Method for extracting precious metal with high selectivity

By using strong alkali, oxidant and thiocyanate compositions in electronic waste, the problems of low selectivity and high toxicity of precious metal extraction in the prior art are solved, and high efficiency precious metal extraction with low cost and low environmental risk are achieved. Recycle.

CN118922566APending Publication Date: 2024-11-08SINGAPORE POLYTECHNIC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029287.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-30
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art has problems of low selectivity, high toxicity, high cost and environmental pollution when extracting gold and silver from electronic waste, especially the toxicity and treatment cost caused by cyanide-based leaching agents under long-term use. .

Method used

Compositions of strong alkali, oxidizing agent and thiocyanate, with alkaline systems with pH values ​​of 12-14, low cyanide content and low lead ion content for solids coated at medium temperatures Selective extraction of precious metals from waste avoids the generation of toxic waste, and improves the extraction efficiency and selectivity through the addition of amine compounds and lead ions.

Benefits of technology

It realizes non-toxic, economical and highly selective precious metal extraction, reduces reagent losses and environmental risks, simplifies downstream recycling processes, and improves the recycling purity and efficiency of precious metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922566A_ABST
    Figure CN118922566A_ABST
Patent Text Reader

Abstract

The present invention relates to a composition comprising a strong base, an oxidizing agent and a thiocyanate, wherein the composition has a pH in the range of 12-14. The invention also relates to a method for preparing such a composition, to a method for extracting precious metals using such a composition, and to the use of such a composition for recovering precious metals.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a composition comprising a strong base, an oxidant and a thiocyanate, wherein the composition has a pH in the range of 12 to 14. The present invention also relates to a method for preparing such a composition, a method for extracting precious metals using such a composition and the use of such a composition for recovering precious metals. Background Art

[0002] For centuries, the demand for the precious metal gold (Au) has been increasing due to its practical uses in industry. Gold has excellent chemical resistance, as it does not react with oxygen or sulfur in air or water, thus ensuring durability in corrosive conditions, which has led to its widespread use in coins and jewelry since ancient times. Gold also has excellent electrical conductivity, making it useful as a coating for electrical contacts. Recent technological innovations have also used gold in the fields of medicine, nanotechnology, engineering, and environmental management.

[0003] Likewise, the demand for metallic silver (Ag) is increasing rapidly across industries due to its use in manufacturing a wide range of products. Silver is widely used in electrical and electronic devices due to its excellent electrical and thermal conductivity. It also plays an important role in photovoltaic modules in the form of conductive paste for efficient power generation. Silver is used in jewelry, silverware, solder, and other industrial applications due to its malleability, ductility, high reflectivity, and high strength. Moreover, the photosensitivity of silver halide makes it used in photography. Silver is also used in pharmaceutical products and consumer products due to its antimicrobial and non-toxic properties.

[0004] According to the United Nations (UN), an average of 7.6 kg of electronic waste will be generated per person in 2021, and 57.4 million tons of electronic waste will be generated worldwide, of which a considerable amount of gold and silver may be recycled. Electronic waste has become a valuable non-traditional resource due to its high metal content, as nearly 40% of electronic waste is composed of metals. In order to meet the growing demand for gold and silver, these metals must be recovered from secondary sources such as printed circuit boards (PCBs), metal fragments, and integrated circuits of discarded computers and mobile phones coated with gold and silver. Since electrical and electronic waste accounts for the majority of secondary sources of gold and silver, methods for leaching gold and silver from such waste need to take into account its complex matrix, which includes a mixture of toxic heavy metals, such as copper (Cu), zinc (Zn), aluminum (Al), tin (Sn) and lead (Pb), as well as hazardous organic components, including brominated flame retardants and polybrominated biphenyls.

[0005] However, the leaching agents currently used in the industry for leaching gold and silver either contain highly corrosive aqua regia or contain free cyanide concentrations (CN -) highly toxic cyanide-based solutions up to 20,000 ppm due to their low cost and historically widespread use. Leaching precious metals using aqua regia is slow and can take days. In addition, aqua regia is non-selective in that it preferentially leach toxic base metals such as copper (Cu) and nickel (Ni) that are more reactive in nature than gold or silver. Leaching gold and silver from electronic waste using aqua regia has only been used in experimental studies and is rarely performed at full scale because of its strong oxidizing and corrosive effects on equipment, relatively high operating costs, and difficulty in treating downstream waste.

[0006] Cyanide-based leaching agents have been used to leach gold ores for centuries and are still used to leach gold from secondary sources due to their efficiency, simplicity and relatively low cost. Cyanide-based leaching agents are faster than aqua regia, typically leaching gold within a day, and are more selective for gold. The free cyanide ion (CN - ) acts as a complexing agent, forming a stable complex with gold at pH values ​​above 10. It is estimated that cyanide leaching has been used for about 90% of primary ore gold production and is also the main leaching agent used in electronic waste recycling in China.

[0007] While cyanide leaching is generally more selective than nitric acid for precious metals such as gold and silver, and with minimal reagent loss in the process, reported leaching yields are modest, with commercial cyanide leaching agents, for example, only 60% of gold was extracted from secondary sources such as crushed waste PCBs, with only 500g of gold recovered per ton of PCB waste. While 88% gold leaching was achieved in 2 hours using commercial cyanide stripping at room temperature, the gold concentration per PCB was not reported. Similarly, leaching yields of only about 60% were reported for silver from secondary sources such as crushed waste PCBs using cyanide-based leaching agents.

[0008] However, interest in non / low-cyanide methods for dissolving gold and silver stems from concerns about the extremely high toxicity of cyanide at high concentrations over long periods of time. In addition, the costs associated with treating downstream waste are high due to toxicity. Due to the high toxicity of cyanide, many countries have strictly regulated or even banned the use of cyanide, especially on a large scale.

[0009] As industrial demand for gold and silver continues to increase, effective technologies are needed to extract and recover gold and silver from secondary sources to meet demand. At the same time, there is an increase in regulations around the world that mandate the recycling of electronic waste, which accounts for the majority of secondary sources of gold and silver.

[0010] In view of the limitations of current methods for extracting gold and / or silver from solid waste containing gold and / or silver, it is necessary to develop leaching agents that are non-toxic, user- and environmentally friendly, economical, and capable of achieving efficient and selective extraction to overcome or at least improve one or more of the above-mentioned shortcomings. SUMMARY OF THE INVENTION

[0012] In one aspect, a composition is provided, comprising:

[0013] i) strong base;

[0014] ii) an oxidizing agent; and

[0015] iii) thiocyanate,

[0016] Wherein the composition has a pH in the range of 12-14.

