embodiment of the present disclosure, a thermosetting resin liquid composition is placed in the dipping tank of a gluing machine, and the first reinforcing material is passed through the dipping tank of the gluing machine for resin impregnation. The thickness of the thermosetting resin liquid film is controlled by a scraper roller to obtain a thermosetting resin liquid film of a certain thickness. After drying, a semi-cured thermosetting resin film is obtained and used as a dielectric film.
[0192] When drying the thermosetting resin liquid film, it can be dried in an oven at a certain drying temperature. The drying temperature is sufficient to remove volatile substances therein, such as organic solvents or the first additive. For example, the drying temperature can be 100°C-150°C, which includes but is not limited to: 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, etc.
[0193] (2.2) The dielectric layer of the copper clad laminate includes a thermosetting resin layer and a low dielectric resin layer, and accordingly, the dielectric film includes a thermosetting resin semi-cured film and a low dielectric resin film. Then, providing the dielectric film includes: providing the thermosetting resin semi-cured film and the low dielectric resin film separately and together as the dielectric film.
[0194] Exemplarily, providing the dielectric film comprises the following steps:
[0195] Step 2.2.1: Using the raw materials for preparing the thermosetting resin matrix, obtain a thermosetting resin liquid composition.
[0196] Step 2.2.2: Combine the thermosetting resin liquid composition with the first reinforcing material, and obtain a thermosetting resin semi-cured film by drying.
[0197] Step 2.2.3: providing a low dielectric resin film.
[0198] When providing the semi-cured thermosetting resin film and the low dielectric resin film, the order of the operations is not critical.
[0199] For step 2.2.1, the raw materials for preparing the thermosetting resin matrix include the following components in percentage by mass: 50%-79% of thermosetting resin, 20%-48% of the first inorganic filler for reinforcement, and 0.2%-2% of the first additive.
[0200] When obtaining a thermosetting resin liquid composition, an organic solvent is required to dissolve the resin so that the thermosetting resin liquid composition has a desired viscosity. Of course, the organic solvent can be effectively removed from the resin system during the subsequent drying process.
[0201] Some suitable organic solvents include, but are not limited to, at least one of acetone, butanone, cyclohexanone, toluene, xylene, N,N-dimethylformamide, and N,N-dimethylacetamide.
[0202] The raw materials for preparing the thermosetting resin matrix and the organic solvent are stirred (for example, in a high-speed stirrer) until they are uniform, thereby obtaining a thermosetting resin liquid composition with uniform texture.
[0203] In step 2.2.2, the thermosetting resin liquid composition may be impregnated and filled with the first reinforcing material in the form of fiber cloth through an impregnation process, so that the thermosetting resin liquid composition is combined with the first reinforcing material.
[0204] For example, in the embodiment of the present disclosure, a thermosetting resin liquid composition is placed in the dipping tank of a gluing machine, and the first reinforcing material is passed through the dipping tank of the gluing machine for resin impregnation. The thickness of the thermosetting resin liquid film is controlled by a scraper roller to obtain a thermosetting resin liquid film of a certain thickness. After drying, a semi-cured thermosetting resin film is obtained and used as a dielectric film.
[0205] When drying the thermosetting resin liquid film, it can be dried in an oven at a certain drying temperature. The drying temperature is sufficient to remove volatile substances therein, such as organic solvents or the first additive. For example, the drying temperature can be 100°C-150°C, which includes but is not limited to: 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, etc.
[0206] For step 2.2.3, a low dielectric resin film is provided, which may include: providing a low dielectric resin finished film material that meets the requirements (for example, both the dielectric properties and the thickness meet the requirements), cutting the low dielectric resin finished film material, and thus preparing a low dielectric resin film with a suitable shape.
[0207] The pressing process involved in step S3 may be performed in a vacuum environment at a set temperature and a set pressure.
[0208] For example, the temperature of the pressing process may be 180°C-250°C, including but not limited to 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, etc.
[0209] The pressure of the pressing process can be 300PSI-600PSI, which includes but is not limited to: 300PSI, 310PSI, 320PSI, 330PSI, 340PSI, 350PSI, 360PSI, 370PSI, 380PSI, 390PSI, 400PSI, 450PSI, 500PSI, 550PSI, etc.
[0210] The time of the pressing treatment can be 1 hour to 4 hours, including but not limited to: 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, etc.
