Copper and manganese containing chabazite SCR catalysts for N2O reduction
By using a catalyst with an appropriate amount of copper and manganese-carried catalyst of CHA skeleton type, the problems of low NOx conversion and high N2O selectivity were solved, and the effects of efficient nitrogen oxide removal and low emissions were achieved.
Patent Information
- Application Number
- CN202380023787.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-23
- Filing Date
- 2023-03-23
- Publication Date
- 2024-11-08
AI Technical Summary
The existing catalysts have low NOx conversion and high N2O selectivity under low temperature conditions, making it difficult to meet the needs of modern engines for high-efficiency nitrogen oxide removal and low emissions.
Crystalline aluminosilicate zeolite with CHA skeleton type is used as the catalytically active composition, with the sum of the molar amounts of copper and manganese, divided by the molar amount of aluminum in the Between 0.11-0.96, it is used to selectively catalytically reduce nitrogen oxides to nitrogen.
It significantly improves the high conversion and selectivity of nitrogen oxides to nitrogen, while reducing the selectivity of N2O, and is suitable for modern low-emission combustion engine exhaust treatment.
Smart Images

Figure BDA0005011538650000101 
Figure BDA0005011538650000231 
Figure BDA0005011538650000241
Abstract
Description
[0001] describe
[0002] The present invention relates to catalytically active compositions for the selective catalytic reduction of nitrogen oxides in exhaust gases from combustion engines exhibiting low N2O emissions. In particular, the present invention relates to chabazites loaded with copper and manganese. Methods for the preparation of these catalytically active compositions and the use of these catalytically active compositions are also envisaged.
[0003] Zeolites are crystalline microporous aluminosilicate materials formed by corner-sharing TO4 tetrahedra (where T represents silicon (Si) or aluminum (Al)) interconnected by oxygen atoms to form pores and cavities of uniform size and shape precisely defined by their crystal structure. Zeolites are also called "molecular sieves" because the pores and cavities have sizes similar to those of small molecules. Such materials have important commercial applications as adsorbents, ion exchangers, and catalysts.
[0004] Zeolites are classified by the International Zeolite Association (IZA) according to the rules of the IUPAC Commission on Zeolite Nomenclature. Once the morphology of a new framework is established, a three-letter code is assigned. This code defines the atomic structure of the framework, from which a clear X-ray diffraction pattern can be described.
[0005] Zeolites are also often classified according to their pore size, which is defined by the ring size of the largest pore opening. Large pore zeolites have a maximum ring size of 12 tetrahedral atoms, medium pore zeolites have a maximum pore size of 10 tetrahedral atoms, and small pore zeolites have a maximum pore size of 8 tetrahedral atoms. Well-known small pore zeolites are particularly of the AEI, CHA (chabazite), ERI (erionite), LEV (intercalated chabazite), and KFI framework types. An example of a zeolite with a large pore size is a faujasite framework type.
[0006] There are a large number of known molecular sieve structures at present.Some known molecular sieves belong to certain structural families with similar characteristics.A specific family, i.e. the ABC-6 family, can be described as a stack of two-dimensional periodic layers of non-connected planar 6-ring primitives composed of 6 T atoms (T=Si, Al, etc.) connected by oxygen atoms.The resulting layer with hexagonal symmetry is also referred to as a periodic construction unit (PerBU).The stacking is typically described by a sequence of letters "A", "B" and "C" indicating the relative positions of adjacent layers. "A", "B" and "C" refer to the relative positions of adjacent layers when stacking hexagonal layers of closely packed spheres.
[0007] The CHA framework belongs to the ABC-6 family and can be described by the repeating stacking sequence AABBCC. This results in a framework morphology characterized by a three-dimensional 8-membered ring pore system containing a double hexacyclic ring (d6R) and a cha cage.
[0008] Small-pore zeolites, especially if they contain cations like copper and iron in the zeolite pores, play an important role as catalysts in the so-called selective catalytic reduction (SCR) of nitrogen oxides with ammonia to form nitrogen and water. The SCR process has been widely used to clean exhaust gases resulting from the combustion of fossil fuels, especially from stationary power plants and vehicles powered by diesel engines.
[0009] Catalytic reduction of NO with NH3 x It can be expressed by different reaction equations. Nitric oxide (NO) is the main NO produced in the engine. x The reduction of NO is known as the "standard" NH3-SCR reaction:
[0010] 4NO+4NH3+O2→4N2+6H20(1)
[0011] NO2 is more reactive than NO. In the presence of a mixture of NO and NO2, the NH3-SCR reaction is more favorable and the so-called "fast" NH3-SCR reaction can occur:
[0012] 2NH3+NO+NO2→2N2+3H2O(2)
[0013] In order to benefit from the fast NH3-SCR reaction, an additional catalyst is needed to facilitate partial oxidation of NO to NO2.
[0014] Furthermore, side reactions may occur and lead to unwanted products or unproductive consumption of ammonia:
[0015] 4NH3+3O2→N2+6H2O(3)
[0016] 2NH3+2O2→N2O+3H2O(4)
[0017] 4NH3+5O2→4NO+6H2O(5)
[0018] 4NH3+7O2→4NO2+6H2O(6)
[0019] 2NH3+2NO2+H2O→NH4NO2+NH4NO3(7)
[0020] The exhaust gas temperatures of the latest generation engines and hybrid vehicles with reduced fuel consumption and low CO2 emissions are significantly lower in the official driving cycle compared to previous generations of engines. Therefore, it is necessary to obtain high low-temperature NO x In general, Cu-containing zeolites show better low-temperature NO conversion than their iron-containing counterparts. xConversion rate. In addition, NH3-SCR catalysts should release as little N2O as possible. During the conversion of NOx with copper-promoted SCR catalysts in the exhaust system of diesel engines in road and off-road applications, the greenhouse gas N2O is formed as a by-product. This is more significant in the case of elevated NO2 content in the exhaust gas feed.
[0021] Besides selectivity and activity, the hydrothermal stability of SCR catalysts is another important parameter, since NH3-SCR catalysts have to withstand the severe temperature conditions at full engine load, and exposure to water vapor at temperatures up to 700°C is known to be critical for many zeolite types.
[0022] WO 2021 / 219628 A1 discloses an SCR catalyst comprising a substrate (which may be a flow-through substrate or a wall-flow filter) and a coating dispersed on the substrate. The coating comprises: a first non-zeolite material comprising aluminum; an 8-membered ring pore zeolite material comprising one or more of copper and iron, selected from CHA, AEI, RTH, LEV, DDR, KFI, ERI, AFX and LTA; and a second non-zeolite oxide material comprising cerium and one or more of zirconium, aluminum, silicon, lanthanum, niobium, iron, manganese, titanium, tungsten, copper, molybdenum, neodymium, cobalt, chromium, tin and praseodymium; wherein at least 65% by weight of the coating consists of an 8-membered ring pore zeolite material comprising one or more of copper and iron. Most preferably, the zeolite material is CHA. The results show that the coating comprising cerium oxide and zirconium oxide has lower back pressure and better NO than other tested coatings. x Conversion. N2O selectivity was not examined.
[0023] WO 2018 / 081682 A1 provides a catalyst composition comprising a zeolite having an LTA structure, wherein iron, manganese or a combination thereof is used as an extra-framework metal. The zeolite has a SAR value of 15 to 70 and may contain 0.5 wt % to 10 wt % of iron, manganese or a combination thereof. Optionally, the catalyst composition may be used with a second catalyst composition comprising a second molecular sieve selected from AEI, AFX, CHA or LTA, the second molecular sieve comprising an extra-framework metal selected from antimony, bismuth, cesium, chromium, cobalt, copper, iron, manganese, molybdenum, nickel, niobium, tin, titanium, tungsten, vanadium, zinc, zirconium and a combination thereof. Studies have shown that fresh and aged Mn-LTA show better NO compared to fresh and aged Mn-CHA and Mn-AFX. x However, the large-pore zeolite Mn-BEA provided better NO conversion at about 150°C to about 200°C than all three Mn-containing small-pore zeolites. x Conversion rate.
[0024] CN 111 375 445A discloses a method for preparing a molecular sieve denitration catalyst loaded with manganese. The molecular sieve-loaded manganese-based denitration catalyst is prepared by mixing a molecular sieve, a soluble aqueous solution of a manganese salt and a ligand to form a mixed solution, wherein the molecular sieve has an electrical property opposite to that of a complex formed by a manganese salt and a ligand; and electrostatic adsorption and other steps are performed on the mixed solution. The molecular sieve-loaded manganese-based denitration catalyst is uniform in terms of the particle size of the active component and the distribution on the surface of the carrier, and is particularly suitable for removing nitrogen monoxide. The molecular sieve can be selected from a long list of molecular sieves, among which AEI, CHA, FAU and ZSM are preferred. In an embodiment, Mn-loaded CHA is synthesized and sulfur-aged. Compared with Mn-CHA obtained by a conventional liquid ion exchange method, sulfur-aged Mn-CHA shows a lower ignition temperature of the NH3-SCR reaction and a better NOx conversion rate. The molecular sieve according to CN 111 375 445A does not contain any other transition metals besides manganese, and the formation of N2O was not investigated.
