Preparation method and application of bismuth sulfide nanocomposite for radioiodine capture

Through the amorphous structure and uniform carbon dispersion of bismuth sulfide nanocomposites, combined with hydrothermal reaction and sodium sulfide solution concentration adjustment, the problem of the degradation of the adsorption capacity of radioactive iodine capture materials in high temperature, high humidity and radiation environments in the prior art is solved. , realizes efficient iodine capture and stable storage.

CN118925652APending Publication Date: 2024-11-12NANJING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411224433.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing radioactive iodine capture materials show a reduced adsorption capacity in high temperature, high humidity and radiation environments, and iodine is easy to escape from the adsorbent, making it difficult to achieve effective iodine capture and stable storage.

Method used

Bismuth sulfide nanocomposite material is used to adjust the sulfur vacancy and carbon uniformly disperse to form amorphous structure and crystal structure bismuth sulfide material, improve the physical and chemical capture ability of adsorbents, and adjust sulfur through hydrothermal reaction and sodium sulfide solution concentration. The number of vacancy places enhances the iodine adsorption capacity and stability of the adsorbent.

Benefits of technology

It realizes efficient iodine capture in high temperature, high humidity and radiation environments, improves the iodine adsorption capacity and chemical adsorption ratio of the adsorbent, ensures stable constraints of iodine and prevents escape, and improves the mechanical properties and durability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925652A_ABST
    Figure CN118925652A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of adsorbents, and discloses a preparation method and application of a bismuth sulfide nano composite material for capturing radioactive iodine, the main body of the bismuth sulfide nano composite material is bismuth sulfide with an amorphous structure and a crystal structure, and carbon is uniformly dispersed in the bismuth sulfide. The iodine trapping agent obtained by the invention has excellent iodine adsorption and glass curing properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of adsorbents, and in particular to a preparation method and application of a bismuth sulfide nanocomposite material for capturing radioactive iodine. Background Art

[0002] Nuclear energy is a clean and efficient energy source, and therefore an important transition technology to effectively deal with the depletion of fossil energy and global warming. However, the radionuclides released during nuclear waste treatment and nuclear accidents seriously hinder the development of nuclear energy. A large amount of volatile radioactive iodine is released during the acid dissolution step of spent fuel reprocessing. Among them, 129 The half-life of I is very long, 1.57×10 7 Years, it is easy to accumulate in the environment and human body and cause long-term effects. 131 I has a short half-life of only 8.02 days, but its mobility and specific activity are high, so it can quickly diffuse into the environment and affect the metabolic processes of organisms. Therefore, it is urgent to develop effective methods and materials for the capture and stable storage of radioactive iodine.

[0003] To meet the challenge of capturing gaseous radioactive iodine, some materials such as silver-based zeolites, activated carbon, and aerogels have been developed and applied in industrial production. However, they have disadvantages such as low iodine capture capacity, high cost, easy desorption, and high biological toxicity. The development of high-performance iodine adsorbents is urgent. So far, researchers have explored and prepared a variety of porous materials, such as metal organic frameworks (MOFs), covalent organic polymers (COFs), and porous aromatic frameworks (PAFs), as adsorbents for solid-phase adsorption of iodine. The high specific surface area, adjustable pore structure, and good chemical stability significantly enhance the gaseous iodine capture performance. However, in addition to their relatively complex synthesis and high cost, the structure of the materials is easily destroyed under high temperature, high humidity, and irradiation environments, resulting in a decrease in adsorption capacity. Therefore, it is particularly important to develop adsorbent materials that can efficiently capture gaseous radioactive iodine under practical conditions (high temperature, high humidity, and radiation exposure).

[0004] Bismuth-based materials have the advantages of high adsorption performance, strong stability, good radiation resistance, strong renewability and environmental protection in the adsorption of radioactive iodine, so they have important application potential in the fields of nuclear waste treatment and nuclear accident post-processing. However, under actual iodine removal conditions, they still face the problem of low adsorption capacity and easy escape of iodine from Bi-based adsorbents. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a method for preparing a bismuth sulfide nanocomposite material for radioactive iodine capture and its application. The adsorbent obtained by the present invention has outstanding iodine adsorption and glass solidification properties.

[0006] The invention provides a bismuth sulfide nanocomposite material for capturing radioactive iodine. The main body of the bismuth sulfide nanocomposite material is bismuth sulfide having both an amorphous structure and a crystal structure, and carbon is uniformly dispersed in the bismuth sulfide.

[0007] Furthermore, the content of sulfur vacancies in the bismuth sulfide nanocomposite material is 29%-44%.

[0008] Furthermore, the specific surface area of ​​the bismuth sulfide nanocomposite material is 40 m 2 / g-54m 2 / g.

[0009] The present invention also provides a method for preparing the bismuth sulfide nanocomposite material, which comprises: adding CAU-17 material to a sodium sulfide solution, performing a hydrothermal reaction, performing solid-liquid separation, washing the separated solid product, and drying the separated solid product to obtain a bismuth sulfide nanocomposite material (AC-Bi2S3-x@C).

[0010] Furthermore, the molar concentration of the sodium sulfide solution is 0.1M-0.3M.

[0011] Furthermore, the mass concentration of the CAU-17 material in the sodium sulfide solution is 100 mg / 30 mL.

[0012] Furthermore, the preparation method of the sodium sulfide solution comprises dissolving sodium sulfide nonahydrate in deionized water.

[0013] Furthermore, the temperature of the hydrothermal reaction is 80°C-100°C, and the time of the hydrothermal reaction is 23h-25h.

[0014] Furthermore, the specific method of washing includes washing with deionized water and ethanol in sequence for at least 3 times.

[0015] Furthermore, the drying temperature is 50°C-70°C.

[0016] It should be understood by those skilled in the art that drying is to remove the deionized water after washing, and therefore, the drying time can be set according to actual conditions.

[0017] The invention also provides application of the bismuth sulfide nanocomposite material in adsorbing iodide ions.

[0018] The embodiments of the present invention have the following technical effects: 1. In the present invention, firstly, by adjusting the sulfur vacancies, not only the ability of the adsorbent to capture iodine ions physically can be improved, but also the ability of the adsorbent to capture iodine ions chemically can be improved. On this basis, first, the amorphous structure can provide a channel for the rapid diffusion of iodine molecules into the adsorbent structure, thereby improving the adsorption equilibrium speed; second, more surface defects and active sites in the amorphous structure make its surface have higher adsorption activity, which can more effectively adsorb gaseous molecules; third, the amorphous structure enhances the charge transfer between sulfur vacancies and iodine molecules, thereby improving the iodine adsorption capacity of the adsorbent and the proportion of chemical adsorption in the iodine capture process; fourth, the amorphous structure can enhance the bonding force between glass particles, help to form a dense glass structure, improve the mechanical properties and durability of the glass after solidification, and also prevent iodine ions from escaping from the adsorbent. In addition, the uniformly dispersed carbon in the bismuth sulfide nanocomposite material is conducive to improving the stability of the overall structure of the adsorbent, thereby ensuring the adsorption capacity of the adsorbent.

