Method for manufacturing inter-blade platform having sacrificial edge

The manufacturing of the turbine engine fan blade platform is simplified through three-dimensional braiding and membrane injection technology, solving the problems of complex processing and material loss in the prior art, and achieving efficient manufacturing and quality assurance.

CN118922296AActive Publication Date: 2024-11-08SAFRAN AIRCRAFT ENGINES SAS
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380027334.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-10
Filing Date
2023-02-01
Publication Date
2024-11-08
Estimated Expiration
2043-02-01

AI Technical Summary

Technical Problem

The manufacturing process of existing turbine engine fan blade platforms is complex and fine, especially the processing operation of composite materials, which is difficult to meet the reference size and surface fit of the components, resulting in material loss and low production efficiency.

Method used

The fiber preform is produced by three-dimensional braiding between multi-layer weft and multi-layer warp yarns, and the components with the shape of a platform to be manufactured are formed by densification of the matrix. The impregnation chamber and compaction chamber are sealed with a flexible film with a flexible film to control the fiber volume Simplify the manufacturing process by comparing and resin injection order.

Benefits of technology

The manufacturing process of the platform between blades is simplified, material losses are reduced, dimensional ratings are met, and production efficiency and component quality are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922296A_ABST
    Figure CN118922296A_ABST
Patent Text Reader

Abstract

The invention relates to a method for manufacturing an inter-blade platform (100) of a turbine engine fan (1), the platform (100) comprising a base (110) having first and second sacrificial side edges (131, 132), the first and second sacrificial side edges (131, 132) having a thickness less than a thickness of a central part (120) of the base (110); the method comprises producing a preform (200) of a platform (100) by three-dimensional weaving, the preform comprising a central component portion (220) and two sacrificial edge portions (231, 232), the thickness of the two sacrificial edge portions being less than the thickness of the central component portion (220), and the thickness of the central component portion (220) being less than the thickness of the sacrificial edge portions (231, 232) being less than the thickness of the sacrificial edge portions (231, 232). Thickness differences between the side edge portions (231, 232) and the central member portion (220) are achieved by removing a plurality of warp yarns located outside the central member portion (220) and not woven with the weft yarns.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a fan of a turbine engine, for example a fan of an aircraft turbojet engine or a turboprop engine, and in particular to an inter-blade platform in a fan of a turbine engine. Background Art

[0002] In a known manner, a turbine engine fan comprises a rotor disk comprising a plurality of blades separated at their radially inner ends by inter-blade platforms. Thus, the inter-blade platforms of a turbine engine fan are arranged between the fan blades in the extension of the inlet cone of the fan. They make it possible in particular to define an annular flow of air at the inlet of the fan on the inside, which is defined on the outside by the casing. These platforms generally comprise a base configured to define an annular flow of air and lugs extending radially towards the rotor disk. These lugs may form part of a box, or correspond to stiffeners.

[0003] Since the blades are not connected to the platform, the mechanical stress on the blade root during operation is greatly reduced. This allows the size of the blade root to be reduced to reduce the weight of the wind turbine, thereby improving the performance of the turbine engine.

[0004] The base of the platform usually includes sacrificial side edges, which are designed to break when strong pressure from the blade acts on the sacrificial edge. These sacrificial side edges are usually thinner than the rest of the base. Therefore, in the event of damage to the wind turbine blade, the sacrificial edges of the two platforms located on both sides of the blade bend (yield) so that part of the energy can be dissipated and the contact force between the blade and the platform can be reduced to limit structural damage. In addition, the two platforms can protect the surrounding wind turbine blades by preventing any fragments of the damaged blade from contacting the radial inner ends of these blades. Therefore, the risk of additional damage to the wind turbine blades and platforms is greatly reduced.

[0005] Therefore, wind turbine platforms are usually made of composite materials and include fiber reinforcements densified by a matrix. It is particularly known to produce a single fiber blank by three-dimensional or multilayer weaving. For example, the three-dimensional weaving production of π (Pi)-shaped fiber blanks for platforms is described in document WO 2013 / 088040. The preform is then densified by the matrix according to conventional methods.