[0017] Advantageously, the composition defined above can be selective for precious metals such as gold and / or silver, can be non-toxic, compatible with downstream recovery processes, non-scalable, and recyclable. More advantageously, the cyanide content in the composition defined above can be very low, the cyanide content is 1 / 20 of that of conventional leaching agents, the lead ion content can be very low, and the leaching of precious metals can be promoted at moderate temperatures in an alkaline system with a pH of about 12-14.

[0018] More advantageously, the composition defined above can provide a simple, low-cost and relatively safe way to selectively and effectively leach precious metals such as gold and / or silver from gold or silver coated solid waste by hydrometallurgy. Unlike conventional leaching agents, the composition defined above can be alkaline (pH 12-14), can be free of aqua regia, and can have a very low cyanide content (1,400 ppm to 1,900 ppm), and the cyanide can be further consumed over time, making it relatively safer to handle without generating large amounts of toxic waste streams.

[0019] Advantageously, thiocyanates can be used in the composition. Thiocyanates can have excellent selectivity for precious metals, low environmental risk, and simple subsequent processing. Compared with other cyanide-free leaching agents, the use of thiocyanates in the leaching process can further enhance adaptability and improve leaching rates. In addition, the toxicity of thiocyanates can be 1 / 1000 of that of cyanide, and thiocyanates can be very strong complexing agents for precious metals. More advantageously, when thiocyanates are used, reagent losses can be lower.

[0020] Advantageously, the composition may be alkaline. The use of a strong base may allow the leaching process of the precious metal to be carried out under alkaline conditions. Since the use of thiocyanates under acidic conditions may generate toxic hydrogen cyanide (HCN) gas during the cyanide release process, the alkaline pH of the composition defined above may advantageously prevent the generation of toxic HCN gas during the extraction process.

[0021] In one embodiment, the composition may further include an amine compound. The addition of an amine compound may increase the amount of extractable precious metals to 3-4 g / L and may also help retard the extraction of base metals. In another embodiment, the composition may advantageously include lead ions to prevent unnecessary side reactions such as passivation of precious metals.

[0022] In another aspect, there is provided a method for preparing the composition defined above, comprising the steps of mixing:

[0023] i) strong base;

[0024] ii) an oxidizing agent; and

[0025] iii) thiocyanate;

[0026] Wherein the composition has a pH in the range of 12-14.

[0027] Advantageously, the process defined above can be carried out at mild temperatures of ≤ 70°C and in a few hours, which means that only moderate energy consumption is required. Even more advantageously, as the leaching proceeds, the alkalinity of the composition can be reduced towards neutrality, so that the resulting leachate becomes even less corrosive over time, simplifying the post-treatment of the waste.

[0028] In another aspect, there is provided a method of extracting precious metals from a solid mixture comprising the precious metals, the method comprising the step of contacting a composition as defined above with the solid mixture to form a leachate solution.

[0029] Advantageously, using the method defined above, more than 95% of gold or silver can be extracted at a temperature of 50-60°C in less than 4 hours at a minimum saturation concentration of 3-4 g / L of gold or silver. The extraction can be relatively selective, with gold and / or silver accounting for 85%-96% of the main extracted metal, thereby reducing the complexity of the downstream recovery process, thereby obtaining high purity gold and silver. More advantageously, the extraction of gold or silver by the method defined above can be carried out batchwise until the composition is saturated.

[0030] Advantageously, the method defined above is broadly applicable to a variety of electronic waste, including gold or silver coated solid waste, such as motherboards, printed circuit boards (PCBs), connectors, thin film battery samples and lead frames.

[0031] In a further aspect, there is provided the use of a composition as defined above for recovering precious metals from a solid mixture comprising a plurality of metals, the metals including the precious metal.

[0032] More advantageously, the extracted precious metals can be recovered from the leachate by conventional methods such as reduction and precipitation, whereby more than 99% of the precious metals can be precipitated at a purity of 90% to 95%.

[0033] definition

[0034] As used herein, the following words and terms shall have the meanings indicated:

[0035] For the purposes of this disclosure, the term "leaching" refers to the process of extracting a substance from a solid mixture into a liquid by dissolution. The term "leachate" should be interpreted accordingly.

[0036] For the purposes of this disclosure, the word "recovery" refers to the process of recovering dissolved substances from solution as solids.

[0037] The word "substantially" does not exclude "completely", for example, a composition "substantially free of" Y may be completely free of Y. If necessary, the word "substantially" may be omitted from the definition of the present invention.

[0038] Unless otherwise stated, the terms "comprising" and "comprise" and grammatical variations thereof are intended to represent "open" or "inclusive" language such that they include the recited elements and also permit the inclusion of additional, unrecited elements.

[0039] As used herein, the term "about", in the context of formulation ingredient concentrations, typically refers to + / - 5% of the stated value, more typically, + / - 4% of the stated value, more typically, + / - 3% of the stated value, more typically, + / - 2% of the stated value, even more typically, + / - 1% of the stated value, and even more typically, + / - 0.5% of the stated value.

[0040] Throughout this disclosure, certain embodiments may be disclosed in range format. It should be understood that the description in range format is only for convenience and brevity and should not be construed as a rigid limitation on the disclosed range. Therefore, the description of a range should be considered to have specifically disclosed all possible subranges and individual values ​​within the range. For example, the description of a range such as 1-6 should be considered to have specifically disclosed subranges such as 1-3, 1-4, 1-5, 2-4, 2-6, 3-6, and individual values ​​within the range, such as 1, 2, 3, 4, 5, and 6. This applies no matter how large the range is.

[0041] This paper may also carry out a broad and general description of certain embodiments. Each narrower category and sub-general grouping falling within the general disclosure scope also constitutes a part of the disclosure. This includes the general description of the embodiment carried out in the case of a proviso or negative restriction, and this proviso or negative restriction deletes any subject from this general concept, regardless of whether this paper specifically describes the material of this deletion.

[0042] Detailed Disclosure of Optional Embodiments

[0043] A composition is provided, comprising:

[0044] i) strong base;

[0045] ii) an oxidizing agent; and

[0046] iii) thiocyanate,

[0047] Wherein the composition has a pH in the range of 12-14.

[0048] The pH can range from about 12 to about 14, about 12 to about 12.5, about 12 to about 13, about 12 to about 13.5, about 12.5 to about 13, about 12.5 to about 13.5, about 12.5 to about 14, about 13 to about 13.5, about 13 to about 14, or about 13.5 to about 14.