[0019] 2. In the present invention, in order to further improve the iodine ion capture capability of the bismuth sulfide nanocomposite material, the number of sulfur vacancies is further adjusted by adjusting the molar concentration of the sodium sulfide solution.

[0020] 3. The adsorbent obtained by the present invention has outstanding iodine adsorption and glass solidification properties, which can not only adsorb trace iodine, but also ensure that the adsorbed iodine ions can be stably bound in the adsorbent to prevent the escape of iodine. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 It is a microscopic picture provided by the embodiments of the present invention and the comparative examples, Figure 1 a is the TEM image of Example 1, Figure 1 b1 is the HRTEM image of Example 1, Figure 1 b2 is the lattice line scanning analysis diagram of Example 1, Figure 1 b3 is the electron diffraction pattern of Example 1, Figure 1 c1 is a microscopic image of Example 1, Figure 1 c2 is the distribution diagram of Bi element in Example 1, Figure 1 c3 is the S element distribution diagram in Example 1, Figure 1 c4 in is the C element distribution diagram in Example 1, Figure 1 d is the TEM image of comparative example 1, Figure 1 e1 is the HRTEM image of comparative example 1, Figure 1 e2 is a lattice line scanning analysis diagram of Example 1, Figure 1 e3 is the electron diffraction pattern of comparative example 1, Figure 1 f1 in the figure is a microscopic picture of comparative example 1. Figure 1 f2 is the Bi element distribution diagram in comparative example 1, Figure 1 f3 is the S element distribution diagram in comparative example 1, Figure 1 f4 in the figure is the C element distribution diagram in comparative example 1, where Figure 1 Figure g is a microscopic image of Example 1. Figure 1 h is a microscopic picture of Example 2, Figure 1 Fig. i is a microscopic image of Example 3, Figure 1 Figure j is a microscopic picture of Example 1. Figure 1 The k in the figure is the microscopic picture of Example 2. Figure 1 Figure 1 is a microscopic image of Example 3.

[0023] Figure 2 This is a microscopic image of CAU-17 material.

[0024] Figure 3 is a data diagram of the embodiments and comparative examples, wherein Figure 3 a is the XRD diagram of the embodiment and the comparative example, Figure 3 b is the Fourier transform infrared spectra of the embodiments and comparative examples, Figure 3 Figure c is the Raman spectra of the embodiments and comparative examples. Figure 3 d in the figure is the XPS graph of the embodiment and the comparative example, Figure 3 e is the XPS graph of the embodiment and the comparative example, Figure 3 f is the XPS graph of Example 1, Figure 3 g in FIG. 1 is the XPS graph of Comparative Example 1.

[0025] Figure 4 is the test data of the embodiment and the comparative example, wherein Figure 4 a is the EPR signal diagram of the embodiment and the comparative example, Figure 4 b is the thermal stability analysis of the embodiments and comparative examples, Figure 4 Figure c is a nitrogen adsorption / desorption isotherm analysis diagram of the embodiment and the comparative example, Figure 4 d in is a physical characteristic diagram of the embodiments and comparative examples.

[0026] Figure 5 are the test results of the embodiments and comparative examples, wherein Figure 5 a is the iodine capture capacity of the embodiment over time, Figure 5 b in the figure shows the iodine capture capacity over time. Figure 5Where c is the physical adsorption capacity and chemical adsorption capacity at different temperatures in the examples and comparative examples, Figure 5 Where d is the fixation capacity of Example 1 for adsorbed iodine, Figure 5 e is the iodine capture capacity of Example 1 after irradiation with different γ-rays.

[0027] Figure 6 : is the pseudo first-order kinetic equation and pseudo second-order kinetic equation fitting diagram of the embodiment and the comparative example, wherein Figure 6 a is the pseudo first-order kinetic equation fitting diagram of Example 1, Figure 6 b is the pseudo first-order kinetic equation fitting diagram of Example 2, Figure 6 c is the pseudo first-order kinetic equation fitting diagram of Example 3, Figure 6 d is the pseudo second-order kinetic equation fitting diagram of Example 1, Figure 6 e is the pseudo second-order kinetic equation fitting diagram of Example 2, Figure 6 f is the pseudo second-order kinetic equation fitting diagram of Example 2, Figure 6 g is the fitting diagram of the pseudo first-order kinetic equation of Example 1, Figure 6 h is the fitting diagram of the pseudo first-order kinetic equation of Example 2, Figure 6 The i in the figure is the fitting diagram of the pseudo first-order kinetic equation of Example 3. Figure 6 The j in the figure is the fitting diagram of the pseudo second-order kinetic equation of Example 1. Figure 6 The k in the figure is the fitting diagram of the pseudo second-order kinetic equation of Example 2. Figure 6 Figure 1 is the fitting diagram of the pseudo-second-order kinetic equation of Example 3.

[0028] Figure 7 is a morphological diagram of Example 1 in different directions after irradiation with a γ-ray dose of 100KGy, wherein Figure 7 Figure a is a morphological diagram of Example 1 after irradiation. Figure 7 Figure b is the morphology of Example 1 after irradiation.

[0029] Figure 8 1 is a graph showing the test results of the embodiment and the comparative example after iodine adsorption, wherein Figure 8 a in the figure is the microscopic image of I-AC-Bi2S3-x@C-1. Figure 8 b1 is the microstructure diagram of I-AC-Bi2S3-x@C-1. Figure 8 b2 is the microstructure diagram of I-AC-Bi2S3-x@C-1. Figure 8 c1 is the distribution diagram of Bi element in I-AC-Bi2S3-x@C-1. Figure 8 c2 is the S element distribution diagram in I-AC-Bi2S3-x@C-1. Figure 8 c3 is the C element distribution diagram in I-AC-Bi2S3-x@C-1. Figure 8c4 is the distribution diagram of I element in I-AC-Bi2S3-x@C-1. Figure 8 (d) is the HRTEM image of I-AC-Bi2S3-x@C-1. Figure 8 e is the SAED pattern of I-AC-Bi2S3-x@C-1, Figure 8 f in the figure is the microscopic image of IC-Bi2S3-x@C-1. Figure 8 In the figure g1 is the microstructure diagram of IC-Bi2S3-x@C-1. Figure 8 In g2, it is the microstructure diagram of IC-Bi2S3-x@C-1. Figure 8 h1 is the distribution diagram of Bi element in IC-Bi2S3-x@C-1. Figure 8 h2 is the distribution diagram of S element in IC-Bi2S3-x@C-1. Figure 8 h3 is the C element distribution diagram in IC-Bi2S3-x@C-1. Figure 8 h4 is the distribution diagram of I element in IC-Bi2S3-x@C-1. Figure 8 The i in the figure is the HRTEM image of IC-Bi2S3-x@C-1. Figure 8 In j, it is the SAED pattern of IC-Bi2S3-x@C-1. Figure 8 k is the XPS graph of the product after iodine adsorption in the example, Figure 8 The first part is the XPS graph of the product after iodine adsorption in the comparative example. Figure 8 Where m is the XPS graph of I-AC-Bi2S3-x@C-1, Figure 8 Where n is the XPS graph of IC-Bi2S3-x@C-1.