[0006] The sacrificial side edges are then produced by machining the edges of the base to obtain the required reduced thickness. However, this machining operation of composite materials is complex and delicate to implement, particularly in order to meet the quoted dimensions and surface fit of the component. Summary of the invention

[0007] Therefore, the main object of the present invention is to remedy the above mentioned drawbacks by facilitating the manufacture of inter-blade platforms.

[0008] To this end, the present invention proposes a method for manufacturing an inter-blade platform of a turbine engine fan, the platform comprising a base and at least two lugs, the base comprising a central portion, the central portion comprising a first surface configured to define a fuel flow of the fan, and a second surface opposite to the first surface; the at least two lugs extend radially from the second surface, the base further comprising a first and a second sacrificial side edge, the first and the second sacrificial side edges extending from either side of the central portion of the base, and having a thickness less than the central portion of the base;

[0009] The method includes producing a fiber preform of the platform by integrally three-dimensionally weaving between multiple layers of weft yarns and multiple layers of warp yarns;

[0010] The method also includes densifying the fiber preform by means of a matrix to form a component having the shape of the platform to be manufactured;

[0011] The method is characterized in that the fiber preform of the platform comprises a base portion of a fiber reinforcement for forming a base of the platform, the base portion of the fiber preform comprising a central component portion and two sacrificial edge portions having a thickness less than the central component portion, a first plurality of weft yarns being continuous between the central component portion and the sacrificial edge portions, the sacrificial edge portions comprising a first plurality of warp yarns woven to the first plurality of weft yarns, the thickness difference between the side edge portions and the central component portion being formed by withdrawing a second plurality of warp yarns located outside the central component portion and not woven with the weft yarns.

[0012] The manufacture of the interblade platform is thus simplified by densifying a fiber preform that already has substantially the same shape as the part to be manufactured. Complex machining steps are thus omitted, thereby also limiting material losses while ensuring that dimensional classes are met.

[0013] According to a particular feature of the invention, the densification of the fiber preform is achieved by placing the fiber preform in an impregnation chamber of a mold comprising a lower surface against which the surface of the fiber preform intended to form the first surface of the central part of the platform base is abutted; the impregnation chamber is closed by a flexible membrane separating it from a compacting chamber; an impregnation fluid is injected into the impregnation chamber and a compressed fluid is injected into the compacting chamber so as to exert pressure on the membrane.

[0014] The impregnation fluid may be, for example, a slurry containing matrix precursor particles or a resin.

[0015] The membrane injection technique offers greater flexibility in the geometry of the injection mould. In fact, the use of a flexible membrane instead of a rigid counter-mould as in RTM technology makes it easier to adapt to the specific geometry of the lug in particular. In addition, the membrane injection technique also allows for better control of the fibre volume ratio, since the exact resin volume required is introduced to obtain a precise and predetermined fibre volume ratio.

[0016] According to another particular feature of the invention, the injection of the impregnating fluid is performed before the injection of the compressed fluid.

[0017] According to another particular feature of the invention, the injection of the compressed fluid begins before the injection of the immersion fluid.

[0018] In this variant, an improved control of the flow of the impregnation fluid and thus of the impregnation of the fiber preform is achieved.

[0019] According to another particular feature of the invention, the injection of the compacting liquid begins before the injection of the impregnation fluid.

[0020] The latter variant advantageously makes it possible to apply a pressure to the fiber preform of such a value that the desired fiber volume fraction can be obtained even before the impregnation fluid is injected. The injection of the impregnation fluid is then started, which can be done while the injection of the compressed fluid continues, in order to compensate for the pressure drop, in particular in the case where the impregnation fluid is a slurry. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 is a partially exploded schematic diagram of an example of a wind turbine including inter-blade platforms.

[0022] Figure 2 yes Figure 1 A cross-sectional view of the inter-blade platform is shown.

