Non-aqueous electrolyte solution for lithium secondary battery and lithium secondary battery comprising same
By using non-aqueous electrolyte of imidazolium sulfonic acid compounds in lithium secondary batteries, a reinforced film is formed, which solves the problem of destruction of the electrode by the electrolyte decomposition product at high temperature, and achieves long life and high temperature stability of the lithium secondary battery sex.
Patent Information
- Application Number
- CN202380027989.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-30
- Publication Date
- 2024-11-08
Smart Images

Figure BDA0005044538330000021 
Figure BDA0005044538330000041 
Figure BDA0005044538330000051
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Korean Patent Application No. 10-2022-0039951, filed on March 30, 2022, the disclosure of which is incorporated herein by reference. Technical Field
[0003] The present invention relates to a non-aqueous electrolyte for a lithium secondary battery and a lithium secondary battery comprising the non-aqueous electrolyte. Background Art
[0004] Lithium secondary batteries are generally prepared by forming an electrode assembly by disposing a separator between a positive electrode containing a positive electrode active material formed of a lithium-containing transition metal oxide and a negative electrode containing a negative electrode active material capable of storing lithium ions, and placing the electrode assembly in a battery case, and then injecting a non-aqueous electrolyte that will become a lithium ion transmission medium therein, and then sealing the battery case.
[0005] Since lithium secondary batteries can be miniaturized and have high energy density and operating voltage, they are being used in various fields such as mobile devices, electronic products, and electric vehicles. As the application fields of lithium secondary batteries diversify, the required physical property conditions are gradually increasing, and in particular, it is necessary to develop lithium secondary batteries that can operate stably even under high temperature conditions and have long life characteristics.
[0006] When lithium secondary batteries are operated under high temperature conditions, PF6 - Anions may be thermally decomposed from lithium salts such as LiPF6 contained in the electrolyte to produce Lewis acids such as PF5, and react with moisture to produce HF. Decomposition products such as PF5 and HF not only destroy the film formed on the electrode surface, but also cause a decomposition reaction of the organic solvent. In addition, the decomposition products of the electrolyte may react with the decomposition products of the positive electrode active material to dissolve the transition metal ions, and the dissolved transition metal ions may be electrodeposited on the negative electrode, thereby destroying the film formed on the negative electrode surface.
[0007] If the electrolyte decomposition reaction continues to occur on the damaged membrane as described above, the battery performance further deteriorates, and therefore, there is a need to develop a secondary battery that can maintain excellent performance even under high temperature conditions.
[0008] [Prior art literature]
[0009] [Patent Document]
[0010] KR 10-2003-0061219A Summary of the invention
[0011] [Technical issues]
[0012] One aspect of the present invention provides a non-aqueous electrolyte and a lithium secondary battery comprising the non-aqueous electrolyte, wherein the non-aqueous electrolyte can remove electrolyte decomposition products and can form a reinforced film on an electrode by comprising an imidazolium sulfonic acid compound, and the lithium secondary battery exhibits long life characteristics even during high temperature operation due to comprising the non-aqueous electrolyte.
[0013] [Technical solution]
[0014] According to one aspect of the present invention, a non-aqueous electrolyte for a lithium secondary battery is provided, which comprises: a lithium salt; an organic solvent; and a compound represented by Formula 1.
[0015] [Formula 1]
[0016]
[0017] In formula 1,
[0018] R is for O - or OR1, wherein R1 is hydrogen or an alkyl group having 1 to 10 carbon atoms,
[0019] L1 is a direct bond; or an alkylene group having 1 to 30 carbon atoms,
[0020] L2 is an alkylene group having 1 to 10 carbon atoms.
[0021] According to another aspect of the present invention, a lithium secondary battery is provided, comprising: a positive electrode comprising a positive electrode active material; a negative electrode comprising a negative electrode active material; a separator disposed between the positive electrode and the negative electrode; and a non-aqueous electrolyte for the lithium secondary battery.
[0022] [Beneficial Effects]
[0023] In the structure of the compound represented by Formula 1 contained as an additive in the non-aqueous electrolyte of the present invention, the nitrogen atom of the cation portion can act as a Lewis base, thereby effectively removing the Lewis acid generated as an electrolyte decomposition product, and the film on the positive electrode or the negative electrode can be formed by the sulfonate group (-RSO3 - ) and propargyl groups (-CH2C≡CH), so when the non-aqueous electrolyte is used in a lithium secondary battery, a lithium secondary battery with improved high-temperature storage characteristics and the degree of self-discharge due to positive electrode dissolution can be achieved. DETAILED DESCRIPTION
[0024] Hereinafter, the present invention will be described in more detail.
[0025] Generally, the anions contained in the lithium salt (such as LiPF6) widely used in the electrolyte for lithium secondary batteries form decomposition products such as hydrogen fluoride (HF) and PF5 due to thermal decomposition or moisture. These decomposition products are acidic and deteriorate the membrane or electrode surface in the battery.
[0026] Due to the decomposition products of the electrolyte and the changes in the positive electrode structure caused by repeated charging and discharging, the transition metal in the positive electrode is easily dissolved into the electrolyte, and the dissolved transition metal will be redeposited on the positive electrode, increasing the resistance of the positive electrode. In addition, in the case where the dissolved transition metal moves to the negative electrode through the electrolyte, the dissolved transition metal is electrodeposited on the negative electrode and grows, causing an internal short circuit. As a result, the negative electrode self-discharges, thus becoming a cause of low voltage failure. In addition, since the dissolved transition metals destroy the solid electrolyte interface (SEI) film when they are electrodeposited on the negative electrode, they become the cause of additional electrolyte decomposition reactions, resulting in problems such as lithium ion consumption and increased resistance.