[0030] Fig. 9 is the test data after iodine adsorption in the embodiment and the comparative example, wherein Fig. 9 a is the XRD diagram of the product after iodine adsorption in the embodiment and the comparative example, Fig. 9 b is the Fourier transform infrared spectra of the embodiment and the comparative example after iodine adsorption, Fig. 9 Figure c is the Raman spectra of the embodiment and the comparative example after iodine adsorption. Fig. 9 d is the XRD diagram of Example 1-Example 3 after iodine adsorption as the temperature changes, Fig. 9 Figure e is the XRD pattern of GAC sample and GC sample before sintering. Fig. 9 Figure f is the XRD pattern of GAC sample and GC sample after sintering. Fig. 9 Where g is the density and Vickers hardness of GAC sample and GC sample, Fig. 9 where h is the retention rate of iodine in GAC sample and GC sample, Fig. 9 Where i is the normalized leaching rate of iodine in GAC samples and GC samples.

[0031] Fig.10 is a simulated iodine capture experiment, in which Fig.10 In the middle, a is a simulation device. Fig.10 b is the color change of the adsorbent over time in Example 1. Fig.10 In c, whether Example 1 can capture reflective iodine is verified.

[0032] Fig.11 Theoretical calculations were performed on the sulfur vacancies and amorphous structures in the examples, where Fig.11 a in the figure is the change of sulfur vacancies, amorphous structure and crystalline structure. Fig.11 Middle b shows the changes of sulfur vacancies and amorphous and crystalline structures.

[0033] Fig.12 is the microscopic picture of GAC sample and GC sample, where Fig.12 The middle a is a microscopic picture of GAC. Fig.12 b is the element distribution diagram of GAC. Fig.12 The middle c is a microscopic picture of GAC. Fig.12 d1 is the distribution diagram of Zn element in GAC. Fig.12 d2 is the distribution diagram of B element in GAC. Fig.12 Figure d3 is the distribution diagram of Bi element in GAC. Fig.12 D4 is the distribution diagram of O element in GAC. Fig.12 D5 is the distribution diagram of C element in GAC. Fig.12 D6 is the distribution diagram of S element in GAC. Fig.12 D7 is the distribution diagram of I element in GAC. Fig.12 The middle e is a microscopic picture of GC. Fig.12 f is the element distribution diagram of GC, Fig.12 The g in the middle is a microscopic picture of GC. Fig.12 h1 is the distribution diagram of Zn element in GC. Fig.12 h2 is the distribution diagram of B element in GC. Fig.12 h3 is the distribution diagram of Bi element in GC. Fig.12 h4 is the distribution diagram of O element in GC. Fig.12 h5 is the distribution diagram of C elements in GC. Fig.12 h6 is the distribution diagram of S element in GC. Fig.12 h7 is the distribution diagram of I element in GC.

[0034] Fig.13 It is the thermal stability analysis diagram of I-CAU-17, I-AC-Bi2S3-x@C-1 and IC-Bi2S3-x@C-1. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.

[0036] In a first aspect, some embodiments of the present invention provide a bismuth sulfide nanocomposite material for radioactive iodine capture, wherein the main body of the bismuth sulfide nanocomposite material is bismuth sulfide having both an amorphous structure and a crystalline structure, and carbon is uniformly dispersed in the bismuth sulfide.

[0037] In the present invention, sulfur vacancies can enhance the physical and chemical capture iodine ion ability of the adsorbent. On this basis, the amorphous structure, first, can provide a channel for the rapid diffusion of iodine molecules into the adsorbent structure, thereby enhancing the adsorption equilibrium speed; second, more surface defects and active sites in the amorphous structure make its surface have higher adsorption activity, which can more effectively adsorb gaseous molecules; third, the amorphous structure enhances the charge transfer between sulfur vacancies and iodine molecules, thereby enhancing the iodine adsorption capacity of the adsorbent and the proportion of chemical adsorption in the iodine capture process; fourth, the amorphous structure can enhance the bonding force between glass particles, help to form a dense glass structure, and improve the mechanical properties and durability of the cured glass. In addition, the uniformly dispersed carbon in the bismuth sulfide nanocomposite material is conducive to improving the stability of the overall structure of the adsorbent, thereby ensuring the adsorption capacity of the adsorbent.

[0038] In some embodiments, the content of sulfur vacancies in the bismuth sulfide nanocomposite material is 29%-44%.

[0039] In some embodiments, the specific surface area of ​​the bismuth sulfide nanocomposite material is 40 m 2 / g-54m 2 / g.

[0040] In a second aspect, some embodiments of the present invention also provide a method for preparing the bismuth sulfide nanocomposite material, which comprises: adding CAU-17 material to a sodium sulfide solution, performing a hydrothermal reaction, performing solid-liquid separation, washing the separated solid product, and drying the separated solid product to obtain a bismuth sulfide nanocomposite material.

[0041] In the present invention, sodium sulfide and hydrothermal reaction are conducive to the formation of an amorphous structure, while the concentration of the sodium sulfide solution is conducive to the formation of sulfur vacancies.

[0042] In some embodiments, the molar concentration of the sodium sulfide solution is 0.1M-0.3M.

[0043] In the present invention, the amount of sulfur vacancies can be adjusted by adjusting the molar concentration of the sodium sulfide solution; when the sulfur vacancy content is small, it will affect the iodine capture ability, and when the sulfur vacancies are too many, the adsorption capacity of the entire adsorption material will be mainly based on bismuth, and the adsorption capacity of the adsorbent will also decrease.

[0044] In some embodiments, the mass concentration of the CAU-17 material in the sodium sulfide solution is 100 mg / 30 mL.

[0045] In some embodiments, the method for preparing the sodium sulfide solution comprises dissolving sodium sulfide nonahydrate in deionized water.

[0046] In some embodiments, the temperature of the hydrothermal reaction is 80° C.-100° C., and the time of the hydrothermal reaction is 23 h-25 h.

[0047] In some embodiments, the specific method of washing includes washing with deionized water and ethanol in sequence for at least 3 times.

[0048] In some embodiments, the drying temperature is 50°C-70°C.

[0049] In a third aspect, some embodiments of the present invention also provide the use of the bismuth sulfide nanocomposite material in the adsorption of iodide ions.