[0025] In H Xue, X Guo, T Meng, Q Guo, D Mao and S Wang: “Cu-ZSM-5 Catalyst Impregnated with Mn-Co Oxide for the Selected Catalytic Reduction of NO: Physicochemical Property–Catalytic Activity Relationship and In Situ DRIFTS Study for the Reaction Mechanism”, ACS Catal 2021, 11, 7702-7718, it was shown that impregnation of Cu-ZSM-5 with copper and manganese improved the NH3-SCR catalytic activity at temperatures below 200°C. The Cu-ZSM-5 zeolite used had a Cu / Al ratio of 38, corresponding to a SAR value of 76, and a copper content of 1.98 wt%. The zeolite was impregnated with manganese and cobalt, and the mass ratio of Mn and Co in the zeolite thus impregnated varied from 1:0.5 to 1:5. The total amount of (Mn+Co) of Cu-ZSM-5 remained constant at 10 wt%.
[0026] In C Song, L Zhang, Z Li, Y Lu and K Li: “Co-Exchange of Mn: A Simple Method to Improve Both the Hydrothermal Stability and Activity of Cu-SSZ-13NH3-SRC Catalysts”, Catalysts 2019, 9, 455-469, a series of Cu-Mn-SSZ-13 were obtained by co-exchanging Mn and Cu into SSZ-13 and compared with the Cu-SSZ-13 catalyst in the selective catalytic reduction (SCR) of nitric oxide (NO) by ammonia. The purpose is to simultaneously improve the low-temperature activity of the catalyst and its tolerance to hydrothermal aging. The higher the copper content of SSZ-13 with a CHA framework structure, the higher the low-temperature activity, but the lower the hydrothermal stability. The zeolite SSZ-13 with a SAR value was ion-exchanged with copper and optionally manganese. The obtained zeolite has a Mn / Cu molar ratio of 0 / 10 (Cu only) to 6 / 10. Based on the results of inductively coupled plasma atomic emission spectroscopy (ICP-AES), the ion exchange degree of the zeolite thus obtained was calculated as mol Cu (or Mn) × 2 / mol Al × 100%. The ion exchange degree of Cu ranged from 0.35 (Mn / Cu ratio = 0 / 10) to 0.13 (Mn / Cu ratio = 6 / 10), and the ion exchange degree of Mn ranged from 0 (Mn / Cu ratio = 0 / 10) to 0.17 (Mn / Cu ratio = 6 / 10). This corresponds to a Cu / Al ratio of 0.175 (Mn / Cu ratio = 0 / 10) to 0.065 (Mn / Cu ratio = 6 / 10) and a Mn / Al ratio of 0 (Mn / Cu ratio = 0 / 10) to 0.085 (Mn / Cu ratio = 6 / 10). Therefore, the (Cu+Mn) / Al ratio ranged from 0.15 to 0.175. The catalysts were studied for NO conversion, NO oxidation, NH3 oxidation, and NH3 desorption. The catalyst known as Cu(0.2)Mn(0.1) showed the highest reactivity in the low temperature range and the best resistance to hydrothermal aging. The catalyst had a Mn / Cu ratio of 6 / 19, a Cu ion exchange degree of 0.2, a Mn ion exchange degree of 0.1, a Cu / Al molar ratio of 0.1, a Mn / Al molar ratio of 0.05, and a (Cu+Mn) / Al molar ratio of 0.15. The catalysts were not studied for N2O formation.
[0027] In J Du, J Wang, X Shi, Y Shan, Y Zhang and H He: “Promoting Ef-fect of Mn on In Situ Synthesized Cu-SSZ-13for NH3-SCR”, Catalysts 2020, 10, 1375-1388, the effect of Mn impregnation on the NH3-SCR activity in in situ synthesized Cu-SSZ-13 was studied. All Cu-SSZ-13 catalysts had a copper content of 4.6 wt% and a Si / Al ratio of 4.8, corresponding to a SAR value of 9.6. The Cu-SSZ-13 catalysts were impregnated with 0%, 3%, 5%, 7%, 10% and 14% Mn. The NH3-SCR catalytic activity, N2 selectivity and N2O formation of all catalysts were studied. Among all catalysts, 5% Mn / Cu-SSZ-13 showed the best catalytic activity in the low temperature range and obtained close to 95% NO at about 140°C. x However, with further increase in Mn content, when compared with 5% Mn / Cu-SSZ-13, the low-temperature NO x The conversion rate starts to decrease. As the Mn content increases, more N2O is produced, which indicates that adding Mn will reduce the N2 selectivity of the catalyst. However, for Mn / Cu-SSZ-13 with Mn content below 7%, N2O formation is below 20 ppm. Among all the prepared catalysts, 5% Mn / Cu-SSZ-13 performs the best.
[0028] WO 2020 / 047356 A1 discloses a catalyst composition comprising a molecular sieve for treating exhaust gas, the molecular sieve comprising exchanged copper and exchanged manganese. In a preferred embodiment, the molecular sieve is selected from AEI, CHA, BEA and MFI. The SAR value is between 5 and 200, most preferably between 10 and 30. The atomic ratio of copper to manganese is between 0.1 and 50, preferably between 0.3 and 3. Copper is present in an amount of 0.1 wt % to 7 wt %, most preferably between 1 wt % and 4 wt %, and manganese is present in an amount of 0.05 wt % to 7 wt %, most preferably between 0.5 wt % and 2.5 wt %. In the experiment, the effect of the amount of copper and manganese on the N2O selectivity of fast, slow and standard SCR, as well as fresh AEI zeolite and aged AEI zeolite was tested. N2O selectivity is defined as the number of moles of N2O formed divided by the number of moles of NO converted x The number of moles (NO x is defined as NO and NO2). This means that the lower the selectivity of N2O, the more xThe amount of copper was kept constant while the manganese content was varied, or vice versa. AEI zeolites containing copper and manganese showed enhanced light-off temperature, lower N2O selectivity and equal or better NO x While keeping the Cu content constant, increasing the Mn content, thus reducing the Cu / Mn ratio, especially in terms of ignition temperature, increases NO x conversion rate without significantly increasing N2O selectivity, which means that the presence of NO x The conversion and N2O production increased proportionally. No SAR values are given for the AEI zeolite. AEI containing 1.5 wt% Cu and 1.5 wt% Mn performed better than CHA containing the same amounts of Cu and Mn. In the experiments comparing AEI and CHA, SAR values are also not given. Experiments conducted on two chabazites with SAR values of 13 and 22 (1.5 wt% Cu and Mn each) each showed that CHA with the lower SAR value showed better NO x BEA and MFI containing 3 wt% or 1.5 wt% Cu and Mn each showed that in the case of BEA, NO x The conversion was not affected by the presence of Mn, while BEA containing Cu and Mn showed lower N2O formation compared to BEA containing Cu alone; and in the case of MFI, zeolite containing only Cu showed better NO formation compared to MFI containing both Cu and Mn. x conversion and lower N2O formation.
[0029] US2015 / 078989 A1 discloses a method for selective catalytic reduction of NO in lean exhaust gas. x The catalyst composition of the present invention comprises an aluminosilicate material comprising silica and alumina in a CHA framework and having a silica to alumina ratio (SAR) of about 10 to about 25, and about 1 wt % to about 5 wt % of a base metal ("BM"), based on the total weight of the zeolite material, wherein the base metal is disposed in the zeolite material as a free and / or extra-framework exchange material, and an alkali metal or alkaline earth metal (collectively referred to as "AM") disposed in the zeolite material as a free and / or extra-framework exchange metal. The base metal is selected from chromium, manganese, iron, cobalt, nickel, copper, and mixtures thereof. The alkali metal or alkaline earth metal is selected from sodium, potassium, rubidium, cesium, magnesium, calcium, strontium, and barium. BM and AM are present in a molar ratio of about 15:1 to about 1:1, respectively. These examples show that the SSZ-13 zeolite has a SAR value of 17 and is promoted with copper and a second metal, the second metal being one of calcium, potassium, magnesium, sodium, cesium, or manganese.
[0030] Always need to show good NO x The invention relates to an SCR catalytically active composition which has a high conversion rate, has a light-off temperature which is as low as possible and at the same time exhibits a low N2O selectivity.
[0031] Problems to be solved by the present invention
[0032] It is therefore an object of the present invention to provide a catalytically active composition for removing nitrogen oxides from the exhaust gases of combustion engines, which exhibits a high conversion of nitrogen oxides to nitrogen via good activity and a good selectivity for this conversion, while exhibiting a low N2O selectivity. Another object of the present invention is to provide a device and a system for treating the exhaust gases of combustion engines, which device and system comprise the catalytically active composition according to the invention. A further object of the present invention is to provide a catalytically active composition for reducing NO from the exhaust gases of internal combustion engines. x Method of emission and optionally also particulate matter.
[0033] Solution to the problem
[0034] The object of the present invention is to provide a catalytically active composition for removing nitrogen oxides from the exhaust gases of combustion engines, which catalytically active composition shows a high conversion of nitrogen oxides to nitrogen via good activity and a good selectivity for this conversion and at the same time shows a low N2O selectivity. This object is solved by a catalytically active composition comprising a crystalline aluminosilicate zeolite having a CHA framework type, wherein the zeolite has a SAR value of between 7 and 25, a copper content of between 3.0 and 4.5% by weight, a manganese content of 0.3 and 4.0% by weight, wherein the copper and manganese are calculated as CuO and MnO and are based on the total weight of the zeolite, and wherein the sum of the molar amounts of copper and manganese divided by the molar amount of aluminum is in the range between 0.11 and 0.96.