[0023] Figure 3 It is a partial schematic diagram of a plane of a fiber blank of a three-dimensionally woven platform.

[0024] Figure 4 is through Figure 3 A partial schematic plan view of a fiber preform obtained by forming a fiber blank.

[0025] Figure 5 is a schematic cross-sectional view of a fiber preform of a platform in a rigid injection tool.

[0026] Figure 6 is a schematic cross-sectional view of a fiber preform of a platform in a tool including a flexible membrane. DETAILED DESCRIPTION

[0027] Figure 1A turbine engine fan 1 is shown in an exploded view and comprises a rotor disk 10 carrying a plurality of fan blades 20, the roots 21 of which engage in axial grooves 11 formed in the rotor disk 10. The blades 20 are separated by inter-blade platforms 100 which are connected to the rotor disk 10.

[0028] The first direction D1 is defined as the general direction corresponding to the airflow of the turbine engine. The second tangential and / or circumferential direction D2 is defined as the direction corresponding to the alternating succession of inter-blade platforms 100 and blades. Finally, the third radial direction D3 is defined as the direction perpendicular to the first direction.

[0029] For simplicity, the first, second and third directions of the wind turbine reference frame are also used for the platform reference frame, the direction of the platform reference frame corresponding to the direction of the wind turbine reference frame when the platform is mounted on the wind turbine.

[0030] Figure 1 and Figure 2 The illustrated inter-blade platform 100 comprises a base 110, which comprises a central part 120 and a first sacrificial side edge 131 and a second sacrificial side edge 132. The central part 120 of the base 110 has a first surface 121 and a second surface 122 opposite to each other. The first surface 121 is used to define a flow path of the wind turbine. When the platform 100 is mounted on the wind turbine, the first surface 121 and the second surface 122 extend longitudinally in a first direction D1, which is the general direction of the airflow of the turbine engine, and extend transversely in a direction D2 between two adjacent blades of the wing-connected platform 100.

[0031] The platform 100 further comprises at least two lugs 150 extending radially from the second surface 122 of the central part 120 of the base 110 and capable of performing a reinforcement function. When the platform 100 is mounted on the wind turbine, the lugs 150 extend along the third direction D3 to the rotor disk. The lugs 150 also extend longitudinally along the first surface 121 and the second surface 122. Thus, when the platform 100 is mounted on the wind turbine, the lugs 150 extend along the first direction D1, that is to say, along the general direction of the airflow of the turbine engine.

[0032] The first and second sacrificial side edges 131 and 132 extend longitudinally along the first and second surfaces 121 and 122 on either side of the central part 120 of the base 110 of the platform 100. Thus, the first and second sacrificial side edges 131 and 132 are connected to the central part 120 of the base 110 of the platform 100.

[0033] Preferably, the first sacrificial side edge 131 and the second sacrificial side edge 132 respectively include extension surfaces 131a and 132a located at the extension portion of the first surface 121 of the central component 120 along the second direction D2. Preferably, the length of the extension surfaces 131a and 132a along the second direction D2 is between 6 mm and 11 mm.

[0034] The thickness D3 of the first sacrificial edge 131 and the second sacrificial edge 132 in the third direction is smaller than the thickness of the central part 120 of the base 110 in the third direction D3. Preferably, the thickness of the first sacrificial edge 131 and the second sacrificial edge 132 is between 1.5 mm and 2.2 mm.

[0035] Preferably, the thickness of the first sacrificial edge 131 and the second sacrificial edge 132 at the free ends 131 b and 132 b thereof along the third direction D3 is less than or equal to 2.2 mm.