[0049] A strong base can be an alkali metal or alkaline earth metal hydroxide. A strong base can completely dissociate in aqueous solution.

[0050] The strong base may be an alkali metal hydroxide. The strong base may be selected from the group consisting of sodium hydroxide, potassium hydroxide, lithium hydroxide, rubidium hydroxide, cesium hydroxide and any mixture thereof.

[0051] The composition may comprise a strong base at a concentration ranging from about 2% w / v to about 5% w / v, from about 2% w / v to about 3% w / v, from about 2% w / v to about 4% w / v, from about 3% w / v to about 4% w / v, from about 3% w / v to about 5% w / v, or from about 4% w / v to about 5% w / v, based on the total volume of the composition.

[0052] The composition may comprise a strong base at a concentration ranging from 2% w / v to 5% w / v based on the total volume of the composition, such that the pH of the composition is in the range of 12-14.

[0053] The oxidizing agent may be selected from the group consisting of persulfates, peroxides, peroxyacids, oxoacids, oxyanions, nitrate compounds, hexavalent chromium compounds, permanganates, cerium (IV) compounds, sodium bismuthate, lead dioxide, and any mixtures thereof.

[0054] The oxidizing agent can be selected from the group consisting of sodium persulfate (Na2S2O8), potassium persulfate (K2S2O8), ammonium persulfate ((NH4)2S2O8), sodium nitrate, potassium nitrate, peroxydisulfuric acid, peroxymonosulfuric acid, hypochlorite, sodium hypochlorite, calcium hypochlorite, chlorite, sodium chlorite, chlorate, sodium chlorate, potassium chlorate, perchlorate, sodium perchlorate, potassium perchlorate, ammonium perchlorate, perchloric acid, chromic acid, dichromic acid, chromium trioxide, pyridinium chlorochromate, chromate compounds, dichromate compounds, sodium permanganate, potassium permanganate, ammonium cerium nitrate, cerium sulfate, sodium perborate, sodium percarbonate, sodium perphosphonate, sodium persulfate, urea peroxide, sodium bismuthate, lead dioxide, and any mixture thereof.

[0055] The oxidizing agent may be a persulfate. The oxidizing agent may be selected from the group consisting of sodium persulfate (Na2S2O8), potassium persulfate (K2S2O8), ammonium persulfate ((NH4)2S2O8) and any mixture thereof.

[0056] Persulfates are probably one of the cheapest oxidants with the highest oxidation potential of all peroxy compounds. This may make them strong oxidants, especially at elevated temperatures in alkaline systems. Therefore, persulfates can promote oxidation reactions in an effective manner in the leaching agents defined above.

[0057] The composition may comprise an oxidant at a concentration ranging from about 2% w / v to 8% w / v, from about 2% w / v to about 4% w / v, from 2% w / v to about 6% w / v, from 4% w / v to about 6% w / v, from 4% w / v to about 8% w / v, or from about 6% w / v to about 8% w / v, based on the total volume of the composition.

[0058] Thiocyanate can be any salt containing the anion [SCN] - The thiocyanate may be an inorganic thiocyanate, an organic thiocyanate or any mixture thereof.

[0059] Thiocyanate can act as a complexing agent for cyanide. Thiocyanate can complex with precious metals.

[0060] The noble metal may be a metal selected from Group 10 or Group 11 of the Periodic Table of Elements. The noble metal may be selected from the group consisting of palladium, platinum, silver, gold and any mixture thereof. The noble metal may be silver, gold or silver and gold. The noble metal may be gold.

[0061] The thiocyanate may be selected from the group consisting of potassium thiocyanate (KSCN), sodium thiocyanate (NaSCN), phenyl thiocyanate, guanidine thiocyanate, and any mixture thereof.

[0062] The composition may comprise a thiocyanate concentration ranging from about 0.5% w / v to 2% w / v, from about 0.5% w / v to about 1% w / v, from about 0.5% w / v to about 1.5% w / v, from about 1% w / v to about 1.5% w / v, from about 1% w / v to about 2% w / v, or from about 1.5% w / v to about 2% w / v, based on the total volume of the composition.

[0063] The amount of thiocyanate in the composition can result in the release of about 1,400 mg / L (ppm) to about 1,900 mg / L (ppm) of free cyanide in the solution. The amount of free cyanide decreases over time as cyanide is consumed during the precious metal extraction process.

[0064] The composition may also include a compound containing a benzoic acid functional group. The compound containing a benzoic acid functional group may function as a non-cyanide related complexing agent that may complex with the noble metal defined above. The benzoic acid group of the benzoic acid containing compound may complex with the noble metal defined above.

[0065] The compound containing a benzoic acid functional group may be selected from the group consisting of phthalic acid, nitrobenzoic acid, 4-nitrobenzoic acid, salicylic acid, anthranilic acid, hydroxybenzoic acid, halogenated benzoic acid, toluic acid and any mixture thereof.

[0066] The compound containing a benzoic acid functional group can be present in a concentration ranging from about 0.5% w / v to about 2% w / v, from about 0.5% w / v to about 1% w / v, from about 0.5% w / v to about 1.5% w / v, from about 1% w / v to about 1.5% w / v, from about 1% w / v to about 2% w / v, or from about 1.5% w / v to about 2% w / v, based on the total volume of the composition.

[0067] The composition may also contain an amine compound.

[0068] The amine group of the amine compound may be a primary amine, a secondary amine or a tertiary amine. The amine compound may contain 1, 2, 3, 4, 5 or 6 amine groups.

[0069] The amine compound may further comprise an alcohol group. The amine compound may comprise 1, 2, 3, 4, 5 or 6 alcohol groups.

[0070] The amine compound can be selected from the group consisting of ethanolamine, hexamethylenetetramine, ethylenediamine, N-(2-hydroxyethyl)ethylenediamine, N,N-dimethylethylenediamine, ethylenediaminetetraacetic acid (EDTA), 5,5-dimethylhydantoin, ammonia, EDTA, nicotinic acid, 1,10-phenanthroline, 4,6-dimethylpyrimidine, 4,7-phenanthroline, benzo[c]cinnoline, 4-(2-pyridyl)pyrimidine and any mixture thereof.

[0071] The amine compound may be selected from the group consisting of ethanolamine, hexamethylenetetramine, ethylenediamine, N-(2-hydroxyethyl)ethylenediamine, N,N-dimethylethylenediamine, and any mixture thereof.