[0035] Explained below are catalytically active compositions for removing nitrogen oxides from the exhaust gases of combustion engines and devices and systems for treating the exhaust gases of combustion engines, the catalytically active compositions showing a high conversion of nitrogen oxides to nitrogen via good activity and good selectivity for this conversion and at the same time showing a low N2O selectivity, the devices and systems comprising the catalytically active compositions, wherein the invention encompasses all embodiments indicated below, both individually and in combination with one another.
[0036] The selective catalytic reduction of nitrogen oxides to nitrogen is hereinafter referred to as "SCR" or "SCR reaction".
[0037] A "catalytically active composition" is a substance or mixture of substances that is capable of converting one or more components of an exhaust gas into one or more other components. Examples of such catalytically active compositions are oxidation catalyst compositions that are, for example, capable of converting volatile organic compounds and carbon monoxide into carbon dioxide or converting ammonia into nitrogen oxides. Another example of such a catalyst is a selective catalytic reduction catalyst (SCR) composition that is, for example, capable of converting nitrogen oxides into nitrogen and water. In the context of the present invention, an SCR catalyst is a catalyst comprising a carrier substrate and a carrier coating containing an SCR catalytically active composition. An ammonia slip catalyst (ASC) is a catalyst comprising a carrier substrate, a carrier coating containing an oxidation catalyst, and a carrier coating containing an SCR catalytically active composition.
[0038] Molecular sieves are materials with pores of uniform size (i.e. with very small pores). These pore sizes are similar in size to small molecules, so large molecules cannot enter or be adsorbed, while smaller molecules can enter or be adsorbed. In the context of the present invention, molecular sieves are zeolites. Zeolites are made of corner-sharing tetrahedral SiO4 and AlO4 units. They are also called "aluminosilicates" or "aluminosilicates". In the context of the present invention, these two terms are used synonymously.
[0039] As used herein, the term "non-zeolitic molecular sieve" refers to a corner-sharing tetrahedral framework in which at least a portion of the tetrahedral sites are occupied by elements other than silicon or aluminum. If a portion of the silicon atoms, but not all of them, are replaced by phosphorus atoms, it is referred to as a so-called "silicoaluminophosphate" or "SAPO". If all of the silicon atoms are replaced by phosphorus, it is referred to as an aluminophosphate or "AlPO".
[0040] "Zeolite framework type" (also referred to as "framework type") refers to the corner-sharing network of tetrahedrally coordinated atoms. Zeolites are generally classified according to their pore size, which is defined by the ring size of the largest pore opening. Large pore zeolites have a maximum ring size of 12 tetrahedral atoms, medium pore zeolites have a maximum pore size of 10 tetrahedral atoms, and small pore zeolites have a maximum pore size of 8 tetrahedral atoms. Well-known small pore zeolites belong in particular to the AEI, CHA (chabazite), ERI (erionite), LEV (chabazite), AFX and KFI frameworks. Examples of zeolites with large pore size are zeolites of the faujasite (FAU) framework type and beta zeolite (BEA).
[0041] A "zeotype" includes any material in a family of materials that is based on the structure of a particular zeolite. Thus, a particular "zeolite type" includes, for example, aluminosilicates, SAPOs, and AlPOs that are based on the structure of a particular zeolite framework type. Thus, for example, chabazite (CHA), aluminosilicates SSZ-13, Linde R, and ZK-14, silicoaluminophosphates SAPO-34, and aluminophosphates MeAlPO-47 all belong to the chabazite framework type. The skilled person knows which aluminosilicates, silicoaluminophosphates, and aluminophosphates belong to the same zeolite type. In addition, zeolites and non-zeolitic molecular sieves that belong to the same zeolite type are listed in the database of the International Zeolite Association (IZA). The skilled person can use this knowledge and the IZA database without departing from the scope of the claims.
[0042] The silica to alumina ratio (SiO2:Al2O3) of a zeolite is hereinafter referred to as the "SAR value".
[0043] A "catalyst support substrate" (also simply referred to as a "support substrate") is a support to which the catalytically active composition is attached and which gives shape to the final catalyst. Thus, the support substrate is a support for the catalytically active composition.
[0044] As used in the present invention, a "washcoat" is an aqueous suspension of the catalytically active composition and optionally at least one binder. Suitable binder materials are, for example, aluminum oxide, titanium dioxide, silicon dioxide, zirconium dioxide or mixtures thereof, for example mixtures of silicon dioxide and aluminum oxide.
[0045] The carrier coating that has been attached to the catalyst support substrate is called a "coating". Two or more carrier coatings can also be attached to the support substrate. The skilled person knows that two or more carrier coatings can be attached to a single support substrate by "layering" or "zoning", and that layering and zoning can also be combined. In the case of layering, the carrier coatings are attached to the support substrate one after another. The carrier coating that is first attached and therefore in direct contact with the support substrate represents the "bottom layer", and the carrier coating that is last attached represents the "top layer". In the case of zoning, the first carrier coating is attached to the support substrate from the first front side A of the support substrate toward the other front side B, but not attached to the entire length of the support substrate, but only to the end point between the front side A and the front side B. Then, the second carrier coating is attached to the support, starting from the front side B, until the end point between the front side B and the front side A. The end points of the first and second carrier coatings do not have to be the same: if they are the same, the two carrier coating areas are adjacent to each other. However, if the end points of the two carrier coating areas, both located between the front side A and the front side B of the support substrate, are not the same, there may be a gap between the first and second carrier coating areas, or they may overlap. As mentioned above, layering and zoning can also be combined if, for example, one washcoat is applied over the entire length of the carrier substrate and another washcoat is applied only from one face side to an end point between the two face sides.
[0046] In the context of the present invention, "washcoat loading" is the mass of catalytically active composition per volume of carrier substrate.
[0047] The skilled person is aware of the preparation of washcoats in the form of suspensions and dispersions.
[0048] Suspensions and dispersions are heterogeneous mixtures comprising solid particles and solvents. The solid particles are not dissolved, but suspended throughout the solvent, floating freely in the medium. If the solid particles have an average particle size of less than or equal to 1 μm, the mixture is called a dispersion; if the average particle size is greater than 1 μm, the mixture is called a suspension. The carrier coating in the sense of the present invention comprises a solvent (usually water) and suspended or dispersed particles represented by particles of one or more catalytically active compositions, and optionally particles of at least one binder as described above. This mixture is generally referred to as a "carrier coating slurry". The slurry is applied to a carrier substrate and then dried to form a coating as described above. In the context of the present invention, the term "carrier coating suspension" is used for a mixture of solvent, particles of one or more catalytically active compositions and optionally particles of at least one binder, regardless of the individual or average particle size. This means that in the "carrier coating suspension" according to the present invention, the size of the individual particles and the average particle size of the one or more catalytically active solid particles may be less than 1 μm, equal to 1 μm and / or greater than 1 μm.
[0049] The term "mixture" as used in the context of the present invention is a material composed of two or more different substances that are physically combined and in which each component retains its own chemical properties and composition. Although its components have not changed chemically, the physical properties of the mixture (such as its melting point) may be different from the physical properties of the components.
[0050] A "catalytic substrate monolith" is a carrier substrate comprising a catalytically active composition. The carrier may be coated with a washcoat comprising the catalytically active composition, wherein the washcoat comprises the catalytically active composition and optionally at least one binder. Alternatively, the catalytically active composition may be a component of the carrier substrate itself.
[0051] A "device" as used in the context of the present invention is a piece of equipment designed to serve a specific purpose or to perform a specific function. The catalytic device according to the present invention serves this purpose and has the function of removing nitrogen oxides from the exhaust gases of an internal combustion engine. A "device" as used in the present invention may consist of one or more catalysts, also referred to as a "catalytic article" or "brick" as defined above.
[0052] "Upstream" and "downstream" are terms relative to the normal flow direction of the exhaust gas in the exhaust pipe. "Zone or catalyst 1 located upstream of zone or catalyst 2" means that zone or catalyst 1 is located closer to the exhaust gas source, i.e., closer to the motor, than zone or catalyst 2. The flow direction is from the exhaust gas source to the exhaust pipe. Therefore, according to this flow direction, the exhaust gas enters each zone or catalyst at its inlet end and leaves each zone or catalyst at its outlet end.
[0053] As used in the context of the present invention, the term "nitrogen oxides" encompasses nitric oxide (NO), nitrogen dioxide (NO2) and nitrous oxide (N2O). In contrast, however, the term "NO x " covers only NO and NO2, but not N2O, although nitrous oxide is also an oxide of nitrogen. However, "nitrogen oxides" and "NO x This distinction between " and " is widely used by technicians.
[0054] The term "NOx conversion rate" as used in the context of the present invention means the NO x The percentage converted to nitrogen.
[0055] “N2O selectivity” (S N2O ) is the NO in the gas feed x and the percentage of NH3 converted to N2O.
[0056] N2O selectivity can be calculated according to the following formula:
[0057]
[0058] in
[0059] N2O 入口 = N2O quantity at the inlet of the catalyst
[0060] N2O 出口 = N2O quantity at the outlet of the catalyst
[0061] NH 3,入口 = NH3 amount at the inlet of the catalyst
[0062] NH 3,出口 = NH3 amount at the outlet of the catalyst
[0063] NO x,入口 = NO at the inlet of the catalyst x quantity
[0064] NO x,出口 = NO at the outlet of the catalyst x quantity
[0065] "Catalytic activity" or just "activity" is the increase in the rate of a chemical reaction caused by the presence of the catalytically active composition.