[0036] The manufacture of the inter-blade platform 100 comprises producing a fiber preform 200 of the platform 100 by three-dimensional weaving between multiple layers of warp yarns and multiple layers of weft yarns. "Three-dimensional weaving" or "3D weaving" here refers to a weaving pattern in which at least some of the warp yarns are connected to the weft yarns over multiple layers of weft yarns. The roles between the warp yarns and the weft yarns are interchangeable. The fiber preform can, for example, have a multiple layer satin weave, that is, a fabric obtained by three-dimensional weaving with multiple layers of weft yarns, wherein the basic weave of each layer corresponds to a classic satin weave, but certain points of the fabric bond the weft yarn layers together.

[0037] The fiber preform may also, for example, have an interlocking weave, ie a fabric obtained by three-dimensional weaving, in which each layer of warp threads is connected to multiple layers of weft threads and all threads of the same row of warp threads perform the same movement in the weaving plane.

[0038] Other three-dimensional weaving methods may be implemented, such as multi-web weave. Different multi-web weaving methods that can be used to form a fiber preform are described in document WO 2006 / 136755.

[0039] The fiber preform 200 includes a lug portion 250 of a fiber reinforcement for forming the lug 150 of the platform 100, and a base portion 210 of a fiber reinforcement for forming the base 110 of the platform 100. In particular, the base portion 210 of the fiber preform 200 includes a fiber reinforcement for forming the central component 120 of the base 110 of the platform 100, and a fiber reinforcement for forming the first sacrificial side edge 131 and the second sacrificial side edge 132, respectively. The central component 220 includes a first surface 221 and a second surface 222, respectively forming the first surface 121 and the second surface 122 of the central component 120 of the base 110 of the platform 100.

[0040] In order to produce the fiber preform 220 of the platform 100 , the fiber blank 300 of the platform 100 may first be produced by three-dimensional weaving.

[0041] The sacrificial edge parts 231 and 232 are produced according to the so-called "layer withdrawal" method. The fiber blank 300 of the fiber preform 200 is manufactured using a jacquard type loom. Such a loom is described, for example, in document FR 3 047 744 A1. With such a loom, it is possible to directly weave the blank of the sacrificial edge part whose thickness is different from the blank of the central component part.

[0042] Thus, in the fiber blank 300, the first plurality of weft yarn layers are continuous between the blank of the central component portion and the two blanks of the sacrificial side edges, that is, the first plurality of weft yarns pass through both the blank of the central component portion and the two blanks of the sacrificial side edges. Thus, in the fiber preform 200, the first plurality of weft yarn layers are continuous between the central component portion 220 and the two sacrificial side edge portions 231 and 232, that is, the first plurality of weft yarns pass through the central component portion 220 and the two sacrificial side edge portions 231 and 232.

[0043] The central component part blank comprises a plurality of warp yarns woven with a plurality of weft yarns. In particular, a plurality of warp yarns are woven with a first plurality of weft yarn layers and a second plurality of weft yarn layers, i.e., the warp yarns belonging to the central component part blank are woven with the first plurality of weft yarn layers and the second plurality of weft yarn layers. Thus, in the fiber preform 200, a plurality of warp yarn layers are woven with the first plurality of weft yarn layers and the second plurality of weft yarn layers, and the warp yarns belonging to the central component part 220 are woven with the first plurality of weft yarns and the second plurality of weft yarns.

[0044] The sacrificial side edge portion blank comprises a first plurality of warp yarn layers woven with a first plurality of weft yarn layers, i.e., within the sacrificial side edge portion blank, the first plurality of warp yarns are woven with the first plurality of weft yarns. The same weaving structure is used for the other sacrificial side edge portion blank. Therefore, in the fiber preform 200, the sacrificial side edge portion 232 comprises a first plurality of warp yarn layers woven with a first plurality of weft yarn layers, i.e., the first plurality of warp yarns are woven with the first plurality of weft yarn layers located within the sacrificial side edge portion 232. The same weaving structure is used for the other sacrificial side edge portion 231.

[0045] The difference in thickness between the blank of the central component part and the two blanks of the sacrificial side edge parts is achieved by removing a second plurality of warp yarns that are located on both sides of the blank of the central component part and are different from the first plurality of warp yarns. In particular, the warp yarns belonging to the second plurality of warp yarns do not belong to the first plurality of warp yarns and vice versa. Thus, the second plurality of warp yarns corresponds to a set of warp yarns that are located outside the central part blank and are not woven into the first plurality of weft yarns.

