Plating solution containing sulfonium group-containing ether compound

By using sulfonyl-containing ether compounds as homogenizers in the plating solution, the problem that plating solution in the prior art is difficult to achieve high flattening, and the excellent hole filling characteristics and the planarization effect of nitrogen-free plating solution is achieved. in various metal plating solutions.

CN118922586APending Publication Date: 2024-11-08JCU CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280092757.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-03-01
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the manufacturing of printed wiring boards and semiconductor wafers, it is difficult for existing plating solutions to achieve a highly flattened hole filling effect. Especially in metal plating solutions other than tin, the smoothing function of the homogenizer is insufficient and often contains nitrogen components, so it cannot be Meets the requirements of nitrogen-free plating solution.

Method used

The plating solution containing water-soluble metal salts and sulfonyl group-containing ether compounds as homogenizers is used. By adding specific sulfonyl group-containing ether compounds to the plating solution, the hole filling characteristics and planarization properties of the plating solution are improved to form a flat surface. plating surface.

Benefits of technology

It realizes a plating solution with excellent hole filling characteristics, which can replace traditional uniform coating agents in the use of nitrogen-free plating solution, significantly improve the flattening performance of the plating surface, and is suitable for various metal plating solutions, especially in metal plating solutions such as copper. Good flattening effect is shown.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005014704780000021
    Figure BDA0005014704780000021
  • Figure BDA0005014704780000051
    Figure BDA0005014704780000051
  • Figure BDA0005014704780000061
    Figure BDA0005014704780000061
Patent Text Reader

Abstract

Provided is a plating solution which has excellent hole filling characteristics and is capable of forming a flat plated surface. A plating solution containing a water-soluble metal salt and a sulfonium group-containing ether compound. The metal salt is preferably a copper-containing salt, and the sulfonium group-containing ether compound is preferably a compound having a mass average molecular weight of 2,000-10,000 (inclusive). The concentration of the sulfonium group-containing ether compound in the plating solution is preferably 0.1 mg / L to 1 g / L.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a plating solution, and more particularly to a plating solution that has excellent hole-filling properties, can form a flat plated surface, and contains a sulfonium group-containing ether compound. Background Art

[0002] In the field of electronic materials, a technique for plating a substrate with a metal is used, and this technique is applied to electronic devices such as liquid crystal displays and semiconductor devices. For example, plating is often used as a technique for applying metal to various parts such as printed electronic circuits such as fine-line circuits and semiconductor wafers. As a metal, copper is mainly used because it has good electrical properties and can be processed in a variety of ways.

[0003] In the manufacture of printed wiring boards, copper and other metals are sometimes used to fill the gaps between wirings, holes such as through holes, etc. In the manufacture of semiconductor wafers, metals are also used to fill the tiny through holes, grooves, etc. formed on the surface of the wafer. In particular, in substrate lamination methods represented by the build-up method, so-called hole-filling plating is often used to fill (fill) the connection holes (holes) between layers.

[0004] As a metal filling technology represented by such hole filling plating, an electrolytic plating method is known, and as a plating solution, for example, an acidic copper sulfate plating solution, an alkaline cyanide or pyrophosphate copper plating solution, etc. are used. Among them, a plating solution containing a metal salt of a strong acid represented by copper sulfate is widely used because it is easier to manage the liquid and control the electrodeposition rate than an alkaline plating solution.

[0005] In the buried plating process, a plating solution containing an organic substance called a leveling agent, an acid, a surfactant, etc. in addition to a metal salt is generally used. By containing a leveling agent, the electrodeposition of the plating can be controlled, and the gaps between through holes, grooves, and wirings can be reliably buried, and a plating process with uniform properties can be performed.

[0006] For example, Patent Document 1 discloses a copper sulfate plating solution containing a polymer surfactant that inhibits electrodeposition reaction, a sulfur-based saturated organic compound such as dithiobisalkanesulfonic acid that promotes electrodeposition speed, and a leveling agent composed of a polymer amine compound. Patent Document 2 discloses a tin plating solution that uses a sulfonium compound having a phenyl group as a leveling agent and further contains a nonionic surfactant. Patent Document 3 discloses a tertiary amine compound obtained by reacting a compound having a glycidyl ether group with a nitrogen-containing heterocyclic compound as a new leveling agent.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2003-105584

[0010] Patent Document 2: Japanese Patent Application Publication No. 2016-183410

[0011] Patent Document 3: International Publication No. 2011 / 135716 Pamphlet Summary of the invention

[0012] Problems to be solved by the invention

[0013] In the recent manufacture of printed wiring boards and semiconductor wafers, it is required to completely fill the gaps and highly flatten the surface by plating. The plating solution disclosed in Patent Document 1 has difficulties in this high level of flattening. In the technology described in Patent Document 2, the smoothness of the tin-plated surface is improved by adding a specific leveling agent, but these leveling agents are difficult to function as smoothing agents in metal plating solutions other than tin. Although such a problem is solved by the amine-based leveling agent disclosed in Patent Document 3, it is hoped that the plated surface will be further flattened. Depending on the application, the plating solution is also required to contain no nitrogen component.

[0014] The present invention has been made in view of such actual circumstances, and an object of the present invention is to provide a plating solution that has excellent hole-filling properties and can form a flat plated surface.

[0015] Means for solving problems

[0016] The present inventors have found that a plating solution having excellent planarization performance can be obtained by including a sulfonium group-containing ether compound as a leveling agent in a plating solution, thereby completing the present invention.

[0017] (1) The first invention of the present invention is a plating solution comprising:

[0018] water-soluble metal salts; and

[0019] Sulfonium-containing ether compounds.

[0020] (2) A second aspect of the present invention is the plating solution of the first aspect, wherein the sulfonium group-containing ether compound has a structure represented by Formula 1.

[0021] [Chemistry 1]

[0022]

[0023] (In Formula 1, R 1 and R 2 are each independently a substituted or unsubstituted aliphatic or aromatic hydrocarbon group, R 1 With R 2 They can be bonded to each other to form a ring structure; E is the ether part in the above-mentioned sulfonium group-containing ether compound, or a substituted or unsubstituted aliphatic or aromatic hydrocarbon group bonded to the above-mentioned ether part.)

[0024] (3) The third invention of the present invention is the plating solution of the second invention, wherein the sulfonium group-containing ether compound has the above R 1 and the above R 2 The reaction product of an organic sulfur compound having the groups shown and an ether compound having a reactive group.

[0025] (4) A fourth aspect of the present invention is the plating solution according to any one of the first to third aspects, wherein the sulfonium group-containing ether compound is a compound having a mass average molecular weight of 2,000 to 10,000.

[0026] (5) A fifth aspect of the present invention is the plating solution according to any one of the first to fourth aspects, wherein the metal salt is a salt containing copper.

[0027] (6) A sixth aspect of the present invention is the plating solution according to any one of the first to fifth aspects, wherein the sulfonium group-containing ether compound is contained at a concentration of 0.1 mg / L to 1 g / L.

[0028] Effects of the Invention

[0029] According to the present invention, a plating solution having excellent hole filling properties and capable of forming a flat plated surface can be provided. In addition, the plating solution of the present invention can also replace a conventional leveling agent in applications requiring a nitrogen-free plating solution. DETAILED DESCRIPTION

[0030] Embodiments of the present invention will be described below, but these are merely illustrative forms, and various modifications are possible without departing from the technical concept of the present invention.