[0211] The disclosed embodiment obtains a copper clad laminate by pressing the laminated intermediate under specific pressing operating conditions. This process is similar to the FR4 epoxy board resin glass fiber board pressing process and has the advantages of simple and convenient operation, low operating cost, high product yield, and ease of large-scale application.
[0212] Some embodiments of the present invention will be described in more detail below, but it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein. If no specific technology or conditions are specified in the examples, the technology or conditions described in the literature in this area or the product specifications are used. If the raw materials or equipment used do not specify the manufacturer, they are all conventional products that can be obtained commercially.
[0213] Example 1
[0214] This embodiment 1 provides a copper clad laminate, as shown in the attached Figure 1As shown, the copper-clad laminate includes a fluororesin layer 1, a copper-clad structural layer symmetrically attached to two opposite surfaces of the fluororesin layer 1, the copper-clad structural layer includes a thermosetting resin layer 2 and a copper foil layer 3, the thermosetting resin layer 2 is attached to the surface of the fluororesin layer 1, and the copper foil layer 3 is attached to the surface of the thermosetting resin layer 2 away from the fluororesin layer 1. The thickness of the fluororesin layer 1 is 80um, the thickness of the thermosetting resin layer 2 is 40um, and the thickness of the copper foil layer 3 is 30um.
[0215] The fluororesin layer 1 includes a fluororesin matrix, and the thermosetting resin layer 2 includes a thermosetting resin matrix and a glass fiber cloth located inside the thermosetting resin matrix, wherein the weight percentage of the glass fiber cloth in the thermosetting resin layer 2 is 30%.
[0216] The copper clad laminate is prepared by the following steps:
[0217] Step 1, providing a fluororesin film, which includes: providing a raw material for preparing a fluororesin matrix in the form of dry powder, which includes the following components in percentage by mass: 40% polytetrafluoroethylene dry powder and 60% silica filler.
[0218] The raw materials of the fluororesin matrix in dry powder form are cast and extruded by calendering and rolling and uniaxial / biaxial stretching processes to obtain a fluororesin green film. Fluorinated copper foils are stacked on both sides of the fluororesin green film, and then the fluororesin green film is hot-pressed and aged. The copper foils on both sides of the aged fluororesin film are completely etched away with an etching solution to obtain a fluororesin film, which is then washed with deionized water for later use.
[0219] Step 2, providing a semi-cured thermosetting resin film, which includes: stirring the raw materials for preparing the thermosetting resin matrix and cyclohexane in a high-speed mixer to obtain a thermosetting resin liquid composition with uniform texture. The raw materials for preparing the thermosetting resin matrix include the following components in percentage by mass: 65% styrene-divinylbenzene copolymer, 33% silica filler, 1% silane coupling agent, and 1% initiator.
[0220] The thermosetting resin liquid composition is placed in the dipping tank of the gluing machine, and the glass fiber cloth is passed through the dipping tank of the gluing machine for resin impregnation. The thickness of the thermosetting resin liquid film is controlled by a scraper to obtain a thermosetting resin liquid film of a certain thickness. After drying, a thermosetting resin semi-cured film is obtained and used as a dielectric film.
[0221] Step 3: providing a copper foil with surface activation treatment, which includes: treating the surface of the copper foil with low roughness with a methoxysilane coupling agent to obtain the copper foil with surface activation treatment.
[0222] Step 4: According to the structure of the copper clad laminate, the fluororesin film, the semi-cured thermosetting resin film and the surface activated copper foil are laminated to obtain a laminated intermediate.
[0223] Step 5: Use a vacuum press to press the laminated intermediate under vacuum to obtain a copper clad laminate, wherein the pressing temperature is 200° C., the pressing pressure is 350 PSI, and the pressing time is 2 hours.
[0224] The performance of the copper clad laminate prepared in Example 1 was tested. Meanwhile, the fluororesin film prepared above and the currently available PTFE-based copper clad laminate were provided as comparative examples and the same performance tests were performed. The relevant test results are shown in Table 1 below.