[0066] As is known to the skilled person, the SCR reaction requires a reducing agent to reduce the nitrogen oxides to nitrogen and water. A suitable reducing agent is ammonia, and the SCR reaction in the presence of ammonia is referred to as "NH3-SCR". The ammonia used as a reducing agent can be obtained by feeding liquid or gaseous ammonia or an ammonia precursor compound into the exhaust gas. If an ammonia precursor is used, it is pyrolyzed and hydrolyzed to form ammonia. Examples of such ammonia precursors are ammonium carbamate, ammonium formate, and preferably urea. Alternatively, ammonia can be formed by a catalytic reaction of an ammonia precursor in the exhaust gas.
[0067] In an embodiment of the present invention, the crystalline aluminosilicate zeolite having a CHA framework structure is selected from the group consisting of zeolite types SSZ-13, LZ-218, Linde D, Linde R, Phi and ZK-14, with SSZ-13 being preferred.
[0068] The crystalline aluminosilicate having a CHA framework structure has a SAR value between 7 and 25, preferably between 9 and 23, more preferably between 11 and 20, even more preferably from 11 to 17, and most preferably from 13 to 17.
[0069] The crystalline aluminosilicate having a CHA framework structure has a copper content of between 3.0 and 4.5 wt.-%, preferably between 3.2 and 4.5 wt.-%, more preferably 3.5 to 4.3 wt.-%, calculated as CuO and based on the total weight of the zeolite.
[0070] The crystalline aluminosilicate having a CHA framework structure has a manganese content of between 0.3 and 4.0 wt.-%, preferably 0.3 to 3.5 wt.-%, more preferably 0.5 to 3.2 wt.-%, calculated as MnO and based on the total weight of the zeolite.
[0071] "Total weight of zeolite" is the sum of the weight of white zeolite and the weight of copper and manganese, wherein the weight of copper and manganese is calculated as their respective oxides CuO and MnO. In the context of the present invention, "white zeolite" is an aluminosilicate zeolite composed of TO4 tetrahedrons and having a CHA framework structure, which contains neither copper nor manganese nor any other transition metal. Due to the absence of transition metals, this zeolite is colorless, also referred to as "white", and the transition metal provides color to the zeolite, for example, blue in the case of copper loading, or mixed colors in the presence of more than one transition metal (such as copper). It is known to those skilled in the art that "white zeolite" generally includes protons and alkali metal cations, although often present in trace amounts. However, protons and alkali metals do not provide color to zeolite. Therefore, the term "white zeolite" also includes aluminosilicate zeolites with a CHA framework structure, which include protons and alkali metal cations.
[0072] The sum of the molar amounts of copper and manganese divided by the amount of aluminum, ie (Cu+Mn) / Al, ranges between 0.11 and 0.96, preferably between 0.20 and 0.80, more preferably between 0.28 and 0.35, even more preferably between 0.31 and 0.35.
[0073] The amounts of copper, manganese, aluminum, silicon and sodium, potassium, rubidium, cesium, magnesium, calcium, strontium and barium can be measured by ICP-AES (Inductively Coupled Plasma Atomic Emission Spectroscopy), ICP-OES (Inductively Coupled Plasma Optical Emission Spectroscopy) or XRF (X-ray Fluorescence Spectroscopy). Energy dispersive X-ray spectroscopy, known as EDS, EDX or EDXS, allows the analysis of elements with an atomic number of 8 or more, and is therefore able to measure the above-mentioned metals and oxygen, etc. The skilled person knows how to perform such an analysis and can apply this knowledge to the zeolite according to the invention without departing from the scope of the claims.
[0074] The SAR value of the zeolite can be determined by NMR (nuclear magnetic resonance), XRF or ICP-OES. The metal to metal molar ratio in the zeolite, such as the copper to aluminum molar ratio or the copper to manganese molar ratio, can be measured by ICP-OES or XRF. These methods are known to those skilled in the art, and they can be applied in the context of the present invention without departing from the scope of the claims.
[0075] Aluminosilicate chabazite and its zeolite type are commercially available. The method for preparing chabazite is disclosed in, for example, EP 2931 406 B1, US2018 / 079650 A1, WO 2017 / 080722 A1, US 2018 / 127282A1 and WO 2018 / 189177 A1. Generally, the synthesis of aluminosilicate zeolite includes mixing a silicon source, an aluminum source, an alkali metal or alkaline earth metal hydroxide, water and at least one organic structure directing agent (OSDA) and an optional salt (such as a copper salt or an iron salt). The mixture forms a gel, and the gel is aged, heat-treated, purified and optionally calcined. Those skilled in the art know how to synthesize aluminosilicate chabazite and its zeolite type. It is also known that some methods for preparing aluminosilicate zeolites (particularly CHA) use OSDA, which is a complex of copper and organic polyamines, such as copper tetraethylene pentamine (Cu-TEPA). If such a complex of copper and an organic polyamine is used, the zeolite obtained therefrom already contains copper. In this case, the zeolite obtained by synthesis already contains copper. In other cases, however, the synthesis gel does not contain copper.
[0076] In the context of the present invention, the amount of copper and manganese can be adjusted according to the desired amount of copper and manganese and according to the sum of the desired molar amounts of copper and manganese divided by the molar amount of aluminum, as indicated above by the ion exchange method. "Adjustment" means that if Cu and Mn are not present in the synthesized zeolite, they can be introduced for the first time, or if they are introduced during the synthesis, their amount can be increased or decreased, but their amount is outside the range required for the crystalline aluminosilicate according to the present invention. Increasing or decreasing the amount of metal is particularly relevant to copper and manganese if they have been introduced by the synthesis method.
[0077] For example, copper can be introduced via ion exchange. In a first step, an ammonium exchange is performed to introduce copper by using NH4 + The cation exchange is used to remove the alkali metal cations or alkaline earth metal cations from the zeolite framework. In the second step, NH4 + is replaced by copper cations. The copper content of the resulting copper-containing zeolite can be easily controlled via the amount of copper salt and the number of ion exchange procedures performed. The copper content can be measured by ICP-AES or XRF as described above.
[0078] Copper and manganese can also be removed by using NH4 + The cations are removed by liquid ion exchange.
[0079] Methods for introducing ammonium, copper and manganese cations and for removing copper and manganese cations are well known to those skilled in the art, respectively. They can be applied to the zeolite according to the present invention without departing from the scope of the claims. For example, ammonium cations can be easily introduced via liquid ion exchange, and copper cations can also be easily introduced via liquid ion exchange, incipient wetness impregnation or solid state ion exchange.
[0080] The methods for introducing copper cations are given below by way of example. These methods are suitable for obtaining the zeolites according to the invention loaded with copper and manganese.
[0081] Liquid ion exchange
[0082] NH4 + Liquid ion exchange can be carried out by treating the zeolite with an aqueous solution of an ammonium salt (eg NH4Cl or NH4NO3).
[0083] Cu 2+ Liquid ion exchange can be carried out by treating the zeolite with an aqueous solution of a copper salt such as copper acetate (Cu(Ac)2), copper nitrate (Cu(NO3)2), copper acetylacetonate (Cu(acac)2) or copper chloride (CuCl2). This procedure can be repeated multiple times to obtain the desired copper content.
[0084] It is obvious to those skilled in the art that the ratio of copper to zeolite in the liquid ion exchange can be adjusted according to the desired copper content of the final zeolite. In general, aqueous solutions with higher copper content produce higher copper-containing zeolites. Without departing from the scope of the claims, the skilled person can easily determine which copper concentration should be selected and how often the procedure will be repeated.
[0085] Optionally, the ammonium exchanged zeolite may be subjected to a heat treatment in order to decompose the ammonium ions. Subsequently, a copper exchange may be performed as described above.
[0086] Initial Wetness Impregnation
[0087] An aqueous solution of a copper salt, such as copper acetate (Cu(Ac)2), copper nitrate (Cu(NO3)2) or copper chloride (CuCl2) is dissolved in a sufficient volume of water. The amount of copper salt is equal to the preferred amount of copper in the zeolite. Incipient wetness impregnation is performed at room temperature. The copper-exchanged zeolite is then dried at a temperature between 60 and 70°C for 8 to 16 hours, and the mixture is subsequently heated to a temperature in the range of 550 to 900°C.
[0088] Solid State Ion Exchange
[0089] Suitable copper salts are, for example, copper acetate (Cu(Ac)2), copper nitrate (Cu(NO3)2), copper chloride (CuCl2), copper (II) oxide (CuO), copper (I) oxide (Cu2O) and copper acetylacetonate (Cu(acac)2). The copper salt and the zeolite are mixed in a dry state and the mixture is subsequently heated to a temperature in the range of 550°C to 900°C. A method for preparing a metal-containing zeolite is disclosed, for example, in US2013 / 0251611A1. This method can be applied to the zeolite of the present invention without departing from the scope of the claims.
[0090] The ion exchange method for exchanging copper ions and ammonium ions described above can also be used for exchanging manganese. As is well known, the introduction of different metal ions (such as copper ions and manganese ions) can be performed sequentially or by co-ion exchange. Sequential ion exchange means that different cations are introduced one by one, such as by introducing copper in the first step and introducing manganese in the second step. Co-ion exchange means that all cations (such as copper and manganese) are exchanged together in one step. If more than two different cations, such as cations of copper, manganese and rare earth metals, will be exchanged, sequential ion exchange and co-ion exchange can also be applied. Those skilled in the art know how to apply the ion exchange method for exchanging copper ions and ammonium ions described above to the exchange of other ions, and those skilled in the art can apply this knowledge to the present invention without departing from the scope of the claims.