[0031] 《1. Plating solution》

[0032] The plating solution of the present invention contains a water-soluble metal salt and a sulfonium group-containing ether compound.

[0033] [Regarding the composition of the plating solution]

[0034] (1) Water-soluble metal salts

[0035] The water-soluble metal salt constituting the plating solution of the present invention is not particularly limited, and includes water-soluble metal salts of copper (Cu), tin (Sn), titanium (Ti), chromium (Cr), manganese (Mn), iron (Fe), nickel (Ni), cobalt (Co), zinc (Zn), silver (Ag), gold (Au), platinum (Pt), palladium (Pd), indium (In), molybdenum (Mo), tungsten (W), lead (Pb), rhenium (Re), rhodium (Rh), ruthenium (Ru), osmium (Os), iridium (Ir), bismuth (Bi), aluminum (Al), etc., and also includes any salt used for plating, such as water-soluble salts of semimetals such as germanium (Ge), arsenic (As), and antimony (Sb). A plurality of metal salts may be used in combination to prepare a plating solution for composite plating such as bronze plating and solder plating.

[0036] It should be noted that, in the present invention, "a plating solution containing a water-soluble metal salt" broadly includes all plating solutions in which a water-soluble metal salt can be detected from the liquid. That is, as long as the metal is ionized and dissolved as described above, for example, a metal salt obtained by dissolving an insoluble metal oxide in an acid is also equivalent to the "water-soluble metal salt" in the present invention. In addition, the plating solution of the present invention is preferably an aqueous solution of these metal salts, but may also contain alcohols such as methanol and ethanol; ethers such as tetrahydrofuran (THF), dioxane, and various glycol dimethyl ethers; carbonates such as ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate; nitrogen-containing solvents such as acetonitrile, dimethylformamide (DMF), and pyrrolidone; organic solvents such as sulfur-containing solvents such as dimethyl sulfoxide (DMSO). Depending on the purpose and the metal salt used, an organic solvent may also be used as the main solvent.

[0037] The types of counter ions with metals in water-soluble metal salts are not particularly limited. For example, anions of inorganic acids such as hydrohalic acids represented by nitric acid, sulfuric acid, and hydrochloric acid, and oxo acids represented by phosphoric acid and chloric acid; anions of organic acids such as alkane sulfonic acids such as methanesulfonic acid and propanesulfonic acid, alkane sulfonic acids such as isethionic acid and propanol sulfonic acid, and aliphatic or aromatic carboxylic acids such as citric acid, tartaric acid, and formic acid, etc., but are not limited to these. The metal salt constituting the plating solution of the present invention may be a salt having a metal element in the anion, such as molybdate and chloroplatinate, and the counter anion in this case may also be any ion such as an alkali metal ion, ammonium ion, etc. In addition, a salt such as nickel molybdate may be contained to prepare a plating solution for nickel-molybdenum alloy plating.

[0038] As described above, the plating solution of the present invention may contain salts of any metal, but considering the use in the field of electronic materials, salts containing metals such as copper, gold, nickel, and tin are preferred. These metals are often used in the manufacture of printed wiring boards and semiconductor wafers, and in a plating solution containing such metal salts, the planarization performance of the present invention becomes significant. In particular, copper salts represented by copper sulfate and copper nitrate are preferred.

[0039] The concentration of the water-soluble metal salt in the plating solution of the present invention is not particularly limited and can be arbitrarily set according to the metal salt contained and the plating object. Generally, in the plating of electronic materials, a concentration of 10 to 80 g / L, particularly 35 to 75 g / L, is used in terms of the mass conversion of metal ions. The plating solution of the present invention can also be set to such an ion concentration.

[0040] It should be noted that the above mentioned embodiment of dissolving the metal oxide in the acid also has the advantages of easy management of the plating solution, control of the electrodeposition rate, etc. In the present invention, even when a water-soluble metal salt is used as a raw material, the plating solution preferably contains an acid. The acid used here is not particularly limited, and the desired substance among the above-mentioned inorganic acids and / or organic acids such as sulfuric acid and nitric acid can be used according to the composition of the plating solution and the plating object. For example, when the water-soluble metal salt is copper sulfate, the plating solution preferably contains sulfuric acid as the acid. The concentration of the acid is also not limited, for example, it can be set to 5 to 200 g / L, especially to 10 to 150 g / L.

[0041] (2) Ether compounds containing sulfonium groups

[0042] The plating solution of the present invention contains the water-soluble metal salt and the ether compound containing a sulfonium group, thereby improving the hole filling property of the plating solution and forming a flat plated surface.

[0043] Here, the sulfonium group-containing ether compound refers to a sulfonium group (R3S + - group: R is a hydrogen atom or an organic group) and an ether bond (-O-), which is a kind of ether compound and a kind of sulfonium compound. The plating solution of the present invention can contain any compound as the ether compound containing a sulfonium group, and its type is not particularly limited. It is also possible to use a plurality of ether compounds containing a sulfonium group in combination.

[0044] Among them, it is particularly preferred that the sulfonium group-containing ether compound contained in the plating solution has a structure represented by the following formula 1. When the sulfonium group-containing ether compound has the structure of formula 1, the planarization performance of the plating solution of the present invention is further excellent.

[0045] [Chemistry 2]

[0046]

[0047] In the above formula 1, R 1 and R 2 are each independently a substituted or unsubstituted aliphatic or aromatic hydrocarbon group, R 1 With R 2 can bond with each other to form a ring structure. 1 and R 2At least one of them is preferably an aliphatic hydrocarbon group, more preferably an alkyl group, especially an alkyl group having 1 to 3 carbon atoms. With such a structure, the plating solution of the present invention is more likely to exhibit planarization performance. 1 With R 2 When they are bonded to each other to form a ring structure, it is preferred that R 1 and R 2 The alkylene group, particularly the alkylene group having 3 to 7 carbon atoms, is bonded to form a 4- to 8-membered ring together with the sulfur atom. 1 and / or R 2 When the aromatic hydrocarbon group is an aromatic hydrocarbon group, the hydrocarbon group is preferably a substituted or unsubstituted phenyl group. Here, the type, number and position of the substituents on the aromatic hydrocarbon group such as the phenyl group and the aliphatic hydrocarbon group are not particularly limited. The planarization performance of the plating solution of the present invention is 1 and / or R 2 The hydrocarbon group, especially the aromatic hydrocarbon group, is not damaged when it has an electron-donating group such as an alkyl group or an alkoxy group, or when it has an electron-withdrawing group such as a halogen group or a halogenated hydrocarbon group.

[0048] In addition, in the above formula 1, E is the ether part in the ether compound containing a sulfonium group as described above, or a substituted or unsubstituted aliphatic or aromatic hydrocarbon group bonded to the ether part. Here, the ether part only needs to have one or more ether bonds (-O-), and its structure is not particularly limited. For example, it can be various oxy groups represented by alkoxy and phenoxy groups, aliphatic or aromatic hydrocarbon groups having such oxy groups as substituents, groups having multiple ether bonds such as polyoxyethylene, amino groups, amide groups, acyl groups, etc. having oxy groups as described above in the side chain. In addition, the aliphatic or aromatic hydrocarbon group having an oxy group as a substituent can be, for example, a smaller group such as methoxymethyl, methoxyethyl, ethoxyethyl, methoxypropyl, methoxyphenyl, or a hydrocarbon group having a long-chain alkoxy group, a long-chain alkyl group or a long-chain alkenyl group having a methoxy group or an ethoxy group, etc., which has a large amount of formula. For polyoxyethylene, there is no particular restriction on the number of carbon atoms, etc.