[0027] In addition, during the initial activation of the battery, a protective film is formed on the positive and negative electrodes by the electrolyte reaction, wherein, when the film becomes unstable due to the above reasons, the electrolyte undergoes additional decomposition during charge-discharge or high temperature exposure, thereby promoting battery degradation and generating gas.
[0028] Therefore, the present inventors have included a compound represented by the following formula 1 in a non-aqueous electrolyte, which contains a sulfonate group (-RSO3 - ) and propargyl groups (-CH2C≡CH), and can effectively strengthen the membrane. Sulfonate (-RSO3 - ) is reduced at the negative electrode while forming a polymeric structure and a LiSO3-like film. For the propargyl group (-CH2C≡CH), it is reduced to form a propargyl radical, and the formed radical forms a thin and dense film on the negative electrode surface by polymerization. In addition, since the compound represented by Formula 1 below contains a Lewis base functional group capable of removing Lewis acid decomposition products such as HF and PF5 generated during the operation of the lithium secondary battery, it has been confirmed that the non-aqueous electrolyte containing the compound represented by Formula 1 below has the effect of preventing battery degradation even under high temperature conditions above 40°C.
[0029] Hereinafter, each component constituting the present invention will be described in more detail.
[0030] Non-aqueous electrolyte
[0031] The present invention provides a non-aqueous electrolyte for a lithium secondary battery, which comprises: a lithium salt; an organic solvent; and a compound represented by Formula 1.
[0032] Hereinafter, each component will be described in detail.
[0033] (1) Compound represented by formula 1
[0034] The non-aqueous electrolyte solution of the present invention contains a compound represented by Formula 1 below.
[0035] [Formula 1]
[0036]
[0037] In formula 1,
[0038] R is for O - or OR1, wherein R1 is hydrogen or an alkyl group having 1 to 10 carbon atoms,
[0039] L1 is a direct bond; or an alkylene group having 1 to 30 carbon atoms,
[0040] L2 is an alkylene group having 1 to 10 carbon atoms.
[0041] The compound represented by Formula 1 has an effect of reinforcing a film on an electrode due to a structure containing a sulfonate group and a propargyl group.
[0042] Sulfonate (-RSO3 - ) can form a polymeric structure and a LiSO3-based film while being reduced at the negative electrode. In addition, by including a sulfonate group in the structure, the lowest unoccupied molecular orbital (LUMO) value of the compound of Formula 1 can be reduced, and the reducibility of the negative electrode can be further improved.
[0043] In addition, the propargyl group (—CH 2 C≡CH ) contained in the structure of Formula 1 is reduced to form a propargyl radical, and the formed radical can form a thin and dense film on the surface of the negative electrode through polymerization.
[0044] In addition, in the compound represented by Formula 1, nitrogen present in the imidazolium can act as a Lewis base. Therefore, since Lewis acids such as HF generated as electrolyte decomposition products can be easily removed, the problem of transition metal dissolution caused by Lewis acid attack on the positive electrode can be significantly prevented.
[0045] Therefore, since the non-aqueous electrolyte of the present invention uses the compound represented by Formula 1 as an additive, a lithium secondary battery having improved life performance as well as resistance reduction and gas reduction effects, particularly at high temperatures, can be obtained.
[0046] In one embodiment of the present invention, the compound represented by Formula 1 may be represented by the following Formula 1-1 or Formula 1-2.
[0047] [Formula 1-1]
[0048]
[0049] [Formula 1-2]
[0050]
[0051] In Formulae 1-1 and 1-2, R1, L1 and L2 are as defined in Formula 1.
[0052] Specifically, when the compound represented by Formula 1 of the present application is a compound having a zwitterionic structure as shown in Formula 1-1 (ie, a neutral molecule having an anion part and a cation part in its structure), the ionic conductivity can be further improved by the zwitterions.
[0053] In the case where the compound represented by Formula 1 of the present application has the structure of Formula 1-2, the nitrogen atom of the cation part in the structure may act as a Lewis base, thereby effectively scavenging Lewis acid generated as an electrolyte decomposition product.
[0054] In one embodiment of the present invention, L1 is -(CH2) n - represents, wherein n may be an integer from 1 to 20, may preferably be an integer from 2 to 10, and may more preferably be 2 or 3.
[0055] L2 is composed of -(CH2) m - represents, wherein m may be an integer from 1 to 10, may preferably be an integer from 1 to 3, and may more preferably be 1.
[0056] In one embodiment of the present invention, the compound represented by Formula 1 may be represented by the following Formula 1A or Formula 1B.
[0057] [Formula 1A]
[0058]
[0059] [Formula 1B]
[0060]
[0061] In one embodiment of the present invention, the amount of the compound represented by Formula 1 may account for 0.1% by weight or more, preferably 0.3% by weight or more, and more preferably 0.5% by weight or more of the total weight of the non-aqueous electrolyte. In this case, it is advantageous that it exhibits a significant effect of removing decomposition products and improving membrane durability.
[0062] In addition, the amount of the compound represented by Formula 1 may be less than 5 wt %, preferably less than 3 wt %, and more preferably less than 2 wt % of the total weight of the non-aqueous electrolyte. In this case, it is advantageous that by-product formation and side reactions caused by excessive additives can be prevented.
[0063] Most preferably, the amount of the compound represented by Formula 1 may account for 1 to 2 weight % of the total weight of the non-aqueous electrolyte.
[0064] (2) Additives
[0065] In order to prevent the electrolyte from decomposing in a high voltage environment and causing electrode disintegration, or to further improve low-temperature high-rate discharge characteristics, high-temperature stability, overcharge protection and battery expansion inhibition effect at high temperatures, the non-aqueous electrolyte of the present invention may optionally further include the following additives if necessary.
[0066] The additive can be at least one selected from the following: cyclic carbonate compounds, halogenated carbonate compounds, sultone compounds, sulfate compounds, phosphate compounds or phosphite compounds, borate compounds, nitrile compounds, benzene compounds, amine compounds, silane compounds and lithium salt compounds.