[0050] The following is described in conjunction with some specific embodiments: Example 1: 100 mg of the prepared CAU-17 precursor was added to 30 ml of 0.1 M Na2S·9H2O aqueous solution. After stirring at room temperature for 30 min, the mixture was transferred to a 50 mL Teflon-lined steel reactor and heated at 90°C for 24 h. The black product was collected by centrifugation, washed with deionized water and ethanol, and dried overnight in vacuum at 60°C, which was recorded as AC-Bi2S3-x@C-1.

[0051] Example 2: 100 mg of the obtained CAU-17 precursor was added to 30 ml of 0.2 M Na2S·9H2O aqueous solution. After stirring at room temperature for 30 min, the mixture was transferred to a 50 mL Teflon-lined steel reactor and heated at 90°C for 24 h. The black product was collected by centrifugation, washed with deionized water and ethanol, and dried overnight in vacuum at 60°C, which was recorded as AC-Bi2S3-x@C-2.

[0052] Example 3: 100 mg of the obtained CAU-17 precursor was added to 30 ml of 0.3 M Na2S·9H2O aqueous solution. After stirring at room temperature for 30 min, the mixture was transferred to a 50 mL Teflon-lined steel reactor and heated at 90°C for 24 h. The black product was collected by centrifugation, washed with deionized water and ethanol, and dried overnight in vacuum at 60°C, which was recorded as AC-Bi2S3-x@C-2.

[0053] Comparative Example 1: Example 1 was calcined at 200°C for 2 h under a nitrogen atmosphere with a heating rate of 5°C / min to obtain a product, which was recorded as C-Bi2S3-x@C-1.

[0054] Comparative Example 2: Example 2 was calcined at 200°C for 2 h under a nitrogen atmosphere with a heating rate of 5°C / min to obtain a product, which was recorded as C-Bi2S3-x@C-2.

[0055] Comparative Example 3: Example 3 was calcined at 200°C for 2 h under a nitrogen atmosphere with a heating rate of 5°C / min to obtain a product, which was recorded as C-Bi2S3-x@C-3.

[0056] Comparative Example 4: 0.309 mmol Bi(NO3)3·5H2O (bismuth nitrate pentahydrate) and 3.659 mmol 1,3,5-benzenetricarboxylic acid (H3BTC) were dissolved in 60 mL of methanol solution. The transparent mixture was transferred to a Teflon-lined steel reactor, heated at 120°C for 24 hours, and the white product was collected by centrifugation, washed several times with methanol, and then vacuum dried at 60°C overnight to obtain the product, which was recorded as: CAU-17.

[0057] The following examples and comparative examples were tested: (1) Batch iodine adsorption experiment: Batch adsorption experiments were used to compare the adsorption characteristics of AC-Bi2S3-x@C and C-Bi2S3-x@C under high temperature, high humidity and irradiation. For safety reasons and the similar chemical properties of isotopes, non-radioactive 127 I replaces radioactive 131 I and 129 I. The iodine adsorption capacity Q (mg / g) is obtained by comparing the change in the mass of the adsorbent before and after adsorption. The corresponding formula is as follows: ; Wherein, “m1” and “m2” represent the mass (mg) of the adsorbent before and after adsorption, respectively. To determine the physical and chemical adsorption of AC-Bi2S3-x@C and C-Bi2S3-x@C, the samples after iodine adsorption were heated at 150 °C for 6 h. The chemical adsorption iodine capacity was calculated by the difference between the final residual mass and the mass of the adsorbent before adsorption, and the physical adsorption iodine capacity was calculated based on the difference between the total adsorption capacity and the chemical adsorption iodine capacity. The schematic diagram of the iodine capture device and the specific experimental steps are shown in the supplementary materials.

[0058] (2) Vitrification experiment of iodine-containing waste: Commercial glass (EG2998) was used as the glass substrate and Bi2O3 was used as the stabilizer to verify the possibility of low-temperature sintering to fix iodine-containing waste. Two forms of glass waste containing I-AC-Bi2S3-x@C and IC-Bi2S3-x@C were prepared, and the corresponding compositions are shown in Table 6. The various components were mixed in an agate mortar in proportion and then pressed into block samples with a diameter of 12 mm by cold pressing at 10 MPa. Finally, the glass solidified body was obtained after sintering at 600°C in air at a heating rate of 1°C / min for 2 hours.

[0059] Results and Analysis: Table 1 XPS results of examples and comparative examples

[0060] Table 2 Physical properties of examples and comparative examples

[0061] Table 3 Iodine adsorption kinetic parameters of the examples and comparative examples

[0062] Table 4 Comparison of adsorbents in the embodiments and prior art

[0063] Table 5 Iodine fixation capacity of each material

[0064] Table 6 Composition of samples before heat treatment

[0065] The present invention prepares CAU-17 precursor by solvothermal method. Then, sodium sulfide is used as sulfur source, and solvothermal sulfurization is performed to obtain a sulfide derivative AC-Bi2S3-x@C in which amorphous and crystalline coexist. The synthesized AC-Bi2S3-x@C is crystallized by heat treatment to obtain crystalline C-Bi2S3-x@C. In this process, by changing the concentration of sodium sulfide solution, we synthesized a series of AC-Bi2S3-x@C containing different sulfur vacancy concentrations (Example 1-Example 3).

[0066] First, the morphology and structural evolution of CAU-17 material to AC-Bi2S3-x@C-1 and C-Bi2S3-x@C-1 were observed by scanning electron microscopy, which is related to the sulfidation-induced crystallization process. Figure 2 As shown in the figure, the CAU-17 material is a uniform hexagonal prism structure with a diameter of about 500nm, a length of about 4μm, and a smooth surface. Figure 1 As shown in (g), after the CAU-17 material was treated with Na2S solution, its hexagonal prism structure was maintained, but its surface was slightly concave inward, and some fine nanoparticles appeared. With the increase of Na2S solution concentration, the size and number of nanoparticles gradually increased, and the surface of the hexagonal prism structure became rougher, as shown in Figure 2. Figure 1 (g)- Figure 1 As shown in (i), it is speculated that Bi2S3 grows on the surface of the hexagonal prism. The surface of C-Bi2S3-x@C obtained by calcination becomes rougher, as shown in Figure 1 (j)- Figure 1 (l) shows that this may be related to the crystallization of Bi2S3 during the calcination process. In order to further verify the in-depth morphology and structural characteristics of AC-Bi2S3-x@C and C-Bi2S3-x@C, TEM and HRTEM analyses were performed on typical AC-Bi2S3-x@C-1 and C-Bi2S3-x@C-1, respectively. Figure 1 (a) and Figure 1 As shown in (d), there are a small number of small nanoparticles on the surface of the hexagonal structure of AC-Bi2S3-x@C-1, while there are more and larger nanoparticles on the surface of C-Bi2S3-x@C-1. HRTEM image of AC-Bi2S3-x@C-1, as shown in Figure 1As shown in (b1), there are fuzzy areas (Amorphous) with no visible lattice fringes and crystal areas (Crystalline) with regular and clear lattice fringes, indicating that it presents an amorphous / crystalline mixed structure, proving that the AC-Bi2S3-x@C-1 material of the present invention has an amorphous structure. In addition, the d spacing of the lattice fringes in the crystal area of ​​AC-Bi2S3-x@C-1 is 0.309nm and 0.563nm, which are consistent with the (230) crystal plane and (020) crystal plane of Bi2S3 (JCPDS 75-1306), respectively. In contrast, C-Bi2S3-x@C-1 presents clear lattice fringes, as shown in Figure 1 (e1), indicating a good crystal structure, with a lattice fringe d spacing of 0.309 nm, corresponding to the (230) crystal plane of Bi2S3 (JCPDS 75-1306). At the same time, the corresponding lattice line scanning analysis shows the loss of many lattice atoms, such as Figure 1 (b2) and Figure 1 (e2), indicating that there are a large number of vacancies in both AC-Bi2S3-x@C-1 and C-Bi2S3-x@C-1. The selected area electron diffraction (SAED) pattern of AC-Bi2S3-x@C-1, as shown in Figure 1 As shown in (b3), the broad diffraction rings and diffraction spots further prove its amorphous and crystalline coexistence structure. In contrast, the SAED pattern of C-Bi2S3-x@C-1, such as Figure 1 The diffraction spots in (e3) are symmetrically distributed, and the center of the bright spot is the transmission spot, indicating that Bi2S3 single crystals have been prepared. The diffraction points can be attributed to the (200) crystal plane and (242) crystal plane of Bi2S3 along the