[0225] Table 1
[0226] project Df Dk CTE / PPM 6L PCB layer deviation / mil Fluorine resin film 0.0002 3.6 20-25 >10 Example 1 Copper Clad Laminate 0.00045 3.1 15 3-4 PTFE based copper clad laminate for sale 0.001 3.0 30-50 Unable to craft
[0227] It can be seen that the copper-clad laminate prepared in Example 1 of the present disclosure effectively improves the mechanical strength of the board and reduces the overall thermal expansion coefficient of the board, thereby reducing its expansion and contraction, compared with the prior art. Based on the copper-clad laminate, a process similar to the FR4 board lamination process can be used to prepare a multi-layer PCB board (Table 1 illustrates the preparation of a 6-layer PCB), and the layer deviation of the PCB multi-layer board is equivalent to the layer deviation of the PCB multi-layer board obtained based on the FR4 board, so that it can be effectively and conveniently used in the preparation of PCB multi-layer boards. In addition, it can be seen from Table 1 that the currently available PTFE-based copper-clad laminate cannot be used to make 6LPCB boards.
[0228] Example 2
[0229] This embodiment 2 provides a copper clad laminate, as shown in the attached Figure 3 As shown, the copper-clad laminate comprises a fluororesin layer 1, a copper-clad structural layer symmetrically attached to two opposite surfaces of the fluororesin layer 1, the copper-clad structural layer comprises a thermosetting resin layer 2, a low dielectric resin layer 4 and a copper foil layer 3, the thermosetting resin layer 2 is attached to the surface of the fluororesin layer 1, the low dielectric resin layer 4 is attached to the surface of the thermosetting resin layer 2 that is away from the fluororesin layer 1, and the copper foil layer 3 is attached to the surface of the low dielectric resin layer 4 that is away from the thermosetting resin layer 2. The thickness of the fluororesin layer 1 is 80um, the thickness of the thermosetting resin layer 2 is 40um, the thickness of the copper foil layer 3 is 30um, and the thickness of the low dielectric resin layer 4 is 15um.
[0230] The fluororesin layer 1 includes a fluororesin matrix, and the thermosetting resin layer 2 includes a thermosetting resin matrix and a glass fiber cloth located inside the thermosetting resin matrix, wherein the weight percentage of the glass fiber cloth in the thermosetting resin layer 2 is 30%.
[0231] The copper clad laminate is prepared by the following steps:
[0232] Step 1, providing a fluororesin film, which includes: providing a raw material for preparing a fluororesin matrix in the form of dry powder, which includes the following components in percentage by mass: 40% polytetrafluoroethylene dry powder and 60% silica filler.
[0233] The raw materials of the fluororesin matrix in dry powder form are cast and extruded by calendering and rolling and uniaxial / biaxial stretching processes to obtain a fluororesin green film. Fluorinated copper foils are stacked on both sides of the fluororesin green film, and then the fluororesin green film is hot-pressed and aged. The copper foils on both sides of the aged fluororesin film are completely etched away with an etching solution to obtain a fluororesin film, which is then washed with deionized water for later use.
[0234] Step 2, providing a semi-cured thermosetting resin film, which includes: stirring the raw materials for preparing the thermosetting resin matrix and cyclohexane in a high-speed mixer to obtain a thermosetting resin liquid composition with uniform texture. The raw materials for preparing the thermosetting resin matrix include the following components in percentage by mass: 65% styrene-divinylbenzene copolymer, 33% silica filler, 1% silane coupling agent, and 1% initiator.
[0235] The thermosetting resin liquid composition is placed in the dipping tank of the gluing machine, and the glass fiber cloth is passed through the dipping tank of the gluing machine for resin impregnation. The thickness of the thermosetting resin liquid film is controlled by a scraper to obtain a thermosetting resin liquid film of a certain thickness. After drying, a thermosetting resin semi-cured film is obtained.
[0236] Step 3: providing a copper foil with surface activation treatment, which includes: treating the surface of the copper foil with low roughness with a methoxysilane coupling agent to obtain the copper foil with surface activation treatment.
[0237] Step 4: Cut the finished PFA film to obtain a low dielectric resin film as a low dielectric resin layer.
[0238] Step 5: According to the structure of the copper clad laminate, the fluororesin film, the thermosetting resin semi-cured film, the low dielectric resin film and the surface activated copper foil are laminated to obtain a laminated intermediate.
[0239] Step 6: Use a vacuum press to press the laminated intermediate under vacuum to obtain a copper clad laminate, wherein the pressing temperature is 200° C., the pressing pressure is 350 PSI, and the pressing time is 2 hours.