[0067] The cyclic carbonate-based compound may be at least one selected from vinylene carbonate (VC) or vinyl ethylene carbonate (VEC), and may specifically be vinylene carbonate.
[0068] The halogenated carbonate compound may be fluoroethylene carbonate (FEC).
[0069] The sultone compound is a material that can form a stable SEI film through a reduction reaction on the surface of the negative electrode, wherein the sultone compound can be at least one compound selected from 1,3-propane sultone (PS), 1,4-butane sultone, ethane sultone, 1,3-propene sultone (PRS), 1,4-butene sultone and 1-methyl-1,3-propene sultone, and can be specifically 1,3-propane sultone (PS).
[0070] The sulfate ester / salt compound is a material that can be electrolyzed on the surface of the negative electrode to form a stable SEI film that does not break even during high-temperature storage, wherein the sulfate ester / salt compound can be at least one selected from ethylene sulfate (Esa), trimethylene sulfate (TMS) or methyl trimethylene sulfate (MTMS).
[0071] The phosphate or phosphite compound may be at least one selected from the group consisting of lithium difluorobis(oxalato)phosphate, lithium difluorophosphate, tris(trimethylsilyl)phosphate, tris(trimethylsilyl)phosphite, tris(2,2,2-trifluoroethyl)phosphate and tris(trifluoroethyl)phosphite.
[0072] The borate ester compound may be lithium tetraphenylborate.
[0073] The nitrile compound can be at least one selected from succinonitrile (SN), adiponitrile (ADN), acetonitrile, propionitrile, butyronitrile, valeronitrile, octanonitrile, heptanenitrile, cyclopentanenitrile, cyclohexanenitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, benzyl cyanide, 2-fluorobenzene acetonitrile, 4-fluorobenzene acetonitrile, ethylene glycol bis(2-cyanoethyl) ether (ASA3), 1,3,6-hexanetrinitrile (HTCN), 1,4-dicyano-2-butene (DCB) and 1,2,3-tris(2-cyanoethyl)propane (TCEP).
[0074] The amine compound may be at least one selected from triethanolamine and ethylenediamine, and the silane compound may be tetravinylsilane.
[0075] The benzene compound may be at least one selected from monofluorobenzene, difluorobenzene, trifluorobenzene and tetrafluorobenzene.
[0076] The lithium salt compound is a compound different from the above-mentioned lithium salt contained in the non-aqueous electrolyte, wherein the lithium salt compound can be at least one compound selected from the following: lithium difluorophosphate (LiDFP; LiPO2F2), lithium bis(oxalate)borate (LiBOB; LiB(C2O4)2), lithium tetrafluoroborate (LiBF4) and lithium difluorobis(oxalate)phosphate (LiDFOP).
[0077] The non-aqueous electrolyte of one embodiment of the present invention may further include at least one additive selected from the group consisting of vinylene carbonate (VC), vinyl ethylene carbonate (VEC), fluoroethylene carbonate (FEC), 1,3-propane sultone (PS), 1,3-propylene sultone (PRS), ethylene sulfate (ESa), succinonitrile (SN), adiponitrile (ADN), ethylene glycol bis(2-cyanoethyl) ether (ASA3), 1,3,6-hexanetrinitrile (HTCN), 1,4-dicyano-2-butene (DCB), 1,2,3-tris(2-cyanoethyl)propane (TCEP), lithium difluoro(oxalato)borate (LiODFB), lithium tetrafluoroborate (LiBF4), lithium difluorobis(oxalato)phosphate (LiDFOP) and lithium difluorophosphate (LiDFP).
[0078] Preferably, the non-aqueous electrolyte may further include at least one additive selected from vinylene carbonate (VC), 1,3-propane sultone (PS), ethylene sulfate (ESa), and lithium difluorophosphate (LiDFP).
[0079] The amount of the additive may be 0.1 wt % to 10 wt %, preferably 0.3 wt % to 5 wt %, and more preferably 1 wt % to 3 wt % of the total weight of the non-aqueous electrolyte. When the amount of the additive is within the above range, there is an effect of suppressing side reactions by forming a film on the positive electrode and the negative electrode.
[0080] (3) Organic solvents
[0081] The non-aqueous electrolyte solution of the present invention contains an organic solvent.
[0082] Various organic solvents commonly used in lithium electrolytes can be used as the organic solvent without restriction. For example, the organic solvent can be a cyclic carbonate solvent, a linear carbonate solvent, a linear ester solvent, a cyclic ester solvent, a nitrile solvent or a mixture thereof, and can preferably include a mixture of at least two selected from a cyclic carbonate solvent, a linear carbonate solvent and a linear ester solvent, and can more preferably include a mixture of a cyclic carbonate solvent and a linear carbonate solvent.
[0083] As a high-viscosity organic solvent, the cyclic carbonate solvent can dissociate the lithium salt in the electrolyte well due to its high dielectric constant, wherein the cyclic carbonate solvent can be at least one selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate and vinylene carbonate, and can preferably include ethylene carbonate (EC) or propylene carbonate (PC).
[0084] In addition, the linear carbonate solvent is an organic solvent with low viscosity and low dielectric constant, wherein the linear carbonate solvent can be at least one selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate and ethyl propyl carbonate, and can preferably include ethyl methyl carbonate (EMC), dimethyl carbonate (DMC) or diethyl carbonate (DEC).
[0085] In order to prepare an electrolyte having high ion conductivity, it is favorable to use a mixture of a cyclic carbonate-based solvent and a linear carbonate-based solvent as the organic solvent.
[0086] The linear ester solvent may be at least one selected from methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, and butyl propionate, and may preferably be methyl propionate, ethyl propionate, or propyl propionate.
