Sputtering target, method for producing sputtering target, crystalline oxide thin film, thin film transistor, and electronic device
By using the oxide sintered sputtering target of In, Ga and O elements, adjusting the Ga/(In+Ga) ratio and In2O3 particle size, the problem of low sputtering target cracks and TFT stability under high power is solved, and the problem of low sputtering target cracks and low TFT stability is achieved. Highly efficient sputtering film formation and high stability thin film transistors.
Patent Information
- Application Number
- CN202380029262.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-06-29
- Filing Date
- 2023-03-20
- Publication Date
- 2024-11-08
AI Technical Summary
During the TFT manufacturing process, abnormal discharge and cracks on the surface of the sputtering target are prone to occur during high-power sputtering film formation, resulting in low productivity and stability, and the prior art is difficult to effectively solve this problem.
Using an oxide sintered sputtering target containing In, Ga and O elements, the atomic composition ratio of Ga/(In+Ga) and the average particle size of the In2O3 crystal structure can improve the flexural strength and crack resistance, and combine appropriately. Manufacturing processes such as sintering and heat treatment are prepared to produce sputtering targets that can operate stably at high power.
Crack suppression during sputtering film formation at high power is achieved, productivity and TFT stability are improved, and high mobility and reliability are ensured.
Smart Images

Figure CN118922580A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a sputtering target, a method for manufacturing the sputtering target, a crystalline oxide film, a thin film transistor and an electronic device. Background Art
[0002] In recent years, in addition to polycrystalline silicon thin films and amorphous silicon thin films, amorphous oxide semiconductors such as InGaZnO are also used as the channel layer of thin film transistors (hereinafter, sometimes referred to as TFTs). The characteristic of oxide semiconductors is that they can achieve large-area uniformity like amorphous silicon. In addition, oxide semiconductors are characterized by the ability to obtain 10cm 2 / Vs or higher, and has a mobility higher than that of amorphous silicon.
[0003] However, in amorphous oxide thin films, the source of carrier supply is oxygen deficiency, and since the behavior of electrons is not necessarily stable relative to external factors such as heat, there is a problem that the operation of thin film transistors becomes unstable. In addition, if a negative bias is continuously applied to a thin film transistor under visible light irradiation, there is also a problem that the threshold voltage shifts to the negative side (photo-negative bias degradation). Therefore, in recent years, research is being conducted on applying crystalline oxide thin films instead of amorphous oxide thin films to the channel layer of thin film transistors.
[0004] Patent document 1 describes a crystalline oxide film, in which the gallium content is greater than 0.15 and less than 0.45 in terms of the Ga / (In+Ga) atomic ratio, and the crystalline phase is composed only of the In2O3 phase of the pyrolusite structure. In addition, the oxide film described in Patent document 1 is obtained by film formation, etching, and annealing using a sputtering target of an oxide sintered body obtained from a raw material composed of indium oxide and gallium oxide. Moreover, Patent document 1 describes a TFT using the oxide film as a channel material. Furthermore, it is described that by selecting a composition range as described in Patent document 1, a film that can be etched with a common weak acid such as oxalic acid instead of a strong acid such as aqua regia can be obtained even without using a special film formation method.
[0005] Patent document 2 describes an oxide sintered body containing indium and gallium as oxides. In the oxide sintered body, the In2O3 phase of the bixbyite structure becomes the main crystal phase, wherein the GaInO3 phase of the β-Ga2O3 structure, or the GaInO3 phase and the (Ga, In)2O3 phase are finely dispersed as crystal grains with an average particle size of 5 μm or less, and the gallium content is 10 atomic % or more and less than 35 atomic % in terms of the Ga / (In+Ga) atomic ratio. In addition, a sputtering target obtained from the oxide sintered body described in Patent document 2 is described.
[0006] Patent Document 3 describes an oxide sintered body having a crystal structure substantially composed of indium oxide showing a bixbyite structure. Gallium atoms are solid-dissolved in the indium oxide in the oxide sintered body, and the atomic ratio Ga / (Ga+In) is 0.10 to 0.15. In addition, a sputtering target obtained from the oxide sintered body described in Patent Document 3 is described.
[0007] Furthermore, Patent Documents 2 and 3 describe that by controlling a sputtering target to have an appropriate crystal phase, it is possible to suppress nodules or prevent abnormal discharge.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: International Publication No. 2015 / 008805
[0011] Patent Document 2: International Publication No. 2009 / 008297
[0012] Patent Document 3: Japanese Patent Application Publication No. 2011-146571 Summary of the invention
[0013] Technical problem to be solved by the invention
[0014] In the manufacturing process of TFT, there is a need to perform film formation at high power (high output) during sputtering film formation in order to improve productivity and stability of TFT. However, if sputtering film formation is performed at high power, abnormal discharge (so-called arc discharge) is likely to occur during film formation. Furthermore, the surface of the sputtering target is exposed to high-energy plasma and becomes highly heated. Therefore, a temperature difference is generated between the surface of the sputtering target and the cooled back side, and thermal stress is generated due to the temperature difference. As a result, cracks are sometimes generated in the sputtering target.
[0015] In conventional sputtering targets, studies on the generation of cracks that occur during film formation by sputtering at high power have not been sufficient, and there is room for further improvement in sputtering targets.
[0016] The object of the present invention is to provide a sputtering target capable of performing sputtering film formation at high power (high output), a method for manufacturing the sputtering target, a crystalline oxide thin film using the sputtering target, a thin film transistor including the crystalline oxide thin film, and an electronic device including the thin film transistor.
[0017] Solutions for solving the above technical problems [1]
[0019] A sputtering target is a sputtering target having an oxide sintered body containing an In element, a Ga element, and an O element.
[0020] The oxide sintered body comprises a crystal structure represented by In2O3,
[0021] The atomic composition ratio of the Ga element in the oxide sintered body satisfies the following formula (1):
[0022] The flexural strength of the oxide sintered body is greater than 140 MPa.
[0023] 8≤Ga / (In+Ga)≤20…(1) [2]
[0025] According to the sputtering target described in [1], the average grain size of the crystal structure represented by In2O3 is 3 μm or less. [3]
[0027] The sputtering target according to [1] or [2], wherein the density measured by the Archimedean method is 6.3 g / cm 3 above. [4]
[0029] In the sputtering target according to any one of [1] to [3], the oxide sintered body includes a crystal structure represented by GaInO 3 . [5]
[0031] The sputtering target according to any one of [1] to [4], wherein the oxide sintered body further includes a crystal structure A in which diffraction peaks are observed at respective positions of the following (A) to (E) at incident angles (2θ) by X-ray (CuKα ray) diffraction measurement.
[0032] (A) 28° or more and 29° or less
[0033] (B) 45° or more and less than 46°
[0034] (C) 46° or more and less than 47°
[0035] (D) 47° or more and 48° or less
[0036] (E) 50° or more and 51° or less [6]
[0038] A method for producing a sputtering target is the method for producing a sputtering target according to any one of [1] to [5], comprising:
[0039] A step of preparing a raw material powder having a particle size of 0.5 μm or less;
[0040] A step of mixing the raw material powders to obtain a raw material mixture, and then granulating the raw material mixture to obtain a raw material granulate;
[0041] The step of forming the raw material granules into a formed body;
[0042] A step of sintering the molded body to obtain the oxide sintered body. [7]
[0044] A crystalline oxide thin film using the sputtering target described in any one of [1] to [5]. [8]
[0046] A thin film transistor comprising the crystalline oxide thin film described in [7]. [9]
[0048] An electronic device comprising the thin film transistor described in [8].
[0049] According to one embodiment of the present invention, there can be provided a sputtering target capable of performing sputtering film formation at high power (high output), a method for manufacturing the sputtering target, a crystalline oxide thin film using the sputtering target, a thin film transistor including the crystalline oxide thin film, and an electronic device including the thin film transistor. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1A This is a perspective view showing the shape of a target according to one embodiment of the present invention.
[0051] Figure 1B This is a perspective view showing the shape of a target according to one embodiment of the present invention.
[0052] Figure 1C This is a perspective view showing the shape of a target according to one embodiment of the present invention.
[0053] Figure 1D This is a perspective view showing the shape of a target according to one embodiment of the present invention.
[0054] Figure 2 It is a longitudinal cross-sectional view showing a thin film transistor according to one embodiment of the present invention.
[0055] Figure 3 It is a longitudinal cross-sectional view showing a thin film transistor according to one embodiment of the present invention.
[0056] Figure 4 It is a longitudinal cross-sectional view showing a quantum tunnel field effect transistor according to one embodiment of the present invention.
[0057] Figure 5 It is a longitudinal sectional view showing another embodiment of a quantum tunnel field effect transistor.
[0058] Fig. 6A It is a longitudinal cross-sectional view for explaining the manufacturing steps of a quantum tunnel field effect transistor.
[0059] Figure 6B It is a longitudinal cross-sectional view for explaining the manufacturing steps of a quantum tunnel field effect transistor.
[0060] Figure 6C It is a longitudinal cross-sectional view for explaining the manufacturing steps of a quantum tunnel field effect transistor.
[0061] Fig.6D It is a longitudinal cross-sectional view for explaining the manufacturing steps of a quantum tunnel field effect transistor.
[0062] Fig. 6E It is a longitudinal cross-sectional view for explaining the manufacturing steps of a quantum tunnel field effect transistor.
[0063] Fig. 7A This is a plan view showing a display device using the thin film transistor according to one embodiment of the present invention.
[0064] Figure 7B 1 is a diagram showing a circuit of a pixel portion of a pixel that can be applied to a VA-type liquid crystal display device.
[0065] Figure 7C This is a diagram showing a circuit of a pixel portion of a display device using an organic EL element.
[0066] Figure 8 This is a diagram showing a circuit of a pixel portion of a solid-state imaging device using a thin film transistor according to one embodiment of the present invention.
[0067] Fig. 9 This is an X-ray diffraction pattern of the oxide sintered body produced in Example 1.
[0068] Fig.10 This is a mapping image of oxygen atoms in the oxide sintered body produced in Example 1. DETAILED DESCRIPTION
[0069] Hereinafter, the embodiments will be described with reference to the accompanying drawings, etc. However, the embodiments can be implemented in a plurality of different schemes, and it is easy for a person skilled in the art to understand that various changes can be made to the embodiments and details without departing from the gist and scope thereof. Therefore, the present invention is not limited to the contents described in the following embodiments for interpretation.
[0070] In the drawings, the size, thickness of the layer, and the region are sometimes exaggerated for clarity. Therefore, the present invention is not limited to the size, thickness of the layer, and the region shown in the drawings. In addition, the drawings schematically show ideal examples, and the present invention is not limited to the shapes and values shown in the drawings.
[0071] Ordinal numbers such as “first”, “second” and “third” used in this specification are added to avoid confusion among components, and components for which no limitation in quantity is described are not limited in quantity.
[0072] In this specification and the like, the term "film" or "thin film" and the term "layer" can be used interchangeably according to circumstances.
[0073] In the sintered body and the oxide thin film in this specification and the like, the term "compound" and the term "crystalline phase" can be used interchangeably according to circumstances.
[0074] In this specification, the "oxide sintered body" may be simply referred to as a "sintered body".
[0075] In this specification, a "sputtering target" may be simply referred to as a "target".
[0076] In this specification, etc., "electrical connection" includes connection via "some substance having an electrical function". Here, "some substance having an electrical function" is not particularly limited as long as it can transmit and receive electrical signals between the connected objects. For example, "some substance having an electrical function" includes electrodes, wiring, switching elements (transistors, etc.), resistors, inductors, capacitors, and other elements having various functions.
[0077] In this specification, etc., the functions of the source or drain of a transistor may be interchanged when transistors of different polarities are used or when the direction of current changes during circuit operation. Therefore, in this specification, etc., the terms source or drain can be used interchangeably.
[0078] In the present specification, a numerical range expressed using "to" means a range including the numerical value described before "to" as the lower limit and the numerical value described after "to" as the upper limit.
[0079] The present inventors invented the present invention based on the following findings.
[0080] It is believed that cracks generated when sputtering is performed at high power (high output) are caused by the surface of the sputtering target exposed to high-energy plasma becoming highly heated, and thermal stress is generated due to the temperature difference between the surface of the target and the back of the cooled target. Parameters related to the generation of cracks include, for example, (1) flexural strength, (2) thermal conductivity, (3) linear expansion coefficient, and (4) Young's modulus.