[0240] The performance of the copper clad laminate prepared in Example 2 was tested. Meanwhile, the fluororesin film, PFA finished film, and currently available PTFE-based copper clad laminate prepared as above were provided as comparative examples and the same performance tests were performed. The relevant test results are shown in Table 2 below.
[0241] Table 2
[0242]
[0243]
[0244] It can be seen that the copper-clad laminate prepared in Example 2 of the present disclosure effectively improves the mechanical strength of the sheet and reduces the overall thermal expansion coefficient of the sheet, thereby reducing its expansion and contraction, compared with the prior art. Based on the copper-clad laminate, a process similar to the FR4 sheet lamination process can be used to prepare a multilayer PCB sheet (Table 2 illustrates the preparation of a 6-layer PCB), and the layer deviation of the PCB multilayer board is equivalent to the layer deviation of the PCB multilayer board obtained based on the FR4 sheet, so that it can be effectively and conveniently used in the preparation of PCB multilayer boards. In addition, it can be seen from Table 2 that the currently available PFA membrane and PTFE-based copper-clad laminate cannot be used to make 6LPCB sheets.
[0245] In addition, compared with Example 1, Example 2 further adds a PFA film as the low dielectric resin layer 4, so that the dielectric properties of the copper clad laminate are more excellent.
[0246] Example 3
[0247] This embodiment 3 provides a copper clad laminate, as shown in the attached Figure 2 As shown, the copper-clad laminate includes a fluororesin layer 1, a copper-clad structural layer symmetrically attached to two opposite surfaces of the fluororesin layer 1, the copper-clad structural layer includes a thermosetting resin layer 2 and a copper foil layer 3, the thermosetting resin layer 2 is attached to the surface of the fluororesin layer 1, and the copper foil layer 3 is attached to the surface of the thermosetting resin layer 2 away from the fluororesin layer 1. The thickness of the fluororesin layer 1 is 95um, the thickness of the thermosetting resin layer 2 is 40um, and the thickness of the copper foil layer 3 is 30um.
[0248] The fluororesin layer 1 includes a fluororesin matrix and a glass fiber cloth located inside the fluororesin matrix, wherein the weight percentage of the glass fiber cloth in the fluororesin layer 1 is 25%, and the thermosetting resin layer 2 includes a thermosetting resin matrix and a glass fiber cloth located inside the thermosetting resin matrix, wherein the weight percentage of the glass fiber cloth in the thermosetting resin layer 2 is 30%.
[0249] The copper clad laminate is prepared by the following steps:
[0250] Step 1, providing a fluororesin film, which includes: providing raw materials for preparing a fluororesin matrix, which includes the following components in percentage by mass: 65% polytetrafluoroethylene, 25% second inorganic filler for reinforcement, and 10% second additive, wherein the second additive is an emulsifier.
[0251] The raw materials and water of the fluororesin matrix are stirred in a high-speed stirrer until they are uniformly stirred to obtain a fluororesin emulsion with uniform texture. The fluororesin emulsion is placed in the dipping tank of the gluing machine, and the glass fiber cloth is passed through the dipping tank of the gluing machine for resin impregnation. The thickness of the fluororesin liquid film is controlled by a scraping stick, and the fluororesin raw film is obtained after drying.
[0252] Fluorinated copper foil is stacked on both sides of the fluororesin green film, and then the fluororesin green film is heat-pressed and aged. The copper foil on both sides of the aged fluororesin film is completely etched away with an etching solution to obtain a fluororesin film, which is then washed with deionized water for later use.
[0253] Step 2, providing a semi-cured thermosetting resin film, which includes: stirring the raw materials for preparing the thermosetting resin matrix and cyclohexane in a high-speed mixer to obtain a thermosetting resin liquid composition with uniform texture. The raw materials for preparing the thermosetting resin matrix include the following components in percentage by mass: 65% styrene-divinylbenzene copolymer, 33% silica filler, 1% silane coupling agent, and 1% initiator.
[0254] The thermosetting resin liquid composition is placed in the dipping tank of the gluing machine, and the glass fiber cloth is passed through the dipping tank of the gluing machine for resin impregnation. The thickness of the thermosetting resin liquid film is controlled by a scraper to obtain a thermosetting resin liquid film of a certain thickness. After drying, a thermosetting resin semi-cured film is obtained.