[0046] In order to be able to remove the second plurality of warp yarns, the second plurality of warp yarns are not woven with the weft yarns. Thus, the second plurality of warp yarns are not woven with the first plurality of weft yarns and are not woven with the second plurality of weft yarns.

[0047] Thus, the second plurality of weft threads weave only with the warp threads present in the center component portion blank. Thus, in the fiber preform 200, the second plurality of weft threads weave only with the warp threads present in the center component portion 220. Thus, the second plurality of weft threads correspond to the weft threads that are not woven with the first plurality of warp threads.

[0048] When the weaving of the fiber blank 300 is completed, two portions of the yarns belonging to the second plurality of weft yarns which are not woven with the blank of the central part portion are cut.

[0049] The lug portion 250 of the fiber preform 200 may be produced by peeling means simultaneously with the production of the side edge portions 231 and 232 . Figure 3 An example of a partial schematic plan view of a fiber blank 300 of a platform 100 is shown, which fiber blank 300 of the platform 100 includes, within its thickness, a base portion blank 310 and a lug portion blank 350, which are separated from each other in the weft direction by a first stripping device 301 and a second stripping device 302 by a portion of the size of the fiber blank 300. The stripping devices 301 and 302 extend from opposite edges 301b, 302b of the fiber blank 300 to the floors 301a, 302a of the stripping devices, and there is no stripping device in the center of the fiber blank 300. The base blank 310 has a first surface 321 and a second surface 322, which are used to form the first surface 221 and the second surface 222 of the central component part 220 of the fiber preform 220, respectively.

[0050] Each of the base portion blank 310 or the lug 350 blank of the fiber blank 300 includes multiple layers of warp yarns, where the number of layers of warp yarns in the base portion 310 blank and the lug 350 blank is different.

[0051] In each plane of the fiber blank 300, the same first warp yarn t 31 ,t 32 ,t 33 ,t 34 The warp yarns in the lug portion blank 350 that extend beyond the second stripping device 302 and the warp yarns in the base portion blank 310 that border the first stripping device 301 are connected together. 35 ,t 36 ,t 37 , 38The warp yarns in the portion of the base portion blank 310 bordering the second stripping device 302 and the warp yarns in the lug portion blank 350 located below the first stripping device 301 are connected together.

[0052] Therefore, the first weft yarn t 31 ,t 32 ,t 33 ,t 34 The path of the second weft yarn t 35 ,t 36 ,t 37 ,t 38 The paths of the stripping devices 301 and 302 intersect in a transition zone 303 , which is located between the bottom layers 301 a and 302 a of the stripping devices 301 and 302 in the center of the fiber blank 300 .

[0053] Note that the first surface 321 of the base portion blank 310 is in contact with the yarn t 39 The surface represented by the satin weave is woven together to provide surface continuity without crossing the warp layers or crossing with other weft yarns.

[0054] Figure 3 and Figure 4 The weaving shown is a block diagram and therefore the number of warp and weft yarns represented is less than the actual number of warp and weft yarns.

[0055] Then, if Figure 4 As shown, the fiber blank 300 of the platform 100 is shaped to obtain the fiber preform 200 of the body 100 having a substantially π (Pi)-shaped cross section, by folding at the stripping devices 301 and 302 to form the lug portions 250 .

[0056] Preferably, the length and width of the first surface 221 of the central component part 220, the length of the lug part 250 and the distance between the two lug parts 250 substantially correspond to the length and width of the first surface of the central component 120, the length of the lug 130 and the distance between the two lugs 130 of the platform 100, respectively.

[0057] Document WO 2013 / 088040 describes in particular an example of a plan view of a fiber blank that can be used to produce a fiber platform preform having lugs.