[0081] The above-mentioned (2) thermal conductivity, (3) linear expansion coefficient and (4) Young's modulus can also slightly change the values of these properties by, for example, changing the crystal structure and changing the ratio of the constituent crystals. On the other hand, (1) flexural strength can be improved by suppressing the pores in the sintered body or reducing the average grain size of the crystal phase. Therefore, in order to improve the crack resistance (hereinafter, this resistance is sometimes referred to as power resistance) when sputtering film formation at high power (high output), it is effective to improve the flexural strength.
[0082] In view of the above, the present inventors have found that in a sputtering target having an oxide sintered body containing In, Ga, and O, by studying the crystal structure contained in the sintered body and the atomic composition ratio of Ga, sputtering film formation at high output is possible.
[0083] In addition, the inventors of the present invention have obtained the following insight: in a sputtering target having an oxide sintered body containing the elements In, Ga and O, by studying the crystal structure contained in the sintered body, the atomic composition ratio of the Ga element, and the average particle size of the crystal structure represented by In2O3, sputtering film formation can be performed at high output and crack resistance can be improved.
[0084] [Sputtering target]
[0085] The sputtering target of the present embodiment includes a sintered body. The sintered body becomes a film raw material when forming a film by sputtering. That is, the sputtering target of the present embodiment includes an oxide sintered body containing In element, Ga element and O element. The sintered body includes a crystal structure represented by In2O3, the atomic composition ratio of the Ga element in the oxide sintered body satisfies the following formula (1), and the flexural strength of the oxide sintered body is greater than 140 MPa.
[0086] 8≤Ga / (In+Ga)≤20…(1)
[0087] In the formula (1), In and Ga represent the number of atoms of the indium element and the gallium element in the sintered body, respectively.
[0088] <Grain size of sintered body>
[0089] In the sintered body included in the target of the present embodiment, the sintered body includes a crystal structure represented by In 2 O 3. In addition to the crystal structure represented by In 2 O 3, the sintered body may include other crystal structures such as GaInO 3.
[0090] The proportion of the crystal structure represented by In2O3 in the sintered body of the present embodiment is preferably substantially 80% or more in terms of area ratio. Therefore, the crystal structure represented by In2O3 is preferably the main phase in the sintered body possessed by the target of the present embodiment. The crystal structure represented by In2O3 is a bixbyite phase. Regarding the proportion of the crystal structure represented by In2O3 in the sintered body, X-ray diffraction (XRD) measurement of the sintered body is performed, and quantification is performed based on the peak area of the strongest line of each crystal phase and the RIR value (Reference Intensity Ratio).
[0091] As one embodiment of a sintered body, when the crystal phase of the sintered body is composed of a crystal structure represented by In2O3 (i.e., schistose manganese phase represented by In2O3) and a crystal structure represented by GaInO3, the ratio of the crystal structure represented by In2O3 is the ratio of the crystal structure represented by In2O3 to the overall crystal structure of the crystal structure represented by In2O3 and the crystal structure represented by GaInO3.
[0092] As one embodiment of a sintered body, when the crystal phase of the sintered body is composed of a crystal structure represented by In2O3, a crystal structure represented by GaInO3 and a crystal structure A described later, the ratio of the crystal structure represented by In2O3 is the ratio of the crystal structure represented by In2O3 to the crystal structure represented by In2O3, the crystal structure represented by GaInO3 and the crystal structure A as a whole.
[0093] In the sintered body of the target of the present embodiment, the average grain size of the crystal structure represented by In2O3 contained in the sintered body is preferably 3 μm or less. That is, the average grain size of the crystal structure represented by In2O3 as the main phase is preferably 3 μm or less. If the average grain size of the crystal structure represented by In2O3 contained in the sintered body is 3 μm or less, the flexural strength of the sintered body is improved, resulting in further improvement in power resistance. The average grain size of the crystal structure represented by In2O3 is more preferably 2.5 μm or less, and further preferably 2 μm or less.
[0094] The lower limit of the average particle size of the crystal structure represented by In2O3 is not particularly limited, and for example, it can be 1 μm or more.
[0095] In addition, in one aspect of the sintered body included in the target of the present embodiment, in addition to the crystal structure represented by In2O3 included as the main phase, for example, in the case where a crystal structure represented by GaInO3 is also included, it is also conceivable to reduce the average grain size of the crystal structure represented by GaInO3 instead of reducing the average grain size of the crystal structure represented by In2O3. However, in the case of reducing the average grain size of the crystal structure represented by GaInO3, if the average grain size of the crystal structure represented by In2O3 as the main phase is large, it is difficult to obtain excellent flexural strength.
[0096] The average particle size of the crystal structure represented by In2O3 can be calculated as follows. First, observe the ground sintered body using SEM, and observe the secondary electron image and the reflected electron image at a magnification of 2000 times. When observing using SEM, use energy dispersive X-ray spectroscopy (EDS: Energy Dispersive X-ray Spectroscopy) to find the atomic ratio of each grain. In addition, the crystalline phase is confirmed by performing X-ray diffraction (XRD) measurement on the sintered body. Then, compare it with the crystal structure identified by X-ray diffraction (XRD) to identify each crystalline phase. Using the obtained SEM image, measure the grains and calculate the average value of the particle size.
[0097] Specifically, the average particle size of the crystal structure represented by In 2 O 3 can be measured, for example, as follows.
[0098] When the planar shape of the sintered body is a quadrilateral, the surface of the sintered body is divided into 16 parts of equal area, and a 1 cm square corner is cut out at 16 positions of the center point of each quadrilateral, and mirror polishing is performed to serve as a measurement sample. The measurement surface of the cut sintered body is further divided into 9 parts of equal area, and secondary electron images and reflected electron images are observed at 9 positions of the center point of each quadrilateral at a magnification of 2000 times. During SEM observation, EDS measurement is performed, and the crystal structure identified by XRD is compared to identify which crystal each grain is. The particle size is measured based on the obtained SEM image, and the average value of the particle size of the particles in the 9 frames is calculated respectively. This operation is performed on the measurement sample cut out from 16 positions, and the average value of the particle size obtained based on a total of 144 SEM images is used as the average particle size.
[0099] Regarding the particle size, for particles with an aspect ratio of less than 2, the particle size of the crystal grain is measured as a circle equivalent diameter based on JIS R 1670:2006. As a measurement procedure for the circle equivalent diameter, specifically, a circular ruler is attached to the particle to be measured in the microstructure photograph, and the diameter corresponding to the area of the particle to be measured is read. For particles with an aspect ratio of more than 2, the average value of the longest diameter and the shortest diameter is taken as the particle size of the particle. More specifically, it can be confirmed by the method described in the embodiments described later.
[0100] <Crystal structure of sintered body>
[0101] In the sintered body of the target of the present embodiment, the crystal phase of the sintered body preferably includes, in addition to the crystal structure represented by In2O3, a crystal structure A in which diffraction peaks are observed at each position of the incident angle (2θ) of (A) to (E) described below by X-ray (CuKα ray) diffraction measurement. In addition, as the crystal phase included in the sintered body, it is also preferred that the sintered body includes, in addition to the crystal structure represented by In2O3 and the crystal structure represented by GaInO3, the above-mentioned crystal structure A.
[0102] (A) 28° or more and 29° or less
[0103] (B) 45° or more and less than 46°
[0104] (C) 46° or more and less than 47°
[0105] (D) 47° or more and 48° or less
[0106] (E) 50° or more and 51° or less
[0107] The observation of X-ray diffraction peaks at the positions (A) to (E) above means that the X-ray (CuKα ray: wavelength ) diffraction measurement, there are peaks at the positions where the incident angle (2θ) is (A) greater than 28° and less than 29°, (B) greater than 45° and less than 46°, (C) greater than 46° and less than 47°, (D) greater than 47° and less than 48°, and (E) greater than 50° and less than 51°.
[0108] The crystal phase of the sintered body of the present embodiment includes the crystal structure A, so that the values of the thermal conductivity, linear expansion coefficient, and Young's modulus of the sintered body can be changed. As a result, even when film formation is performed at high power, the occurrence of cracks can be more easily suppressed.
[0109] The observation of X-ray diffraction peaks at the respective positions of (A) to (E) can be confirmed by X-ray diffraction (XRD) measurement. The details will be described in detail in the Examples described below.
[0110] The sintered body of the target of the present embodiment has a crystal structure with different contents of O element (oxygen element) in the element mapping image, that is, a region with a relatively low content of O element (oxygen element) and a region with a relatively high content of O element (oxygen element), and it is preferred that the region with a relatively low content of O element is continuously connected. The resistance value of the structure with a low content of O element, that is, more oxygen defects, becomes lower. The crystal structure with a low content of O element is continuously connected (continuously connected), so that the overall resistance value of the sintered body can be kept low, and as a result, it is easier to suppress the generation of cracks even if the film is formed at high power. In the case where the resistance value of the sintered body is high, it becomes a cause of abnormal discharge and becomes the main cause of cracks when the film is formed at high power (high output).
[0111] The element mapping image of the sintered body can be evaluated using a scanning electron microscope (SEM: Scanning electron microscope)-energy dispersive X-ray spectroscopy (EDS: Energy Dispersive X-ray Spectroscopy). Hereinafter, scanning electron microscope-energy dispersive X-ray spectroscopy is referred to as SEM-EDS.
[0112] In the sintered body of the target of the present embodiment, the surface roughness Ra (arithmetic mean roughness) of the sintered body is preferably less than 0.5 μm. In addition, the sintered body of the target of the present embodiment preferably has a surface roughness Ra (arithmetic mean roughness) of 0.5 μm or less, and has a grinding surface without directionality. The surface roughness Ra of the sintered body is more preferably less than 0.5 μm, and further preferably less than 0.25 μm. In the case where the surface roughness Ra of the sintered body of the target of the present embodiment is less than 0.5 μm, and the surface roughness Ra of the sintered body of the target of the present embodiment is preferably less than 0.5 μm and has a grinding surface without directionality, abnormal discharge and the generation of particles can be prevented. Furthermore, in the sintered body of the target of the present embodiment, the surface roughness Rz (maximum height roughness) of the surface of the sintered body is preferably less than 2.0 μm. If the surface roughness Rz is less than 2.0 μm, it is easy to obtain a sputtering target with improved crack resistance. As a method of adjusting the surface roughness Ra and the surface roughness Rz of the sintered body, the method described in the production process of the sputtering target described later may be mentioned.
[0113] <Atomic composition ratio of Ga element>
[0114] As described above, in the sintered body included in the target of the present embodiment, the atomic composition ratio of the Ga element satisfies the following formula (1).
[0115] 8≤Ga / (In+Ga)≤20…(1)
[0116] In the sintered body of the target of the present embodiment, if the atomic composition ratio of Ga (Ga / (In+Ga)) represented by the above formula (1) is 8 or more, in the film formation using a mixed gas of Ar gas and O2 gas commonly used, it is possible to suppress the situation where the thin film just after film formation becomes a complete crystalline film and the situation where the thin film just after film formation becomes a thin film mixed with microcrystals, and the generation of residues in the patterning process during TFT production is suppressed. In the case where the thin film just after film formation becomes a complete crystalline film or a thin film mixed with microcrystals, when manufacturing TFTs, residues are generated due to etching using a weak acid such as oxalic acid, making it difficult to obtain the target TFT characteristics. Ga / (In+Ga) is more preferably 10 or more, and even more preferably 12 or more.
[0117] If the atomic composition ratio of Ga (Ga / (In+Ga)) represented by the above formula (1) is 20 or less, the formed thin film can be easily crystallized by heat treatment (annealing) at about 300°C to 450°C even if the formed thin film is not subjected to special annealing treatments such as high-temperature annealing and laser annealing. Furthermore, the thin film can be made larger even without using expensive equipment. In the case where the crystallization of the thin film after annealing is insufficient, the TFT containing the insufficiently crystallized thin film may not be able to ensure high mobility and stability. Ga / (In+Ga) is more preferably less than 18, and even more preferably less than 16.