[0087] The cyclic ester solvent may be at least one selected from the group consisting of γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone.
[0088] The nitrile solvent may be at least one selected from succinonitrile, acetonitrile, propionitrile, butyronitrile, valeronitrile, octanonitrile, heptanenitrile, cyclopentanenitrile, cyclohexanenitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, benzyl cyanide, 2-fluorophenyl cyanide and 4-fluorophenyl cyanide, and succinonitrile may be preferred.
[0089] Unless otherwise specified, the remaining amount of the non-aqueous electrolyte excluding other components (eg, the compound represented by Formula 1, additives, and lithium salt) other than the organic solvent may be entirely the organic solvent.
[0090] (4) Lithium salt
[0091] The non-aqueous electrolyte of the present invention contains a lithium salt.
[0092] Any lithium salt commonly used in an electrolyte for a lithium secondary battery may be used as the lithium salt without limitation, and specifically, the lithium salt may include Li + as a cation, and may contain at least one selected from the following as an anion: F - , Cl - Br - ,I - 、NO3 - 、N(CN)2 - 、BF4 - 、ClO4 - , B 10 Cl 10 - 、AlCl4 - 、AlO4 - PF6 - CF3SO3 - 、CH3CO2 - CF3CO2 - 、AsF6 - 、SbF6 - 、CH3SO3 - 、(CF3CF2SO2)2N - 、(CF3SO2)2N - 、(FSO2)2N - 、BF2C2O4 - , BC4O8 - 、BF2C2O4CHF - PF4C2O4 - PF2C4O8 - PO2F2 - 、(CF3)2PF4 - 、(CF3)3PF3 - 、(CF3)4PF2 - 、(CF3)5PF - 、(CF3)6P - 、C4F9SO3 - CF3CF2SO3 - CF3CF2(CF3)2CO- 、(CF3SO2)2CH - CF3(CF2)7SO3 - and SCN - .
[0093] Specifically, the lithium salt can be at least one selected from LiPF6, LiClO4, LiBF4, LiN(FSO2)2(LiFSI), LiN(SO2CF3)2(LiTFSI), lithium bis(pentafluoroethanesulfonyl)imide (LiBETI), LiSO3CF3, LiPO2F2, lithium bis(oxalate)borate (LiBOB), lithium difluoro(oxalate)borate (LiFOB), lithium difluoro(bisoxalate)phosphate (LiDFOP), lithium tetrafluoro(oxalate)phosphate (LiTFOP) and lithium fluoro(difluoro)borate (LiFMDFB), and LiPF6 can be preferred.
[0094] In one embodiment of the present invention, the concentration of the lithium salt in the non-aqueous organic solution containing the lithium salt and the organic solvent may be in the range of 0.5 M to 4.0 M, particularly 0.5 M to 3.0 M, and more particularly 0.8 M to 2.0 M. When the concentration of the lithium salt is within the above range, sufficient electrolyte impregnation can be obtained by preventing excessive increases in viscosity and surface tension, while sufficiently ensuring the effects of improving low-temperature output and improving cycle characteristics.
[0095] Lithium secondary battery
[0096] Next, the lithium secondary battery of the present invention will be described.
[0097] The lithium secondary battery of the present invention comprises: a positive electrode comprising a positive electrode active material, a negative electrode comprising a negative electrode active material, a separator disposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte. In this case, the non-aqueous electrolyte is the non-aqueous electrolyte of the present invention described above. Since the non-aqueous electrolyte has been described above, its description will be omitted and other components will be described below.
[0098] (1) Positive electrode
[0099] The positive electrode of the present invention includes a positive electrode active material, and may be prepared by coating a positive electrode collector with a positive electrode slurry including the positive electrode active material, a binder, a conductive agent, and a solvent, and then drying and roll-pressing the coated positive electrode collector.
[0100] The positive electrode collector is not particularly limited as long as it has conductivity without causing adverse chemical changes in the battery, and for example, stainless steel; aluminum; nickel; titanium; sintered carbon; or aluminum or stainless steel surface-treated with one of carbon, nickel, titanium, silver, etc. can be used.
[0101] The positive electrode active material is a compound capable of reversibly inserting and extracting lithium. Among them, the positive electrode active material can be at least one selected from LCO (LiCoO2); LNO (LiNiO2); LMO (LiMnO2); LiMn2O4; LiCoPO4; LFP (LiFePO4); and lithium composite transition metal oxides containing nickel (Ni), cobalt (Co), and manganese (Mn).
[0102] The molar ratio of nickel in the positive electrode active material among the transition metals can be 60 mol% or more, preferably 70 mol% or more, and more preferably 80 mol% or more.
[0103] In one embodiment of the present invention, the lithium composite transition metal oxide can be a compound represented by Formula 2 below. That is, the positive electrode active material of the embodiment of the present invention may include the lithium composite transition metal oxide represented by Formula 2.
[0104] [Formula 2]
[0105] Li 1+x (Ni a Co b Mn c M d )O2
[0106] In Formula 2,
[0107] M is at least one selected from tungsten (W), copper (Cu), iron (Fe), vanadium (V), chromium (Cr), titanium (Ti), zirconium (Zr), zinc (Zn), aluminum (Al), indium (In), tantalum (Ta), yttrium (Y), lanthanum (La), strontium (Sr), gallium (Ga), scandium (Sc), gadolinium (Gd), samarium (Sm), calcium (Ca), cerium (Ce), niobium (Nb), magnesium (Mg), boron (B), and molybdenum (Mo), and
[0108] 1 + x, a, b, c, and d are the atomic fractions of each independent element,
[0109] wherein, -0.2 ≤ x ≤ 0.2, 0.6 ≤ a < 1, 0 < b ≤ 0.3, 0 < c ≤ 0.3, 0 ≤ d ≤ 0.1, and a + b + c + d = 1.