[0058] Preferably, the fiber preform 200 corresponds to a "dry" fiber structure, that is to say not impregnated with resin or the like. The fiber preform 200 may comprise a plurality of different kinds of yarns, in particular ceramic or carbon yarns or even a mixture of such yarns. Preferably, the fiber preform 200 may be made of silicon carbide fibers. In general, the fiber preform 200 may also be made of fibers comprising alumina, mullite, silica, aluminosilicates, borosilicates, carbon or a mixture of several of these materials.

[0059] Once the fiber preform 200 of the platform 100 is obtained, said fiber preform 200 is densified by means of a matrix in order to form a component comprising a fiber reinforcement constituted by the fiber preform 200 .

[0060] Densification can be achieved by the well-known resin transfer molding (abbreviated as "RTM"), or by slurry transfer molding (abbreviated as "STM"). Figure 5 As shown, a fiber preform 200 for forming a fiber reinforcement of a platform 100 is arranged in a cavity defined by a first part 61 and a second part 62 of a mold 60. The cavity has the shape of the part to be manufactured, which has the general shape of the platform 100 to be manufactured.

[0061] Typically, a slurry 6 of matrix precursor particles or resin is injected into the cavity housing the fiber preform 200 so as to pass through said fiber preform 200 due to the application of a pressure gradient P. In the case of a slurry, the mold in which the injection of the slurry 6 is carried out comprises a filter 63 at the outlet orifice of the slurry 6 in the mold 60, thus making it possible to retain any particles of the matrix precursor in the mold 60 and gradually impregnate the fiber preform 200 during the deposition of the matrix precursor particles into the mold 60.

[0062] Densification can also be achieved in a known manner by injection under the membrane, such as Figure 6 The injection method enables full control over the quality of the injected resin or slurry, thus ensuring an accurate and appropriate fiber volume ratio. As a result, the properties of the resulting parts are improved and there is less variability between parts.

[0063] A fiber preform 200 for forming a fiber reinforcement of the platform 100 is arranged in the mold 70. In particular, the fiber preform 200 may be arranged directly on the lower surface of the impregnation chamber 71. The lower surface of the impregnation chamber 71 may include a filter ( Figure 6 not shown).

[0064] The mold 70 comprises, on the one hand, an impregnation chamber 71 into which the fiber preform 200 is placed in order to be densified by the matrix by injecting an impregnation fluid 8, and, on the other hand, a compaction chamber 72 into which a compressed fluid 9 is injected in order to apply pressure to the preform 200 during the densification of the preform 200 by the matrix. The impregnation chamber 71 and the compaction chamber 72 are separated by a flexible membrane 73. The membrane 73 makes it possible to apply pressure to the fiber preform 200 installed in the impregnation chamber 71, the compressed fluid 9 exerting a pressure Q on the membrane 73, which deforms and thus in turn applies pressure to the fiber preform 200.

[0065] Preferably, if Figure 6 As shown, the membrane cooperates with the lug portions 250 of the fiber preform 200 and the second surface 222 of the central part 220, while the first surface 221 of the central part 220 abuts against a wall of the impregnation chamber 71, which is opposite to the membrane 73. The insert 74 can be used to facilitate the impregnation of the fiber preform 200 of the platform 100.

[0066] The flexible film 73 is made of silicone, for example.

[0067] like Figure 6 As shown, for example, the resin 8 can be introduced into the impregnation chamber 71 through the inlet hole, and the compression liquid 9 can be introduced into the compaction chamber 72 through the inlet hole.

[0068] Depending on the size, thickness and shape of the platform 100 to be manufactured, the injection sequence of the different compression and impregnation fluids will be preferred.

[0069] For example, an impregnation fluid (e.g., resin) may first be injected into an impregnation chamber in which the fiber preform is arranged. Once the impregnation fluid is injected, a compressed fluid (e.g., water) is injected into the compacting chamber to apply pressure to the flexible membrane. Thus, the flexible membrane applies pressure to the fiber preform, thereby causing the impregnation fluid to penetrate into the preform.