[0118] In the sintered body of the target of the present embodiment, the sintered body may be substantially composed of only In (indium) element, Ga (gallium) element and O (oxygen) element. Here, "substantially" means that the sintered body of the present embodiment may also contain other components within the scope of the effect of the present invention brought about by the combination of the above-mentioned In element, Ga element and O element. In this case, in the sintered body of the target of the present embodiment, the sintered body may contain elements as impurities. As metal elements in the sintered body, the total content of In element and Ga element relative to the total of the metal elements in the sintered body (100 atomic %) is preferably 99 atomic % or more, more preferably 99.5 atomic % or more, and further preferably 99.9 atomic % or more. The total content of In element and Ga element relative to the total of the metal elements in the sintered body can be 100 atomic %. In addition, in this specification, atomic % is sometimes recorded as at%.
[0119] Impurities refer to elements that are not intentionally added, and refer to elements mixed in raw materials and manufacturing processes. That is, impurities are inevitable impurities that are inevitably contained. The same applies to the following description. As examples of impurities, for example, at least one element selected from the group consisting of alkali metal elements (elements such as Li (lithium), Na (sodium), K (potassium), Rb (rubidium)), alkaline earth metal elements (elements such as Mg (magnesium), Ca (calcium), Sr (strontium), Ba (barium)), H element (hydrogen element), B element (boron element), C element (carbon element), N element (nitrogen element), F element (fluorine element), Si element (silicon element) and Cl element (chlorine element), Zr element (zirconium element), Al element (aluminum element), and Sn element (tin element) can be cited.
[0120] The sintered body included in the target of the present embodiment may contain H element (hydrogen element). When the sintered body contains H element, the atomic concentration of H element in the sintered body is preferably 1×10 16 cm -3 More than and less than 1×10 18 cm -3 .
[0121] The atomic concentration of H element in the sintered body is more preferably 3×10 16 cm -3 More preferably, 5×10 16 cm -3 above.
[0122] If the H element concentration in the sintered body is too low, the H element degassed from the anti-deposition plate of the sputtering chamber during film formation has a greater impact, and the degassed H element is unevenly mixed into the formed film, which sometimes easily reduces the in-plane uniformity of TFT characteristics.
[0123] The atomic concentration of H element in the sintered body is more preferably 5×10 17 cm -3 Below, more preferably 3×10 17 cm -3 the following.
[0124] If the H element concentration in the sintered body is too high, a large amount of H element is mixed into the formed film and forms a donor level or an acceptor level, which may result in significant deterioration of the reliability of the TFT.
[0125] The sintered body of the target of the present embodiment may contain C element (carbon element). When the sintered body contains C element, the lower limit of the atomic concentration of C in the sintered body is not particularly limited, and the amount of impurities during the manufacture of the target may contain 1×10 16 cm -3When the sintered body contains C element, the atomic concentration of C element is preferably 1×10 16 cm -3 More than and less than 1×10 18 cm -3 The atomic concentration of C in the sintered body is more preferably 7×10 17 cm -3 Below, more preferably 4×10 17 cm -3 the following.
[0126] If the atomic concentration of the C element is too high, a large amount of the C element is mixed into the formed film, and the C element forms a donor level or an acceptor level, which may result in significant degradation of the reliability of the TFT.
[0127] In the sintered body of the target of the present embodiment, the sintered body may contain H element (hydrogen element) and C element (carbon element). When the sintered body contains both H element and C element, the atomic concentration of each of H element and C element is preferably 1×10 16 cm -3 More than and less than 1×10 18 cm -3 In addition, in this specification, the unit of atomic concentration of H element and C element is [atoms / cm 3 ]Sometimes recorded as [cm -3 ].
[0128] The atomic concentration of the H element and the atomic concentration of the C element contained in the sintered body can be determined by secondary ion mass spectrometry (SIMS) measurement. A dynamic SIMS apparatus can be used for SIMS measurement.
[0129] The sintered body included in the target of the present embodiment may contain one or more elements (X elements) selected from the group consisting of positive trivalent, positive tetravalent, and positive pentavalent elements as an additive element within a range not impairing the effect.
[0130] In this case, as one scheme, the sputtering target of the present embodiment may include an oxide sintered body containing In element, Ga element and O element, and one or more X elements selected from the group consisting of positive trivalent, positive tetravalent and positive pentavalent. Even in this case, in one scheme, the oxide sintered body also includes a crystal structure represented by In2O3, the atomic composition ratio of the Ga element in the oxide sintered body satisfies the above-mentioned formula (1), and the flexural strength of the oxide sintered body is greater than 140 MPa. In addition, the sintered body of the sputtering target in this scheme may include a crystal structure represented by GaInO3, and may also include the above-mentioned crystal structure A. Furthermore, in the sintered body of the sputtering target in this scheme, the average particle size of the crystal structure represented by In2O3 may be less than 3 μm.
[0131] The X element as an additive element is preferably, for example, at least one element selected from the group consisting of Zn (zinc) element, Mg (magnesium) element, Ti (titanium) element, Fe (iron) element, Zr (zirconium) element, Nb (niobium) element, Hf (hafnium) element, Sn (tin) element, Si (silicon) element, Ge (germanium) element, Ta (tantalum) element, W (tungsten) element, Al (aluminum) element, B (boron) element, Y (yttrium) element, Sc (scandium) element and Ln (lanthanide) element. Among them, the X element as an additive element is more preferably at least one of Zn (zinc) element and Sn (tin) element. The sintered body of the sputtering target in this embodiment can be substantially composed of In (indium) element, Ga (gallium) element, O (oxygen) element and X element. "Substantially" means the same as above. For example, as the metal elements in the sintered body, the total content of the In element, the Ga element, and the X element is preferably 99 atomic % or more, more preferably 99.5 atomic % or more, and further preferably 99.9 atomic % or more relative to the total of the metal elements in the sintered body (100 atomic %). The total content of the In element, the Ga element, and the X element may be 100 atomic % relative to the total of the metal elements in the sintered body.
[0132] The amount of the X element as the added element is preferably 2 at% (2 atomic %) or less, more preferably 1 at% or less, and further preferably 0.5 at% or less. If the amount of the added element is 2 at% or less, when the target of this embodiment is used to manufacture a TFT, it is easy to obtain a TFT with high mobility and high stability. If the amount of the added element is large, the obtained TFT may cause undesirable conditions such as reduced mobility or reduced stability.
[0133] The amount of the element X as an additional element is represented by the following formula (2).
[0134] 0.02≥(X / (In+Ga+X))…(2)
[0135] In the formula (2), In, Ga and X represent the number of atoms of indium element, gallium element and X element in the sintered body, respectively.
[0136] The amount of each element can be measured by ICP (Inductive Coupled Plasma) measurement or XRF (X-ray Fluorescence) measurement to determine the content (atomic ratio) of each metal element in the sintered body. ICP measurement can be performed using an inductively coupled plasma emission spectrometer. XRF measurement can be performed using a thin film fluorescence X-ray analyzer.
[0137] <Physical properties of sintered body>
[0138] In the sintered body included in the target of the present embodiment, the density of the sintered body measured by the Archimedean method is preferably 6.3 g / cm 3 The measured density of the sintered body by the Archimedean method is more preferably 6.5 g / cm 3 above.
[0139] The relative density of the sintered body is preferably 97% or more, more preferably 99% or more. The relative density refers to the percentage of the value obtained by dividing the actual density of the oxide sintered body measured by the Archimedean method by the theoretical density of the oxide sintered body.
[0140] In the sintered body of the target of the present embodiment, the thickness of the sintered body is usually preferably 2 mm or more and 20 mm or less. The thickness of the sintered body is more preferably 3 mm or more, and further preferably 4 mm or more. The thickness of the sintered body is more preferably 12 mm or less, further preferably 9 mm or less, and further preferably 6 mm or less.
[0141] The sintered body included in the target of the present embodiment has a flexural strength of 140 MPa or more, preferably 150 MPa or more, and more preferably 160 MPa or more.
[0142] When the flexural strength is 140 MPa or more, the flexural strength of the sintered body is sufficient to suppress the occurrence of cracks when sputtering is performed at high power (high output) to form a film.
[0143] The flexural strength of the sintered body was determined based on JIS R1601:2008 as an average value of three-point bending strength measurement values of 30 test pieces.
[0144] The sintered body included in the target of the present embodiment also shows excellent characteristics in terms of various physical properties such as thermal conductivity, linear expansion coefficient, and Young's modulus.
[0145] The linear expansion coefficient of the sintered body can be measured in accordance with JIS R 1618:2002 at a measurement temperature of 30° C. to 500° C., a heating rate of 10 K / min, and in an atmosphere of air.
[0146] The Young's modulus of the sintered body can be measured at room temperature in the atmosphere using an ultrasonic flaw detector in accordance with JIS R 1602:1995.
[0147] The thermal conductivity of the sintered body can be calculated from the following equation (1) by measuring the specific heat capacity by a laser flash method (room temperature, in vacuum) and measuring the thermal diffusivity by a laser flash method (room temperature, in air) in accordance with JIS R 1611:2010.
[0148] λ(thermal conductivity) = Cp(specific heat) × ρ(density) × α(thermal diffusivity)…(Equation 1)
[0149] ρ is the density of the oxide sintered body.
[0150] The sputtering target of this embodiment includes an oxide sintered body and a cooling and holding member such as a backing plate provided on the oxide sintered body as needed. The material of the backing plate as a member for holding or cooling the oxide sintered body is preferably a material having excellent thermal conductivity such as copper.
[0151] In the case where the target of the present embodiment has a cooling and holding component such as a backing plate, the sintered body of the sputtering target of the present embodiment has a bonding surface mounted on the holding component and a surface opposite to the bonding surface, i.e., a sputtering surface to be sputtered. In the present embodiment, the sputtering surface is preferably a smooth surface (i.e., a smooth surface such as the surface roughness Ra of 0.5 μm or less), and the surface opposite to the sputtering surface is set as the bonding surface.
[0152] The shape of the sputtering target is not particularly limited. For example, the sputtering target may be Figure 1A The plate-like shape shown in the figure numeral 1 may also be as shown in Figure 1B In the case of a plate-like shape, the planar shape may be Figure 1A The rectangle shown in the figure 1 can also be Figure 1C The oxide sintered body may be formed integrally or as a circle as shown in the figure 1B. Figure 1D As shown, it is a multi-division type in which a plurality of divided oxide sintered bodies (reference numeral 1C) are respectively fixed to a backing plate 3 .
[0153] <Method for producing sputtering target>
[0154] An example of a preferred method for producing the target according to the present embodiment will be described.
[0155] The method for producing the sputtering target according to the present embodiment preferably includes the following steps, for example.
[0156] A step of preparing a raw material powder having a particle size of 0.5 μm or less (hereinafter, sometimes referred to as a raw material powder preparation step).
[0157] A step of mixing the raw material powders to obtain a raw material mixture and then granulating the raw material mixture to obtain a raw material granulated product (hereinafter, sometimes referred to as a granulation step).
[0158] A step of molding the raw material granules to obtain a molded body (hereinafter, sometimes referred to as a molding step).
[0159] A step of sintering the molded body to obtain a sintered body (hereinafter, sometimes referred to as a sintering step).
[0160] The preferred manufacturing method of the target of this embodiment may also have at least one process selected from the group consisting of the following processes, a process of heat treating the sintered body (annealing process), a process of at least grinding the sintered body (hereinafter, sometimes referred to as the grinding process), a process of cleaning the ground sintered body (hereinafter, sometimes referred to as the cleaning process), and a process of joining the sintered body to a backing plate (hereinafter, sometimes referred to as the joining process).
[0161] (Raw material powder preparation process)
[0162] In the raw material powder preparation step, raw material powder used as a raw material of a sintered body possessed by the sputtering target of the present embodiment is prepared. The raw material powders prepared in the raw material powder preparation step are indium oxide having an average particle size of 0.5 μm or less and gallium oxide having an average particle size of 0.5 μm or less. The raw material powder may also be prepared as needed to be a raw material powder of a compound containing one or more elements selected from the group consisting of positive trivalent, positive tetravalent and positive pentavalent elements having an average particle size of 0.5 μm or less. The raw material powder may be prepared by obtaining a raw material powder having an average particle size of 0.5 μm or less, or by obtaining a raw material powder having an average particle size exceeding 0.5 μm, and adjusting the average particle size of the obtained raw material powder to be less than 0.5 μm.