[0049] In addition, the substituent E may have other sulfonium groups at the terminal and / or side chain. Here, the "other sulfonium groups" may be of the same type as the previous sulfonium group to which the substituent E is bonded, or may be different. The number of sulfonium groups in the sulfonium group-containing ether compound is not particularly limited, and by containing an ether compound preferably having 1 to 20, particularly 2 to 10 sulfonium groups in the molecule, the planarization performance of the plating solution can be made particularly excellent.

[0050] The ether compound containing a sulfonium group is particularly preferably one having an alkylene oxide structure, such as an ethylene oxide structure, and particularly a polyethylene oxide structure at the ether portion. The ether compound containing a sulfonium group having an alkylene oxide structure is generally well water-soluble, and therefore can be contained in a large amount in the plating solution. Therefore, the planarization performance of the plating solution can be further improved. In addition, the ether compound having an alkylene oxide structure can be prepared relatively easily as described later. As a specific example of the ether compound containing a sulfonium group having a polyoxyalkylene structure, for example, a compound such as the following formula 1-1 can be cited.

[0051] [Chemistry 3]

[0052]

[0053] In the compound of formula 1-1, the compound corresponding to R in formula 1 1 and R 2 The groups of R are all methyl groups, and the group corresponding to E is an aromatic hydrocarbon bonded to the ether portion. Generally, aromatic sulfonyl compounds are more stable than aliphatic sulfonyl compounds, so in the sulfonium group-containing ether compound used in the present invention, the substituent R is also preferably 1 , R 2 The sulfur atom-side position of E is a substituted or unsubstituted aromatic hydrocarbon group, particularly a substituted or unsubstituted phenyl group. However, the sulfonium group-containing ether compound is not limited to such a structure.

[0054] As described above, the sulfonium-containing ether compound may be a compound having a chain length of a certain degree and a large molecular weight. The molecular weight of the sulfonium-containing ether compound is not particularly limited, and the mass average molecular weight is preferably 500 to 100,000, particularly preferably 1,000 to 15,000, and particularly preferably 2,000 to 10,000. As shown in the examples described below, a plating solution containing a sulfonium-containing ether compound of such a molecular weight exhibits excellent planarization performance. In particular, the hole filling performance generally tends to be better as the molecular weight of the sulfonium-containing ether compound in the plating solution increases, and is particularly good in the case of a plating solution containing a sulfonium-containing ether compound having a mass average molecular weight of 2,000 or more. In addition, if the mass average molecular weight of the sulfonium-containing ether compound is less than 10,000, sufficient water solubility can also be ensured, so that it can be contained in a larger amount in the plating solution of the present invention, and the planarization performance can be made better. The molecular weight of the sulfonium group-containing ether compound can be measured, for example, by gel permeation chromatography (GPC) or the like using monodisperse polyethylene oxide, polyethylene glycol, or the like as a standard.

[0055] (Preparation of sulfonium group-containing ether compound)

[0056] The sulfonium group-containing ether compound can be prepared, for example, by reacting an organic sulfur compound with an ether compound having a reactive group. In a preferred embodiment of the present invention, the sulfonium group-containing ether compound is an ether compound having the above R 1 and R 2 The reaction product of an organic sulfur compound having the groups shown and an ether compound having a reactive group.

[0057] Here, the reactive group on the ether compound is not particularly limited, and a desired group can be selected from various reactive groups such as epoxy, sulfonyl, sulfonyloxy, carboxyl, and amino. Alternatively, the sulfonium-containing ether compound can be prepared by bonding an ether compound having an allyl group with an allyl-containing sulfonium compound using a peroxide or the like. Among them, from the perspective of reliable and rapid reaction, the reactive group is preferably an epoxy group or a sulfonyloxy group, and particularly preferably an epoxy group.

[0058] When the reactive group is an epoxy group, for example, as shown in the following reaction formula α, by reacting an organic sulfur compound represented by formula 2α with an epoxy-containing ether compound represented by formula 3 in the presence of an acid such as methanesulfonic acid, a sulfonium group-containing ether compound such as formula 1α1 and / or formula 1α2 can be prepared.

[0059] [Chemistry 4]

[0060]

[0061] Here, R 1 and R 2 R in the above formula 1 1 and R 2 The same; Eo and Er are groups containing an ether portion; -CH2-CH(OH)-Er and the like are groups corresponding to -E in Formula 1, i.e., the ether portion in the sulfonium group-containing ether compound shown in Formula 1. It should be noted that the group Er in Formulas 1α1 and 1α2 is represented by a symbol different from that of the group Eo in Formula 3, because sometimes Eo itself reacts and changes into other groups (for example, Eo also has epoxy groups, and polymerization is carried out starting from these epoxy groups, etc.).

[0062] Alternatively, for example, as shown in the following reaction formula β, a sulfonium compound having a hydroxyl group represented by formula 2β and an epoxy-containing ether compound represented by formula 3 may be reacted in the presence of a catalyst such as potassium carbonate to prepare a sulfonium group-containing ether compound such as formula 1β1 and / or formula 1β2.

[0063] [Chemistry 5]

[0064]

[0065] Here, R 1 and R 2R in the above formula 1 1 and R 2 The same; A is a substituted or unsubstituted aliphatic or aromatic divalent hydrocarbon group; Eo and Er are groups containing an ether portion; -AO-CH2-CH(OH)-Er and the like are groups corresponding to -E in Formula 1. The compounds represented by Formula 1β1 and Formula 1β2 are equivalent to compounds in which E is a substituted or unsubstituted aliphatic or aromatic hydrocarbon group bonded to the ether portion in the sulfonium group-containing ether compound represented by Formula 1.

[0066] In addition, when the reactive group is a sulfonyloxy group, for example, as shown in the following reaction formula γ, a sulfonium compound having a hydroxyl group represented by formula 2β and an ether compound containing a sulfonyloxy group represented by formula 4 can be reacted in the presence of a catalyst such as potassium carbonate to prepare a sulfonium group-containing ether compound such as formula 1γ.

[0067] [Chemistry 6]

[0068]

[0069] Here, R 1 and R 2 , A, Eo and Er are the same as the substituents in the above reaction formula β, R 3 It is a substituted or unsubstituted aliphatic or aromatic hydrocarbon group, for example, a methyl group.

[0070] It should be noted that in the reaction represented by reaction formula α, acids other than methanesulfonic acid may be used, such as sulfuric acid, phosphoric acid, acetic acid, etc. In the reactions represented by reaction formulas β and γ, catalysts other than potassium carbonate, such as sodium hydroxide, triethylamine, etc. may be used.

[0071] (2-1) Organic sulfur compounds

[0072] In addition, the sulfonium group-containing ether compound may also be composed of a substituent R 1 and R 2 The method can be prepared by using any organic sulfur compound represented by formula 2α and / or the organic sulfur compound represented by formula 2β.