[0110] 1 + x represents the molar ratio of lithium in the lithium composite transition metal oxide. Among them, x can satisfy -0.1 ≤ x ≤ 0.2 or 0 ≤ x ≤ 0.2. When the molar ratio of lithium satisfies the above range, the crystal structure of the lithium composite transition metal oxide can be stably formed.
[0111] a represents the molar ratio of nickel among all metals other than lithium in the lithium composite transition metal oxide, where a can satisfy 0.70 ≤ a < 1, 0.80 ≤ a < 1, or 0.85 ≤ a < 1. When the molar ratio of nickel satisfies the above ranges, high energy density can be exhibited, and thus high capacity can be achieved.
[0112] b represents the molar ratio of cobalt among all metals other than lithium in the lithium composite transition metal oxide, where b can satisfy 0 < b ≤ 0.20, 0 < b ≤ 0.15, or 0 < b ≤ 0.10. When the molar ratio of cobalt satisfies the above ranges, good resistance characteristics and output characteristics can be achieved.
[0113] c represents the molar ratio of manganese among all metals other than lithium in the lithium composite transition metal oxide, where c can satisfy 0 < c ≤ 0.20, 0 < c ≤ 0.15, or 0 < c ≤ 0.10. When the molar ratio of manganese satisfies the above ranges, the structural stability of the positive electrode active material is excellent.
[0114] In one embodiment of the present invention, the lithium composite transition metal oxide may contain at least one doping element selected from W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo, and Al may preferably be contained as the doping element. In other words, d represents the molar ratio of the doping element among all metals other than lithium in the lithium composite transition metal oxide, which can satisfy 0 < d ≤ 0.10, 0 < d ≤ 0.08, or 0 < d ≤ 0.05.
[0115] Preferably, a, b, c, and d in Formula 2 can respectively satisfy 0.70 ≤ a < 1, 0 < b ≤ 0.2, 0 < c ≤ 0.2, and 0 ≤ d ≤ 0.1.
[0116] The content of the positive electrode active material may account for 80% to 99% by weight, specifically 90% to 99% by weight, of the total weight of the solid components in the positive electrode paste. When the amount of the positive electrode active material is 80% by weight or less, the capacity may decrease due to the reduction in energy density.
[0117] The binder is a component that helps the adhesion between the active material and the conductive agent and the adhesion to the current collector. Among them, the addition amount of the binder can generally be 1% to 30% by weight of the total weight of the solid components in the positive electrode paste. Examples of the binder can be polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber, fluororubber, or various copolymers thereof.
[0118] In addition, the conductive agent is a material that provides conductivity without causing adverse chemical changes in the battery, wherein the conductive agent may be added in an amount of 0.5 wt % to 20 wt % of the total weight of the solid components in the positive electrode slurry.
[0119] For example, the conductive agent can be selected from conductive materials such as: carbon black, such as acetylene black, Ketjen black, channel black, furnace black, lamp black and thermal black; graphite powder, such as natural graphite, artificial graphite, carbon nanotubes and graphite; conductive fibers, such as carbon fibers and metal fibers; conductive powders, such as fluorocarbon powder, aluminum powder and nickel powder; conductive whiskers, such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides, such as titanium oxide; and polyphenylene derivatives.
[0120] In addition, the solvent of the positive electrode slurry may include an organic solvent such as N-methyl-2-pyrrolidone (NMP), and the amount used may be such that the desired viscosity is obtained when the positive electrode active material, the binder and the conductive agent are included. For example, the content of the solvent may be such that the concentration of the solid component in the positive electrode slurry containing the positive electrode active material, the binder and the conductive agent is 40 wt % to 90 wt %, preferably 50 wt % to 80 wt %.
[0121] (2) Negative electrode
[0122] The negative electrode of the present invention includes a negative electrode active material, and may be prepared by coating a negative electrode collector with a negative electrode slurry including the negative electrode active material, a binder, a conductive agent, and a solvent, and then drying and roll-pressing the coated negative electrode collector.
[0123] The thickness of the negative electrode collector is generally 3 μm to 500 μm. The negative electrode collector is not particularly limited as long as it has high conductivity without causing adverse chemical changes in the battery, and for example, copper; stainless steel; aluminum; nickel; titanium; sintered carbon; copper or stainless steel surface-treated with one of carbon, nickel, titanium, silver, etc.; or aluminum-cadmium alloy. In addition, similar to the positive electrode collector, the negative electrode collector may have fine surface irregularities to improve the bonding strength with the negative electrode active material, and the negative electrode collector may be used in various shapes, such as films, sheets, foils, nets, porous bodies, foams, non-woven fabrics, etc.
[0124] In addition, the negative electrode active material may include at least one selected from a carbon material capable of reversibly inserting / deinserting lithium ions; a metal or an alloy of lithium and the metal; a metal composite oxide; a material that can be doped and dedoped with lithium; lithium metal; and a transition metal oxide.
[0125] As a carbon material capable of reversibly embedding / de-embedding lithium ions, a carbon-based negative electrode active material commonly used for lithium ion secondary batteries can be used without particular limitation, and as a typical example, crystalline carbon, amorphous carbon or both thereof can be used. An example of crystalline carbon can be graphite, such as natural graphite or artificial graphite in an irregular, planar, flaky, spherical or fibrous form, and an example of amorphous carbon can be soft carbon (low temperature sintered carbon) or hard carbon, mesophase pitch carbide and fired coke.
[0126] As the metal or the alloy of lithium and the metal, a metal selected from the group consisting of copper (Cu), nickel (Ni), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), francium (Fr), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), silicon (Si), antimony (Sb), lead (Pb), indium (In), zinc (Zn), barium (Ba), radium (Ra), germanium (Ge), aluminum (Al) and tin (Sn), or an alloy of lithium and the above metals can be used.