[0072] Amine compounds, which are derivatives of ammonia, have been shown to achieve highly selective extraction of precious metals. Amine compounds are preferred over ammonia because they are easier to handle and generally consume less than volatile ammonia. Amine compounds can form stable complexes with precious metals, thereby improving the extraction of precious metals while reducing the oxidation and extraction of base metals.

[0073] Base metals can be more abundant, lower cost common metals such as copper (Cu), zinc (Zn), nickel (Ni), aluminum (Al), tin (Sn), lead (Pb) and any mixture thereof. Base metals can often be plated underneath precious metals such as silver (Ag), gold (Au) and / or palladium (Pd) in the underlying layer of electronic components.

[0074] The amine compound can be present in a concentration ranging from about 0.05% w / v to about 1% w / v, about 0.05% w / v to about 0.1% w / v, about 0.05% w / v to about 0.2% w / v, about 0.05% w / v to about 0.5% w / v, about 0.1% w / v to about 0.2% w / v, about 0.1% w / v to about 0.5% w / v, about 0.1% w / v to about 1% w / v, about 0.2% w / v to about 0.5% w / v, about 0.2% w / v to about 0.5% w / v, about 0.2% w / v to about 1% w / v, or about 0.5% w / v to about 1% w / v, based on the total volume of the composition.

[0075] The composition may also include lead ions. The lead ions may be present in the form of lead (II) salts. The lead ions may function as surfactant inhibitors to prevent the surface of the noble metal from reacting undesirably during the extraction process, such as passivation of the noble metal. The lead salt may be at least partially soluble in water.

[0076] The lead ions may be present in the form of a lead salt selected from the group consisting of lead (II) nitrate, lead (II) carbonate, lead (II) oxide, lead (II) acetate, lead (II) methanesulfonate, lead (II) citrate, and any mixture thereof.

[0077] The lead ion or lead salt form may be present in a concentration ranging from about 0.02% w / v to about 0.05% w / v, from about 0.02% w / v to about 0.03% w / v, from about 0.02% w / v to about 0.04% w / v, from about 0.03% w / v to about 0.04% w / v, from about 0.03% w / v to about 0.05% w / v, or from about 0.04% w / v to about 0.05% w / v, based on the total volume of the composition.

[0078] Advantageously, the amount of lead ions in the composition may be lower compared to conventionally known leaching agents.

[0079] The composition may be substantially free of iron (Fe) ions. The iron ions may be Fe 2+ or Fe 3+ The composition may not contain any iron ions. The iron ions may be in the form of an iron salt. The iron salt may be ferrous sulfate.

[0080] The composition may also contain water.

[0081] The total % w / v of the strong base, oxidizing agent, thiocyanate, water, optional benzoic acid functional group-containing compound, optional amine compound, and optional lead ions in the composition may be 100% w / v.

[0082] A composition is provided, comprising:

[0083] i) 2% w / v to 5% w / v of a strong base;

[0084] ii) 2% w / v to 8% w / v of an oxidizing agent;

[0085] iii) 0.5% w / v to 2% w / v thiocyanate; and

[0086] iv) 85% w / v to 95.5% w / v water,

[0087] Wherein, the composition has a pH of 12-14, and the total %w / v of the composition is 100%w / v. Provided is a composition, which consists essentially of:

[0088] i) 2% w / v to 5% w / v of a strong base;

[0089] ii) 2% w / v to 8% w / v of an oxidizing agent;

[0090] iii) 0.5% w / v to 2% w / v thiocyanate; and

[0091] iv) 85% w / v to 95.5% w / v water,

[0092] Wherein, the composition has a pH of 12-14, and the total %w / v of the composition is 100%w / v. A composition is provided, comprising:

[0093] i) 2% w / v to 5% w / v of a strong base;

[0094] ii) 2% w / v to 8% w / v of an oxidizing agent;

[0095] iii) 0.5% w / v to 2% w / v thiocyanate;

[0096] iv) 0.5% w / v to 2% w / v of a compound containing a benzoic acid functional group;

[0097] v) 0.05% w / v to 1% w / v of an amine compound;

[0098] vi) 0.02% w / v to 0.05% w / v lead ions; and

[0099] vii) 81.95% w / v to 94.93% w / v water,

[0100] Wherein, the composition has a pH of 12-14, and the total %w / v of the composition is 100%w / v. Provided is a composition, which consists essentially of:

[0101] i) 2% w / v to 5% w / v of a strong base;

[0102] ii) 2% w / v to 8% w / v of an oxidizing agent;

[0103] iii) 0.5% w / v to 2% w / v thiocyanate;

[0104] iv) 0.5% w / v to 2% w / v of a compound containing a benzoic acid functional group;

[0105] v) 0.05% w / v to 1% w / v of an amine compound;

[0106] vi) 0.02% w / v to 0.05% w / v lead ions; and

[0107] vii) 81.95% w / v to 94.93% w / v water,

[0108] Wherein, the composition has a pH in the range of 12-14, and the total % w / v of the composition is 100% w / v.

[0109] The combination of a strong base, an oxidant, and a thiocyanate at specific concentrations may be critical for high yield and selective extraction of precious metals, as deprivation of any one of these components or use of any one of these components at different concentrations may adversely affect the performance of the composition.

[0110] The composition may be a lixiviant (extraction or leaching medium) for extracting a precious metal from a solid mixture comprising the precious metal. The composition may be a lixiviant for extracting a precious metal from a solid mixture comprising the precious metal.

[0111] There is also provided a method for preparing the composition defined above, comprising the steps of mixing:

[0112] i) strong base;

[0113] ii) an oxidizing agent; and

[0114] iii) thiocyanate,

[0115] Wherein the composition has a pH in the range of about 12-14.

[0116] The method may further comprise the step of adding a compound containing a benzoic acid functional group to the composition.

[0117] The method may further comprise the step of adding an amine compound to the composition.

[0118] The method may further comprise the step of adding lead ions to the composition.

[0119] There is also provided a method of extracting precious metals from a solid mixture comprising a plurality of metals including the precious metal, the method comprising the step of contacting the composition defined above with the solid mixture to form a leachate.

[0120] The contacting step can be carried out at a temperature in the range of about 40°C to about 70°C, about 40°C to about 50°C, about 40°C to about 60°C, about 50°C to about 60°C, about 50°C to about 70°C, or about 60°C to about 70°C.

[0121] Compared to conventionally known methods, the temperature of the method can be relatively low. The temperature of the method can be an important consideration related to energy consumption, workplace safety and equipment considerations. Therefore, the method defined above can advantageously reduce energy consumption and improve the safety of the method.