[012] zone axis, and the angle between the two crystal planes is 61.27 degrees; in addition, the diffraction pattern shows clear diffraction points, confirming that the crystallinity of Bi2S3 is good. Figure 1 (c1)- Figure 1 (c4) and Figure 1 (f1)- Figure 1 The element mapping diagram shown in (f4) reflects the uniform distribution of Bi, S and C on the surface of AC-Bi2S3-x@C-1 and C-Bi2S3-x@C-1, indicating that the phase composition is uniform. It can be seen that the composite material obtained by the present invention has a disordered amorphous structure, which can promote the electron transfer between the active site and iodine and provide a large number of unsaturated sites for the adsorption of iodine, which is expected to significantly improve the capture performance of the composite material for iodine.

[0067] exist Figure 3In (a), the crystallinity and phase structure of the original CAU-17 material, AC-Bi2S3-x@C, and C-Bi2S3-x@C were observed by XRD. The CAU-17 material showed typical and sharp diffraction peaks; after the sulfurization process, the characteristic peaks originally belonging to CAU-17 in the obtained AC-Bi2S3-x@C completely disappeared, indicating that CAU-17 had been completely converted into a sulfurized derivative. At the same time, low-intensity broad diffraction peaks appeared at 25.04°, 28.73°, and 42.82°, belonging to the (130) crystal plane, (230) crystal plane, and (421) crystal plane of Bi2S3 (JCPDS NO. 75-1360), indicating that the sample was an amorphous bismuth sulfide structure. In order to further determine the structure of the sample, the synthesized AC-Bi2S3-x@C was crystallized at high temperature to obtain C-Bi2S3-x@C. The annealed sample showed enhanced diffraction peaks. The diffraction peaks at 17.67°, 22.47°, 25.04°, 28.73°, 31.92°, 33.05°, 35.75°, 40.08°, 42.82° and 46.64° correspond to the (120) crystal plane, (220) crystal plane, (130) crystal plane, (230) crystal plane, (221) crystal plane, (301) crystal plane, (240) crystal plane, (141) crystal plane, (421) crystal plane and (431) crystal plane of Bi2S3, respectively. Fourier transform infrared spectroscopy (FTIR) shows the changes in the functional groups of CAU-17 materials during the sulfurization and crystallization process, such as Figure 3 (b) 527cm -1 、843cm -1 and 1115cm -1 The peak at 1619 cm is the stretching vibration of Bi-O in CAU-17. -1 and 1365cm -1 Two strong peaks were observed at 3- ) in the carboxylate anion. After sulfurization, the peak belonging to the Bi-O bond disappears, and at 1108cm -1 and 1375cm -1 The new vibration modes related to Bi-S bonds appeared, which revealed that CAU-17 was effectively converted into Bi2S3. In addition, after high temperature annealing, the -1 A new vibration mode belonging to the Bi-S bond appears, which may be related to the transformation of the structure from an amorphous state to a crystalline state after annealing.

[0068] Raman spectroscopy further confirmed the structural transformation between CAU-17 and AC-Bi2S3-x@C and C-Bi2S3-x@C. Figure 3(c) The Raman spectrum of CAU-17 shows a 162 cm -1 and 446cm -1 、846cm -1 and 1002cm -1 、1463cm -1 and 1609cm -1 These characteristic peaks can be attributed to the stretching mode of Bi-O bond, BTC 3- Aromatic CC and COC stretching vibration modes in the ligands. Compared with CAU-17 materials, AC-Bi2S3-x@C does not show Bi-O bonds and BTC 3- The characteristic peak of the ligand is at 128 cm -1 、437cm -1 and 965cm -1 New bands appeared, which were attributed to the vibration modes of Bi-S bonds.

[0069] XPS analysis was used to further understand the valence state and chemical composition of the sulfide derivatives. The XPS survey spectrum showed that CAU-17 contained Bi, O, and C. After sulfidation, AC-Bi2S3-x@C-1 and C-Bi2S3-x@C-1 samples showed S, such as Figure 3 (d) shows that sulfur was successfully introduced. Figure 3 In (e), the S 2s peak of AC-Bi2S3-x@C-1 shifted by 0.1 eV after annealing, indicating that the chemical environment of sulfur changed after crystallization. Figure 3 (f) and Figure 3 In (g), the high-resolution Bi 4f spectra of AC-Bi2S3-x@C and C-Bi2S3-x@C can be decomposed into two groups of peaks, indicating that there are two different types of Bi in the samples. The peaks at 159.0eV and 164.3eV belong to the bonding of lattice Bi and S (Bi-S bond), and the binding energy difference is 5.3eV, which confirms that the Bi element is Bi 3+ The shoulder peaks at 160.1eV and 165.4eV can be attributed to the antisite Bi of Bi-S defect. In addition, the peaks near 161.4eV and 162.6eV (spin-orbit double separation of 1.2eV) belong to S 2p3 / 2 and S 2p1 / 2, respectively, indicating the presence of S 2- . The results of quantitative XPS elemental analysis (Table 1) show that the atomic concentration ratio of Bi to S in AC-Bi2S3-x@C and C-Bi2S3-x@C is higher than the stoichiometric ratio of Bi2S3 of 0.67, indicating the presence of a large number of sulfur vacancies. The present invention has confirmed the existence of vacancies by HRTEM, Raman spectroscopy and EPR spectroscopy, while we have confirmed the existence of vacancies by XPS ( Figure 3 (f) and Figure 3 The content of sulfur vacancies was determined by the peak area ratio of Bi-S defects in Bi 4f (g). The contents of sulfur vacancies in AC-Bi2S3-x@C-1, AC-Bi2S3-x@C-2 and AC-Bi2S3-x@C-3 were 43.6%, 38.5% and 29.4%, respectively.