[0163] The average particle size of the raw material powder prepared in the raw material powder preparation step is preferably 0.1 μm or more and 0.5 μm or less. If the average particle size of the raw material powder is 0.1 μm or more, it is easy to suppress the aggregation of the raw material powders, and the raw material powders can be mixed into a nearly uniform state. If the average particle size of the raw material powder is 0.5 μm or less, it is easy to control the average particle size of the crystal structure represented by In2O3 contained in the sintered body after sintering to be 3 μm or less. The average particle size of the raw material powder can be calculated by at least one of the particle size evaluation using a particle size distribution measuring device and the specific surface area obtained by the BET method. In addition, the average particle size of the raw material powder can also be confirmed by a SEM device.
[0164] When the average particle size of the obtained raw material powder exceeds 0.5 μm, it is preferred to pre-crush the raw material powder to adjust the average particle size of the raw material powder to 0.5 μm or less.
[0165] The pre-crushing can be performed using a bead mill, a ball mill, a jet mill, etc. The material of the pot used in the pre-crushing is not particularly limited, and for example, materials such as agate and aluminum oxide can be cited. The material of the pulverizing medium (ball) used in the pre-crushing is not particularly limited, and for example, materials such as aluminum oxide and zirconium oxide can be cited.
[0166] The crushing time in the pre-crushing is preferably more than 30 minutes and less than 6 hours. If the crushing time in the pre-crushing is more than 30 minutes, a sufficient crushing effect can be obtained, and it is easy to adjust to a predetermined average particle size. If the crushing time in the pre-crushing is less than 6 hours, it is difficult to cut off the material of the tank and the material of the ball and mix in foreign matter (difficult to cause pollution), and when using the target of this embodiment to make TFT, it is easy to obtain a TFT with high mobility and high stability. During the pre-crushing, a binder, a dispersant, a defoaming agent, etc. can be appropriately added as needed for crushing.
[0167] The raw material powders of indium oxide and gallium oxide prepared in the raw material powder preparation step are preferably high-purity. The purity of the raw material powders is preferably 99% by mass or more, more preferably 99.9% by mass or more, and further preferably 99.99% by mass or more. In addition, when a raw material powder of a compound containing one or more elements selected from the group consisting of positive trivalent, positive tetravalent and positive pentavalent is used, the raw material powder is also preferably high-purity like the raw material powders of indium oxide and gallium oxide. For example, the purity of the raw material powder of a compound containing one or more elements selected from the group consisting of positive trivalent, positive tetravalent and positive pentavalent is preferably 99% by mass or more, more preferably 99.9% by mass or more, and further preferably 99.99% by mass or more.
[0168] If a high-purity raw material powder is used, a sintered body with a dense structure can be obtained, and the volume resistivity of a sputtering target having the sintered body becomes low. In addition, when a TFT is made using a sputtering target having the sintered body, the formation of defect levels caused by impurities can be suppressed, and a TFT with high mobility and high stability can be obtained.
[0169] (Granulation process)
[0170] In the granulation step, first, the raw material powders prepared in the raw material powder preparation step are mixed to prepare mixed raw material powders, and a dispersant and a thickener are added as needed to prepare a raw material mixture. The mixed raw material powders may also be used directly as a raw material mixture. Next, the raw material mixture is granulated to obtain a raw material granulate. Hereinafter, the raw material granulate may be referred to as raw material granulated powder.
[0171] [Mixing of raw material powders]
[0172] In the raw powder prepared in the raw powder preparation process, a dispersant for removing agglomeration and a thickener for adjusting the viscosity of the granulation suitable for the spray dryer are added as needed, and mixed by a wet ball mill, a planetary ball mill, a bead mill and a jet mill, etc. to obtain a raw material mixture. Wherein, the device for water mixing is preferably a bead mill. If a bead mill is used, the raw powder can be uniformly mixed, so even at the sintering temperature described later, it can be fully sintered, and it is easy to obtain a sputtering target that can be sputtered and film-formed with high power (high output). As a dispersant, for example, an acrylic acid methacrylic acid copolymer ammonia neutralizer, etc. can be exemplified, and as a thickener, for example, polyvinyl alcohol, etc. can be exemplified.
[0173] As long as the raw material powders can be fully mixed, the mixing time of the raw material powders is not particularly limited. The mixing time of the raw material powders is, for example, preferably more than 2 hours and less than 48 hours. If the mixing time is more than 2 hours, the raw material powders are easily fully mixed. If the mixing time is less than 48 hours, it is easy to suppress the re-agglomeration of the raw material powders. In addition, if the mixing time is less than 48 hours, the mixing (contamination) of foreign matter such as the material of the tank and the material of the ball can be suppressed.
[0174] [Granulation of raw material powder]
[0175] The granulation treatment for granulating the raw material mixture can be performed using a spray dryer, etc. The shape of the raw material granules obtained in the granulation step is not particularly limited, but is preferably a true spherical shape in order to uniformly fill the mold in the molding step described later.
[0176] The granulation conditions can be appropriately selected by adjusting the concentration of the raw material mixture after mixing the raw material powders introduced into the spray dryer, the rotation speed of the spray dryer, the temperature of the hot air used for drying, and the like.
[0177] When a raw material mixture that has not been pre-calcined is used and the raw material mixture is granulated by a spray drying method, the raw material granules can be prepared by using the raw material mixture obtained above as it is. When a raw material mixture that has been pre-calcined is used, the raw material mixture that has been pre-calcined can be prepared as a raw material mixture that has been crushed again by the method described in the preliminary crushing of the raw material powder.
[0178] In the target manufacturing method of the present embodiment, the particle size of the raw material granules formed by the granulation treatment is not particularly limited, for example, it is preferably controlled within the range of 25 μm to 150 μm. If the particle size of the raw material granules is 25 μm or more, the sliding property of the raw material granules relative to the surface of the mold used in the forming process described later is improved, and the raw material granules can be fully filled into the mold. If the particle size of the raw material granules is 150 μm or less, it is possible to suppress the reduction of the filling rate in the mold due to excessive particle size. The particle size of the raw material granules is more preferably 25 μm to 75 μm.
[0179] The method for obtaining a raw material granulation with a particle size within the desired range is not particularly limited. For example, a method of sieving the raw material granulation to which a granulation treatment has been applied to screen the raw material granulation belonging to the desired particle size range can be cited. The sieve used in this method is preferably a sieve with an opening of a size through which the raw material granulation of the desired particle size can pass. The sieve used in this method preferably uses a first sieve for screening the raw material granulation based on the lower limit of the particle size range, and a second sieve for screening the raw material granulation based on the upper limit of the particle size range. For example, when the particle size of the raw material granulation is controlled within a range of 25 μm to 150 μm, first, a sieve (first sieve) having an opening of a size through which raw material granulation less than 25 μm can pass and raw material granulation above 25 μm cannot pass is used to screen the raw material granulation with a particle size of 25 μm or more. Next, the raw material granules after screening are screened using a sieve (second sieve) having an opening of a size that allows raw material granules of 150 μm or less to pass through but prevents raw material granules of more than 150 μm from passing through to screen raw material granules within a range of 25 μm to 150 μm. Alternatively, the second sieve may be used first and then the first sieve may be used.
[0180] The method of controlling the particle size range of the raw material granules is not limited to the above-mentioned method using a sieve, and any method may be used as long as the raw material granules to be supplied to the molding step can be controlled within a desired range.
[0181] (Forming process)
[0182] In the forming process, the raw material granules are formed into a formed body by die stamping, casting or injection molding. As a sputtering target, in the case of obtaining a sintered body with a high sintering density, it is preferred to further consolidate the granules by cold isostatic pressing (CIP) or the like after pre-forming by die stamping or the like in the forming process.
[0183] (Sintering process)
[0184] In the sintering step, the molded body obtained in the forming step is sintered to obtain a sintered body. In the sintering step, a commonly used sintering method such as normal pressure sintering, hot pressing sintering, or hot isostatic pressing (HIP) sintering can be used. The obtained sintered body becomes a sputtering target material.
[0185] The sintering temperature is preferably 1300°C to 1400°C. If the sintering temperature is 1300°C or higher, the sintering of the compact is easily and fully carried out, thereby suppressing the generation of a large number of pores in the sintered body and easily improving the flexural strength. If the sintering temperature is 1400°C or lower, it is easy to control the average particle size of the crystal structure represented by In2O3 contained in the sintered body to a range of 3 μm or less, and easily improve the flexural strength.
[0186] The sintering time is preferably 12 hours or more and 48 hours or less. If the sintering time is 12 hours or more, the sintering of the compact is easy to be fully carried out, thereby suppressing the large-scale generation of pores in the sintered body, and the flexural strength is easy to improve. If the sintering time is 48 hours or less, it is easy to control the average particle size of the crystal structure represented by In2O3 contained in the sintered body to a range of less than 3 μm, and the flexural strength is easy to improve.
[0187] In the sintering step, the temperature increase rate from room temperature to the sintering temperature is not particularly limited, but is preferably 0.1° C. / minute to 3° C. / minute.
[0188] In the process of heating, the temperature may be maintained at 700° C. to 800° C. for 1 to 10 hours, and after maintaining the predetermined temperature for a predetermined time, the temperature may be raised to the sintering temperature.
[0189] As the atmosphere during sintering, for example, an atmosphere of air or oxygen, an atmosphere containing air or oxygen and a reducing gas, or an atmosphere containing air or oxygen and an inert gas can be mentioned. As the reducing gas, for example, hydrogen gas, methane gas, and carbon monoxide gas can be mentioned. As the inert gas, for example, argon gas and nitrogen can be mentioned.
[0190] (Heat treatment process (annealing process))
[0191] In the heat treatment step (annealing step), the obtained sintered body is annealed. In the target manufacturing method of the present embodiment, the annealing step is a step provided as needed. When the annealing step is performed, the sintered body is usually treated at a holding temperature of 700° C. to 1100° C. and a holding time of 1 hour to 5 hours.
[0192] In the annealing step, the sintered body may be cooled once and then heated again for annealing, or the annealing may be performed while the temperature is lowered from the sintering temperature.
[0193] As the atmosphere during annealing, for example, air or oxygen atmosphere, an atmosphere containing air or oxygen and a reducing gas, or an atmosphere containing air or oxygen and an inert gas can be mentioned. As the reducing gas, for example, hydrogen gas, methane gas, and carbon monoxide gas can be mentioned. As the inert gas, for example, argon gas and nitrogen can be mentioned.
[0194] (Grinding process)
[0195] In the grinding step, the obtained sintered body is cut into an appropriate shape, and the surface of the oxide sintered body is ground. Specifically, the sintered body is cut into a shape suitable for attachment to a sputtering device, and the surface of the oxide sintered body is ground.
[0196] The abrasive grain size of the grinding wheel used in the grinding process is preferably 100 μm or less. If the abrasive grain size of the grinding wheel is 100 μm or less, the rupture of the sintered body can be prevented. The grinding wheel used in the grinding process is preferably a diamond grinding wheel. The grinding depth of grinding in the grinding process is preferably 0.3 mm or more, more preferably 0.5 mm or more, and further preferably 2 mm or more. By grinding the surface of the sintered body by more than 0.3 mm, the variable part of the crystal structure near the surface can be removed.
[0197] The surface of the sintered body after the grinding process preferably has a surface roughness Ra (arithmetic mean roughness) of 5 μm or less. The surface of the sintered body after the grinding process preferably has a surface roughness Rz (maximum height roughness) of less than 2.0 μm. In addition, the surface of the sintered body after the grinding process preferably has a surface roughness Ra (arithmetic mean roughness) of 5 μm or less and has a non-directional ground surface.
[0198] The sintered body can further implement mirror finishing on the sputtering surface. The mirror finishing (grinding) can use known grinding techniques such as mechanical grinding, chemical grinding and mechanochemical grinding (using mechanical grinding and chemical grinding in combination). For example, it can be polished with a fixed abrasive polisher (polishing liquid is water) with #2000 or above, or it can be ground with a free abrasive grinding disc (grinding material is SiC abrasive paste, etc.), and then the abrasive material is replaced with diamond abrasive paste, thereby grinding. The grinding method is not limited to these methods.