[0255] Step 3: providing a copper foil with surface activation treatment, which includes: treating the surface of the copper foil with low roughness with a methoxysilane coupling agent to obtain the copper foil with surface activation treatment.
[0256] Step 4: According to the structure of the copper clad laminate, the fluororesin film, the semi-cured thermosetting resin film and the surface activated copper foil are laminated to obtain a laminated intermediate.
[0257] Step 5: Use a vacuum press to press the laminated intermediate under vacuum to obtain a copper clad laminate, wherein the pressing temperature is 200° C., the pressing pressure is 350 PSI, and the pressing time is 2 hours.
[0258] The performance of the copper clad laminate prepared in Example 3 was tested. Meanwhile, the fluororesin film prepared above and the currently available PTFE-based copper clad laminate were provided as comparative examples and the same performance tests were performed. The relevant test results are shown in Table 3 below.
[0259] Table 3
[0260] project Df Dk CTE / PPM 6L PCB layer deviation / mil Fluorine resin film 0.001 3.0 30-50 Unable to process Example 3 Copper Clad Laminate 0.0008 3.1 14-15 3-4 PTFE based copper clad laminate for sale 0.001 3.0 30-50 Unable to craft
[0261] It can be seen that the copper clad laminate prepared in Example 3 of the present disclosure effectively improves the mechanical strength of the board and reduces the overall thermal expansion coefficient of the board, thereby reducing its expansion and contraction, compared with the prior art. Based on the copper clad laminate, a process similar to the FR4 board lamination process can be used to prepare a multi-layer PCB board, and the layer deviation of the PCB multi-layer board is equivalent to the layer deviation of the PCB multi-layer board obtained based on the FR4 board, so that it can be effectively and conveniently used in the preparation of PCB multi-layer boards.
[0262] In addition, compared with Example 1, in Example 3, glass fiber cloth is added to the fluororesin layer 1, so that the mechanical strength of the fluororesin layer 1 is improved, thereby reducing the overall thermal expansion coefficient of the copper clad laminate.
[0263] Example 4
[0264] This embodiment 4 provides a copper clad laminate, as shown in the attached Figure 4 As shown, the copper-clad laminate comprises a fluororesin layer 1, a copper-clad structural layer symmetrically attached to two opposite surfaces of the fluororesin layer 1, the copper-clad structural layer comprises a thermosetting resin layer 2, a low dielectric resin layer 4 and a copper foil layer 3, the thermosetting resin layer 2 is attached to the surface of the fluororesin layer 1, the low dielectric resin layer 4 is attached to the surface of the thermosetting resin layer 2 that is away from the fluororesin layer 1, and the copper foil layer 3 is attached to the surface of the low dielectric resin layer 4 that is away from the thermosetting resin layer 2. The thickness of the fluororesin layer 1 is 95 microns, the thickness of the thermosetting resin layer 2 is 40um, the thickness of the copper foil layer 3 is 30um, and the thickness of the low dielectric resin layer 4 is 15um.
[0265] The fluororesin layer 1 includes a fluororesin matrix and a glass fiber cloth located inside the fluororesin matrix, wherein the weight percentage of the glass fiber cloth in the fluororesin layer 1 is 25%, and the thermosetting resin layer 2 includes a thermosetting resin matrix and a glass fiber cloth located inside the thermosetting resin matrix, wherein the weight percentage of the glass fiber cloth in the thermosetting resin layer 2 is 30%.
[0266] The copper clad laminate is prepared by the following steps:
[0267] Step 1, providing a fluororesin film, which includes: providing raw materials for preparing a fluororesin matrix, which includes the following components in percentage by mass: 65% polytetrafluoroethylene, 25% second inorganic filler for reinforcement, and 10% second additive, wherein the second additive is an emulsifier.
[0268] The raw materials and water of the fluororesin matrix are stirred in a high-speed stirrer until they are uniformly stirred to obtain a fluororesin emulsion with uniform texture. The fluororesin emulsion is placed in the dipping tank of the gluing machine, and the glass fiber cloth is passed through the dipping tank of the gluing machine for resin impregnation. The thickness of the fluororesin liquid film is controlled by a scraping stick, and the fluororesin raw film is obtained after drying.