[0091] Suitable manganese salts for introducing manganese by ion exchange are, for example, manganese(II) acetate (Mn(CH3COO)2), manganese(II) acetylacetonate (Mn(acac)2), manganese(III) acetylacetonate (Mn(acac)3), manganese(II) chloride (MnCl2), manganese(II) sulfate (MnSO4) and manganese(II) nitrate (Mn(NO3)2).
[0092] The crystalline aluminosilicate zeolite having a CHA framework type according to the present invention can be used to remove NO from combustion exhaust gases. x In this process, also known as SCR (Selective Catalytic Reduction), these zeolites are used to convert NO x The use of the zeolite according to the invention as a catalytically active composition for NOx conversion is therefore applicable to exhaust gas purification systems of mobile and stationary combustion engines. Mobile internal combustion engines are, for example, gasoline and diesel engines and hydrogen internal combustion engines (H2 ICE). The skilled person knows that the combustion process usually takes place under oxidizing conditions and that the fuel also contains nitrogen or nitrogen compounds, which can be oxidized to NO x, and / or the combustion occurs in the presence of air, wherein the oxygen present in the air acts as an oxidant and at least a portion of the nitrogen present in the air may be oxidized to NO x .
[0093] Mobile internal combustion engines may be engines for on-road and off-road applications, such as gasoline and diesel engines as well as hydrogen internal combustion engines, used in passenger cars, agricultural machinery such as agricultural and forestry tractors and harvesters, construction wheel loaders, bulldozers, highway excavators, forklifts, road maintenance equipment, snowplows, ground support equipment at airports, aerial lifts and mobile cranes.
[0094] Stationary internal combustion engines are, for example, power stations, industrial heaters, combined heat and power plants including wood-burning boilers, stationary diesel and gasoline engines, industrial and municipal waste incinerators, industrial drilling rigs, compressors, plants for the manufacture of glass, steel and cement, plants for the manufacture of nitrogen-containing fertilizers, plants for the production of nitric acid (for example plants using the Ostwald process), and ammonia burners for supplying fuel to gas turbines for the production of nitric acid.
[0095] In a preferred embodiment, the crystalline aluminosilicate small pore zeolite according to the present invention can be used to remove NO from automobile combustion exhaust. x In the method, the exhaust gas comes from a diesel or gasoline engine.
[0096] The object of providing a device for treating exhaust gases of combustion engines is solved by a catalytic substrate monolith comprising a catalyst for use in treating automobile combustion exhaust gases for converting NO x SCR catalytically active composition, wherein for converting NO x The SCR catalytically active composition is a crystalline aluminosilicate zeolite having a CHA framework according to the invention.
[0097] In some embodiments of the SCR catalytically active composition according to the invention, the SCR catalytically active composition is present in the form of a coating on a carrier substrate, i.e. as a carrier coating on a carrier substrate. The carrier substrate can be a so-called honeycomb flow-through substrate and a wall-flow filter as well as a corrugated substrate, a wound or filled fiber filter, an open-cell foam and a sintered metal filter. In a preferred embodiment, the carrier substrate is a honeycomb flow-through substrate or a honeycomb wall-flow filter.
[0098] Flow-through substrates and wall-flow filters can be composed of inert materials such as silicon carbide, aluminum titanate, and cordierite. Such carrier substrates are well known to the skilled person and are commercially available. Corrugated substrates are made of ceramic E-glass fiber paper. They are also well known to the skilled person and are commercially available.
[0099] When the SCR catalytically active composition is present in the form of a coating on a carrier substrate, it is typically present on or in the substrate in an amount of about 10 g / L to about 600 g / L, preferably about 100 g / L to about 300 g / L, as calculated by molecular sieve weight per volume of total catalyst article.
[0100] The SCR catalytically active composition can be coated on or into a substrate using known carrier coating techniques. In this method, the molecular sieve powder is suspended in a liquid medium together with a binder and a stabilizer. The carrier coating can then be applied to the surface and walls of the substrate. The carrier coating optionally also contains a binder based on TiO2, SiO2, Al2O3, ZrO2, CeO2 and a combination thereof. In addition, the carrier coating may optionally include additives. The additive may be present with the binder, as mentioned above, or the carrier coating may contain only a binder or only an additive. Suitable additives are polysaccharides, polyvinyl alcohol, glycerol; linear or branched multifunctional organic molecules having two or more carbon atoms in the chain, having up to about 12 carbon atoms (C n ; wherein 2≤n≤12); a salt of a basic quaternary ammonium, wherein one or more quaternary ammonium groups are attached to a length of C n on four carbon chains of , where 1≤n≤5, and where the cations are balanced as salts using, but not limited to, one of the following anions: hydroxide, fluoride, chloride, bromide, iodide, carbonate, sulfate, sulfite, oxalate, maleate, phosphate, aluminate, silicate, borate or other suitable organic or inorganic counterions; an inorganic base selected from, but not limited to, the following list: lithium hydroxide, sodium hydroxide, potassium hydroxide, magnesium hydroxide, calcium hydroxide, strontium hydroxide and barium hydroxide; and simple salts of transition elements or rare earth elements, including, but not limited to, the following: nitrates, carbonates, sulfates, phosphates, borates of rare earth elements with atomic numbers 57 (La) to 71 (Lu) and including Sc, Y, Ti, Zr and Hf, as mentioned above.
[0101] In a preferred embodiment, the additive is a polysaccharide selected from the group consisting of galactomannan gum, xanthan gum, guar gum, curdlan, schizophyllan, scleroglucan, Diutan gum, Welan gum, starch, cellulose or alginate, or derived from starch, cellulose (i.e. cellulosic) or alginate, and mixtures thereof. The cellulose additive may be selected from the group consisting of carboxymethyl cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, methyl cellulose, methyl hydroxyethyl cellulose, methyl hydroxypropyl cellulose and ethyl hydroxyethyl cellulose.
[0102] More preferably, the additive is xanthan gum, guar gum or a mixture thereof. Even more preferably, the additive is xanthan gum.
[0103] In case the first and / or second washcoat comprises an additive, the additive is present in an amount of up to 20 wt.-%, preferably 3 to 15 wt.-%, more preferably 6 to 10 wt.-%, based on the total weight of the oxides, wherein the "total weight of the oxides" is the sum of the weight of the zeolite and the binder. It should be understood that if the washcoat does not comprise a binder, the "total weight of the oxides" corresponds to the weight of the zeolite.
[0104] In other embodiments, the support substrates themselves may be catalytically active, and they may also contain the catalytically active composition, i.e. the crystalline aluminosilicate zeolite according to the invention. In addition to the catalytically active composition, these support substrates contain a matrix component. In this case, all inert materials used for the production of catalyst substrates can be used as matrix components. They are, for example, silicates, oxides, nitrides or carbides, with magnesium aluminum silicates being particularly preferred.
[0105] In a further embodiment of the SCR catalytically active composition according to the invention, the catalyst itself forms part of a support substrate, for example as part of a flow-through substrate or a wall-flow filter. Such a support substrate additionally comprises the above-mentioned matrix components.
[0106] The carrier substrate containing the SCR catalytically active composition according to the present invention can be used as it is for exhaust gas purification. Alternatively, it can be coated with a catalytically active composition, for example, coated with an SCR catalytically active composition. As long as these materials exhibit SCR catalytic activity, the SCR catalytically active composition mentioned above is a suitable material.
[0107] In one embodiment, the catalytically active support material is produced by mixing 10% to 95% by weight of at least one inert matrix component and 5% to 90% by weight of a catalytically active composition and then extruding the mixture according to well-known protocols. As already described above, the inert materials conventionally used for the production of catalyst substrates can be used as the matrix component in this embodiment. Suitable inert matrix materials are, for example, silicates, oxides, nitrides and carbides, among which magnesium aluminum silicates are particularly preferred. The catalytically active support material obtainable by such a process is referred to as an "extruded catalytic substrate monolith".
[0108] The application of the catalytically active catalyst to an inert support substrate or to a support substrate which is itself catalytically active, and the application of the catalytically active coating to a support substrate which comprises the catalyst according to the invention, can be carried out according to the production methods familiar to the person skilled in the art, for example by the widely used dip coating, pump coating and draw coating, followed by subsequent thermal aftertreatment (calcination).
[0109] The skilled person knows that in the case of a wall-flow filter, the average pore size and the average particle size of the catalytically active component according to the invention can be adjusted to one another in the following manner: the coating thus obtained is located on the porous walls of the channels forming the wall-flow filter (coating on the wall). However, preferably, the average pore size and the average particle size are adjusted to one another in the following manner: the catalyst according to the invention is located within the porous walls of the channels forming the wall-flow filter. In this preferred embodiment, the inner surface of the pores is coated (coating in the wall). In this case, the average particle size of the catalyst according to the invention must be small enough to be able to pass through the pores of the wall-flow filter. A wall-flow filter coated with an SCR catalytically active composition is also referred to as a "SDPF" (SCR on DPF, i.e. an SCR catalytically active composition coated on a diesel particulate filter) or a "SCRF" (SCR on a filter). Therefore, the present invention covers a catalytic substrate monolith, wherein the monolith is a wall-flow filter and the SCR catalytic composition comprises a crystalline aluminosilicate zeolite according to the invention.