[0127] As the metal composite oxide, at least one selected from the group consisting of PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, Bi2O5, Li x Fe2O3(0≤x≤1), Li x WO2(0≤x≤1) and Sn x Me 1-x Me' y O z (Me: Mn, Fe, Pb or Ge; Me': Al, B, phosphorus (P), Si, elements of Groups I, II and III of the periodic table, or halogen; 0 <x≤1;1≤y≤3;1≤z≤8)。
[0128] Materials that can be doped and dedoped with lithium may include Si, SiO x(0 < x < 2), Si-Y alloy (where Y is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Si), Sn, SnO2, and Sn-Y (where Y is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Sn). A mixture of SiO2 and at least one of them can also be used. Element Y can be selected from Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.
[0129] Examples of transition metal oxides can be lithium-containing titanium composite oxide (LTO), vanadium oxide, and lithium vanadium oxide.
[0130] In one embodiment of the present invention, the negative electrode active material can be a mixture of a carbon-based material and a silicon-based material, and preferably can be a mixture of graphite and SiO.
[0131] The content of the negative electrode active material can account for 80% to 99% by weight of the total weight of the solid components in the negative electrode slurry.
[0132] The binder is a component that helps the adhesion between the conductive agent, the active material, and the current collector. Among them, the addition amount of the binder usually accounts for 1% to 30% by weight of the total weight of the solid content in the negative electrode slurry. Examples of the binder can be polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber, fluororubber, or various copolymers thereof.
[0133] The conductive agent is a component for further improving the conductivity of the negative electrode active material, wherein the conductive agent may be added in an amount of 1 to 20 weight percent of the total weight of the solid components in the negative electrode slurry. Any conductive agent may be used without particular limitation as long as it has conductivity and does not cause adverse chemical changes in the battery, such as the following conductive materials: carbon black, such as acetylene black, ketjen black, channel black, furnace black, lamp black, or thermal carbon black; graphite powder, such as natural graphite, artificial graphite, carbon nanotubes, or graphite having a developed crystal structure; conductive fibers, such as carbon fibers or metal fibers; conductive powders, such as fluorocarbon powders, aluminum powders, or nickel powders; conductive whiskers, such as zinc oxide whiskers or potassium titanate whiskers; conductive metal oxides, such as titanium oxide; or polyphenylene derivatives.
[0134] The solvent of the negative electrode slurry may include water; or an organic solvent such as NMP and alcohols, and the amount used may be such that the desired viscosity is obtained when the negative electrode active material, the binder and the conductive agent are included. For example, the content of the solvent may be such that the concentration of the solid component in the slurry containing the negative electrode active material, the binder and the conductive agent is 30 wt % to 80 wt %, preferably 40 wt % to 70 wt %.
[0135] (3) Diaphragm
[0136] The lithium secondary battery of the present invention includes a separator between a positive electrode and a negative electrode.
[0137] The separator separates the negative electrode from the positive electrode and provides a migration path for lithium ions, wherein any separator can be used without particular limitation as long as it is commonly used as a separator in lithium secondary batteries, and in particular, a separator having high moisture retention ability for the electrolyte and excellent safety and low resistance to the transmission of electrolyte ions can be used.
[0138] Specifically, a porous polymer film, for example, a porous polymer film prepared from a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure having two or more layers thereof can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric formed of a high melting point glass fiber or a polyethylene terephthalate fiber can be used. In addition, a coated diaphragm containing a ceramic component or a polymer material can be used to ensure heat resistance or mechanical strength, and a diaphragm having a single-layer or multi-layer structure can be used.
[0139] The lithium secondary battery of the present invention as described above can be applied to portable devices such as mobile phones, notebook computers, and digital cameras; and electric vehicles such as hybrid electric vehicles (HEVs).
[0140] Therefore, according to another embodiment of the present invention, a battery module including the above-mentioned lithium secondary battery as a unit cell and a battery pack including the battery module are provided.
[0141] The battery module or battery pack can be used as a power source for at least one of the following medium to large devices: power tools; electric vehicles, including electric vehicles (EV), hybrid electric vehicles (HEV) and plug-in hybrid electric vehicles (PHEV); or power storage systems.
[0142] The shape of the lithium secondary battery of the present invention is not particularly limited, but a cylindrical type using a can, a prismatic type, a pouch type, or a coin type may be used.
[0143] The lithium secondary battery of the present invention can be used not only as a battery cell used as a power source for small-sized devices but also as a unit cell in a medium or large-sized battery module including a plurality of battery cells.
[0144] Hereinafter, the present invention will be described in detail according to specific embodiments.
[0145] <Example: Preparation of lithium secondary battery>
[0146] Example 1
[0147] (Preparation of non-aqueous electrolyte)
[0148] Ethylene carbonate (EC): dimethyl carbonate (DMC) was mixed in a volume ratio of 30:70, and then LiPF6 was dissolved so that the concentration of LiPF6 was 1.2 M, thereby preparing a non-aqueous organic solution. A 100 wt % non-aqueous electrolyte was prepared as follows: 2 wt % of the compound represented by Formula 1A, 2 wt % of vinylene carbonate (VC) and the remainder of the non-aqueous organic solution were mixed.
[0149] (Preparation of lithium secondary battery)
[0150] As the positive electrode active material, Li(Ni 0.8 Co 0.1 Mn 0.1 )O2, a conductive agent (carbon black) and a binder (polyvinylidene fluoride) were added to N-methyl-2-pyrrolidone (NMP) at a weight ratio of 97.5:1:1.5 to prepare a positive electrode slurry (solid content: 60 wt%). A 15 μm thick aluminum (Al) film as a positive electrode current collector was coated with the positive electrode slurry, dried and then roll-pressed to prepare a positive electrode.