[0199] (Cleaning process)
[0200] In the cleaning process, the sintered body ground in the grinding process is cleaned. As a method of cleaning, for example, any method such as air blowing and running water cleaning can be cited. When removing foreign matter by air blowing, the foreign matter can be removed more effectively by sucking air from the opposite side of the air blowing nozzle using a vacuum cleaner.
[0201] In addition, in the cleaning process, in addition to the cleaning process using air blowing or running water cleaning, ultrasonic cleaning etc. can also be implemented. As ultrasonic cleaning, a method of performing multiple oscillations between a frequency of 25 kHz or more and 300 kHz or less is effective. For example, it is preferred to perform a method of ultrasonic cleaning by performing multiple oscillations at 12 frequencies every 25 kHz between a frequency of 25 kHz or more and 300 kHz or less.
[0202] (Joining process)
[0203] The bonding step is a step of bonding the sintered body after the processing step to the back plate using a low melting point metal (such as metal indium and metal gallium).
[0204] In terms of maintaining the cooling efficiency during sputtering, the bonding rate is preferably 90% or more, more preferably 95% or more, and further preferably 98% or more. The bonding rate referred to herein refers to the area ratio of the surface where the target material and the target support material are bonded via the bonding layer relative to the area of the overlapping surface of the target material and the target support. The bonding rate can be confirmed, for example, by X-ray CT (X-ray Computed Tomography) or ultrasonic flaw detection.
[0205] When sputtering film formation is performed using the sputtering target of the present embodiment, crack resistance is improved, and thus an oxide thin film can be stably produced.
[0206] Furthermore, according to the sputtering target of the present embodiment, since a target having the same atomic composition as the sintered body of the present embodiment is used, a TFT obtained by sputtering has high mobility and high stability.
[0207] [Crystalline oxide thin films]
[0208] The crystalline oxide thin film of the present embodiment is a crystalline oxide thin film using the sputtering target of the present embodiment. The crystalline oxide thin film of the present embodiment is obtained by forming a film using the sputtering target of the present embodiment. The crystalline oxide thin film of the present embodiment is preferably obtained by a manufacturing method including a step of forming an oxide thin film by sputtering (hereinafter, sometimes referred to as an oxide thin film forming step) and a step of heat-treating the oxide thin film (hereinafter, sometimes referred to as a heat treatment step) using, for example, the sputtering target of the present embodiment. According to the crystalline oxide thin film of the present embodiment, since the film is formed using a target having the same atomic composition as the sintered body of the present embodiment, the processability during TFT manufacturing is excellent, and a TFT with high mobility and high stability can be obtained.
[0209] The crystalline oxide thin film of this embodiment is a crystalline oxide thin film. The crystalline oxide thin film of this embodiment is an amorphous (non-crystalline) oxide thin film after sputtering film formation and before heat treatment (annealing treatment). By performing annealing treatment after sputtering film formation, the crystallinity is improved to become a crystalline oxide thin film. The crystalline oxide thin film of this embodiment is a crystalline oxide thin film, and thus a thin film transistor (TFT) including the crystalline oxide thin film of this embodiment has high mobility and high stability.
[0210] Whether the oxide thin film is amorphous or crystalline can be confirmed by X-ray diffraction (XRD) measurement. When XRD measurement is performed on an oxide thin film, if no peak is observed, the oxide thin film can be judged to be amorphous, and if a peak is observed, it can be judged to be crystalline.
[0211] In the oxide thin film forming process, a gas that does not substantially contain impurity gases is used. Specifically, in the oxide thin film forming process, one or more gases selected from the group consisting of argon, hydrogen and oxygen that do not substantially contain impurity gases are used as sputtering gases. Among them, the sputtering gas is preferably a mixed gas of argon and oxygen that does not substantially contain impurity gases. The sputtering gas "substantially does not contain impurity gases" means that, except for adsorbed water brought in with the insertion of the gas, and gases that cannot be removed (inevitable impurity gases) such as leakage or adsorbed gases in the chamber, no impurity gases other than argon, hydrogen and oxygen are actively introduced. In this embodiment, as the sputtering gas, for example, a mixed gas of commercially available high-purity argon and high-purity oxygen can be used. If achievable, it is preferred to remove impurities from the sputtering gas.
[0212] The proportion of the impurity gas in the sputtering gas is preferably 0.1 volume % or less, and more preferably 0.05 volume % or less. When the proportion of the impurity gas is 0.1 volume % or less, crystallization of the oxide thin film proceeds smoothly.
[0213] The purity of high-purity argon and high-purity oxygen is preferably 99% by volume or more, more preferably 99.9% by volume or more, and even more preferably 99.99% by volume or more.
[0214] The oxygen partial pressure in the mixed gas of argon and oxygen as the sputtering gas is preferably in the range of 0 volume % to 50 volume %, and more preferably in the range of 5 volume % to 30 volume %. If the oxygen partial pressure is in the above range, it is easy to crystallize and semiconductorize when heated. The degree of oxidation, i.e., the degree of crystallization, of the obtained thin film can be adjusted by changing the oxygen partial pressure. The oxygen partial pressure can be appropriately selected as needed.
[0215] In the heat treatment step, the heat treatment temperature for crystallizing the formed amorphous thin film is preferably in the range of 300° C. to 450° C., more preferably 300° C. to 350° C. When the heat treatment temperature is 300° C. or higher, the oxide thin film is easily crystallized.
[0216] When the heat treatment temperature is 450° C. or lower, abnormal crystal growth can be suppressed and the crystal grains can be enlarged.
[0217] In the heat treatment step, the heat treatment time for crystallizing the formed amorphous thin film is preferably 0.1 to 5 hours, more preferably 0.3 to 3 hours, and even more preferably 0.5 to 2 hours.
[0218] When the heat treatment time is 0.1 hour or longer, crystallization does not occur, and the oxide thin film is easily crystallized.
[0219] When the heat treatment time is 5 hours or less, excellent economic efficiency is achieved.
[0220] In the heat treatment step, the temperature increase rate is preferably 2° C. / minute to 40° C. / minute, and more preferably 3° C. / minute to 20° C. / minute.
[0221] When the temperature increase rate in the heat treatment step is 2° C. / minute or more, the production efficiency of the oxide thin film is improved compared to a case where the temperature increase rate is less than 1° C. / minute.
[0222] If the heating rate in the heat treatment step is 40° C. / min or less, the metal element diffuses uniformly during crystallization, and crystals in which the metal is not segregated at the grain boundaries can be formed.
[0223] The crystalline oxide thin film of this embodiment can also be applied to various integrated circuits such as logic circuits, storage circuits and differential amplifier circuits, and these can be applied to electronic devices, etc. In addition, the crystalline oxide thin film of this embodiment can be applied as a layer of a part of a solar cell, and a layer of a part of a display device such as a liquid crystal element, an organic electroluminescent element, an inorganic electroluminescent element, a micro organic EL display, a micro LED (Light Emitting Diode: light emitting diode) display, and a mini LED display. Furthermore, the crystalline oxide thin film of this embodiment can be applied as a layer of a part of a solid-state imaging element, an X-ray sensor, a power semiconductor element, a touch panel, an LSI (Large Scale Integrated circuits: large-scale integrated circuits), a variable resistance memory, a DRAM (Dynamic Random Access Memory: dynamic random access memory), a ferroelectric memory, a BEOL (Back End of Line: back end line), and a part of a microprocessor. The crystalline oxide thin film of this embodiment can also be suitable as a semiconductor layer of a field effect transistor, an electrostatic induction transistor, a quantum tunnel field effect transistor, a Schottky barrier transistor, a Schottky diode, a PN diode and a resistor element, and a part of them.
[0224] [Thin film transistor and electronic device]
[0225] As the thin film transistor of this embodiment, a thin film transistor including the crystalline oxide thin film of this embodiment can be exemplified. The crystalline oxide thin film of this embodiment is preferably an oxide semiconductor thin film.
[0226] As a channel layer of a thin film transistor, the crystalline oxide thin film of this embodiment mode is preferably used.
[0227] When the thin film transistor of this embodiment has the crystalline oxide thin film of this embodiment as a channel layer, other element structures in the thin film transistor are not particularly limited, and a known element structure can be adopted.
[0228] The thin film transistor of this embodiment can be suitably used in electronic devices.
[0229] Specifically, the thin film transistor of this embodiment can be suitably used in display devices such as liquid crystal displays and organic EL displays.
[0230] The film thickness of the channel layer in the thin film transistor of this embodiment is usually 10 nm to 300 nm, and preferably 20 nm to 250 nm.
[0231] The channel layer in the thin film transistor of this embodiment is generally used in an N-type region, but can be combined with various P-type semiconductors such as P-type Si-based semiconductors, P-type oxide semiconductors, and P-type organic semiconductors to be used in various semiconductor devices such as PN junction transistors.
[0232] The thin film transistor of this embodiment can also be applied to various integrated circuits such as field effect transistors, logic circuits, storage circuits, and differential amplifier circuits. Furthermore, in addition to field effect transistors, it can also be suitable for electrostatic induction transistors, Schottky barrier transistors, Schottky diodes, and resistors. That is, the thin film transistor of this embodiment can be applied to the uses exemplified in the "Uses of Thin Film Transistors" described later.
[0233] The thin film transistor of this embodiment mode can adopt a structure selected from well-known structures such as a bottom gate, a bottom contact, a top gate, and a top contact without limitation.
[0234] The thin film transistor of this embodiment can be suitably used in a display device.
[0235] Specific examples of thin film transistors are Figure 2 and Figure 3 Shown.
[0236] like Figure 2 As shown, the thin film transistor 100 includes a silicon wafer 20 , a gate insulating film 30 , an oxide thin film 40 , a source electrode 50 , a drain electrode 60 , and interlayer insulating films 70 , 70A.
[0237] The silicon wafer 20 is a gate electrode. The gate insulating film 30 is an insulating film that blocks conduction between the gate electrode and the oxide thin film 40 , and is provided on the silicon wafer 20 .
[0238] The oxide thin film 40 is a channel layer, and is provided on the gate insulating film 30. As the oxide thin film 40, the crystalline oxide thin film of this embodiment is used.
[0239] The source electrode 50 and the drain electrode 60 are conductive terminals for allowing source current and drain current to flow through the oxide film 40 , and are provided in contact with the vicinity of both ends of the oxide film 40 .
[0240] The interlayer insulating film 70 is an insulating film that blocks conduction between the source electrode 50 and the drain electrode 60 and the oxide thin film 40 except for the contact portions.
[0241] The interlayer insulating film 70A is an insulating film that blocks conduction except for the contact portion between the source electrode 50 and the drain electrode 60 and the oxide thin film 40. The interlayer insulating film 70A is also an insulating film that blocks conduction between the source electrode 50 and the drain electrode 60. The interlayer insulating film 70A is also a channel layer protection layer.
[0242] like Figure 3 As shown, although the structure of the thin film transistor 100A is the same as that of the thin film transistor 100, it is different in that the source electrode 50 and the drain electrode 60 are provided in contact with both the gate insulating film 30 and the oxide thin film 40. It is also different in that the interlayer insulating film 70B is provided integrally in a manner covering the gate insulating film 30, the oxide thin film 40, the source electrode 50, and the drain electrode 60.
[0243] The materials forming the drain electrode 60, the source electrode 50, and the gate electrode are not particularly limited, and any commonly used material can be selected. Figure 2 and Figure 3 In the examples cited above, a silicon wafer is used as a substrate and the silicon wafer also functions as an electrode, but the electrode material is not limited to silicon.
[0244] For example, transparent electrodes such as indium tin oxide (ITO), indium zinc oxide (IZO), ZnO and SnO2, or metal electrodes such as Al, Ag, Cu, Cr, Ni, Mo, Au, Ti and Ta, or metal electrodes or stacked electrodes containing alloys of these metals can be used.
[0245] In addition, Figure 2 and Figure 3 In the present invention, a gate electrode can also be formed on a substrate such as glass.
[0246] The material for forming the interlayer insulating films 70, 70A, and 70B is not particularly limited, and any commonly used material can be selected. x MN x and MN x O y A compound represented by (wherein M in the formula is a metal element, and x and y are real numbers greater than 0. The same applies to x and y in the compounds exemplified below.) Specifically, the material can be SiO2, SiO x 、SiN x and SiN x O y Furthermore, the material may also include compounds such as Al2O3, Ta2O5, TiO2, MgO, ZrO2, CeO2, K2O, Li2O, Na2O, Rb2O, Sc2O3, Y2O3, HfO2, CaHfO3, PbTiO3, BaTa2O6, SrTiO3, Sm2O3, and AlN. The valence of anions (oxygen anions and nitrogen anions) in these oxide compounds and nitride compounds is not particularly limited as long as it is a real number greater than 0.