[0110] Furthermore, the present invention encompasses an ammonia slip catalyst (ASC). It is well known to the skilled person that in an exhaust gas purification system, the ASC is preferably located downstream of the SCR, since due to the dynamic driving conditions, a discernible amount of NH3 leaves the SCR. Therefore, converting the excess ammonia leaving the SCR is mandatory, since ammonia is also an emission regulating gas. The oxidation of ammonia leads to the formation of NO as the main product, which therefore has an impact on the NOx of the entire exhaust system. x The ASC can therefore be located downstream of the SCR to reduce the emission of additional NO. The ASC catalyst combines the critical NH3 oxidation function with the SCR function. Ammonia entering the ASC is partially oxidized to NO. The newly oxidized NO and the not yet oxidized NH3 within the ASC can therefore react with N2 according to the usual SCR reaction scheme. In doing so, the ASC is able to eliminate trace amounts of ammonia by converting them into N2 in a parallel mechanism.
[0111] Those skilled in the art will appreciate that the SCR catalyst and the ASC catalyst may exist as two continuous catalytic products, or the SCR function and the ASC function may exist on a single catalytic product. In the case of two continuous catalytic products, the upstream catalytic product is an SCR catalyst comprising a carrier substrate and a carrier coating comprising an SCR catalytically active composition, and the downstream catalytic product is an ASC catalyst comprising a carrier substrate, a carrier coating comprising an oxidation catalyst, and a carrier coating comprising an SCR catalytically active composition. In the case where the SCR catalyst and the ASC catalyst are present on a single substrate, the carrier coating comprising the SCR catalytically active composition but without the oxidation catalyst is coated on the upstream region of the carrier substrate, and the downstream region of the carrier substrate contains a bottom layer having a carrier coating comprising an oxidation catalyst and a top layer having a carrier coating comprising an SCR catalytically active composition. In all embodiments in which the SCR catalyst is combined with a downstream ASC catalyst, the SCR catalytically active composition of the SCR catalyst is preferably a crystalline aluminosilicate zeolite according to the present invention. The SCR catalytically active composition of the ASC may be selected from crystalline aluminosilicate zeolites according to the present invention, other zeolites and non-zeolitic molecular sieves as described above, and mixed oxides comprising vanadium oxide and titanium oxide. When other zeolites and non-zeolitic molecular sieves are used, they are preferably loaded with at least one transition metal, preferably copper and / or iron. When a mixed oxide comprising vanadium oxide and titanium oxide is used, it may also optionally comprise oxides of one or more elements selected from tungsten, silicon, aluminum, zirconium, molybdenum, niobium and antimony.
[0112] Platinum group metals are used as oxidation catalysts in ASCs, and zeolites can be used for SCR functions. The noble metal is a platinum group metal selected from ruthenium, rhodium, palladium, osmium, iridium, platinum and mixtures thereof. Preferably, the noble metal is selected from palladium, platinum, rhodium and mixtures thereof, more preferably, the noble metal is platinum. In a preferred embodiment, the platinum group metal is added to the carrier coating slurry in the form of a precursor salt and applied to the carrier monolith. The platinum group metal is present in a concentration of 0.01 wt % to 10 wt %, preferably 0.05 wt % to 5 wt %, and even more preferably 0.1 wt % to 3 wt %, calculated as the corresponding platinum group metal and based on the total weight of the carrier coating load. In a preferred embodiment, the platinum group metal is platinum and is present in a concentration of 0.1 wt % to 1 wt % calculated as Pt and based on the total weight of the carrier coating load.
[0113] In one embodiment, the ASC catalyst is a catalytic substrate monolith, wherein the monolith is a flow-through monolith coated with a bottom layer comprising the oxidation catalyst and a top layer comprising a crystalline aluminosilicate zeolite having a CHA framework type according to the present invention.
[0114] In all devices for treating exhaust gases of combustion engines comprising a crystalline aluminosilicate zeolite according to the invention as an SCR catalytically active composition, one or more of these SCR catalytically active compositions can be used. If more than one SCR catalytically active composition is present, they may be present in a carrier coating in the form of two or more different layers, two or more different regions as a mixture of two or more different SCR catalytically active compositions. In addition, the layers or regions may independently of one another contain a single SCR catalytically active composition or a mixture of two or more SCR catalytically active compositions. If two or more crystalline aluminosilicate zeolites according to the invention differ in at least one parameter selected from the group consisting of framework type, SAR value, copper content and / or manganese content, they are "different".
[0115] Furthermore, the present invention provides an emissions treatment system for removing NOx emissions and optionally also for removing particulate matter from the exhaust gas of an internal combustion engine, the system comprising, from upstream to downstream, in the following order:
[0116] a) a device for injecting ammonia or an ammonia precursor solution into the exhaust gas stream,
[0117] b) A catalytic substrate monolith comprising an SCR catalytically active composition for converting NOx in automobile combustion exhaust gas, wherein the SCR catalytically active composition for converting NOx is a crystalline aluminosilicate zeolite having a CHA framework type according to the present invention, and wherein the substrate monolith is selected from a honeycomb flow-through substrate, a honeycomb wall-flow filter, a corrugated substrate, a wound or filled fiber filter, an open-cell foam, a sintered metal filter and an extruded catalytic substrate monolith.
[0118] Those skilled in the art will appreciate that where the substrate monolith is a flow-through monolith or a corrugated substrate, the corresponding catalytic substrate monolith will only remove NOx emissions. However, if the substrate monolith is a wall-flow filter, the corresponding catalytic substrate monolith will also remove particulate matter.
[0119] It is known to those skilled in the art that the SCR reaction requires the presence of ammonia as a reducing agent. Ammonia can be supplied in a suitable form, for example in the form of liquid ammonia or in the form of an aqueous solution of an ammonia precursor, and added to the exhaust gas stream via a device for injecting ammonia or an ammonia precursor as required. Suitable ammonia precursors are, for example, urea, ammonium carbamate or ammonium formate. Alternatively, ammonia can be formed by a catalytic reaction in the exhaust gas.
[0120] A common method is to carry an aqueous urea solution and dose it to the catalyst according to the invention via an upstream injector and a metering unit as required. Means for injecting ammonia, such as an upstream injector and a metering unit, are well known to the skilled person and can be used in the present invention without departing from the scope of the claims.
[0121] Furthermore, it will be appreciated that for removing NO from the exhaust gas of an internal combustion engine x Emission treatment systems that remove particulate matter and optionally also remove particulate matter may include additional catalytic articles such as a diesel oxidation catalyst (DOC), an ammonia slip catalyst (ASC), a catalyzed or non-catalyzed particulate filter, a passive NO x Adsorber (PNA) and / or lean NO x The system includes a catalytic substrate monolith, the catalytic substrate monolith comprising a catalyst for converting NO in automobile combustion exhaust gas. x SCR catalytically active composition, wherein for converting NO x The SCR catalytically active composition is a crystalline aluminosilicate zeolite according to the invention. A catalyzed particulate filter may be coated with a diesel oxidation catalyst, thereby forming a "catalyzed diesel particulate filter (CDPF)", or it may be coated with a SCR catalytically active composition, thereby forming a SDPF.
[0122] In one embodiment of the present invention, an emission treatment system comprising a catalytic substrate monolith comprising an SCR catalytically active composition according to the present invention is arranged in a close-coupled position. The term "closely coupled" refers to a position in the exhaust gas treatment system of the engine in which the catalytic device is located less than 1 meter downstream of the exhaust manifold or turbocharger of the engine. In a preferred embodiment, the emission treatment system comprising a catalytic substrate monolith comprising an SCR catalytically active composition according to the present invention further comprises one or more particulate filters. In this embodiment, the "first" filter is the filter arranged closest to the engine. The "second" filter, if present, is located downstream of the first filter, either directly after the first filter or at a further downstream position. In this embodiment, the catalytic substrate monolith comprising an SCR catalytically active composition according to the present invention, which is arranged in a close-coupled position, is arranged upstream of the first filter.
[0123] As mentioned above, the substrate monolith can be a honeycomb flow-through substrate, a honeycomb wall-flow filter, a corrugated substrate, a wound or filled fiber filter, an open-cell foam or a sintered metal filter. Preferably, it is a honeycomb flow-through substrate or a honeycomb wall-flow filter. If the catalytic substrate monolith is a honeycomb wall-flow filter comprising an SCR catalytically active composition according to the invention, it is a SDPF.
[0124] In yet another embodiment of the present invention, the emission treatment system is arranged in an underfloor position. Underfloor catalyst elements are also known in the prior art and are located downstream of any close-coupled and / or medium-coupled catalysts, adjacent to the muffler of the vehicle or in combination with the muffler of the vehicle, located under the floor of the vehicle. In this embodiment, a catalytic substrate monolith comprising an SCR catalytically active composition according to the present invention is arranged downstream of the first filter. The catalytic substrate monolith comprising an SCR catalytically active composition according to the present invention is the same as those mentioned above for close-coupled arrangements.
[0125] In yet another embodiment of the present invention, an emission treatment system comprising a catalytic substrate monolith comprising a SCR catalytically active composition according to the present invention is arranged upstream of a first particulate filter, but 1 meter or more downstream of an exhaust manifold or a turbocharger of an engine. In this embodiment, the catalytic substrate monolith comprising a SCR catalytically active composition according to the present invention is preferably the first brick downstream of an exhaust manifold or a turbocharger of an engine.
[0126] In yet another embodiment of the invention, an emission treatment system comprising a catalytic substrate monolith comprising an SCR catalytically active composition according to the invention is arranged downstream of a first particulate filter.