[0070] The electron paramagnetic resonance (EPR) method was used to study whether vacancy defects were introduced during the phase evolution process and the changes in the vacancy concentration in the sample before and after crystallization. Figure 4 As shown in (a), all AC-Bi2S3-x@C and C-Bi2S3-x@C samples show obvious EPR signals at g=2.003, which corresponds to sulfur vacancy defects. With the increase of sulfur source, the EPR signal intensity of AC-Bi2S3-x@C and C-Bi2S3-x@C composites gradually decreases, which is mainly due to the interaction between sulfur and Bi 3+ The sufficient reaction reduces the sulfur vacancy concentration. Combined with the TEM, XRD, XPS and EPR characterization results, AC-Bi2S3-x@C composites have an amorphous structure and a large number of sulfur vacancy defects. This can provide a large number of unsaturated coordination sites at the metal center for iodine molecules, which is beneficial to significantly improve the iodine capture performance of Bi2S3.

[0071] In addition, the thermal stabilities of CAU-17, AC-Bi2S3-x@C-1, and C-Bi2S3-x@C-1 were investigated by thermogravimetric analysis. Figure 4 (b) As shown. AC-Bi2S3-x@C-1 and C-Bi2S3-x@C-1 have better thermal stability than CAU-17 materials, which is attributed to the decomposition of the organic linker in CAU-17 at high temperature. It is worth noting that from 200°C to 800°C, AC-Bi2S3-x@C-1 has basically no mass loss, which may be because AC-Bi2S3-x@C-1 has an amorphous structure and irregular atomic arrangement, which makes it difficult to undergo phase change at high temperatures. In contrast, the crystal structure is prone to phase change at high temperatures, causing the crystalline C-Bi2S3-x@C-1 to lose stability. It can be seen that the amorphous structure is also conducive to the structural stability of the adsorbent.

[0072] The Brunauer-Emmett-Teller (BET) surface areas and pore size distributions of CAU-17 materials, AC-Bi2S3-x@C, and C-Bi2S3-x@C were analyzed by nitrogen adsorption / desorption isotherms, as shown in Figure 4(c). The isotherm of CAU-17 rises sharply at low adsorption pressure (P / P0 < 0.01) and shows a typical H4-type hysteresis loop at medium adsorption pressure (0.4 < P / P0 < 0.9), indicating the presence of micropores and mesopores. The isotherms of AC-Bi2S3-x@C and C-Bi2S3-x@C present typical type-IV isotherms with an H3 hysteresis loop at high adsorption pressure (P / P0 = 0.8 - 1.0), indicating their mesoporous characteristics. As Figure 4 (d) and Table 2 show, with the increase of sulfur source, the specific surface area and pore size of the sulfide derivatives gradually decrease. This is because in addition to filling the pores, the increase of sulfur source also promotes the in-situ transformation inside CAU-17 to form bismuth sulfide. In addition, after high-temperature crystallization of AC-Bi2S3-x@C to obtain C-Bi2S3-x@C, both its specific surface area and pore size decrease. This may be because the originally amorphous material shows the phenomenon of crystal grain growth, and the formation of the crystal structure makes the atomic arrangement inside the material more closely ordered, resulting in a decrease in the specific surface area.

[0073] To clarify the synergistic effect of the amorphous structure and sulfur vacancies on iodine capture, the iodine adsorption performances of AC-Bi2S3-x@C and C-Bi2S3-x@C were systematically compared. First, the adsorption kinetics of AC-Bi2S3-x@C and C-Bi2S3-x@C were investigated at 80 °C under ambient pressure, as Figure 5 (a)- Figure 5 (b) shows. The iodine capture capacities of AC-Bi2S3-x@C and C-Bi2S3-x@C both increase rapidly in the initial stage of adsorption. AC-Bi2S3-x@C reaches the adsorption equilibrium at about 15 min, and C-Bi2S3-x@C reaches the adsorption equilibrium at about 50 min. The equilibrium adsorption capacities of AC-Bi2S3-x@C-1, AC-Bi2S3-x@C-2, and AC-Bi2S3-x@C-3 are 1763.9 mg / g, 1654.5 mg / g, and 1408.3 mg / g respectively. After crystallization (C-Bi2S3-x@C), the equilibrium adsorption capacities decrease to 1583.1 mg / g, 1447.8 mg / g, and 1263.2 mg / g respectively. The faster adsorption equilibrium time and higher adsorption capacity of AC-Bi2S3-x@C may be attributed to its amorphous structure, higher sulfur vacancy concentration, and higher specific surface area in the structure. To further clarify the adsorption process, the pseudo-first-order kinetic equation and pseudo-second-order kinetic equation were used to fit the experimental results, and the results are as Figure 6and Table 3. According to the fitting results, the pseudo-second-order kinetics has a higher correlation coefficient (R2) for the experimental data of AC-Bi2S3-x@C and C-Bi2S3-x@C, and the iodine adsorption capacity obtained by model fitting is more consistent with the experimental results. This indicates that the two adsorbents mainly achieve iodine removal by chemical reaction with iodine molecules, rather than a simple mass transfer process caused by physical adsorption.

[0074] In the actual spent fuel reprocessing process, due to the presence of water vapor, the actual iodine removal temperature is usually higher than 140°C. Therefore, the iodine adsorption characteristics of AC-Bi2S3-x@C and C-Bi2S3-x@C at high temperatures (80°C, 140°C and 200°C) were studied. Figure 5 As shown in (c), with the increase of temperature, the chemical adsorption capacity of iodine increases slightly, which indicates that high temperature is conducive to the reaction of bismuth sulfide with iodine molecules and promotes the stable capture of iodine. At 200 ° C, the chemical adsorption ratios of AC-Bi2S3-x@C-1, AC-Bi2S3-x@C-2 and AC-Bi2S3-x@C-3 are 93.4%, 90.8% and 86.3%, respectively. After crystallization, the chemical adsorption ratios of the samples (C-Bi2S3-x@C) decreased to 88.2%, 84.8% and 80.7%, respectively. It is worth noting that the trend of the chemical adsorption ratio is consistent with the sulfur vacancy concentration, which indicates that sulfur vacancy defects play an important role in iodine capture. In addition, the adsorption capacity of AC-Bi2S3-x@C with amorphous structure is greater than that of crystalline C-Bi2S3-x@C, which indicates that the amorphous structure is conducive to the capture of iodine. In the present invention, the maximum adsorption capacity of AC-Bi2S3-x@C is 1763.9 mg / g (AC-Bi2S3-x@C-1 at 80°C) and the equilibrium time is 15 min. Its adsorption performance is significantly better than similar adsorbents reported (Table 4), including silver-based, copper-based and bismuth-based adsorbents. Although its iodine capture capacity is still somewhat lower than that of reported organic adsorbent materials, the high chemical adsorption ratio is conducive to the stable solidification of iodine-containing waste in the glass substrate during the subsequent low-temperature sintering process.