[0122] The contacting step can be performed for a duration of less than 1 hour, less than 45 minutes, less than 30 minutes, less than 15 minutes, or less than 1 minute. The contacting step can be performed for a duration ranging from about 1 minute to about 1 hour, about 1 minute to about 15 minutes, about 1 minute to about 30 minutes, about 1 minute to about 45 minutes, about 15 minutes to about 30 minutes, about 15 minutes to about 45 minutes, about 15 minutes to about 1 hour, about 30 minutes to about 45 minutes, about 30 minutes to about 1 hour, or about 45 minutes to about 1 hour.

[0123] The contacting step may be performed until the leachate solution is saturated. After saturation, the pH of the leachate may have a pH in the range of about 8-10.

[0124] The method can be used to extract precious metals from the surface of solid mixtures, as well as to extract precious metals embedded in or integrated into solid mixtures.

[0125] The plurality of metals may be selected from the group consisting of silver, palladium, aluminum, gold, platinum, copper, iron, nickel, lead, tin, zinc, and any mixture thereof.

[0126] The solid mixture may also comprise base metals as defined above.

[0127] The solid mixture may also contain silicon dioxide, silicates or organic compounds.

[0128] The silicon dioxide or silicates may be in the form of rocks.

[0129] The solid mixture may be an ore containing precious metals.

[0130] The solid mixture may also contain an organic compound. The organic compound may be a polymer. The polymer may be selected from the group consisting of epoxy resins, acrylates, polyamides, poly(ether sulfone) (PES), polyetherimide (PEI), poly(phenylene sulfide) (PPS), polyethylene terephthalate and any mixture thereof. The organic compound may be a brominated flame retardant or a polybrominated biphenyl.

[0131] The solid mixture may be electronic waste or industrial waste. Electronic waste may be selected from the group consisting of TV board waste, PC board waste, central processing unit (CPU), mobile phone waste, portable audio waste, DVD player waste, calculator waste, PC motherboard waste, printed circuit board (PCB) waste, solar panel wafers, connectors, thin film battery samples and lead frames and any mixture thereof. Industrial waste may be film.

[0132] The solid mixture may be selected from precious metal coated electronic waste such as printed circuit boards (PCBs), connectors, thin film battery samples and lead frames.

[0133] The method may also comprise a step of pre-treating the solid mixture before contacting it with the composition as defined above.

[0134] The pre-treatment step may include the step of washing the solid mixture with an organic solvent and / or a strong acid prior to contacting with the composition.

[0135] The organic solvent may be selected from the group consisting of methanol, ethanol, propanol, acetone, chloroform, dichloromethane, dimethyl sulfoxide, dimethylformamide, toluene, tetrahydrofuran, acetone, acetonitrile, and any mixture thereof.

[0136] The strong acid may be selected from the group consisting of hydrochloric acid, nitric acid, sulfuric acid, hydrobromic acid, hydroiodic acid, perchloric acid, chloric acid, and any mixture thereof.

[0137] If the solid mixture comprises organic compounds, the pre-treatment step may include a step of separating the solid mixture into the organic compounds and the plurality of metals to form a solid metal mixture.

[0138] The pre-treatment step may include a size reduction step, wherein the solid mixture or solid metal mixture may be comminuted or cut.

[0139] It will be appreciated by those skilled in the art that the solid mixture or solid metal mixture can be ground into particles or ground to a specific average size by various well-known crushers or grinders (e.g., hammer mills, ball mills, ring mills, and pulverizers), or a combination of two or more such devices. For example, the grinding step can include a cutting stage, followed by a two-step grinding and crushing stage. The particle size can be reduced to a range of millimeters to centimeters. The particle size can be reduced to less than 10 cm, less than 5 cm, less than 2 cm, less than 1 cm, or less than 1 mm. The particle size can be reduced to an average of about 1 mm to about 10 cm, about 1 mm to about 2 mm, about 1 mm to about 5 mm, about 1 mm to about 1 cm, about 1 mm to about 2 cm, about 1 mm to about 5 cm, about 2 mm to about 5 mm, about 2 mm to about 1 cm, about 2 mm to about 2 cm, about 2 mm to about 5 cm, about 2 mm to about 10 cm, about 5 mm to about 1 cm, about 5 mm to about 2 cm, about 5 mm to about 5 cm, about 5 mm to about 10 cm, about 5 mm to about 1 cm, about 5 mm to about 2 cm, about 5 mm to about 5 cm, about 5 mm to about 10 cm, about 1 cm to about 2 cm, about 1 cm to about 5 cm, about 1 cm to about 10 cm, about 2 cm to about 5 cm, about 2 cm to about 10 cm, or about 5 cm to about 10 cm.

[0140] The size reduction step may follow the separation step.

[0141] The pretreatment step may include a start-up step in which the optionally crushed or cut solid mixture or solid metal mixture is contacted with a strong acid. The strong acid may be sulfuric acid.

[0142] The priming step may follow the size reduction step.

[0143] The pretreatment step may comprise a washing step, wherein the optionally comminuted, cut or started solid mixture or solid metal mixture may be rinsed with water.

[0144] A wash step may follow the priming step.

[0145] The contacting step may be repeated multiple times for the same solid mixture. That is, the solid mixture may be contacted with a first batch of the composition defined above to form a first leachate solution, and after contacting the first batch of the composition, the same solid mixture may be contacted with a second batch of the composition defined above to form a second leachate solution. The second batch of the composition may not have been previously contacted with any solid mixture. Likewise, after contacting the second batch of the composition, the same solid mixture may be contacted with a third batch of the composition defined above to form a third leachate solution. The third batch of the composition may not have been previously contacted with any solid mixture.

[0146] The first leachate solution and the second leachate solution may be combined.The third leachate solution may be combined with the first leachate solution and the second leachate solution.

[0147] The method may further comprise the step of contacting the leachate solution with a reducing agent to precipitate the precious metal.The precious metal may be precipitated as a solid in elemental form, an oxide of the precious metal, or a mixture thereof.

[0148] If the solid precipitates as an oxide of the noble metal, or as a mixture of the noble metal in elemental form and the noble metal oxide, the solid may be further purified to obtain the noble metal in elemental form.

[0149] The reducing agent can be H2, hydrazine, sodium borohydride (NaBH4), lithium aluminum hydride (LiAlH4), sodium acetate, citrate, and any mixture thereof. The citrate can be selected from the group consisting of ammonium ferric citrate, sodium citrate, trisodium citrate, potassium citrate, zinc citrate, magnesium citrate, and any mixture thereof.