[0127] In these embodiments in which the catalytic substrate monolith comprising the SCR catalytically active composition according to the invention is located upstream or downstream of the first particulate filter, the catalytic substrate monolith comprising the SCR catalytically active composition according to the invention is the same as the catalytic device mentioned above for the close-coupled arrangement and the underfloor arrangement.
[0128] Furthermore, the present invention provides a method for removing NOx emissions and optionally also particulate matter from the exhaust gas of an internal combustion engine, the method comprising, from upstream to downstream, in the following order:
[0129] a) injecting ammonia or an ammonia precursor solution into the exhaust gas stream,
[0130] b) introducing the exhaust gas from step a) into a catalytic substrate monolith comprising an SCR catalytically active composition for converting NOx in automobile combustion exhaust gases, wherein the SCR catalytically active composition for converting NOx is a crystalline aluminosilicate zeolite having a CHA framework type according to the present invention, and wherein the substrate monolith is selected from a honeycomb flow-through substrate, a honeycomb wall-flow filter, a corrugated substrate, a wound or filled fiber filter, an open-cell foam, a sintered metal filter and an extruded catalytic substrate monolith.
[0131] As mentioned above, for the emission treatment system, those skilled in the art will understand that, in the case where the substrate monolith used in step b) of the above method is a flow-through monolith or a corrugated substrate, the corresponding catalytic substrate monolith will only remove NOx emissions. However, if the substrate monolith used in step b) of the above method is a wall-flow filter, the corresponding catalytic substrate monolith will also remove particulate matter. BRIEF DESCRIPTION OF THE DRAWINGS
[0132] Figure 1 The NO in the standard SCR reaction of Comparative Example 1 and Examples 1, 2, 3 and 4 in the fresh state is shown. x Percent conversion ("NO only").
[0133] Figure 2 The N2O concentration in ppm for Comparative Example 1 and Examples 1, 2, 3 and 4 in the fresh state in a standard SCR reaction ("NO only") is shown.
[0134] Figure 3 The N2O selectivity percentages for Comparative Example 1 and Examples 1, 2, 3 and 4 in the fresh state in the standard SCR reaction ("NO only") and at 25% and 50% NO2 are shown.
[0135] Figure 4 The percentage N2O selectivity in the standard SCR reaction ("NO only") and 25% and 50% NO2 in the aged state is shown for Comparative Example 1 and Examples 1, 2, 3 and 4. Aging was performed at 750°C for 16 h.
[0136] Figure 5 The NO in the standard SCR reaction of Comparative Example 1 and Examples 1, 2, 3 and 4 under the aged state is shown. x Percent conversion ("NO only"). Aging was performed at 750°C for 16 h.
[0137] Figure 6 The N2O concentration in ppm in the standard SCR reaction ("NO only") in the aged state is shown for Comparative Example 1 and Examples 1, 2, 3 and 4. Aging was performed at 750°C for 16 h.
[0138] Figure 7 The NO in the SCR reaction in only NO at 180° C. in the fresh state of Comparative Example 2 and Examples 5, 6, 7, 8 and 9 are shown. x Conversion rate percentage.
[0139] Figure 8 The N2O concentration in ppm for Comparative Example 2 and Examples 5, 6, 7, 8 and 9 in the SCR reaction in NO only at 250°C in the fresh state is shown.
[0140] Fig. 9 It shows that ΔNO x , i.e., in the fresh state, the NO in Examples 5 to 9 in the SCR reaction with 50% NO2 at 180°C x The conversion rate (in percent) is minus the corresponding NO of Comparative Example 2. x The difference in conversion rate.
[0141] Fig.10 ΔN2O, ie the difference in N2O formation (in ppm) of Comparative Example 2 in an SCR reaction with 50% NO2 at 250°C minus the corresponding N2O formation of Examples 5 to 9 in the fresh state, is shown.
[0142] Fig.11 The NO in the SCR reaction in NO only at 180°C in the aged state of Comparative Example 2 and Examples 5, 6, 7, 8 and 9 are shown. x Conversion percentage. Aging was carried out at 750°C for 16 h.
[0143] Fig.12 The N2O concentration in ppm in the SCR reaction in NO only at 250° C. in the aged state is shown for Comparative Example 2 and Examples 5, 6, 7, 8 and 9. Aging was performed at 750° C. for 16 h.
[0144] Fig.13 It shows that ΔNO x , i.e., in the aged state, the NO in the SCR reaction with 50% NO2 at 180°C for Examples 5 to 9 x The conversion rate (in percent) is minus the corresponding NO of Comparative Example 2. x The aging was carried out at 750°C for 16 h.
[0145] Fig.14 ΔN2O is shown, i.e. the difference in N2O formation (in ppm) in the aged state in the SCR reaction with 50% NO2 at 250°C for Comparative Example 2 minus the corresponding N2O formation of Examples 5 to 9. Aging was performed at 750°C for 16 h.
[0146] Implementation
[0147] Preparation of Powders of Comparative Example 1, Comparative Example 2 and Examples 1 to 9 :
[0148] The purchased H with CHA skeleton structure +-form zeolite powder was used as the base zeolite material, with a SAR value of 13. 1.2 kg of the base zeolite was impregnated with an aqueous solution of Cu(NO3)2, which was metered in over 30 min while the powder was constantly mixed in a closed stainless steel container. The Cu(NO3)2 aqueous solution was prepared from a mixture of 540 g of deionized water and 122.1 g of Cu(NO3)2*3H2O, in which the Cu salt was completely dissolved before addition to the zeolite powder. After impregnation, the Cu-loaded zeolite was dried at 120°C for 8 h and calcined at 600°C for 2 h.
[0149] To prepare the powders of Examples 1 to 4, an aqueous solution containing 122.1 g of Cu(NO3)2*3H2O and X g of a Mn(NO3)2 solution containing 15 wt% Mn was mixed with deionized water to a total of 540 g of water. For Examples 1 to 4, the values of X were 46.2 g, 92.3 g, 138.5 g, and 184.7 g, respectively.
[0150] The preparation of powders of Comparative Example 2 (CE2) and Examples 5 to 9 (Ex5 to Ex9) was carried out in a similar manner to Examples 1 to 4. The compositions are listed in Table 1. Comparative Example 2 corresponds to Example 1g of US 2015 / 078989A1.
[0151] Preparation of coated catalysts of Comparative Example 1 and Examples 1 to 4:
[0152] The powders prepared in Comparative Example 1 and Examples 1 to 4 were each coated onto their individual commercial extruded monolithic support materials having dimensions of 5.66" diameter and 3.0" length, a channel size of 400 cpsi and a wall thickness of 4 mils. A slurry consisting of HO, AlO as a binder and the prepared Cu / Mn-zeolite powder was mixed and stirred overnight. The commercial monolithic support was immersed in the slurry and subsequently dried by a stream of hot air. The process was repeated until the loading of the dry coating reached 150 g / L.
[0153] Table 1: Compositions of Comparative Example 1 and Examples 1 to 4
[0154]
[0155]
[0156] Measurement of Aging, NOx Conversion and N2O Formation of Comparative Example 1 and Examples 1 to 4
[0157] After preparation and after aging, the coated catalysts were measured in a hydrothermal atmosphere (10% H2O, 10% O2, the remainder N2). The holding time and aging temperature in the hydrothermal atmosphere was 16 h at 750°C.
[0158] In the so-called NOx conversion test, the NOx conversion of a catalyst is determined in a model gas reactor as a function of the temperature upstream of the catalyst.
[0159] The NOx conversion test consists of a test program that includes pre-conditioning and a test cycle run for various target temperatures.
[0160] Testing Procedure:
[0161] 1. Pre-treatment in N2 at 600°C for 10 min
[0162] 2. Repeat the test cycle for the target temperature
[0163] a. Approaching target temperature in gas mixture 1
[0164] b. Add NO x (Gas mixture 2)
[0165] c. Add NH3 (gas mixture 3) and wait until NH3 breaks through > 20ppm, or a maximum duration of 30 minutes
[0166] d. Programmed temperature desorption temperature up to 500°C (gas mixture 3)
[0167] In the case of NO measurement only (Table 2a), in the case of measurement of NOx concentration of 25% NO2 (Table 2b) and in the case of NO x In the case of measurements with a concentration of 50% NO2 (Table 2c), the NOx concentration in the gas composition in test procedure ranges 3 and 4 was adjusted accordingly.
[0168] Table 2a: NO under NO-only conditions x Gas mixture for conversion test
[0169]
[0170]
[0171] Table 2b: In NO x When the concentration is 25% NO2 x Gas mixture for conversion test
[0172] Gas mixture 1 2 3 <![CDATA[N2]]> balance balance balance <![CDATA[O2]]> 10% by volume 10% by volume 10% by volume NOx 0ppm 375ppm 375ppm <![CDATA[NO2]]> 0ppm 125ppm 125ppm <![CDATA[NH3]]> 0ppm 0ppm 750ppm <![CDATA[H2O]]> 5% by volume 5% by volume 5% by volume
[0173] Table 2c: In NO x When the concentration is 50% NO2 x Gas mixture for conversion test
[0174] Gas mixture 1 2 3 <![CDATA[N2]]> balance balance balance <![CDATA[O2]]> 10% by volume 10% by volume 10% by volume NOx 0ppm 250ppm 250ppm <![CDATA[NO2]]> 0ppm 250ppm 250ppm <![CDATA[NH3]]> 0ppm 0ppm 750ppm <![CDATA[H2O]]> 5% by volume 5% by volume 5% by volume
[0175] The gas hourly space velocity (GHSV) used for the catalyst measurements was 60,000 h-1 at all measurement temperatures. -1 .