[0073] In the organic sulfur compounds represented by formula 2α and 2β, R 1 and R 2 Each is independently a substituted or unsubstituted aliphatic or aromatic hydrocarbon group, and may be bonded to each other to form a cyclic structure. As described in the description of Formula 1, preferably R 1 and R 2 At least one of them is an aliphatic hydrocarbon group, more preferably an alkyl group, especially an alkyl group having 1 to 3 carbon atoms. 1 With R 2 When they are bonded to each other, R1 and R 2 Together with the sulfur atom, it forms a 4- to 7-membered ring. 1 and / or R 2 In the case of an aromatic hydrocarbon group, the hydrocarbon group is preferably a substituted or unsubstituted phenyl group.

[0074] In the organic sulfur compound represented by formula 2β, A can be a substituted or unsubstituted aliphatic or aromatic divalent hydrocarbon group, preferably a substituted or unsubstituted aromatic hydrocarbon group, and more preferably a substituted or unsubstituted phenylene group. If it is an organic sulfur compound having a phenolic hydroxyl group, it is easy to react with reactive groups such as epoxy groups and sulfonyloxy groups in ether compounds. The -A-OH group is particularly preferably p-hydroxyphenyl.

[0075] In addition, in the organic sulfur compound represented by formula 2β, R 1 and R 2 It is preferably a hydrocarbon group having 1 to 6 carbon atoms, and among them, an alkyl group having 1 to 3 carbon atoms is preferred. 1 and R 2 Both are methyl groups. One particularly preferred embodiment of the organic sulfur compound represented by Formula 2β is a compound represented by the following Formula 2-1. Of course, organic sulfur compounds other than these can also be preferably used.

[0076] [Chemistry 7]

[0077]

[0078] It should be noted that the counter anion of the organic sulfonium compound represented by formula 2β is not particularly limited and can be any type of anion such as an alkyl sulfonate anion represented by a methanesulfonate anion, a borate anion represented by a tetrafluoroborate anion, a phosphate anion represented by a hexafluorophosphate anion, a sulfate anion, a nitrate anion, a halide ion, etc.

[0079] As particularly preferred embodiments of the organic sulfur compound represented by Formula 2α, for example, compounds represented by the following Formulas 2-2 to 2-7 can be mentioned.

[0080] [Chemistry 8]

[0081]

[0082] Of course, organic sulfur compounds other than those of Formula 2-2 to Formula 2-7 may also be preferably used. It should be noted that the compound represented by Formula 2-3 may also react with an ether compound via the hydroxyl group (phenolic hydroxyl group) in the molecule as shown in Reaction Formula β.

[0083] (2-2) Ether compound having a reactive group

[0084] The ether compound that reacts with the organic sulfur compound may be any compound as long as it has a reactive group as described above, but preferably contains an epoxy group or a sulfonyloxy group as a reactive group. More preferably, the ether compound represented by the above formula 3 or formula 4 is used. It is particularly preferred that the substituent Eo in formula 3 and formula 4 has an alkylene oxide structure, such as an ethylene oxide structure, particularly a polyethylene oxide structure. The molecular weight is also not particularly limited, but the mass average molecular weight is preferably 50 to 10,000, particularly preferably 70 to 5,000, and particularly preferably 100 to 1,000.

[0085] In addition, the ether compound preferably has two or more epoxy groups in the molecule. If there are multiple epoxy groups, when reacting with the organic sulfur compound, the polymerization reaction between the ether compounds also proceeds, and a sulfonium group-containing ether compound having a polyoxyalkylene structure can be generated. As a result, the obtained sulfonium group-containing ether compound has a high molecular weight and good water solubility, which can make the planarization performance of the plating solution more excellent.

[0086] As particularly preferred embodiments of the ether compound having a reactive group represented by Formula 3, for example, compounds represented by the following Formulas 3-1 to 3-4 can be mentioned.

[0087] [Chemistry 9]

[0088]

[0089] Of course, epoxy-containing ether compounds other than those mentioned above can also be used as the compound of formula 3. In formula 3-1, m and n are preferably integers of 0 to 10, particularly preferably 1 to 6; m+n is preferably 1 to 20, particularly preferably 2 to 10. It should be noted that a plurality of compounds represented by formula 3-1 can also be used in combination. At this time or when the compounds represented by formula 3-1 are polymerized with each other, the average values ​​of m and n are not necessarily integers, but such an embodiment is also included in the scope of the present invention.

[0090] As a particularly preferred embodiment of the ether compound having a reactive group represented by Formula 4, for example, there can be mentioned a compound represented by the following Formula 4-1.

[0091] [Chemistry 10]

[0092]

[0093] Of course, other sulfonyloxy-containing ether compounds may also be preferably used. It should be noted that in Formula 4-1, n is preferably an integer of 1 to 10,000, particularly preferably an integer of 2 to 1,000. Multiple compounds represented by Formula 4-1 may also be used in combination. In this case, the average value of n is not necessarily an integer, but such an embodiment is also included in the scope of the present invention.

[0094] By reacting these ether compounds with the above-mentioned organic sulfur compounds, sulfonium group-containing ether compounds can be synthesized. For example, by reacting the organic sulfur compound represented by Formula 2-1 with the ether compound represented by Formula 3-1 according to Reaction Formula β, the compound represented by Formula 1-1 can be prepared. It should be noted that the molar ratio of the organic sulfur compound to the reactive group in the ether compound during the reaction does not necessarily need to be 1:1, for example, 1:0.9 to 1:1.1. Depending on the structure and molecular weight of the target sulfonium group-containing ether compound, the equivalent ratio of the reactive group in the ether compound: the organic sulfur compound can be, for example, 1:0.1 to 1:0.9, especially 1:0.2 to 1:0.8, so that the ether compounds are polymerized with each other.

[0095] (Content of sulfonium group-containing ether compound)

[0096] In the plating solution of the present invention, the content of the sulfonium group-containing ether compound is not particularly limited and can be arbitrarily set according to the plating object and the metal salt used. For example, the sulfonium group-containing ether compound can be contained in a concentration of about 0.1 mg / L to 1 g / L, more preferably in a concentration of about 1 to 700 mg / L, and particularly preferably in a concentration of about 1 to 500 mg / L. If the content of the sulfonium group-containing ether compound is above 0.1 mg / L, the plating solution exhibits good planarization performance, and if the content is below 1 g / L, it is cost-effective.

[0097] (3) Additives

[0098] As described above, the plating solution of the present invention contains a water-soluble metal salt and a sulfonium group-containing ether compound. In addition, in order to facilitate the management of the plating solution and control the electrodeposition rate, it may further contain an acid such as sulfuric acid as described above as desired.

[0099] In addition, the plating solution of the present invention may contain additives such as halide ions, brighteners, surfactants, complexing agents, antioxidants, conductive salts, wetting agents, and pigments represented by phthalocyanine compounds and Janus green as desired. Several of these additives are described below, but the additives that can be contained in the plating solution of the present invention are not limited to these.