[0075] In order to investigate the stability of iodine adsorption on AC-Bi2S3-x@C, taking AC-Bi2S3-x@C-1 as an example, the desorption experiment of the adsorbed sample was carried out at room temperature. Figure 5As shown in (d), AC-Bi2S3-x@C-1 still maintains excellent retention capacity for adsorbed iodine after 7 days (94.3% and 92.4% in air and humidity environments, respectively). This shows that AC-Bi2S3-x@C can stably fix the captured iodine and has potential for practical applications. Given that AC-Bi2S3-x@C will be irradiated by radioactive rays in actual iodine removal applications, its stability under γ-ray irradiation was investigated using Co-60 as the radioactive source. The irradiated AC-Bi2S3-x@C-1 was characterized by SEM, FT-IR and XRD to investigate the effect of γ-ray irradiation on its morphology and crystal structure. As shown in Figure 7 As shown in Figure 2, the morphology of AC-Bi2S3-x@C-1 was maintained after irradiation with γ-rays at a dose of 100KGy. Figure 5 As shown in (e), the iodine capture performance of AC-Bi2S3-x@C-1 in air and humidity environments did not change significantly after irradiation with different doses, which indicates that the prepared AC-Bi2S3-x@C has excellent irradiation stability.

[0076] AC-Bi2S3-x@C exhibits outstanding adsorption performance and stability under high temperature, high humidity and irradiation environments. In addition, adsorption performance studies have shown that the amorphous structure and sulfur vacancy defects in the AC-Bi2S3-x@C structure make important contributions to iodine capture. Adsorption kinetics studies have shown that it mainly achieves the transformation of iodine vapor from gas phase to solid phase through chemical adsorption between bismuth sulfide and iodine gas. In order to further clarify the synergistic effect of amorphous structure and sulfur vacancy defects in iodine capture, a series of characterization analyses were performed on the adsorption products of AC-Bi2S3-x@C and C-Bi2S3-x@C.

[0077] First, the morphology and microstructure of the adsorbed samples were studied by SEM and TEM. Figure 8 (a) and Figure 8 As shown in (f), the nanorod-like structures of AC-Bi2S3-x@C-1 and C-Bi2S3-x@C-1 are maintained after iodine adsorption. AC-Bi2S3-x@C-1 becomes I-AC-Bi2S3-x@C-1 after iodine adsorption, and C-Bi2S3-x@C-1 becomes IC-Bi2S3-x@C-1 after iodine adsorption. A large number of sheet-like structures grow on the surface of I-AC-Bi2S3-x@C-1, while the nanoparticles originally existing on the surface of IC-Bi2S3-x@C-1 become larger. TEM image ( Figure 8 (b1)- Figure 8 (b2) and Figure 8 (g1)- Figure 8(g2) shows that the structure of I-AC-Bi2S3-x@C-1 is looser than that of IC-Bi2S3-x@C-1, which is attributed to the fact that iodine molecules can easily diffuse in the amorphous structure of AC-Bi2S3-x@C and react with the bismuth sulfide inside. Figure 8 (c1)- Figure 8 (c4) and 8(h1) - Figure 8 As shown in (h4), the corresponding elemental map image shows that Bi, S, C and I are evenly distributed on the sample surface. In addition, the distribution area of ​​I is consistent with that of Bi, which confirms the formation of BiI3. Figure 8 As shown in (d), the HRTEM image of I-AC-Bi2S3-x@C-1 shows obvious single lattice fringes with a d-spacing of 0.214 nm, which is attributed to the (103) crystal plane of BiI3. Figure 8 The SAED pattern of (e) also shows the characteristics of single crystal. Figure 8 In (i), the HRTEM image of IC-Bi2S3-x@C-1 shows lattice fringes belonging to BiI3 as well as (200) lattice fringes belonging to I2. Figure 8 The diffraction rings in the SAED pattern of (j) also have a very good correspondence with the (103) and (102) crystal planes of BiI3 and the (400) and (200) crystal planes of I2. This indicates that the proportion of chemical adsorption during the iodine removal process of AC-Bi2S3-x@C is significantly higher than that of C-Bi2S3-x@C. It can be seen that the amorphous structure provides a channel for the diffusion of iodine molecules inside the adsorbent, promoting the binding of iodine molecules to the internal active sites.

[0078] XPS spectroscopy was used to study the chemical composition and valence state changes of the samples after adsorption. Figure 8 (m)- Figure 8 As shown in (n), the peaks belonging to I 3d appeared in the XPS full scan spectra of I-AC-Bi2S3-x@C-1 and IC-Bi2S3-x@C-1, which confirmed that iodine was successfully captured. In addition, the intensity of the I 3d peak of I-AC-Bi2S3-x@C-1 is greater than that of IC-Bi2S3-x@C-1, indicating that I-AC-Bi2S3-x@C-1 has a larger iodine adsorption capacity. Figure 8 (k)- Figure 8As shown in (l), after adsorption, the proportion of peaks corresponding to anti-site Bi belonging to Bi-S defects in the high-resolution Bi 4f spectra of I-AC-Bi2S3-x@C-1 and IC-Bi2S3-x@C-1 decreased significantly, indicating that sulfur vacancies play an important role in the iodine capture process. In addition, the proportion of sulfur vacancies decreased in AC-Bi2S3-x@C-1 was 28.1%, 28.7% and 22.5%, respectively, which were significantly higher than 16.6%, 12.1% and 12.4% of C-Bi2S3-x@C, which proves that sulfur vacancies in amorphous structures are more conducive to iodine adsorption. At the same time, the higher iodine adsorption capacity of AC-Bi2S3-x@C-1 also proves this. Figure 8 (m)- Figure 8 As shown in (n), the high-resolution I 3d spectrum can be fitted with two groups of peaks, which are attributed to I2 (631.6 eV and 620.3 eV) and I3 - or I - (630.8eV and 619.4eV). This indicates that the iodine adsorption process mainly involves the chemical reaction of bismuth and iodine to form BiI3, and the physical adsorption of I2. - or I - The proportion of I3 in the I 3d spectrum of I-AC-Bi2S3-x@C-1 is significantly higher than that of I2, which indicates that chemical adsorption plays a dominant role in the iodine removal process. - The ratios of AC-Bi2S3-x@C-1 are all higher than those of the corresponding IC-Bi2S3-x@C-1, which may be because the amorphous structure and higher sulfur vacancy content in AC-Bi2S3-x@C-1 enhance the interaction between bismuth sulfide and iodine molecules.