[0070] Then, while maintaining the pressure applied by the membrane, the preform is heat treated to form a matrix in the pores of the fiber preform.

[0071] According to another example, it is possible to start by injecting a compressed fluid into the compaction chamber. Thus, even before the impregnation fluid is injected, a pressure is already applied to the fiber preform through the flexible membrane, the value of which makes it possible to obtain the desired fiber volume ratio. Then the injection of the impregnation fluid is started, which can be carried out while continuing to inject the compressed fluid in order to compensate for the pressure drop, in particular in the case where the impregnation fluid is a slurry. Such an injection sequence is described, for example, in document WO 2019 / 197757 A1.

[0072] When the densification step is completed, a composite material part is obtained, the fiber reinforcement of which consists of the fiber preform 200 and whose shape generally corresponds to the inter-blade platform 100 to be manufactured. Trimming or light machining steps can be performed on the produced part to obtain the inter-blade platform 100 to be manufactured. In addition, other elements can be mounted or welded to the produced part to obtain the inter-blade platform 100 to be manufactured, in particular Figure 1 Element 140 is shown attached to a rotor disk.

[0073] The expression "between... and..." must be understood as including the boundaries.

Claims

1. A method for manufacturing an inter-blade platform (100) of a turbine engine fan (1), the platform (100) comprising a base (110) and at least two lugs (150); the base (110) comprising a central part (120) comprising a first surface (121) configured to define a flow path of the fan and a second surface (122) opposite to the first surface (121); the at least two lugs (150) extending radially from the second surface, the base (110) further comprising first and second sacrificial side edges (131, 132), the first and second sacrificial side edges (131, 132) extending on both sides of the central part (120) of the base (110) and having a thickness less than the thickness of the central part (120) of the base (110); the method comprising producing a fiber preform (200) of the platform (100) by three-dimensionally weaving between multiple layers of weft yarns and multiple layers of weft yarns into a single piece; The method also comprises densifying the fiber preform (200) with a matrix to form a component having the shape of the platform (100) to be manufactured, The method is characterized in that the fiber preform (200) of the platform (100) comprises a base portion (210) of a fiber reinforcement for forming a base (110) of the platform (100), the base portion (210) of the fiber preform (200) comprising a central component portion (220) and two sacrificial edge portions (231, 232), the thickness of which is less than the thickness of the central component portion (220), a first plurality of weft yarns being continuous between the central component portion (220) and the sacrificial edge portions (231, 232), the sacrificial edge portions (231, 232) comprising a first plurality of warp yarns woven to the first plurality of weft yarns, and the thickness difference between the side edge portions (231, 232) and the central component portion (220) being achieved by removing a second plurality of warp yarns located outside the central component portion (220) and not woven with the weft yarns.

2. The manufacturing method according to claim 1, wherein: Densification of the fiber preform (200) is carried out by arranging the fiber preform (200) in an impregnation chamber (71) of a mold (70) comprising a lower surface, by pressing a surface (221) of the fiber preform (200) intended to form a first surface (121) of a central part (120) of a base (110) of a platform (100) against said lower surface (221) of the fiber preform (200), the impregnation chamber (71) being closed by a flexible membrane (73) separating said impregnation chamber (71) from a compacting chamber (72), an impregnation fluid (8) being injected into the impregnation chamber (71), and a compressed fluid (9) being injected into the compacting chamber (72) so as to exert a pressure (Q) on the membrane (73).

3. The method according to claim 2, wherein: The injection of the immersion fluid (8) starts before the injection of the compressed fluid (9).

4. The method according to claim 2, wherein: The injection of the compressed fluid (9) starts before the injection of the immersion fluid (8).

Citation Information

Patent Citations

  • Inter-blade platform with sacrificial box

    FR3097904A1

  • Method for manufacturing a fibrous preform for reinforcing parts made of composite material with significant local thickness variation

    FR3098435A1