[0100] (Halide Ion)

[0101] In addition, halide ions are sometimes added to the usual acidic metal plating solution for the purpose of glossy metal plating and leveling. In the present invention, halide ions such as chlorine, bromine, and iodine may also be added to the plating solution as needed. Chloride ions (Cl - ) In this case, the concentration of the halide ions can be, for example, about 0.01 to 150 mg / L, preferably about 10 to 100 mg / L, in terms of ion mass concentration in the entire plating solution.

[0102] (Glossing agent)

[0103] The brightener not only imparts gloss to the plated film, but also promotes the precipitation of metal in the recessed portion, and can contribute to the flattening of the plated surface. The type of brightener is not particularly limited, and examples thereof include benzaldehyde, o-chlorobenzaldehyde, 2,4,6-trichlorobenzaldehyde, m-chlorobenzaldehyde, p-nitrobenzaldehyde, p-hydroxybenzaldehyde, furfural, 1-naphthaldehyde, 2-naphthaldehyde, 2-hydroxy-1-naphthaldehyde, 3-acenaphthaldehyde, benzylideneacetone, pyridylideneacetone, furfurylideneacetone, and acenaphthaldehyde. Various aldehydes such as furfurylideneacetone, cinnamaldehyde, anisaldehyde, salicylaldehyde, crotonaldehyde, acrolein, glutaraldehyde, paraldehyde, and vanillin; triazine, imidazole, indole, quinoline, 2-vinylpyridine, aniline, phenanthroline, neocuprous reagent, picolinic acid, thiourea, N-(3-hydroxybutylene)-p-sulfanilic acid, N-butylenesulfanilic acid, N-cinnamoylidenesulfanilic acid (cinnamoylidene sulfanilic acid, cinnamoylidene sulfanilic acid) acid), 2,4-diamino-6-(2'-methylimidazolyl(1'))ethyl-1,3,5-triazine, 2,4-diamino-6-(2'-ethyl-4-methylimidazolyl(1'))ethyl-1,3,5-triazine, 2,4-diamino-6-(2'-undecylimidazolyl(1'))ethyl-1,3,5-triazine, phenyl salicylate; or benzothiazole, 2-mercaptobenzothiazole, 2-methylbenzothiazole, 2-aminobenzothiazole, 2-amino-6-methoxybenzothiazole, 2-methyl-5-chlorobenzothiazole, 2-hydroxybenzothiazole, 2-amino-6-methylbenzothiazole, 2-chlorobenzothiazole, 2,5-dimethylbenzothiazole, 5-hydroxy-2-methylbenzothiazole and the like, sulfides such as bis(sodium 3-sulfopropyl) disulfide, etc. Among them, by containing a sulfide compound as a brightener, the planarization characteristics of the plating solution of the present invention can be further improved. Bis(3-sulfopropylsodium) disulfide is particularly preferred. It should be noted that when a brightener is contained, its concentration is preferably about 0.01 mg / L to 50 mg / L, and particularly preferably about 0.1 mg / L to 10 mg / L.

[0104] (Surfactant)

[0105] There are no particular restrictions on the surfactant, and a desired surfactant can be selected from common anionic surfactants, cationic surfactants, nonionic surfactants, amphoteric surfactants, etc. When a surfactant is contained, its concentration is preferably 10 mg / L to 50 g / L, and particularly preferably 50 mg / L to 500 mg / L.

[0106] Examples of the anionic surfactant include polyoxyalkylene alkyl ether sulfates such as sodium polyoxyethylene nonyl ether sulfate, polyoxyalkylene alkyl phenyl ether sulfates such as sodium polyoxyethylene dodecylphenyl ether sulfate, alkylbenzene sulfonates such as sodium dodecylbenzene sulfonate, naphthol sulfonates such as sodium 1-naphthol-4-sulfonate and disodium 2-naphthol-3,6-disulfonate, (poly)alkylnaphthalene sulfonates such as sodium diisopropylnaphthalene sulfonate and sodium dibutylnaphthalene sulfonate, and alkyl sulfates such as sodium lauryl sulfate and sodium oleyl sulfate.

[0107] Examples of the cationic surfactant include mono- to trialkylamine salts, dimethyldialkylammonium salts, trimethylalkylammonium salts, dodecyltrimethylammonium salts, hexadecyltrimethylammonium salts, octadecyltrimethylammonium salts, dodecyldimethylammonium salts, octadecyldimethylethylammonium salts, dodecyldimethylbenzylammonium salts, hexadecyldimethylbenzylammonium salts, octadecyldimethylbenzylammonium salts, trimethylbenzylammonium salts, triethylbenzylammonium salts, hexadecylpyridinium salts, dodecylpyridinium salts, dodecylmethylpyridinium salts, dodecylimidazolium salts, oleylimidazolium salts, octadecylamine acetate, and dodecylamine acetate.

[0108] Examples of the nonionic surfactant include addition condensates of sugar esters, fatty acid esters, alkoxyphosphates (salts), sorbitan esters, aliphatic amides, etc. with ethylene oxide and / or propylene oxide, silicon-based polyoxyethylene ethers, silicon-based polyoxyethylene esters, fluorine-based polyoxyethylene ethers, fluorine-based polyoxyethylene esters, sulfated or sulfonated addition products of condensation products of ethylene oxide and / or propylene oxide with alkylamines or diamines, and the like.

[0109] Examples of the amphoteric surfactant include betaine, carboxybetaine, imidazolinium betaine, sulfobetaine, and aminocarboxylic acid.

[0110] (Complexing agent)

[0111] Complexing agents are additives that can help stabilize metal ions in the plating solution and homogenize the composition of the precipitated alloy in the alloy plating layer. In particular, in plating solutions containing precious metals such as silver, complexing agents such as hydroxycarboxylic acids, polycarboxylic acids, and monocarboxylic acids are generally used. When a complexing agent is included, its concentration can be, for example, 0.1 g / L to 500 g / L, particularly 1 g / L to 100 g / L. Specific examples of the complexing agent include gluconic acid, citric acid, glucoheptonic acid, gluconolactone, gluconolactone, formic acid, acetic acid, propionic acid, butyric acid, ascorbic acid, oxalic acid, malonic acid, succinic acid, glycolic acid, malic acid, tartaric acid, diglycolic acid, thioglycolic acid, thiodiglycolic acid, thioglycol, thiodiglycol, mercaptosuccinic acid, 3,6-dithia-1,8-octanediol, 3,6,9-trithiodecane-1,11-disulfonic acid, thiobis(dodecanediol), di(6-methylbenzothiazolyl) disulfide trisulfonic acid, di(6-chlorobenzothiazolyl) disulfide disulfonic acid, glucose Sugar acid, citric acid, glucoheptonic acid, gluconolactone, gluconolactone, dithiodiphenylamine, dipyridyl disulfide, mercaptosuccinic acid, sulfite, thiosulfate, ethylenediamine, ethylenediaminetetraacetic acid (EDTA), diethylenetriaminepentaacetic acid (DTPA), nitrilotriacetic acid (NTA), iminodiacetic acid (IDA), iminodipropionic acid (IDP), hydroxyethylethylenediaminetriacetic acid (HEDTA), triethylenetetraaminehexaacetic acid (TTHA), ethylenedioxybis(ethylamine)-N,N,N',N'-tetraacetic acid, glycines, nitrilotrimethylphosphonic acid, or salts thereof, etc. In addition, sulfur-containing compounds such as thioureas, tris(3-hydroxypropyl)phosphine, etc. may also be contained.