[0247] When the thin film transistor of this embodiment is a back channel etch type (bottom gate type), it is preferred to provide a protective film on the drain electrode, the source electrode and the channel layer. By providing a protective film, the durability is easily improved even when the TFT is driven for a long time. In addition, in the case of a top gate type TFT, for example, a gate insulating film is formed on the channel layer.
[0248] The protective film or insulating film can be formed by, for example, CVD, which may be a high-temperature process. In addition, the protective film or insulating film often contains impurity gases just after film formation, so it is preferable to perform a heat treatment (annealing treatment). The impurity gases are removed by heat treatment, thereby forming a stable protective film or insulating film, and it is easy to form a TFT element with high durability.
[0249] By using the crystalline oxide thin film of this embodiment, the film is less susceptible to the influence of the temperature in the CVD process and the influence of the subsequent heat treatment. Therefore, even when a protective film or an insulating film is formed, the stability of TFT characteristics can be improved.
[0250] Among transistor characteristics, the on / off characteristic is a factor that determines the display performance of the display. When a thin film transistor is used as a switch for liquid crystal, the on / off ratio is preferably above 6 digits. In the case of OLED, since it is current driven, the on current is important, but the on / off ratio is also preferably above 6 digits.
[0251] The on-off ratio of the thin film transistor of this embodiment is preferably 1×10 6 above.
[0252] The on-off ratio was obtained by setting the value of Id at Vg=-10V as the off current value and the value of Id at Vg=20V as the on current value and determining the ratio [on current value / off current value].
[0253] In addition, the mobility of the TFT of this embodiment is preferably 5 cm 2 / Vs or more, more preferably 10cm 2 / Vs or above.
[0254] The saturation mobility is obtained from the transfer characteristics when a drain voltage of 20 V is applied. Specifically, the saturation mobility can be obtained from the formula of the saturation region by making a graph of the transfer characteristics Id-Vg, calculating the transconductance (Gm) of each Vg. Id is the current between the source and drain electrodes, and Vg is the gate voltage when a voltage Vd is applied between the source and drain electrodes.
[0255] The threshold voltage (Vth) is preferably -3.0V to 3.0V, more preferably -2.0V to 2.0V, and further preferably -1.0V to 1.0V. If the threshold voltage (Vth) is -3.0V or higher, a thin film transistor with high mobility can be obtained. If the threshold voltage (Vth) is 3.0V or lower, a thin film transistor with a small off current and a large on-off ratio can be obtained.
[0256] The threshold voltage (Vth) can be calculated from the transfer characteristic graph using the current value Id between the source and the drain = 10 -9 It is defined by the gate voltage Vg under A.
[0257] The on-off ratio is preferably 10 6 above 10 12 Below, more preferably 10 7 above 10 11 Below, more preferably 10 8 above 10 10 If the on-off ratio is 10 6 If the on-off ratio is 10 12 Below, it is possible to drive an organic EL with a large contrast ratio. 12 Below, the shutdown current can be 10 -11 A or less, when a thin film transistor is used for a transfer transistor or a reset transistor of a CMOS image sensor, it is possible to extend the image retention time or improve the sensitivity.
[0258] <Quantum Tunneling Field Effect Transistor>
[0259] The crystalline oxide thin film of this embodiment can also be used for a quantum tunnel field effect transistor (FET). In addition, a quantum tunnel field effect transistor is sometimes referred to as a quantum tunnel field effect type transistor.
[0260] exist Figure 4 A schematic diagram (longitudinal cross-sectional view) of a quantum tunnel field effect transistor (FET) according to one embodiment is shown.
[0261] The quantum tunnel field effect transistor 501 includes a p-type semiconductor layer 503 , an n-type semiconductor layer 507 , a gate insulating film 509 , a gate electrode 511 , a source electrode 513 , and a drain electrode 515 .
[0262] The p-type semiconductor layer 503 , the n-type semiconductor layer 507 , the gate insulating film 509 , and the gate electrode 511 are stacked in this order.
[0263] The source electrode 513 is provided on the p-type semiconductor layer 503 . The drain electrode 515 is provided on the n-type semiconductor layer 507 .
[0264] The p-type semiconductor layer 503 is a p-type Group IV semiconductor layer, and is a p-type silicon layer in this case.
[0265] The n-type semiconductor layer 507 is the n-type oxide thin film in the above-mentioned embodiment. The source electrode 513 and the drain electrode 515 are conductive films.
[0266] Although in Figure 4 Although not shown in the figure, an insulating layer may be formed on the p-type semiconductor layer 503. In this case, the p-type semiconductor layer 503 and the n-type semiconductor layer 507 are connected via a contact hole in a region where the insulating layer is partially opened. Figure 4 Although not shown in the figure, the quantum tunnel field effect transistor 501 may also include an interlayer insulating film covering its upper surface.
[0267] The quantum tunnel field effect transistor 501 is a quantum tunnel field effect transistor (FET) that switches current, and controls the current tunneling through the energy barrier formed by the p-type semiconductor layer 503 and the n-type semiconductor layer 507 by the voltage of the gate electrode 511. In this structure, the band gap of the oxide semiconductor constituting the n-type semiconductor layer 507 becomes larger, and the off current can be reduced.
[0268] exist Figure 5 A schematic diagram (longitudinal cross-sectional view) of a quantum tunnel field effect transistor 501A according to another embodiment is shown.
[0269] The configuration of the quantum tunneling field effect transistor 501A is the same as that of the quantum tunneling field effect transistor 501, but differs in that a silicon oxide layer 505 is formed between the p-type semiconductor layer 503 and the n-type semiconductor layer 507. The presence of the silicon oxide layer can reduce the off current.
[0270] The thickness of the silicon oxide layer 505 is preferably 10 nm or less. By making the thickness of the silicon oxide layer 505 10 nm or less, it is possible to prevent the tunnel current from not flowing, or the energy barrier formed from being difficult to form or the barrier height from changing, thereby preventing the tunnel current from decreasing or changing. The thickness of the silicon oxide layer 505 is preferably 8 nm or less, more preferably 5 nm or less, further preferably 3 nm or less, and further preferably 1 nm or less.
[0271] In the quantum tunneling field effect transistors 501 and 501A, the n-type semiconductor layer 507 is also an n-type oxide semiconductor.
[0272] The oxide thin film constituting the n-type semiconductor layer 507 may also be amorphous. By making the oxide thin film constituting the n-type semiconductor layer 507 amorphous, it can be etched with an organic acid such as oxalic acid, the difference in etching speed with other layers becomes larger, and it will not affect the metal layer such as the wiring, so that etching can be performed well.
[0273] The oxide thin film constituting the n-type semiconductor layer 507 may also be crystalline. By making the oxide thin film constituting the n-type semiconductor layer 507 crystalline, the band gap becomes larger than in the case of amorphous and the off current can be reduced. Since the work function can also be increased, it is easy to control the current that tunnels through the energy barrier formed by the p-type IV group semiconductor material and the n-type semiconductor layer 507.
[0274] The method for manufacturing the quantum tunneling field effect transistor 501 is not particularly limited, and the following method can be exemplified.
[0275] First, if Fig. 6A As shown in FIG. 1 , an insulating film 505A is formed on the p-type semiconductor layer 503 , and a part of the insulating film 505A is opened by etching or the like to form a contact hole 505B.
[0276] Then, if Figure 6B As shown in FIG. 5 , an n-type semiconductor layer 507 is formed on the p-type semiconductor layer 503 and the insulating film 505A. At this time, the p-type semiconductor layer 503 and the n-type semiconductor layer 507 are connected via a contact hole 505B.
[0277] Then, if Figure 6C As shown, a gate insulating film 509 and a gate electrode 511 are sequentially formed on the n-type semiconductor layer 507 .
[0278] Then, if Fig.6D As shown, an interlayer insulating film 519 is provided to cover the insulating film 505A, the n-type semiconductor layer 507 , the gate insulating film 509 , and the gate electrode 511 .
[0279] Then, if Fig. 6E As shown, a contact hole 519A is formed by opening a portion of the insulating film 505A and the interlayer insulating film 519 on the p-type semiconductor layer 503, and a source electrode 513 is provided in the contact hole 519A.
[0280] Furthermore, if Fig. 6E As shown, a contact hole 519B is formed by opening a portion of the gate insulating film 509 and the interlayer insulating film 519 on the n-type semiconductor layer 507, and a drain electrode 515 is formed in the contact hole 519B.
[0281] The quantum tunnel field effect transistor 501 can be manufactured through the above steps.
[0282] After forming the n-type semiconductor layer 507 on the p-type semiconductor layer 503, heat treatment is performed at a temperature of 150°C to 600°C to form the silicon oxide layer 505 between the p-type semiconductor layer 503 and the n-type semiconductor layer 507. By adding this step, the quantum tunnel field effect transistor 501A can be manufactured.
[0283] The thin film transistor of this embodiment is preferably a channel-doped thin film transistor. A channel-doped thin film transistor is a transistor that properly controls the carriers in the channel through n-type doping, rather than oxygen deficiency that is easily changed by external stimuli such as atmosphere and temperature, and can achieve the effect of both high mobility and high reliability.
[0284] <Applications of Thin Film Transistors>
[0285] The thin film transistor of this embodiment can be suitably used in solar cells, display elements (liquid crystal elements, organic electroluminescent elements and inorganic electroluminescent elements, etc.) and power semiconductor elements. The thin film transistor of this embodiment can be suitably used as a transistor for devices using an active matrix method, such as display devices (liquid crystal display, organic EL (Electro Luminescence: electroluminescence) display, micro organic EL display, micro LED (Light Emitting Diode: light emitting diode) display and mini LED display, etc.), solid-state imaging elements and touch panels. The thin film transistor of this embodiment can also be applied to various integrated circuits such as field effect transistors, logic circuits, storage circuits and differential amplifier circuits, and these can be applied to electronic devices, etc. The electronic device of this embodiment preferably includes a thin film transistor. Furthermore, in addition to being suitable for field effect transistors, the thin film transistor of this embodiment can also be suitable for electrostatic induction transistors and Schottky barrier transistors. The thin film transistor of this embodiment can also be suitable as a transistor for sensors such as image sensors, X-ray sensors and biosensors.
[0286] Hereinafter, a case where the thin film transistor of this embodiment is used for a display device and a solid-state imaging element will be described.
[0287] First, refer to Figure 7A to Figure 7C A case where the thin film transistor of this embodiment mode is used in a display device is described.
[0288] Fig. 7A It is a top view of the display device of this embodiment. Figure 7B 2 is a circuit diagram for explaining a circuit of a pixel portion when a liquid crystal element is applied to the pixel portion of the display device of this embodiment. Figure 7CThis is a circuit diagram for explaining a circuit of a pixel portion in the case where an organic EL element is applied to the pixel portion of the display device of this embodiment.
[0289] The thin film transistor of this embodiment can be used as the transistor configured in the pixel portion. Since the thin film transistor of this embodiment can be easily set to an n-channel type, a part of the driving circuit that can be composed of n-channel transistors is formed on the same substrate as the transistor of the pixel portion. By using the thin film transistor described in this embodiment in the pixel portion or the driving circuit, a display device with high reliability can be provided.
[0290] exist Fig. 7A An example of a top view of an active matrix display device is shown. A pixel portion 301, a first scan line driving circuit 302, a second scan line driving circuit 303, and a signal line driving circuit 304 are formed on a substrate 300 of the display device. In the pixel portion 301, a plurality of signal lines are extended from the signal line driving circuit 304, and a plurality of scan lines are extended from the first scan line driving circuit 302 and the second scan line driving circuit 303. Pixels having display elements are arranged in a matrix at the intersection of the scan lines and the signal lines. The substrate 300 of the display device is connected to a timing control circuit (also called a controller, a control IC) via a connection portion such as an FPC (Flexible Printed Circuit).