[0151] The negative electrode active material (composed of 96 wt % graphite and 4 wt % SiO), a binder (SBR-CMC) and a conductive agent (carbon black) were added to water as a solvent at a weight ratio of 95:3.5:1.5 to prepare a negative electrode slurry (solid content: 60 wt %). A 6 μm thick copper (Cu) film as a negative electrode current collector was coated with the negative electrode slurry, dried and then rolled to prepare a negative electrode.
[0152] The positive electrode, the polyolefin-based porous separator coated with inorganic particles (Al2O3), and the negative electrode were sequentially stacked to prepare an electrode assembly.
[0153] The prepared electrode assembly was housed in a cylindrical battery case, and the non-aqueous electrolyte prepared above was injected therein, thereby preparing a lithium secondary battery.
[0154] Example 2
[0155] A lithium secondary battery was prepared in the same manner as in Example 1, except that the amount of the compound represented by Formula 1A was changed to 1 wt % during the preparation of the non-aqueous electrolyte.
[0156] Example 3
[0157] A lithium secondary battery was prepared in the same manner as in Example 1, except that during the preparation of the nonaqueous electrolyte, the amount of the compound represented by Formula 1A was changed to 1 wt %, and 1 wt % of 1,3-propane sultone (PS) was further added.
[0158] Example 4
[0159] A lithium secondary battery was prepared in the same manner as in Example 1, except that the amount of the compound represented by Formula 1A was changed to 0.3 wt % during the preparation of the non-aqueous electrolyte.
[0160] Example 5
[0161] A lithium secondary battery was prepared in the same manner as in Example 1, except that, in the process of preparing the non-aqueous electrolyte, the compound represented by Formula 1B was used instead of the compound represented by Formula 1A.
[0162] Example 6
[0163] A lithium secondary battery was prepared in the same manner as in Example 5, except that the amount of the compound represented by Formula 1B was changed to 1 wt % during the preparation of the non-aqueous electrolyte.
[0164] Example 7
[0165] A lithium secondary battery was prepared in the same manner as in Example 5, except that during the preparation of the nonaqueous electrolyte, the amount of the compound represented by Formula 1B was changed to 1 wt %, and 1 wt % of 1,3-propane sultone (PS) was further added.
[0166] Example 8
[0167] A lithium secondary battery was prepared in the same manner as in Example 5, except that the amount of the compound represented by Formula 1B was changed to 0.3 wt % during the preparation of the non-aqueous electrolyte.
[0168] Comparative Example 1
[0169] A lithium secondary battery was prepared in the same manner as in Example 1, except that the compound represented by Formula 1A was not added during the preparation of the non-aqueous electrolyte.
[0170] Comparative Example 2
[0171] A lithium secondary battery was prepared in the same manner as in Example 1, except that, during the preparation of the non-aqueous electrolyte, the compound represented by Formula 1A was not added, and 1 wt % of 1,3-propane sultone (PS) was further added.
[0172] Comparative Example 3
[0173] A lithium secondary battery was prepared in the same manner as in Example 3, except that in the preparation of the nonaqueous electrolyte, the compound represented by the following Formula C was used instead of the compound represented by Formula 1A and the amount thereof was changed to 0.3 wt %.
[0174] [Formula C]
[0175]
[0176] Comparative Example 4
[0177] A lithium secondary battery was prepared in the same manner as in Example 1, except that in the preparation of the nonaqueous electrolyte, a compound represented by the following Formula D was used instead of the compound represented by Formula 1A and the amount thereof was changed to 2 wt %.
[0178] [Formula D]
[0179]
[0180] <Test example: battery performance evaluation>
[0181] Test Example 1. Measurement of capacity and resistance after high temperature storage
[0182] After the lithium secondary batteries prepared in the embodiments and comparative examples were subjected to a formation process, the lithium secondary batteries were charged with a constant current / constant voltage (CC / CV) charge (0.05C cut-off) to 4.25 V at a 0.5C rate at 25°C, and discharged with a constant current (CC) to 2.50 V at a 0.5C rate, and then the initial discharge capacity and initial resistance were measured.
[0183] Thereafter, each battery was fully charged to 100% of the state of charge (SOC) under the same conditions and stored at high temperature (55°C) for 8 weeks. Thereafter, after each battery was transferred to a charger and discharger at room temperature (25°C), the capacity and resistance were measured again, and the capacity retention rate and resistance increase rate were calculated by the following equations 1 and 2, and the results are shown in the following Table 1.
[0184] Equation 1: Capacity retention rate (%) = (discharge capacity after high temperature storage / initial discharge capacity) × 100
[0185] Equation 2: Resistance increase rate (%) = {(resistance after high temperature storage - initial resistance) / initial resistance} × 100
[0186] Test Example 2. Measurement of gas generation after high temperature storage
[0187] After the lithium secondary battery prepared in the embodiment and the comparative example is subjected to the formation process, the lithium secondary battery is charged to 4.25V at a rate of 0.5C under constant current / constant voltage conditions (0.05C cut-off) at 25°C, so that the lithium secondary battery is fully charged to 100% SOC. After the fully charged battery is stored at 72°C for 4 weeks, it is transferred to a charger and discharger at room temperature (25°C), and then the gas collected in the cylindrical tank is analyzed using a gas chromatography-thermal conductivity detector (GC-TCD), and the gas generation measured in Comparative Example 1 is set to 100%, and the relative gas generation of each battery is calculated and shown in Table 1 below.
[0188] Test Example 3. High Temperature Life Evaluation
[0189] After the lithium secondary batteries prepared in the examples and comparative examples were subjected to a formation process, they were charged to 4.25 V at 40° C. at a constant current / constant voltage (CC / CV) rate of 0.3C (0.05C cutoff) and discharged to 2.85 V at a constant current (CC) rate of 0.5C.