[0112] (Antioxidant)

[0113] Antioxidants are used to prevent oxidation of metal salts and are important in tin plating solutions and the like. Antioxidants can be contained in a concentration of, for example, 0.1 g / L to 500 g / L, particularly 1 g / L to 100 g / L. Examples of antioxidants include hypophosphorous acids, ascorbic acid, phenolsulfonic acid, cresolsulfonic acid, hydroquinonesulfonic acid, hydroquinone, α or β-naphthol, catechol, resorcinol, phloroglucinol, hydrazine, phenolsulfonic acid, catecholsulfonic acid, hydroxybenzenesulfonic acid, naphtholsulfonic acid, and salts thereof.

[0114] [About the preparation of plating solution]

[0115] The plating solution of the present invention can be prepared from the above-mentioned components by a conventional method, and the details thereof can be appropriately determined in consideration of the composition and blending amount of each component.

[0116] 《2. Plating treatment》

[0117] As described above, by performing a plating treatment using the plating solution of the present invention, it is possible to flatten the gaps in a printed wiring board, a semiconductor wafer, or the like, and form a flat plated surface.

[0118] (Plating object)

[0119] The plating solution of the present invention can be used for any object such as various substrates and wafers. According to the plating solution of the present invention, a flat plated surface can be formed. The plating solution of the present invention is also excellent in uniform electroplating properties, and can also flatten gaps of various sizes ranging from sub-μm to hundreds of μm. Furthermore, the plating solution of the present invention is also excellent in anisotropy, and can mainly plate only the target part, so it is useful for plating electronic components and the like. As electronic components, printed circuit boards, flexible printed circuit boards, film carriers, semiconductor integrated circuits, resistors, capacitors, filters, inductors, thermistors, crystal oscillators, switches, leads, etc. can be cited, but the objects of the plating solution of the present invention are not limited to these. The plating solution of the present invention can also be applied to a part of an electronic component to form a film, such as a bump electrode of a wafer.

[0120] When the plating solution of the present invention is used to plate a substrate, the target substrate is not particularly limited. For example, a substrate having a conductive layer of metal or the like formed and patterned on a substrate made of resin or the like, a semiconductor substrate such as a silicon wafer having a fine circuit pattern on the surface, an electronic circuit substrate such as a printed circuit board, etc. can be used as the plating target.

[0121] In these substrates, blind holes, grooves (trench) for fine wiring, through holes that penetrate the substrate, etc. may also be mixed. The plating solution of the present invention has excellent hole-filling properties and is therefore suitable for plating substrates having through holes and grooves. The plating solution of the present invention can also be used for wiring formation of substrates.

[0122] Specific examples of these substrates include printed circuit boards such as package substrates on which IC bare chips are directly mounted, silicon wafers on which LSIs are directly mounted, and silicon wafer substrates for the purpose of manufacturing semiconductor chips themselves.

[0123] (Plating Operation)

[0124] The plating solution of the present invention can be used to plate the above-mentioned substrate by, for example, a normal plating operation. Hereinafter, an embodiment of the plating operation using the plating solution of the present invention will be described, but the present invention is not limited to such an embodiment.

[0125] For example, the substrate to be plated is subjected to pretreatment such as formation of a barrier layer as desired, and then the substrate is subjected to a conductive treatment such as forming a metal seed layer to become a power supply layer. The conductive treatment can be performed by a common conductive treatment method, such as a metal (including carbon) coating treatment using electroless plating, a so-called direct plating treatment method using carbon or palladium, sputtering, evaporation or chemical vapor deposition (CVD).

[0126] Next, the conductive substrate is plated using the plating solution of the present invention. The conditions at this time are not particularly limited, and the usual plating conditions may be used. For example, the liquid temperature is about 20 to 30°C, the cathode current density is 0.05 to 3A / dm 2 The plating can be performed to a certain extent. In addition, the plating time can be appropriately set according to the purpose of plating. Furthermore, during the plating, it is preferred to stir the liquid by aeration, pump circulation, paddle stirring, etc.

[0127] According to the embodiment described above, blind holes, through holes, grooves, silicon through electrodes, etc. located on the above-mentioned substrate can be filled in a state where the surface plating thickness (the plating thickness of the substrate portion without these, which is plated simultaneously with the blind holes, through holes, grooves, silicon through electrodes) is thin.

[0128] Specifically, for example, in order to completely fill a through hole by plating a patterned substrate having a blind hole with a diameter of 50 μm and a depth of 30 μm, the current can be 1.5 A / dm. 2 The plating is performed for about 30 minutes at a cathode current density of . The surface plating thickness at this time can be, for example, about 10 μm.

[0129] In addition, for the purpose of semiconductor manufacturing, for example, in order to completely fill the through-holes and grooves of a silicon wafer having a diameter of 0.1 to 0.5 μm and a depth of 0.2 to 1 μm by plating, the through-holes and grooves can also be plated at 2 A / dm 2 The plating is performed for about 150 seconds at a cathode current density of about 1 μm. The surface plating thickness at this time is, for example, about 1 μm.

[0130] Furthermore, for the purpose of three-dimensional mounting, for example, in order to fill and plate a silicon through-electrode with a diameter of 10 μm and a depth of 20 μm, the plating can be carried out at 2 A / dm. 2 The cathode current density is 0.2A / dm for plating for about 10 minutes. The surface plating thickness at this time is, for example, about 5 μm. In addition, for example, in order to fill the silicon through electrode with a diameter of 20 μm and a depth of 100 μm, the cathode current density can also be 0.2A / dm 2 The plating is performed for about 60 minutes at a cathode current density of . The surface plating thickness at this time is, for example, about 3 μm.

[0131] The operation and conditions in the plating method using the plating solution of the present invention are not limited to the above contents, and the plating solution of the present invention can be applied to various plating processes or apparatuses.

[0132] Example

[0133] Hereinafter, the present invention will be described in further detail by way of examples, but the present invention is not limited to these descriptions at all.

[0134] "Synthesis Examples 1 to 11"

[0135] Before preparing the plating solution of the present invention, various sulfonium-containing ether compounds are synthesized as follows. It should be noted that in the following synthesis examples, the structure of the product is represented by 1 The mass average molecular weight was analyzed by GPC. The GPC analysis was performed using monodisperse polyethylene oxide and polyethylene glycol as standard samples and a differential refractive index detector (RI). In addition, NMR measurement was performed at 400 MHz.

[0136] <Synthesis example 1>

[0137] Into the reaction container, add 2.87 g of polyglycerol polyglycidyl ether represented by formula 3-1 (n+m=6), 5 g of pure water, 3.41 g of 4-hydroxyphenyldimethylsulfonium methanesulfonate represented by formula 2-1 (0.8 equivalents of reactive groups relative to epoxy groups), and 1.76 g of potassium carbonate in the order described. After raising the internal temperature to 70°C, stir at 70°C±5°C for 3 hours. Return the reaction solution to room temperature, and add 4.34 g of 50% sulfuric acid to stop the reaction. Adjust the total volume to 40 mL with water, and obtain a sulfonium-containing ether compound (SE-1) in the form of an aqueous solution with a concentration of 157 g / L. It is inferred that SE-1 has the structure shown in formula 1-1. 1 In H-NMR (solvent: heavy water), the peak derived from the methyl group that appeared at 3.08 ppm in the compound of formula 2-1 as the raw material appeared as a broad peak at 3.21 ppm, and the peak derived from the aromatic ring that appeared near 6.7 and 7.6 ppm appeared as a broad peak near 7.2-7.3 and 7.9 ppm. In addition, the mass average molecular weight of SE-1 was 7,800 as measured by GPC.