[0291] exist Fig. 7A In the embodiment of the present invention, the first scanning line driving circuit 302, the second scanning line driving circuit 303 and the signal line driving circuit 304 are formed on the same substrate 300 as the pixel portion 301. Therefore, the number of components such as the driving circuit provided outside is reduced, so that cost reduction can be achieved. In addition, when the driving circuit is provided outside the substrate 300, it is necessary to extend the wiring, and the number of connections between the wirings increases. When the driving circuit is provided on the same substrate 300, the number of connections between the wirings can be reduced, thereby achieving improved reliability or improved yield.
[0292] In addition, Figure 7B An example of a circuit configuration of a pixel is shown. Here, a circuit of a pixel portion that can be applied to a pixel portion of a VA type liquid crystal display device is shown.
[0293] The circuit of the pixel unit can be applied to a structure having multiple pixel electrodes in one pixel. Each pixel electrode is connected to a different transistor, and each transistor is configured to be driven by a different gate signal. Thus, the signal applied to each pixel electrode of the pixel of the multi-domain design can be independently controlled.
[0294] The gate wiring 312 of the transistor 316 and the gate wiring 313 of the transistor 317 are separated so that different gate signals can be provided to the two. On the other hand, the source electrode or the drain electrode 314 functioning as a data line is shared by the transistor 316 and the transistor 317. The thin film transistor of this embodiment can be used for the transistor 316 and the transistor 317. Thus, a liquid crystal display device with high reliability can be provided.
[0295] The first pixel electrode is electrically connected to the transistor 316, and the second pixel electrode is electrically connected to the transistor 317. The first pixel electrode and the second pixel electrode are separated. The shapes of the first pixel electrode and the second pixel electrode are not particularly limited. For example, the first pixel electrode may be V-shaped.
[0296] The gate electrode of transistor 316 is connected to gate wiring 312, and the gate electrode of transistor 317 is connected to gate wiring 313. Different gate signals are supplied to gate wiring 312 and gate wiring 313 to make transistor 316 and transistor 317 operate at different timings, thereby controlling the alignment of liquid crystal.
[0297] Alternatively, a storage capacitor may be formed using the capacitor wiring 310 , a gate insulating film functioning as a dielectric, and a capacitor electrode electrically connected to the first pixel electrode or the second pixel electrode.
[0298] The multi-domain structure includes a first liquid crystal element 318 and a second liquid crystal element 319 in one pixel. The first liquid crystal element 318 is composed of a first pixel electrode, a counter electrode, and a liquid crystal layer therebetween, and the second liquid crystal element 319 is composed of a second pixel electrode, a counter electrode, and a liquid crystal layer therebetween.
[0299] The pixel portion is not limited to Figure 7B The composition shown. Figure 7B The pixel portion shown in the figure is further provided with a switch, a resistor, a capacitor, a transistor, a sensor, or a logic circuit.
[0300] exist Figure 7C Another example of the circuit configuration of a pixel is shown. Here, the configuration of a pixel portion of a display device using an organic EL element is shown.
[0301] Figure 7C 3 is a diagram showing an example of a circuit of an applicable pixel unit 320. Here, an example of using two n-channel transistors in one pixel is shown. The crystalline oxide thin film of this embodiment can be used in the channel formation region of the n-channel transistor. The circuit of the pixel unit can be applied to digital time grayscale driving.
[0302] The thin film transistor of this embodiment can be used as the switching transistor 321 and the driving transistor 322. Thus, a highly reliable organic EL display device can be provided.
[0303] The circuit configuration of the pixel portion is not limited to Figure 7C The composition shown. Figure 7C A switch, a resistor, a capacitor, a sensor, a transistor, or a logic circuit is added to the circuit of the pixel portion shown.
[0304] The above is the description of the case where the thin film transistor of this embodiment is used in a display device.
[0305] Next, refer to Figure 8 A case where the thin film transistor of this embodiment is used for a solid-state imaging element will be described.
[0306] CMOS (Complementary Metal Oxide Semiconductor) image sensors are solid-state imaging elements that maintain a potential in a signal charge storage unit and output the potential to a vertical output line via an amplifier transistor. If there is leakage current in the reset transistor and / or transfer transistor included in the CMOS image sensor, the potential of the signal charge storage unit changes due to charging or discharging caused by the leakage current. If the potential of the signal charge storage unit changes, the potential of the amplifier transistor also changes, becoming a value that deviates from the original potential, causing the captured image to deteriorate.
[0307] The effect of operation when the thin film transistor of this embodiment is applied to a reset transistor and a transfer transistor of a CMOS image sensor will be described. The amplifier transistor can be either a thin film transistor or a bulk transistor.
[0308] Figure 8 : This is a diagram showing an example of the pixel structure of a CMOS image sensor. The pixel is composed of a photodiode 3002 as a photoelectric conversion element, a transfer transistor 3004, a reset transistor 3006, an amplifier transistor 3008 and various wirings, and a plurality of pixels are arranged in a matrix to form a sensor. A selection transistor electrically connected to the amplifier transistor 3008 may also be provided. The "OS" marked in the transistor reference numeral represents an oxide semiconductor (Oxide Semiconductor), and "Si" represents silicon, indicating the preferred material when applied to each transistor. The same is true for subsequent drawings.
[0309] The photodiode 3002 is connected to the source side of the transfer transistor 3004, and a signal charge storage unit 3010 (also referred to as FD: Floating diffusion) is formed on the drain side of the transfer transistor 3004. The source of the reset transistor 3006 and the gate of the amplifier transistor 3008 are connected to the signal charge storage unit 3010. As another configuration, the reset power supply line 3110 can also be deleted. For example, there is also a method of connecting the drain of the reset transistor 3006 to the power supply line 3100 or the vertical output line 3120 instead of the reset power supply line 3110.
[0310] In addition, the crystalline oxide thin film of this embodiment mode can also be used for the photodiode 3002 , and the same material as the oxide thin film used for the transfer transistor 3004 and the reset transistor 3006 can be used.
[0311] Example
[0312] Hereinafter, the present invention will be described in detail based on Examples. However, the present invention is not limited to the Examples.
[0313] [1] Manufacturing of sputtering targets
[0314] (Example 1, Example 2, Example 5 and Example 6)
[0315] A sputtering target including an oxide sintered body containing In element, Ga element, and O element is prepared. The specific steps are as follows.
[0316] First, In2O3 with an average particle size of 0.3 μm and Ga2O3 with an average particle size of 1 μm were prepared and weighed to obtain the atomic composition ratios (at %) shown in Tables 1 and 2 to prepare raw material powders.
[0317] In Tables 1 and 2, the description of "metal composition ratio [at%]" corresponds to the above-mentioned atomic composition ratio (at%). The numerical value shown in "at%" shows the ratio obtained by expressing the atomic composition ratio of indium element, gallium element, zinc element and tin element in percentage. The same applies to the description of "metal composition ratio [at%]" in Tables 3 to 8 described later.
[0318] Next, water, a binder, a dispersant, and a defoaming agent were added to Ga2O3 to pre-crush Ga2O3. In the pre-crushing, a bead mill (manufactured by Ashizawa Finetech) was used as a pulverizer, zirconia beads with a diameter of 0.1 mm were used as pulverizing media, the circumferential speed of the bead mill was set to 14 m / s, and the pulverization was performed for 3 hours.
[0319] The particle size of the pre-crushed Ga2O3 was 0.28 μm or less. The particle size of the pre-crushed Ga2O3 was confirmed using a particle size distribution measuring device (LA950 manufactured by HORI BA) and a SEM device.
[0320] Next, the prepared raw material powder of In2O3 and the pre-crushed raw material powder of Ga2O3 were mixed to obtain a mixed raw material powder, and then an acrylic acid-methacrylic acid copolymer ammonia neutralized product (BANSTAR X754B manufactured by Sanmei Chemical Co., Ltd.) as a dispersant, polyvinyl alcohol as a thickener, and water were added to the mixed raw material powder, and mixed and crushed with a bead mill for 2 hours to obtain a raw material mixture with a solid content concentration of 70% by mass. The obtained raw material mixture was supplied to a spray dryer and granulated at a rotation speed of 12,000 rpm and a hot air temperature of 150°C to obtain a raw material granulated powder.
[0321] Next, the raw granulated powder was passed through a 100-mesh sieve to remove raw granulated powder with a particle size exceeding 150 μm, and then passed through a 500-mesh sieve to remove raw granulated powder with a particle size less than 25 μm, thereby adjusting the particle size of the raw granulated powder to a range of 25 μm to 150 μm.
[0322] Next, the raw material granulated powder after adjusting the particle size was uniformly filled into a mold with an inner diameter of 300 mm×600 mm×9 mm, and pressed using a cold press. After the pressing, a cold isostatic pressing device (CIP device) was used to press at a pressure of 294 MPa to obtain a molded body.
[0323] Three compacts were prepared, and the obtained three compacts were heated to 780°C in a sintering furnace under an oxygen atmosphere, and then kept at 780°C for 5 hours, and then further heated to 1350°C and kept at the sintering temperature (1350°C) for 20 hours. Then, the oxide sintered body was obtained by cooling in the furnace. In addition, the heating rate was 2°C / min.
[0324] The three sintered bodies were cut and surface-ground to obtain three oxide sintered body plates of 142 mm × 305 mm × 5 mm t, one of which was used for property evaluation and two for G1 targets [142 mm × 610 mm (divided into 2 equal parts) × 5 mm t].
[0325] The surface grinding was performed on the oxide sintered body using a surface grinder and a diamond grinding wheel with a grinding wheel grain size of 80 μm. The surface grinding processing conditions were as follows.
[0326] Surface grinding processing conditions:
[0327] Feed speed v of grinding object: 1m / min
[0328] Grinding wheel peripheral speed V: 500m / min
[0329] Grinding wheel cutting depth (cutting depth t): 5μm
[0330] Grinding wheel abrasive particle size d: 80μm
[0331] Type of grinding wheel: diamond grinding wheel
[0332] After grinding under the above-mentioned surface grinding conditions, grinding was performed under the above-mentioned surface grinding conditions in the order of grinding wheels with abrasive grain sizes from large to small using a diamond grinding wheel with a grinding grain size of 40 μm and then a diamond grinding wheel with a grinding grain size of 20 μm.
[0333] The two obtained oxide sintered plates (142mm×305mm×5mmt) were used to bond with a backing plate made of Cu (copper) to manufacture a G1 target. The bonding is to set the surface after plane grinding as the sputtering surface, and the surface on the opposite side of the sputtering surface (the surface after rough grinding with a grinding wheel with an abrasive grain size of 130μm) as the bonding surface, and bond the bonding surface side of the oxide sintered plate to the backing plate. In all targets, the bonding rate is more than 98%. When the oxide sintered body plate is bonded to the backing plate, no cracks are generated on the oxide sintered body plate, and the sputtering target can be manufactured well. The bonding rate (bonding rate) is confirmed by X-ray CT.
[0334] (Example 3, Example 4)
[0335] In addition to the same In2O3 and Ga2O3 as in Example 1, ZnO with an average particle size of 0.8 μm and SnO2 with an average particle size of 0.4 μm were prepared and weighed as raw material powders in such a manner as to obtain the atomic composition ratios (at%) shown in Tables 1 and 2. ZnO was pre-crushed under the same conditions as Ga2O3. The average particle size of the pre-crushed ZnO was 0.32 μm. A sintered body was obtained in the same manner as in Example 1 except for the above. Then, the obtained sintered body was ground and joined in the same manner as in Example 1 to prepare a sputtering target, which was evaluated in the same manner as in Example 1.
[0336] (Comparative Example 1 to Comparative Example 3)
[0337] First, the same In2O3 and Ga2O3 as those in Example 1 were prepared and weighed as raw material powders so as to have the atomic composition ratios (at%) shown in Table 3. In Comparative Examples 1 to 3, premixing of the raw material powders was not performed.
[0338] Next, the raw material powders were mixed for 4 hours using a planetary ball mill. The mixed raw material powders were dried and classified to obtain a raw material mixture. The obtained raw material mixture was molded in the same manner as in Example 1. Three compacts were made, and the obtained three compacts were heated to 780°C in a sintering furnace under an oxygen atmosphere, maintained at 780°C for 5 hours, further heated to 1400°C, and maintained at the sintering temperature (1400°C) for 20 hours. Then, an oxide sintered body was obtained by cooling in the furnace. In addition, the heating rate was 2°C / min. Then, grinding and joining were performed in the same manner as in Example 1 to make a sputtering target, which was evaluated in the same manner as in Example 1.