[0176] For each temperature point below 500°C, the conversion rate for an NH3 slip of 20 ppm was determined for test program range 2c. For the temperature point of 500°C, the conversion rate at equilibrium was determined in test program range 2c. Plotting this NOx conversion rate for each temperature point yields the following: Figure 1 and Figure 3 The drawing shown.
[0177] The following table shows the NOs given in Tables 2a to 2c. x Conversion test conditions, NO in percentage x Conversion, N2O concentration in ppm and N2O selectivity in percent.
[0178] CE1 = Comparative Example 1, Ex1 to Ex4 = Examples 1 to 4
[0179] Table 3: For Comparative Example 1 and Examples 1, 2, 3 and 4, the SCR reaction of 25% NO2 in the fresh state NO in percentage x Conversion rate and N2O concentration in ppm
[0180]
[0181] Table 4: For Comparative Example 1 and Examples 1, 2, 3 and 4, the SCR reaction of 50% NO2 in the fresh state NO in percentage x Conversion rate and N2O concentration in ppm
[0182]
[0183] Table 5: For Comparative Example 1 and Examples 1, 2, 3 and 4, the SCR reaction of 25% NO2 under the aged state NO in percentage x Conversion and N2O concentration in ppm. Aging was performed at 750 °C for 16 h. .
[0184]
[0185] Table 6: For Comparative Example 1 and Examples 1, 2, 3 and 4, the SCR reaction of 50% NO2 under the aged state NO in percentage x Conversion and N2O concentration in ppm. Aging was performed at 750 °C for 16 h. .
[0186]
[0187] The data in Tables 3 to 6 show that, in the fresh state, the CHA aluminosilicate zeolite according to the present invention exhibits NO x The disproportionate reduction in conversion and N2O formation means that in the fresh state, the N2O formation of the CHA zeolite according to the invention is higher than that of the corresponding NO x In the aged state, the CHA zeolite according to the invention shows an increased NO x Concomitant reduction in conversion and N2O formation.
[0188] Measurement of Aging, NOx Conversion and N2O Formation of Comparative Example 2 and Examples 5 to 9
[0189] The NO values of Comparative Example 2 and Examples 5 to 9 were measured at 180°C in the fresh and aged states of the catalyst powders. xConversion rate.
[0190] The formation of N2O was measured at 250 °C in the fresh and aged state of the catalyst powder.
[0191] The measurements were carried out using a conventional plug flow model. In these measurements, a gas flow simulating lean burn exhaust from an engine was passed through and through the mesh particles of the test sample at different temperature conditions, and the effectiveness of the sample in NOx reduction was determined by an online FTIR (Fourier Transform Infrared) spectrometer.
[0192] Table 7 below details all experimental parameters used to generate the data included herein.
[0193] Table 7: Model gas test conditions
[0194] Components / Parameters Concentration / setting (NO only) <![CDATA[NH3]]> 750ppm NO 500ppm <![CDATA[H2O]]> 4% <![CDATA[O2]]> 5% temperature Ramp from 600°C to 100°C at -2°C / min Sample quality 180mg Particle size of the sample 300-500μm GHSV <![CDATA[250,000h -1 ]]>
[0195] The results are listed in Tables 8 and 9.
[0196] Through the NO from Ex5 to Ex9 x The conversion value is subtracted from the NO in CE2 x The corresponding value of conversion rate is used to calculate "ΔNO x ”.
[0197] "ΔN2O" was calculated by subtracting the corresponding values of N2O formation of Ex5 to Ex9 from the values of N2O formation of CE2.
[0198] Positive Δ values indicate that Examples Ex5 to Ex9 each exhibited better NO x The negative Δ values indicate that CE2 shows better NO conversion or lower N2O formation compared to Ex5 to Ex9, respectively. x conversion or lower N2O formation.
[0199] The results are shown in Figures 7 to 14 middle.
[0200] Table 8: Comparative Example 2 and Examples 5 to 9 (abbreviated as CE2 and Ex5 to Ex9) in the fresh state at 50% NO2 NO in percent at 180°C in the SCR reaction x Conversion rate and N2O concentration in ppm at 250 °C, and the difference between CE2 and Ex5 and Ex9 (expressed as "ΔNO x ” and “ΔN2O”) .
[0201]
[0202] Table 9: Comparative Example 2 and Examples 5 to 9 (abbreviated as CE2 and Ex5 to Ex9) in the aged state in 50% NO2 NO in percent at 180°C in the SCR reaction x Conversion rate and N2O concentration in ppm at 250 °C, and the difference between CE2 and Ex5 and Ex9 (expressed as "ΔNO x ” and “ΔN2O”) .
[0203]
Claims
1. A catalytically active composition comprising a crystalline aluminosilicate zeolite of the CHA framework type, wherein the zeolite has a SAR value between 7 and 25, a copper content between 3.0% and 4.5% by weight, a manganese content of 0.3% to 4.0% by weight, wherein the copper and manganese are calculated as CuO and MnO and are based on the total weight of the zeolite, and wherein the sum of the molar amounts of copper and manganese divided by the molar amount of aluminum is in the range between 0.11 and 0.
96.
2. The catalytically active composition according to claim 1, wherein the crystalline aluminosilicate having the CHA framework structure is selected from the group consisting of the zeolites SSZ-13, LZ-218, Linde D, Linde R, Phi and ZK-14. 3 . The catalytically active composition according to claim 1 , wherein the crystalline aluminosilicate having the CHA framework structure has a SAR value of between 10 and 23. 4 .
4. The catalytically active composition according to any one of claims 1 to 3, wherein the crystalline aluminosilicate having the CHA framework structure has a copper content of between 3.3% and 3.7% by weight, calculated as CuO and based on the total weight of the zeolite.
5. The catalytically active composition according to any one of claims 1 to 4, wherein the crystalline aluminosilicate having the CHA framework structure has a manganese content of between 0.6% and 4.0% by weight, calculated as MnO and based on the total weight of the zeolite.
6. Catalytically active composition according to any one of claims 1 to 5, wherein the sum of the molar amounts of copper and manganese divided by the amount of aluminum is in the range between 0.25 and 0.
40.
7. A method for removing NO from combustion exhaust gas x A method wherein the crystalline aluminosilicate zeolite according to any one of claims 1 to 6 having a CHA framework type is used as a catalyst for converting NO x SCR catalytically active composition.
8. A catalytic substrate monolith comprising a catalyst for converting NO in treating automobile combustion exhaust gas. x SCR catalytically active composition, wherein for converting NO x The SCR catalytically active composition is a crystalline aluminosilicate zeolite according to any one of claims 1 to 6.
9. The catalytic substrate monolith according to claim 8, wherein the crystalline aluminosilicate zeolite according to any one of claims 1 to 6 is present on a carrier substrate in the form of a washcoat.
10. The catalytic substrate monolith of claim 8, wherein the carrier substrate is a flow-through substrate, a wall-flow filter, or a corrugated substrate.
11. The catalytic substrate monolith according to claim 8, wherein the catalytic substrate monolith is an extruded catalytic substrate monolith.
12. The catalytic substrate monolith according to claim 9, wherein the monolith is a flow-through monolith coated with a bottom layer and a top layer, the bottom layer comprising an oxidation catalyst, the bottom layer comprising a crystalline aluminosilicate zeolite according to any one of claims 1 to 6 having a CHA framework type.
13. A method for removing NO from the exhaust gas of an internal combustion engine x An emission treatment system for removing particulate matter and optionally also for removing particulate matter, the system comprising, from upstream to downstream, in the following order: a) a device for injecting ammonia or an ammonia precursor solution into the exhaust gas stream, b) a catalytic substrate monolith, the catalytic substrate monolith comprising a catalyst for converting NO in automobile combustion exhaust gas x SCR catalytically active composition, wherein for converting NO x The SCR catalytically active composition is a crystalline aluminosilicate zeolite according to any one of claims 1 to 6 having a CHA framework type, and wherein the substrate monolith is selected from a honeycomb flow-through substrate, a honeycomb wall-flow filter, a corrugated substrate, a wound or filled fiber filter, an open-cell foam, a sintered metal filter and an extruded catalytic substrate monolith.
14. The emissions treatment system of claim 13, wherein the emissions treatment system is arranged in a close coupled position.
15. The emissions treatment system of claim 13, wherein the emissions treatment system is disposed in an under-floor location.
16. A method for removing NO from the exhaust gas of an internal combustion engine x A method for removing particulate matter from an exhaust gas and optionally also for removing particulate matter, the method comprising, from upstream to downstream, the following order: a) injecting ammonia or an ammonia precursor solution into the exhaust gas stream, b) introducing the exhaust gas from step a) into a reactor comprising a reactor for converting NO in automobile combustion exhaust gas x A catalytic substrate monolith of an SCR catalytically active composition, wherein the catalytic substrate monolith is used to convert NO x The SCR catalytically active composition is a crystalline aluminosilicate zeolite according to any one of claims 1 to 6 having a CHA framework type, and wherein the substrate monolith is selected from a honeycomb flow-through substrate, a honeycomb wall-flow filter, a corrugated substrate, a wound or filled fiber filter, an open-cell foam, a sintered metal filter and an extruded catalytic substrate monolith.