[0150] The contacting step to precipitate the precious metal may be performed at a temperature in the range of about 60°C to about 80°C, about 60°C to about 70°C, or about 70°C to about 80°C.

[0151] If the step of contacting the composition with the solid mixture is repeated multiple times on the same solid mixture, the combined leachate solutions may be subjected to the contacting step for precipitating the precious metal.

[0152] Those skilled in the art will appreciate that the pH, the temperature of the contacting step, the duration of the contacting step, and the shape and / or volume of the leaching agent may be adjusted to improve the performance of the leaching agent, depending on the composition type of the solid mixture.

[0153] There is also provided the use of a composition as defined above for recovering precious metals from a solid mixture comprising a plurality of metals including the precious metal.

[0154] BRIEF DESCRIPTION OF THE DRAWINGS

[0155] The accompanying drawings illustrate the disclosed embodiments and are used to explain the principles of the disclosed embodiments. However, it should be understood that the accompanying drawings are designed for illustration purposes only and are not intended to limit the scope of the present invention.

[0156] Figure 1

[0157] [ Figure 1 ] shows a photographic image of gold recovered in the form of brown particles using the leaching agent of the present invention.

[0158] Figure 2

[0159] [ Figure 2 ] shows a photographic image of gold coated electronic waste using the leaching agent of the present invention. Figure 2 A is the motherboard, Figure 2 BPrinted circuit board (PCB).

[0160] Figure 3

[0161] [ Figure 3 ] shows photographic images of gold coated electronic waste before and after exposure to the leaching agent of the present invention. Figure 3 A shows a sample of a gold-coated random access memory (RAM), Figure 3 B shows a sample of gold-coated pins, Figure 3 C shows a sample of a gold-coated central processing unit (CPU), Figure 3 D shows a sample of a gold-coated master plate.

[0162] Figure 4

[0163] [ Figure 4 ] shows a curve chart showing the extraction performance of the extractant of the present invention for gold and silver changing over time. Example

[0164] Non-limiting examples of the present invention will be described in further detail with reference to specific examples, which should not be construed as limiting the scope of the present invention in any way.

[0165] Methods and Materials

[0166] Potassium hydroxide (99.5%), potassium persulfate (95%), and guanidine thiocyanate (≥98%) were purchased from Shanghai MacLean Biochemical Co., Ltd. (Shanghai, China). Lead (II) oxide (≥99%) and ethanolamine (≥98%) were purchased from Sigma-Aldrich (St. Louis, MO, USA). Potassium thiocyanate (analytical grade) and 4-nitrobenzoic acid (analytical grade) were purchased from Sinopharm Chemical Reagent Co., Ltd. (Shanghai, China). Glycine (99%) was purchased from Alfa Aesar (Heysham, Lancashire, UK).

[0167] Inductively Coupled Plasma-Optical Emission Spectroscopy (ICP-OES) was performed using a Thermo Scientific cCAP6300. The element wavelengths used were: gold 242.795 nm, silver 328.068 nm, copper 324.754 nm, aluminum 309.271 nm, nickel 221.647 nm, palladium 340.458 nm, tin 189.989 nm, and zinc 213.856 nm. Three calibration standards (5 ppm, 10 ppm, and 15 ppm) were prepared for each element. The concentrations (mg / L) of dissolved elements were quantified using ICP-OES.

[0168] Energy dispersive X-ray fluorescence (XRF) was performed using Shimadzu's EDX-720, using an aluminum plate (A750) for energy calibration. XRF was used to quantify the percentage of metal element composition.

[0169] According to the Standard Methods for the Examination of Water and Wastewater (23) published by the American Public Health Association (APHA), rd Voltammetric analysis was performed to quantify the free cyanide concentration (mg / L) using the 4500CN F method specified in the Standard Methods for the Examination of Water and Wastewater (2017 23rd Edition).

[0170] Metal Extraction

[0171] Discarded motherboards and printed circuit boards (PCBs) were obtained from electrical component manufacturers and electronic waste recyclers. Prior to leaching, the waste was rinsed with 10% sulfuric acid (H2SO4) to remove any oxide layer that could interfere with extraction, then washed with deionized water and air-dried.

[0172] The mixture of electronic waste samples was immersed in a leaching bath at 50°C to 60°C in batches (i.e., 50g of electronic waste at laboratory scale) and removed as soon as the precious metals were observed to be leached (no effervescence). This process was repeated until the solution was saturated and no new batch of immersed samples could be leached. The duration of immersion for each batch of samples ranged from 1 minute to 30 minutes, depending on the sample type, because the concentration of the leaching bath gradually increased and the dissolution rate slowed down. After rinsing and drying, all leached samples were subjected to a second leaching using the same formulation and conditions as the first leaching to ensure complete dissolution of the precious metals in the samples. This was to obtain the amount of residual precious metals remaining after the first leaching to determine the total amount of precious metals present, which was subsequently used to calculate the extraction rate / recovery rate. The concentration of metal ions in all leachates was analyzed by inductively coupled plasma-optical emission spectroscopy (ICP-OES). The purity of the solid samples after reducing the saturated leaching bath to obtain pure precious metals was analyzed by X-ray fluorescence (XRF).

[0173] Extraction efficiency

[0174] The extraction efficiency of the preparation was determined by Equation 1.

[0175] Formula 1. Determination of extraction rate

[0176]

[0177] Metal Recycling

[0178] First, about 300 g of hydrazine was added to 5 L of saturated leaching agent (concentration: 60 g / L or 2 mol / L hydrazine) at 70 ° C to reduce the gold. After stirring for 20 minutes, a mixture of 100 g of sodium borohydride (NaBH4) and 100 g of sodium acetate was slowly added to further reduce the gold (concentration: 20 g / L or 0.5 mol / L NaBH4 and 20 g / L or 0.25 mol / L sodium acetate), which was stirred for another hour. Over time, brown gold particles ( Figure 1 ) precipitates out of solution and the gold particles are then filtered and dried.