[0269] Fluorinated copper foil is stacked on both sides of the fluororesin green film, and then the fluororesin green film is heat-pressed and aged. The copper foil on both sides of the aged fluororesin film is completely etched away with an etching solution to obtain a fluororesin film, which is then washed with deionized water for later use.
[0270] Step 2, providing a semi-cured thermosetting resin film, which includes: stirring the raw materials for preparing the thermosetting resin matrix and cyclohexane in a high-speed mixer to obtain a thermosetting resin liquid composition with uniform texture. The raw materials for preparing the thermosetting resin matrix include the following components in percentage by mass: 65% styrene-divinylbenzene copolymer, 33% silica filler, 1% silane coupling agent, and 1% initiator.
[0271] The thermosetting resin liquid composition is placed in the dipping tank of the gluing machine, and the glass fiber cloth is passed through the dipping tank of the gluing machine for resin impregnation. The thickness of the thermosetting resin liquid film is controlled by a scraper to obtain a thermosetting resin liquid film of a certain thickness. After drying, a thermosetting resin semi-cured film is obtained.
[0272] Step 3: providing a copper foil with surface activation treatment, which includes: treating the surface of the copper foil with low roughness with a methoxysilane coupling agent to obtain the copper foil with surface activation treatment.
[0273] Step 4: Cut the finished PFA film to obtain a low dielectric resin film as a low dielectric resin layer.
[0274] Step 5: According to the structure of the copper clad laminate, the fluororesin film, the thermosetting resin semi-cured film, the low dielectric resin film and the surface activated copper foil are laminated to obtain a laminated intermediate.
[0275] Step 6: Use a vacuum press to press the laminated intermediate under vacuum to obtain a copper clad laminate, wherein the pressing temperature is 200° C., the pressing pressure is 350 PSI, and the pressing time is 2 hours.
[0276] The performance of the copper clad laminate prepared in Example 4 was tested. Meanwhile, the fluororesin film, PFA finished film, and currently available PTFE-based copper clad laminate prepared as above were provided as comparative examples and the same performance tests were performed. The relevant test results are shown in Table 4 below.
[0277] Table 4
[0278] project Df Dk CTE / PPM 6L PCB layer deviation / mil Fluorine resin film 0.001 3.0 30-50 Unable to craft PFA membrane 0.0003 2.1 15PPM Unable to craft Example 4 Copper Clad Laminate 0.0005 3.1 15 3-4 PTFE based copper clad laminate for sale 0.001 3.0 30-50 Unable to craft
[0279] It can be seen that the copper clad laminate prepared in Example 4 of the present disclosure effectively improves the mechanical strength of the laminate, reduces the overall thermal expansion coefficient of the laminate, and thus reduces its expansion and contraction, compared with the prior art.
[0280] The copper clad laminate can be used to prepare multi-layer PCB boards using a process similar to the FR4 board lamination process. The layer deviation of the PCB multi-layer board is equivalent to the layer deviation of the PCB multi-layer board obtained based on the FR4 board, so that it can be effectively and conveniently used in the preparation of PCB multi-layer boards.
[0281] In addition, compared with Example 3, Example 4 further adds a PFA film as the low dielectric resin layer 4, so that the dielectric properties of the copper clad laminate are more excellent.
[0282] The above description is only for the purpose of facilitating those skilled in the art to understand the technical solution of the present disclosure and is not intended to limit the present disclosure. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present disclosure shall be included in the protection scope of the present disclosure.
Claims
1. A copper clad laminate, characterized in that: The copper-clad laminate comprises: a fluororesin layer and a copper-clad structural layer located on at least one surface of the fluororesin layer; The copper-clad structural layer comprises a dielectric layer and a copper foil layer bonded to each other, and the dielectric layer is bonded to the fluororesin layer; The medium layer includes a thermosetting resin layer, and the thermosetting resin layer includes a thermosetting resin matrix and a first reinforcing material located inside the thermosetting resin matrix.
2. The copper clad laminate according to claim 1, characterized in that: The first reinforcing material includes fiber cloth.
3. The copper clad laminate according to claim 1, characterized in that: The weight percentage of the thermosetting resin matrix is 50%-80%; The weight percentage of the first reinforcing material is 20%-50%.
4. The copper clad laminate according to claim 1, characterized in that: The raw material for preparing the thermosetting resin matrix includes thermosetting resin, and the thermosetting resin includes at least one of polyolefin resin and hydrocarbon resin.