[0138] <Synthesis example 2>

[0139] Into the reaction container, add 0.5 g of glycerol polyglycidyl ether (Formula 3-2), 1 g of pure water, 0.47 g of 4-hydroxyphenyldimethylsulfonium methanesulfonate (Formula 2-1) (0.5 equivalents of reactive groups relative to epoxy groups), and 0.24 g of potassium carbonate in the order described. Raise the internal temperature to 70°C and stir at 70°C±5°C for 3 hours. Return the reaction solution to room temperature and add 1.57 g of 50% sulfuric acid to stop the reaction. Adjust the total volume to 20 mL with water, and obtain the sulfonium-containing ether compound (SE-2) in the form of an aqueous solution with a concentration of 49 g / L. By 1 H-NMR confirmed that a sulfonium group different from that of the raw material was generated after the reaction. The mass average molecular weight of SE-2 was 4,120.

[0140] <Synthesis example 3>

[0141] Into the reaction container, add 3.24 g of ethylene glycol diglycidyl ether (Formula 3-3), 3 g of pure water, 1.99 g of 4-hydroxyphenyldimethylsulfonium methanesulfonate (Formula 2-1) (0.3 equivalents of reactive groups relative to epoxy groups), and 1.03 g of potassium carbonate in the order described. Raise the internal temperature to 70°C and stir at 70°C±5°C for 3 hours. Return the reaction solution to room temperature and add 3.9 g of 50% sulfuric acid to stop the reaction. Adjust the total volume to 40 mL with water, and obtain a sulfonium-containing ether compound (SE-3) in the form of an aqueous solution with a concentration of 131 g / L. By 1 H-NMR confirmed that a sulfonium group different from that of the raw material was generated after the reaction. The mass average molecular weight of SE-3 was 2,710.

[0142] <Synthesis example 4>

[0143] Into the reaction container, add 1.17 g of polyethylene glycol (molecular weight 600) terminal mesylate (Formula 4-1), 2 g of pure water, 1.04 g of 4-hydroxyphenyldimethylsulfonium methanesulfonate (Formula 2-1) (1.0 equivalent of reactive group amount relative to epoxy group), and 0.54 g of potassium carbonate in the order described. After raising the internal temperature to 70°C, stir at 70°C±5°C for 3 hours. Return the reaction solution to room temperature, add about 10 mL of pure water, and then add 2.2 g of 50% sulfuric acid to stop the reaction. Adjust the total volume to 30 mL with water, and obtain the sulfonium-containing ether compound (SE-4) in the form of an aqueous solution with a concentration of 74 g / L. By 1 H-NMR confirmed that a sulfonium group different from that of the raw material was generated after the reaction. The mass average molecular weight of SE-4 was 3,160.

[0144] <Synthesis example 5>

[0145] Into the reaction container, add 0.95 g of polyglycerol polyglycidyl ether (Formula 3-1: n+m=6), 4 g of acetonitrile, 0.54 g of methyl phenyl sulfide (Formula 2-2) (0.8 equivalents of reactive groups relative to epoxy groups), and 0.52 g of methanesulfonic acid in the order described. After raising the internal temperature to 80°C, stir at 80°C±5°C for 4 hours. Return the reaction solution to room temperature, and add 5 g of pure water and 2.35 g of 50% sulfuric acid to stop the reaction. Adjust the total volume to 50 mL with water, and obtain a sulfonium-containing ether compound (SE-5) in the form of an aqueous solution with a concentration of 30 g / L. It should be noted that SE-5 was confirmed to be a sulfonium compound by NMR. 1 In H-NMR (solvent: DMSO-d6), the peak derived from the aromatic ring that appeared at 7.27 to 7.31 ppm in the compound of formula 2-2 as the raw material appeared at 7.71 to 8.09 ppm. The mass average molecular weight of SE-5 was 7,020.

[0146] <Synthesis example 6>

[0147] Into the reaction container, add 1.39 g of sorbitol polyglycidyl ether (Formula 3-4), 4 g of acetonitrile, 0.81 g of methyl phenyl sulfide (Formula 2-2) (0.8 equivalents of reactive groups relative to epoxy groups), and 0.78 g of methanesulfonic acid in the order described. After raising the internal temperature to 80°C, stir at 80°C±5°C for 4 hours. Return the reaction solution to room temperature, and add 5 g of pure water and 2.35 g of 50% sulfuric acid to stop the reaction. Adjust the total volume to 50 mL with water, and obtain a sulfonium-containing ether compound (SE-6) in the form of an aqueous solution with a concentration of 44 g / L. It should be noted that through 1 H-NMR confirmed that SE-6 was a sulfonium compound. The mass average molecular weight of SE-6 was 5,360.

[0148] <Synthesis Example 7>

[0149] Into the reaction container, add 0.88 g of polyglycerol polyglycidyl ether (Formula 3-1: n+m=6), 4 g of acetonitrile, 0.57 g of 4-(methylthio)phenol (Formula 2-3) (0.8 equivalent of reactive groups relative to epoxy groups), and 0.49 g of methanesulfonic acid in the order described. After raising the internal temperature to 80°C, stir at 80°C±5°C for 4 hours. Return the reaction solution to room temperature, and add 5 g of pure water and 2.35 g of 50% sulfuric acid to stop the reaction. Adjust the total volume to 50 mL with water, and obtain a sulfonium-containing ether compound (SE-7) in the form of an aqueous solution with a concentration of 29 g / L. It should be noted that by 1 H-NMR confirmed that SE-7 was a sulfonium compound. The mass average molecular weight of SE-7 was 7,360.

[0150] <Synthesis example 8>

[0151] Into the reaction container, add 2.01 g of polyglycerol polyglycidyl ether (Formula 3-1: n+m=6), 7 g of acetonitrile, 1.28 g of 4-(methylthio)toluene (Formula 2-4) (0.8 equivalent of reactive groups relative to epoxy groups), and 1.11 g of methanesulfonic acid in the order described. After raising the internal temperature to 80°C, stir at 80°C±5°C for 4 hours. Return the reaction solution to room temperature, and add 5 g of pure water and 2.35 g of 50% sulfuric acid to stop the reaction. Adjust the total volume to 250 mL with water, and obtain a sulfonium-containing ether compound (SE-8) in the form of an aqueous solution with a concentration of 14 g / L. It should be noted that by 1 H-NMR confirmed that sulfonium groups were generated after the reaction. The mass average molecular weight of SE-8 was 6,360.