[0190] Performing one charge / discharge was defined as one cycle, and after repeating the same charge / discharge 250 times, the resistance increase rate (DCIR increase) was measured by the following Equation 3. The measurement results are shown in Table 1 below.
[0191] Equation 3: Resistance increase rate (%) = {(resistance after 250 cycles - resistance after one cycle) / resistance after one cycle} × 100
[0192] Test Example 4. Thermal Safety Assessment
[0193] After the lithium secondary batteries prepared in the examples and comparative examples were subjected to the formation process, the lithium secondary batteries were charged to 4.25V at a rate of 0.5C under constant current / constant voltage conditions (0.05C cutoff) at 25°C, so that the lithium secondary batteries were fully charged to 100% SOC. The following hot box evaluation test was performed: the fully charged battery was heated to 130°C at a heating rate of 5°C / min, and then left to stand for 30 minutes to confirm whether the battery caught fire.
[0194] The results are shown in Table 1 below, where the battery that did not catch fire was indicated as "pass", and the battery that caught fire was indicated as "failure".
[0195] [Table 1]
[0196]
[0197] According to the results of Table 1, when the compound represented by Formula 1 is used as the electrolyte additive of the lithium secondary battery of the present invention, it can be confirmed that the high temperature durability is improved compared with Comparative Examples 1 and 2 in which the compound represented by Formula 1 is not used and Comparative Example 3 in which the compound represented by Formula C having a structure similar to Formula 1 but not containing a sulfonate group is used, and not only the gas generation amount is reduced, but also the resistance characteristics are improved. For Comparative Example 4, since Formula D does not contain a propargyl group that can form a SEI film on the negative electrode by polymerization with vinylene carbonate (VC), it can be confirmed that the high temperature durability is reduced.
[0198] In particular, it was confirmed that the best results were obtained in all evaluation items when the amount of the compound represented by Formula 1 was 1 wt% or more, and most preferably 2 wt% or more. By comparing Example 2 with Example 3 and Example 6 with Example 7, it was confirmed that, when the same amount was used, further addition of PS showed better results, but by comparing Example 1 with Example 3 and Example 5 with Example 7, it was confirmed that the increase in the amount of the compound represented by Formula 1 was more advantageous than the use of PS.
Claims
1. A non-aqueous electrolyte for a lithium secondary battery, the non-aqueous electrolyte comprising a lithium salt; an organic solvent; and a compound represented by Formula 1: [Formula 1] Wherein, In Formula 1, R is for O - or OR1, wherein R1 is hydrogen or an alkyl group having 1 to 10 carbon atoms, L1 is a direct bond; or an alkylene group having 1 to 30 carbon atoms, and L2 is an alkylene group having 1 to 10 carbon atoms.
2. The non-aqueous electrolyte for a lithium secondary battery according to claim 1, Wherein, The compound represented by Formula 1 is represented by Formula 1-1 or Formula 1-2: [Formula 1-1] [Formula 1-2] Wherein, in Formulas 1-1 and 1-2, R1, L1 and L2 are as defined in Formula 1.
3. The non-aqueous electrolyte for a lithium secondary battery according to claim 1, Wherein, L1 is composed of -(CH 2 ) n - represents, wherein n is an integer from 1 to 20.
4. The non-aqueous electrolyte for a lithium secondary battery according to claim 1, Wherein, L2 is composed of -(CH 2 ) m - represents, wherein m is an integer from 1 to 10.
5. The non-aqueous electrolyte for a lithium secondary battery according to claim 1, Wherein, The amount of the compound represented by Formula 1 is 0.1% by weight to 5% by weight of the total weight of the non-aqueous electrolyte.
6. The non-aqueous electrolyte for a lithium secondary battery according to claim 1, Wherein, The amount of the compound represented by Formula 1 is 0.5% by weight to 5% by weight of the total weight of the non-aqueous electrolyte.
7. The non-aqueous electrolyte for a lithium secondary battery according to claim 1, which further comprises at least one additive selected from vinylene carbonate, 1,3-propane sultone, ethylene sulfite and lithium difluorophosphate.
8. The non-aqueous electrolyte for a lithium secondary battery according to claim 1, Wherein, The organic solvent comprises a mixture of at least two selected from cyclic carbonate solvents, linear carbonate solvents and linear ester solvents.
9. A lithium secondary battery, comprising: A positive electrode comprising a positive electrode active material; a negative electrode comprising a negative electrode active material; a separator disposed between the positive electrode and the negative electrode; and the non-aqueous electrolyte according to claim 1.
10. The lithium secondary battery according to claim 9, Wherein, The positive electrode active material comprises a lithium composite transition metal oxide represented by Formula 2: [Formula 2] Li 1+x (Ni a Co b Mr c M d )O 2 Wherein, in Formula 2, M is at least one selected from tungsten (W), copper (Cu), iron (Fe), vanadium (V), chromium (Cr), titanium (Ti), zirconium (Zr), zinc (Zn), aluminum (Al), indium (In), tantalum (Ta), yttrium (Y), lanthanum (La), strontium (Sr), gallium (Ga), scandium (Sc), gadolinium (Gd), samarium (Sm), calcium (Ca), cerium (Ce), niobium (Nb), magnesium (Mg), boron (B) and molybdenum (Mo), and 1+x, a, b, c and d are atomic fractions of respective independent elements, Wherein, -0.2 ≤ x ≤ 0.2, 0.6 ≤ a < 1, 0 < b ≤ 0.3, 0 < c ≤ 0.3, 0 ≤ d ≤ 0.1, and a + b + c + d = 1.
11. The lithium secondary battery according to claim 10, Wherein, a, b, c and d in Formula 2 respectively satisfy 0.70 ≤ a < 1, 0 < b ≤ 0.2, 0 < c ≤ 0.2 and 0 ≤ d ≤ 0.1.