5. The copper clad laminate according to claim 1, characterized in that: The raw materials for preparing the thermosetting resin matrix also include a first inorganic filler for reinforcement.
6. The copper clad laminate according to claim 5, characterized in that: The first inorganic filler for reinforcement includes a ceramic filler.
7. The copper clad laminate according to any one of claims 1 to 6, characterized in that: The dielectric layer further includes a low dielectric resin layer, and the low dielectric resin layer is located between the thermosetting resin layer and the copper foil layer.
8. The copper clad laminate according to claim 7, characterized in that: The low dielectric resin layer includes at least one of polytetrafluoroethylene resin, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, and fluorinated ethylene propylene copolymer.
9. The copper clad laminate according to any one of claims 1 to 8, characterized in that: The fluororesin layer comprises a fluororesin matrix, and the raw material for preparing the fluororesin matrix comprises at least one of polytetrafluoroethylene resin and tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer.
10. The copper clad laminate according to claim 9, characterized in that: The raw materials for preparing the fluororesin matrix also include a second inorganic filler for reinforcement.
11. The copper clad laminate according to claim 10, characterized in that: The second inorganic filler for reinforcement includes a ceramic filler.
12. The copper clad laminate according to any one of claims 9 to 11, characterized in that: The fluororesin layer further includes a second reinforcing material located inside the fluororesin.
13. The copper clad laminate according to claim 12, characterized in that: The second reinforcing material includes fiber cloth.
14. A circuit board, characterized in that: The circuit board comprises at least one layer of the copper clad board according to any one of claims 1 to 13.
15. An electronic device, characterized in that: The electronic device comprises the circuit board according to claim 14.
16. A method for preparing a copper clad laminate, characterized in that: The copper clad laminate is as described in any one of claims 1 to 13, and the preparation method of the copper clad laminate comprises: Provide fluororesin film, dielectric film and copper foil with surface activation treatment respectively; According to the structure of the copper-clad laminate, the fluororesin film, the dielectric film and the copper foil treated with surface activation are laminated to obtain a laminated intermediate; The laminated intermediate is subjected to a pressing process, so that the fluororesin film is cured to form a fluororesin layer and the dielectric film is cured to form a dielectric layer, thereby obtaining the copper clad laminate.
17. The method for preparing a copper clad laminate according to claim 16, characterized in that: The dielectric layer is a thermosetting resin layer; Providing the dielectric film comprises: Using the raw materials for preparing the thermosetting resin matrix, obtaining a thermosetting resin liquid composition; The thermosetting resin liquid composition is combined with the first reinforcing material and dried to obtain a thermosetting resin semi-cured film as the dielectric film.
18. The method for preparing a copper clad laminate according to claim 16, characterized in that: The dielectric layer includes a thermosetting resin layer and a low dielectric resin layer bonded to each other; Providing the dielectric film includes: providing a thermosetting resin semi-cured film and a low dielectric resin film respectively and both of them serve as the dielectric film; Providing the semi-cured film of thermosetting resin comprises: Obtaining a thermosetting resin liquid composition according to the raw materials for preparing the thermosetting resin matrix; The thermosetting resin liquid composition is combined with the first reinforcing material and dried to obtain the thermosetting resin semi-cured film.
19. The method for preparing a copper clad laminate according to any one of claims 16 to 18, characterized in that: The fluororesin layer includes a fluororesin matrix; Providing the fluororesin film comprises: Providing raw materials for preparing fluororesin matrix in dry powder form; By means of a dry film-making process, a fluororesin green film is prepared using the fluororesin matrix preparation raw material in dry powder form; The fluororesin raw film is subjected to a aging treatment under the protection of the protective plate, and the protective plate is removed to obtain the fluororesin film.
20. The method for preparing a copper clad laminate according to any one of claims 16 to 18, characterized in that: The fluororesin layer includes a fluororesin matrix and a second reinforcing material located inside the fluororesin matrix; Providing the fluororesin film comprises: Using the raw materials for preparing the fluororesin matrix, a fluororesin emulsion is obtained; Combining the fluororesin emulsion with the second reinforcing material, and subjecting the mixture to drying treatment to obtain a fluororesin green film; The fluororesin raw film is subjected to a aging treatment under the protection of the protective plate, and the protective plate is removed to obtain the fluororesin film.