[0152] <Synthesis Example 9>

[0153] Into the reaction container, add 1.24 g of polyglycerol polyglycidyl ether (Formula 3-1: n+m=6), 5 g of acetonitrile, 0.81 g of 4-fluoromethylphenyl sulfide (Formula 2-5) (0.8 equivalent of reactive groups relative to epoxy groups), and 0.69 g of methanesulfonic acid in the order described. After the internal temperature is raised to 80°C, stir at 80°C±5°C for 4 hours. The reaction solution is returned to room temperature, and 5 g of pure water and 2.35 g of 50% sulfuric acid are added to stop the reaction. The total volume is adjusted to 100 mL with water, and a sulfonium-containing ether compound (SE-9) is obtained in the form of an aqueous solution with a concentration of 21 g / L. It should be noted that by 1 H-NMR confirmed that a sulfonium group was generated after the reaction. The mass average molecular weight of SE-9 was 6,520.

[0154] <Synthesis example 10>

[0155] Into the reaction container, add 2.94 g of polyglycerol polyglycidyl ether (Formula 3-1: n+m=6), 11 g of acetonitrile, 2.00 g of isopropyl sulfide (Formula 2-6) (0.8 equivalents of reactive groups relative to epoxy groups), and 1.62 g of methanesulfonic acid in the order described. After raising the internal temperature to 80°C, stir at 80°C±5°C for 4 hours. Return the reaction solution to room temperature, and add 5 g of pure water and 2.35 g of 50% sulfuric acid to stop the reaction. Adjust the total volume to 70 mL with water, and obtain a sulfonium-containing ether compound (SE-10) in the form of an aqueous solution with a concentration of 71 g / L. It should be noted that SE-10 was confirmed to be a sulfonium compound by NMR. 1 In H-NMR (solvent: DMSO-d6), the peak derived from the methyl group that appeared at 1.18 to 1.20 ppm in the compound of formula 2-6 as the raw material appeared at 1.45 to 1.48 ppm. The mass average molecular weight of SE-10 was 6,450.

[0156] <Synthesis Example 11>

[0157] Into the reaction container, add 2.98 g of polyglycerol polyglycidyl ether (Formula 3-1: n+m=6), 11 g of acetonitrile, 1.21 g of tetrahydrothiophene (Formula 2-7) (0.8 equivalents of reactive groups relative to epoxy groups), and 1.64 g of methanesulfonic acid in the order described. After raising the internal temperature to 80°C, stir at 80°C±5°C for 4 hours. Return the reaction solution to room temperature, and add 5 g of pure water and 2.35 g of 50% sulfuric acid to stop the reaction. Adjust the total volume to 40 mL with water, and obtain a sulfonium-containing ether compound (SE-11) in the form of an aqueous solution with a concentration of 105 g / L. It should be noted that by 1 H-NMR confirmed that sulfonium groups were generated after the reaction. The mass average molecular weight of SE-11 was 7,460.

[0158] 《Examples 1 to 11》

[0159] (Preparation of copper sulfate plating solution)

[0160] As a leveling agent for the plating solution, the sulfonium group-containing ether compounds SE-1 to SE-11 obtained in Synthesis Examples 1 to 11 were used, respectively, to prepare copper sulfate plating solutions of the following compositions according to the present invention.

[0161] <Copper sulfate plating solution composition>

[0162] ·Copper sulfate pentahydrate: 200g / L (Cu 2+ Concentration: 50g / L)

[0163] Sulfuric acid: 100g / L

[0164] Chloride ion: 40mg / L (Cl - concentration, added as hydrochloric acid)

[0165] Polyethylene glycol (molecular weight 6000) (surfactant): 500 mg / L

[0166] Bis(3-sulfopropyl sodium) disulfide (brightening agent): 1 mg / L (2 mg / L for Example 7 only)

[0167] ·SE-1 to SE-11 (leveling agent): concentrations are shown in Table 1 below

[0168] (Copper sulfate plating)

[0169] Resin substrates having blind holes with an opening diameter of φ120 μm and a depth of 75 μm and electroless copper plating were placed in the copper sulfate plating solution, and copper sulfate plating was performed under the following conditions.

[0170] <Copper sulfate plating conditions>

[0171] Current density: 1.5A / dm 2

[0172] Duration: 45 minutes

[0173] Bath volume: 500mL

[0174] ·Stirring: Aeration 1.5L / min

[0175] (Evaluation of hole filling properties)

[0176] The amount of dishing was measured for each substrate after the plating, and the hole filling property was evaluated. The evaluation results are shown in Table 1 described below together with the composition of each plating solution.

[0177] Comparative Examples 1 to 3

[0178] The same operation as in Examples 1 to 11 was carried out except that the following compounds were used as leveling agents, and the filling properties were evaluated. The evaluation results are shown in Table 1 described later together with the composition of each plating solution.

[0179] Comparative Examples 1 and 2: 4-Hydroxyphenyldimethylsulfonium methanesulfonate (Formula 2-1)

[0180] Comparative Example 3: Janus Green (JGB: a compound having the following structure generally used as a leveling agent for copper sulfate plating)

[0181] [Chemistry 11]

[0182]

[0183] [Table 1]

[0184] [Table 1 Leveling agents used in each example and evaluation results]

[0185]

[0186] *Symbol name (*1), structure (*2, *3) and molecular weight of the leveling agent used in each example and comparative example

[0187] *1 Examples 1 to 11 are ether compounds containing a sulfonium group, and Comparative Examples 1 to 2 are sulfonium compounds

[0188] *2The structure of the sulfonium group is represented by the formula of the organic sulfur compound used in the preparation.

[0189] *3 The structure of the ether part is represented by the formula of the ether compound used in the preparation

[0190] As shown in the results in Table 1, it can be seen that according to the plating solution containing a water-soluble metal salt (copper sulfate) and a sulfonium-containing ether compound according to the present invention, the substrate after plating can be made extremely flat. On the other hand, in Comparative Examples 1 and 2 using a sulfonium compound without an ether bond, the depressions on the substrate were almost not filled after plating. Even if the concentration of the leveling agent was increased as in Comparative Example 2, the flattening effect was not exerted, showing the importance of containing a sulfonium-containing ether compound as a leveling agent. In addition, the plating solutions of Examples 1 to 11 of the present invention all showed excellent flattening performance compared with the plating solution of Comparative Example 3 containing JGB as a general leveling agent.

Claims

1. A plating solution comprising: water-soluble metal salts; and Sulfonium-containing ether compounds.

2. The plating solution according to claim 1, wherein The sulfonium group-containing ether compound has a structure shown in Formula 1, [Chemistry 1] In formula 1, R 1 and R 2 are each independently a substituted or unsubstituted aliphatic or aromatic hydrocarbon group, R 1 With R 2 They may be bonded to each other to form a cyclic structure; E is an ether portion in the sulfonium group-containing ether compound, or a substituted or unsubstituted aliphatic or aromatic hydrocarbon group bonded to the ether portion.

3. The plating solution according to claim 2, wherein The sulfonium group-containing ether compound has the R 1 and the R 2 The reaction product of an organic sulfur compound having the groups shown and an ether compound having a reactive group.

4. The plating solution according to any one of claims 1 to 3, wherein The sulfonium group-containing ether compound is a compound having a mass average molecular weight of 2,000 to 10,000.

5. The plating solution according to any one of claims 1 to 4, wherein The metal salt is a salt containing copper.

6. The plating solution according to any one of claims 1 to 5, wherein The sulfonium group-containing ether compound is contained at a concentration of 0.1 mg / L to 1 g / L.