[0179] Example 1: Leaching agent

[0180] Basically, the low cyanide leaching agent developed for extracting gold and / or silver from gold and / or silver coated solid waste disclosed herein is an alkaline aqueous system (pH 13-14) comprising:

[0181] i) 2.0-8.0% w / v potassium persulfate (K2S2O8), acting as the primary oxidant for leaching gold and / or silver;

[0182] ii) 2.0-5.0% w / v potassium hydroxide (KOH), which provides an alkaline medium for the dissolution of the reagents;

[0183] iii) 0.5%-2.0% w / v potassium thiocyanate (KSCN) and guanidine thiocyanate, acting as cyanide-related complexing agents;

[0184] iv) 0.5%-2.0% w / v nitrobenzoic acid, acting as a non-cyanide related complexing agent;

[0185] v) 0.05-1.0% w / v amine additives to enhance gold and / or silver extraction and / or reduce base metal leaching; and

[0186] vi) 0.03% w / v lead (II) oxide as a surfactant inhibitor to prevent undesirable reactions on metal surfaces during the extraction process (i.e., passivation of gold or silver).

[0187] The leaching agent was prepared using a 5% w / v (i.e. 50 g / L) stock solution consisting of potassium hydroxide, 12.5 g / L 4-nitrobenzoic acid, 0.3 g / L lead (II) oxide, 5-10 g / L guanidine thiocyanate, 0-5 g / L potassium thiocyanate, 3-4 g / L amine additive, and finally 60 g / L potassium persulfate. The remainder of the leaching agent consisted of deionized water.

[0188] Example 2: Gold Leaching

[0189] The leaching agent of the present invention is used to extract the gold coating on discarded motherboards and printed circuit boards (PCBs) ( Figure 2 ), discarded motherboards and printed circuit boards were obtained from electrical component manufacturers and electronic waste recyclers. The main base metals in these materials were Cu, Ni, Zn and Sn. Trace amounts of Pd (<0.5%) were also detected.

[0190] The amount of gold leached from electronic waste depends on the composition of the electronic waste sample. It was found that for samples with more Cu or samples with gold plated directly on copper (such as PCBs), the amount of leached gold was lower because Cu was easily leached into the bath once exposed. This resulted in a higher proportion of base metals in the leachate, thereby reducing the proportion of leached gold. On the other hand, for samples with less copper, the amount of leached gold was higher, and other base metals (such as Ni and Sn) had little effect on the performance of the bath.

[0191] Table 2 summarizes the results of small-scale (i.e., 100 mL of lixiviant) leaching of gold from electronic waste samples containing less copper (>3 g / L gold at saturation) by varying the concentration of the main reagent in the leaching bath. Bath 1 exhibited the highest concentration of leached gold at 3.925 g / L at saturation, and Bath 1 included 60 g / L oxidant, 15 g / L cyanide-related complexing agent, 12.5 g / L non-cyanide-related complexing agent, and 1-2 g / L performance enhancing additives. Voltammetric analysis of free cyanide in freshly prepared Bath 1 recorded concentrations in the range of 1,800-1,900 ppm, which is less than 1 / 10 of the amount of cyanide used in industry. At saturation, no cyanide may be detected in the bath, which may indicate that the cyanide is fully complexed with the metal ions.

[0192]

[0193] Using Bath 1 as a baseline, slightly higher levels of the performance enhancing additive were tested in Bath 2 in an attempt to increase the amount of gold that could be leached. While the gold extraction efficiency increased from 89.0% to 90.9%, the actual amount of gold leached at saturation decreased by 3.2% from 3.925 g / L to 3.80 g / L. For Baths 3, 4, and 5, the amount of cyanide was reduced by changing the cyanide-related complexing agent to 10 g / L. While the free cyanide concentration decreased slightly in Baths 3, 4, and 5 compared to Bath 1, the actual amount of gold leached at saturation did not improve. This may illustrate the effect of the cyanide-related complexing agent. The gold extraction efficiency in Bath 3 was calculated to be 95.1%. Interestingly, Bath 5 provided the highest gold extraction efficiency of 96.2% using elevated levels of the performance enhancing additive. Additionally, the proportion of gold in the leachate varied from 85% to 96% at saturation, indicating that the extraction was relatively selective for gold.

[0194] Example 3: Effect of amine additives

[0195] Using the same base leaching agent as in Example 2, the effects of different amine-based performance enhancing additives on gold leaching performance were examined and summarized in Table 3. Among these additives, ethanolamine provided the highest amount of gold at saturation, ≥3.80 g / L, while hexamethylenetetramine provided the highest percentage of gold in the leachate, 93.2%. However, hexamethylenetetramine is flammable, while ethanolamine is less hazardous than the other additives. Therefore, ethanolamine is considered to be the best choice for amine-based additives.

[0196] Table 3. In the saturated leaching test, the same basic leaching agent (a) Extraction performance of various amine performance enhancing additives under the following conditions

[0197]

[0198] Note: (a) The composition of the base leaching agent pair is: 5% w / v KOH, 0.03% w / v PbO, 1.25% w / v 4-nitrobenzoic acid, 6% w / v K2S2O8, 0.5% w / v KSCN, 1% w / v C2H6N4S and 0.02% w / v glycine; (b) Base metals include Cu, Ni, Zn, Sn and Al.

[0199] Example 4: Recovery of gold metal

[0200] After developing the leaching agents of Examples 2 and 3, the use of the leaching agents was tested in cooperation with two companies using electronic waste provided by the companies in a volume of up to 5 L. The electronic waste was mechanically broken into smaller sizes and divided into small batches of about 200 g to 1000 g. Each batch was placed in an inert mesh basket made of polytetrafluoroethylene (PTFE) with a pore size of 3 mm to 10 mm so that it could be loaded into a beaker with a capacity of 5 L with a magnetic stirrer, so that the electronic waste was completely immersed in the leaching agent.

[0201] Figure 3 A section of gold coated e-waste is shown before and after leaching testing. The leaching process was performed by batch leaching, where the duration, mass and sample type were recorded. After saturation, the amount of gold and base metals in the leachate was characterized, and the gold was then recovered by reduction using conventional reduction methods.

[0202] The results of two test runs for both companies are listed in Table 4. An example of gold recovery calculations for Company A’s Test 2 is summarized in Table 5.