[0339] (Comparative Examples 4 to 6)
[0340] A sputtering target was obtained in the same manner as in Example 1 except that the same In2O3 and Ga2O3 as in Example 1 were prepared and weighed so as to have the atomic composition ratio (at %) shown in Table 4 as raw material powders.
[0341] [1-1] Evaluation of sintered body
[0342] <1-A> Atomic composition ratio
[0343] The atomic composition ratio of the sintered body was analyzed by an inductively coupled plasma atomic emission spectrometer (ICP-AES, manufactured by Shimadzu Corporation). The obtained sintered body was confirmed to have the atomic composition ratio shown in Tables 1 to 4.
[0344] <1-B> XRD measurement and crystal phase identification
[0345] The obtained sintered body was subjected to XRD measurement using an X-ray diffraction measuring apparatus to investigate the crystal structure.
[0346] The measurement conditions of the above-mentioned X-ray diffraction measurement (XRD) are as follows.
[0347] Device: D8 DISCOVER Plus (Bruker Japan Co., Ltd.)
[0348] X-ray: CuKα
[0349] <1-C> Measurement of crystal particle size
[0350] The crystal grain size is measured as follows: A surface of a sintered body produced in the same batch as the sputtering target is divided into 16 equal-area portions, and a 1 cm square corner is cut out at the center point 16 of each quadrilateral.
[0351] The cut sputtering target was embedded in resin and mirror-polished using a grinding device (Buehler). After the surface was made conductive by osmium coating, it was put into a scanning electron microscope (SEM) device (Hitachi High-Technologies Corporation), and the measurement surface was further divided into 9 equal areas. At the center point 9 of each quadrilateral, secondary electron images and reflected electron images were observed at a magnification of 2000 times. In addition, EDS measurement was performed during SEM measurement to obtain the atomic ratio of each grain.
[0352] By comparing with the crystal structure identified by XRD, it is identified which crystal each grain belongs to.
[0353] The particle size was measured from the obtained SEM images, and the average particle size of the particles in the 9 frames was calculated. This operation was performed on each sample cut out from 16 locations, and the average particle size obtained from a total of 144 SEM images was taken as the average particle size.
[0354] For particles with an aspect ratio of less than 2, the particle size of the crystal grain is measured as a circle equivalent diameter based on JIS R1670: 2006. Specifically, as a measurement procedure for the circle equivalent diameter, a circular ruler is attached to the particle to be measured in the microstructure photograph, and the diameter corresponding to the area of the particle to be measured is read. For particles with an aspect ratio of more than 2, the average value of the longest diameter and the shortest diameter is taken as the particle size of the particle.
[0355] <1-D> Density
[0356] The actual density of the obtained oxide sintered body was measured by the Archimedean method. Specifically, the density was measured using water at room temperature.
[0357] <1-E>Flexural strength
[0358] Thirty prism test pieces with a thickness of 3 mm × a width of 4 mm × a total length of 36 mm and a rectangular cross-section were cut out from the obtained oxide sintered body. The three-point bending strength was measured using a material testing machine (EZ Graph manufactured by Shimadzu Corporation) based on JIS R 1601:2008, and the average value of the three-point bending strength measurement values of the 30 test pieces was taken as the flexural strength (flexural strength).
[0359] <1-F> Power resistance
[0360] The produced sputtering target was mounted on a sputtering device and subjected to DC discharge to check for the presence or absence of cracks.
[0361] Power resistance is a value expressed as the maximum sputtering power at which no cracks occur in the sputtering target. After discharging at a sputtering power of DC1.5kW for 1 hour, open the chamber and visually observe whether there are any cracks. Then, increase the sputtering power to 1.75kW, discharge at this sputtering power for 1 hour, open the chamber and visually observe whether there are any cracks. Confirm the cracks by increasing the sputtering power by 0.25kW each time, and do this until cracks are confirmed in the sputtering target. The maximum power at which no cracks are confirmed is used as an indicator of power resistance. In addition, the sputtering power varies depending on the device, so the value obtained by dividing the switched-on power by the target area is standardized as the power density. The evaluation conditions for power resistance are as follows.
[0362] <Device>
[0363] ULVAC SMO-200I
[0364] <Sputtering conditions>
[0365] Atmosphere gas: Ar (argon) + O2 (oxygen)
[0366] Oxygen partial pressure during discharge: 20%
[0367] Back pressure before discharge: 2×10 -4 Pa
[0368] Sputtering pressure during discharge: 0.5Pa
[0369] Fig. 9 The X-ray diffraction pattern of the sintered body used in the target produced in Example 1 is shown. Fig. 9 As shown, it can be seen that the sintered body obtained in Example 1 shows peaks at positions where the incident angle (2θ) is (A) 28° to 29°, (B) 45° to 46°, (C) 46° to 47°, (D) 47° to 48°, and (E) 50° to 51°, in addition to In2O3 and GaInO3. Therefore, it can be seen that the sintered body obtained in Example 1 contains crystal structure A.
[0370] Fig.10 The mapping image of oxygen atoms in the sintered body used in the target produced in Example 1 is shown. Fig.10 As shown in the figure, it can be seen that the regions with relatively low O content are continuously connected. Fig.10 In the figure, the relatively dark portion is a region having a relatively low content of the O element.
[0371] [Table 1]
[0372]
[0373] [Table 2]
[0374]
[0375] [Table 3]
[0376]
[0377] [Table 4]
[0378]
[0379] [2] Fabrication of oxide thin films and TFTs
[0380] [2-1] Oxide thin film
[0381] (Example 1 to Example 6 and Comparative Example 1 to Comparative Example 6)
[0382] Using the sputtering targets prepared in Examples 1 to 6 and Comparative Examples 1 to 6, a 40 nm oxide thin film (oxide semiconductor thin film layer) was formed on a silicon wafer with a 100 nm thermal oxide film (gate insulating film) through a metal mask by sputtering. At this time, high-purity argon and high-purity oxygen were used as sputtering gases for sputtering.
[0383] In addition, a sample in which only an oxide thin film layer with a film thickness of 40 nm was formed on a glass substrate was also manufactured at the same time under the same conditions. ABC-G manufactured by Nippon Electric Glass Co., Ltd. was used as the glass substrate.
[0384] [2-2] Formation of source-drain electrodes
[0385] Next, titanium metal was sputtered using a metal mask in the shape of a source-drain contact hole on the oxide thin film in the sample on which a silicon wafer, a gate insulating film, and an oxide thin film were sequentially formed, and a titanium electrode was formed as a source-drain electrode to form a laminate to manufacture a thin film transistor (TFT). The obtained laminate was subjected to a heat treatment (annealing treatment) at 350°C for 1 hour in the atmosphere to evaluate the performance of the thin film transistor (TFT).
[0386] <2-A> Crystal properties of semiconductor films
[0387] For the sample composed of a glass substrate and an oxide thin film layer (i.e., a sample in which only an oxide thin film layer with a film thickness of 40 nm was formed on a glass substrate), the crystallinity of both the unheated film after sputtering (immediately after film deposition) and the film after heat treatment after film formation under the conditions described in Tables 5 to 8 was evaluated by X-ray diffraction (XRD) measurement. The film quality of the film before heating and the film quality of the film after heating were recorded as amorphous when no peak was observed in the XRD measurement, and as crystalline when a peak was observed in the XRD measurement and crystallization occurred.
[0388] <2-B> TFT characteristic evaluation
[0389] The linear mobility of the TFT prepared in the above [2-2] before the formation of the protective insulating film (SiO2 film) was evaluated.
[0390] The linear mobility is obtained from the transfer characteristics when a drain voltage of 0.1 V is applied. Specifically, a transfer characteristic Id-Vg graph is prepared, the transconductance (Gm) of each Vg is calculated, and the mobility is derived from the formula in the linear region. In addition, Gm is given by Indicates that the applied voltage is Vg of -10V to 20V, and the maximum mobility within this range is defined as linear mobility. Unless otherwise specified in the present invention, the linear mobility is evaluated by this method. The above Id is the current between the source and drain electrodes, and Vg is the gate voltage when the voltage Vd is applied between the source and drain electrodes.
[0391] [Table 5]
[0392]
[0393] [Table 6]
[0394]
[0395] [Table 7]
[0396]
[0397] [Table 8]
[0398]
[0399] Description of Reference Numerals
[0400] 1.1A, 1B, 1C oxide sintered body
[0401] 3 Back Panel
[0402] 20 Silicon Wafer
[0403] 30Gate insulating film
[0404] 40 oxide film
[0405] 50 Source Electrode
[0406] 60 drain electrode
[0407] 70 interlayer insulation film
[0408] 70A interlayer insulation film
[0409] 70B interlayer insulation film
[0410] 100 Thin Film Transistors
[0411] 100A Thin Film Transistor
[0412] 300 substrates
[0413] 301 Pixel Department
[0414] 302 1st scanning line driving circuit
[0415] 303 second scanning line driving circuit
[0416] 304 signal line driver circuit
[0417] 310 capacitor wiring
[0418] 312 Gate wiring
[0419] 313 Gate wiring
[0420] 314 drain electrode
[0421] 316 transistors
[0422] 317 transistors
[0423] 318 No.1 Liquid Crystal Element
[0424] 319 Second Liquid Crystal Element
[0425] 320 pixels
[0426] 321 Switching Transistor
[0427] 322 driving transistor
[0428] 3002 Photodiode
[0429] 3004 transfer transistor
[0430] 3006 Reset transistor
[0431] 3008 Amplifier Transistor
[0432] 3010 signal charge storage unit
[0433] 3100 Power Cord
[0434] 3110 Reset Power Cord
[0435] 3120 vertical output lines
[0436] 501 Quantum Tunnel Field Effect Transistor
[0437] 501A Quantum Tunneling Field Effect Transistor
[0438] 503 p-type semiconductor layer
[0439] 505 silicon oxide layer
[0440] 505A Insulation Film
[0441] 505B contact hole
[0442] 507 n-type semiconductor layer
[0443] 509 gate insulation film
[0444] 511 gate electrode
[0445] 513 source electrode
[0446] 515 drain electrode
[0447] 519 interlayer insulation film
[0448] 519A, 519B contact holes.
Claims
1. A sputtering target comprising an oxide sintered body containing In element, Ga element and O element, characterized in that: The oxide sintered body comprises a crystal structure represented by In2O3, The atomic composition ratio of the Ga element in the oxide sintered body satisfies the following formula (1): The flexural strength of the oxide sintered body is above 140 MPa, 8≤Ga / (In+Ga)≤20…(1).
2. The sputtering target according to claim 1, wherein The average particle size of the crystal structure represented by In2O3 is less than 3 μm.
3. The sputtering target according to claim 1 or 2, wherein: The measured density based on the Archimedean method is 6.3 g / cm 3 above.
4. The sputtering target according to any one of claims 1 to 3, wherein The oxide sintered body includes a crystal structure represented by GaInO 3 .
5. The sputtering target according to any one of claims 1 to 4, wherein: The oxide sintered body further includes a crystal structure A in which diffraction peaks are observed at respective positions of the following (A) to (E) at incident angles (2θ) by X-ray, i.e., CuKα-ray diffraction measurement, (A) 28° or more and 29° or less (B) 45° or more and less than 46° (C) 46° or more and less than 47° (D) 47° or more and 48° or less (E)Above 50° and below 51°.
6. A method for producing a sputtering target, the method for producing a sputtering target according to any one of claims 1 to 5, characterized in that: have: A step of preparing a raw material powder having a particle size of 0.5 μm or less; A step of mixing the raw material powders to obtain a raw material mixture, and then granulating the raw material mixture to obtain a raw material granulate; The step of forming the raw material granules into a formed body; A step of sintering the molded body to obtain the oxide sintered body.
7. A crystalline oxide thin film, characterized in that: The sputtering target according to any one of claims 1 to 5 is used.
8. A thin film transistor, characterized in that: A crystalline oxide thin film comprising the crystalline oxide thin film according to claim 7.
9. An electronic device, characterized in that: A thin film transistor comprising the thin film transistor according to claim 8.