[0203] Table 4 Results of gold leaching agent test bedding at two electronic waste recycling companies in Singapore

[0204]

[0205] Note: (#) = leaching process is slow, but the leaching agent is not fully saturated; (^) = insufficient sample

[0206] Table 5. Results of gold recovery from leachate in Company A's Experiment 2

[0207] Volume of leachate used 2.35L Au concentration at saturation (first leaching) 2.82g / L Theoretical mass of gold present 2.35L×2.82g / L=5.64g Residual Au concentration (second leaching) 0.54g / L Extraction efficiency 5.64 / (5.64+0.54)=91.2% Quality of recovered gold metal 5.6g Purity of recovered gold metal 95.8% Actual mass of gold metal recovered 95.8%×5.6g=5.36g Gold recovery percentage (5.36 / 5.64)=95.0% Total recovery rate 91.2%×95.0=86.6%

[0208] As can be seen from Table 4, the gold saturation was as high as 3.5 g / L, the gold in the saturated bath was 94.4%, the extraction rate was as high as 95.0%, and the leaching duration was as short as 2 hours. By using a combination of hydrazine and sodium borohydride to reduce the gold, the gold recovery percentage was 95.0%, as shown in Table 5, and the purity was ≥ 95% according to X-ray fluorescence (XRF) analysis. As shown in Table 2, these results are crucial for validating the leaching agent of the present invention under small-scale experimental conditions.

[0209] Example 5: Leaching Agent Extraction of Gold and Silver Metals

[0210] To further demonstrate the effect of the leaching agent on the extraction of precious metals, the leaching agent was tested using a mixture of about 1300 mg / L of gold (89% purity) powder and 1100 mg / L of silver (93% purity) powder.

[0211] By extracting and recovering gold from electronic waste in the same manner as shown in Examples 2 and 4 in a volume of 0.1 L, gold powder was obtained.

[0212] Silver powder was obtained by extracting silver from electronic waste from the same company as in Example 4 using a known method. Briefly, the electronic waste was immersed in a leaching agent containing 0.4% w / v acetic acid (CH3COOH), 1.1% w / v monochloroacetic acid (C2H3ClO2), 0.1% w / v peptone, 7.5% w / v hydrogen peroxide (H2O2), 0.25% w / v sodium phenolsulfonate (C6H5NaO4S), 0.2% w / v ethanolamine and 0.2% w / v 5,5-dimethylhydantoin at 40°C. The extracted silver was recovered by precipitation after contact with 1M sodium chloride and further reduced to metallic silver in the presence of sodium borohydride (NaBH4).

[0213] The same extraction and recovery process as in Examples 2 and 4 was applied to the mixture of gold and silver powders. The results are shown in Tables 6 and Figure 4 shown.

[0214] Table 6. Changes in the extraction performance of leaching agents for gold and silver over time

[0215]

[0216] The gold and silver can be extracted within 240 minutes using the leaching agent. Figure 4 As shown, in the presence of a mixture of gold and silver powders, the leaching agent has a clear selectivity for gold, with almost all of the gold being extracted within 4 minutes of the start of the test. In contrast, the extraction of silver proceeded gradually over time, requiring 240 minutes to be complete. This demonstrates the ability of the leaching agent to extract both gold and silver simultaneously.

[0217] Industrial Applicability

[0218] The composition defined above can be applied to the extraction and recovery of precious metals such as gold and / or silver from electronic and industrial waste such as motherboards, printed circuit boards, connectors, central processing units (CPUs), in the recycling and waste management industries, in the extraction of precious metals from spent catalysts (spent catalyst recovery), and in the extraction of precious metals from precious metal-containing ores in the mining industry.

[0219] Various other modifications and adaptations of the present invention will be apparent to those skilled in the art after reading the foregoing disclosure without departing from the spirit and scope of the invention, and all such modifications and adaptations are intended to fall within the scope of the appended claims.

Claims

1. A composition comprising: i) strong base; ii) an oxidizing agent; and iii) thiocyanate, wherein the composition has a pH in the range of 12-14.

2. The composition according to claim 1, wherein the strong base is present in a concentration ranging from 2% w / v to 5% w / v based on the total volume of the composition.

3. The composition according to claim 1 or 2, wherein the strong base is selected from the group consisting of potassium hydroxide, sodium hydroxide, lithium hydroxide, rubidium hydroxide, cesium hydroxide and any mixture thereof.

4. A composition according to any one of the preceding claims, wherein the oxidising agent is present in a concentration ranging from 2% w / v to 8% w / v based on the total volume of the composition.

5. A composition according to any one of the preceding claims, wherein the oxidizing agent is a persulfate, preferably selected from the group consisting of sodium persulfate (Na2S2O8), potassium persulfate (K2S2O8), ammonium persulfate ((NH4)2S2O8) and any mixture thereof.

6. A composition according to any one of the preceding claims, wherein the thiocyanate is present in a concentration ranging from 0.5% w / v to 2% w / v based on the total volume of the composition.

7. The composition according to any one of the preceding claims, wherein the thiocyanate is an inorganic thiocyanate, an organic thiocyanate or a mixture thereof, preferably selected from the group consisting of potassium thiocyanate (KSCN), sodium thiocyanate (NaSCN), phenyl thiocyanate, guanidine thiocyanate and mixtures thereof.

8. A composition according to any one of the preceding claims, further comprising a compound containing a benzoic acid functional group.

9. The composition according to claim 8, wherein the compound containing a benzoic acid functional group is present in a concentration ranging from 0.5% w / v to 2% w / v based on the total volume of the composition.

10. The composition of any preceding claim further comprising an amine compound.

11. The composition according to claim 10, wherein the amine compound is present in a concentration ranging from 0.05% w / v to 1% w / v based on the total volume of the composition.

12. A composition according to any preceding claim further comprising lead ions.

13. The composition of claim 12, wherein the lead ions are present in a concentration ranging from 0.02% w / v to 0.05% w / v based on the total volume of the composition.

14. A method for preparing a composition according to any one of the preceding claims, comprising the steps of mixing: i) strong base; ii) an oxidizing agent; and iii) thiocyanate, wherein the composition has a pH in the range of 12-14.

15. The method of claim 15, further comprising the step of adding a benzoic acid functional group-containing compound, an amine compound and / or lead ions to the composition.

16. A method of extracting precious metals from a solid mixture comprising precious metals, the method comprising the step of contacting a composition according to any one of claims 1 to 13 with the solid mixture to form a leachate solution.

17. The method of claim 16, wherein the solid mixture further comprises base metals, silicon dioxide, silicates, organic compounds, or any mixture thereof.

18. The method of claim 16 or 17, wherein the contacting step is performed at a temperature in the range of 40°C to 70°C, or for a duration of about 1-5 hours.

19. The method according to any one of claims 16 to 18, further comprising a pre-treatment step, wherein the solid mixture is washed with an organic solvent and / or a strong acid before contacting with the composition.

20. The method of any one of claims 16 to 19, further comprising the step of contacting the leachate solution with a reducing agent to precipitate the precious metal.

21. Use of the composition according to any one of claims 1 to 13 for recovering precious metals from a solid mixture comprising a plurality of metals including precious metals.