[0079] In order to determine the phase composition of AC-Bi2S3-x@C and C-Bi2S3-x@C after adsorption, XRD detection was carried out. Fig. 9 As shown in (a), characteristic diffraction peaks corresponding to the (001), (200), (-1-12), (103), (-1-13), (-2-21), (004), (-2-22) and (-4-11) planes of BiI3 (JCPDS No. 76-1742) were detected at 2θ values ​​of 12.83°, 27.08°, 35.34°, 41.69°, 46.29°, 50.34°, 553.01°, 55.71° and 67.28° for all samples. With the increase of sulfur source, the peak intensity belonging to BiI3 in I-AC-Bi2S3-x@C and IC-Bi2S3-x@C gradually decreased, which is because the decrease in sulfur vacancy concentration reduces the adsorption capacity. In addition, Fig. 9In (d), as the iodine adsorption temperature increases, the diffraction peak intensity corresponding to BiI3 gradually increases, which indicates that high temperature enhances the interaction between bismuth sulfide and iodine molecules. At the same time, the proportion of chemical adsorption in the iodine capture process is higher at high temperature.

[0080] In addition, FT-IR was used to study the changes in the molecular structure and chemical composition of AC-Bi2S3-x@C and C-Bi2S3-x@C after adsorption. Fig. 9 (b) As we know, after adsorption, the Bi-S bond in the adsorbent is at 1108 cm -1 and 1375cm -1 The characteristic peak at disappeared, which proves that bismuth sulfide is involved in the iodine capture process.

[0081] also, Fig. 9 (c) Raman spectroscopy was used to analyze the existence form of iodine in the sample after adsorption. The results showed that the iodine ions at 115 cm-1 appeared in both I-AC-Bi2S3-x@C and IC-Bi2S3-x@C. -1 and 141cm -1 I3 - The symmetric stretching and intrinsic vibration of I2 are shown in Figure 2. This indicates that the prepared adsorbent captures iodine through chemical adsorption and physical adsorption. And with the increase of sulfur source, the intensity of the characteristic peak belonging to I2 after adsorption increases, which indicates that the reduction of sulfur vacancies increases the proportion of physical adsorption.

[0082] The thermal stability of the material after iodine capture was analyzed by TGA. Fig.13 As shown, I-CAU-17, I-AC-Bi2S3-x@C-1 and IC-Bi2S3-x@C-1 lose 18.1wt%, 7.0wt% and 7.1wt% respectively below 200℃, which is due to the physical adsorption of iodine molecules. The weight loss of the second part is 32.2wt%, 86.0wt% and 79.7wt% from 200℃ to 800℃, which corresponds to chemical adsorption. The chemical adsorption proportions of I-AC-Bi2S3-x@C-1 and IC-Bi2S3-x@C-1 obtained from thermal stability analysis are 92.47% and 91.82%, respectively, which are consistent with the adsorption experimental results.

[0083] Encouraged by the high adsorption capacity and fast adsorption rate of AC-Bi2S3-x@C, we evaluated its performance in capturing iodine in a simulated spent fuel reprocessing plant waste gas stream. Fig.10 As shown in (a), we built a simulated actual dynamic iodine removal device consisting of an I2 generator, an adsorption tube, and tail gas treatment. The I2 generated by the reaction of KI (potassium iodide) solution and concentrated nitric acid solution is driven by argon gas into the adsorption tube, and the excess I2 is collected by Na2S2O3 solution. Fig.10As shown in (b), the color of AC-Bi2S3-x@C-1 in the adsorption tube gradually changes from black to dark brown as the adsorption process proceeds. Fig.10 As shown in (c), the tail gas that has not been treated by AC-Bi2S3-x@C-1 adsorption can make the starch test paper turn blue, indicating that a large amount of I2 and water vapor are produced. After the tail gas treated by AC-Bi2S3-x@C-1 adsorption, almost no I2 is detected, indicating that AC-Bi2S3-x@C-1 can effectively capture reflective iodine under simulated exhaust gas conditions. The above results show that AC-Bi2S3-x@C has the potential to be used in the actual reprocessing of spent nuclear fuel.

[0084] The adsorption experimental results show that the amorphous structure and sulfur vacancy defects of AC-Bi2S3-x@C play an important role in its efficient and rapid capture of iodine. In order to further reveal the synergistic effect of amorphous regions and sulfur vacancy defects, we performed DFT theoretical calculations.

[0085] The adsorption energies of iodine molecules on crystalline and amorphous Bi2S3 surfaces with different sulfur vacancy concentrations were compared. Fig.11 As shown in (a), with the increase of sulfur vacancy concentration, the absolute value of the adsorption energy of iodine molecules on the crystalline and amorphous Bi2S3 surfaces increases continuously. In addition, the absolute value of the adsorption energy of iodine molecules on the amorphous Bi2S3 surface is higher. This means that both amorphous structure and sulfur vacancies can enhance the adsorption of iodine.

[0086] It is worth noting that with the increase of the same concentration of sulfur vacancies, the absolute value of the adsorption energy of iodine molecules on the amorphous Bi2S3 surface increases more, which indicates that the sulfur vacancies in the amorphous structure have a greater enhancing effect on iodine adsorption, which corresponds to the conclusion drawn from the XPS analysis results. The sulfur vacancies in AC-Bi2S3-x@C with an amorphous structure are more involved in the iodine adsorption process than the sulfur vacancies in the crystalline C-Bi2S3-x@C.

[0087] In order to further clarify the mechanism of the enhancement of iodine adsorption by sulfur vacancies in the amorphous structure on AC-Bi2S3-x@C, the details of the charge transfer between iodine molecules and the adsorbent were compared. Fig.11 As shown in (b), the charge density difference diagram also shows enhanced charge transfer with increasing sulfur vacancy concentration, indicating a stronger interaction between the adsorbent and the iodine molecules, which is also reflected in the higher adsorption energy and iodine capture capacity. In addition, at the same sulfur vacancy concentration, the charge transfer between the iodine molecules and the amorphous Bi2S3 is stronger, indicating a stronger interaction between the sulfur vacancies in the amorphous structure and the target pollutant iodine molecules. In addition, the excess charge generated by the sulfur vacancies is transferred from the adsorbent to I2, prompting the physically adsorbed captured I2 to form triiodide I3 -, thereby increasing the proportion of iodine captured by chemical adsorption and achieving efficient, rapid and stable capture of iodine.

[0088] Combining the results of adsorption experiments, characterization analysis and theoretical simulation calculations, AC-Bi2S3-x@C achieves efficient and stable capture of iodine mainly through the following three pathways. Some iodine molecules are attached to the surface of the adsorbent by physical adsorption (path one). In addition, BiI3 is generated through the strong chemical reaction between Bi2S3 in the adsorbent and the iodine molecules, realizing the transformation of iodine vapor from the gas phase to the solid phase (path two). In addition, the large number of sulfur vacancies in the adsorbent structure generate excess electrons, causing the physically captured iodine molecules to react to form triiodide (I3 - ) (Path three).

[0089] More importantly, the amorphous structure in the AC-Bi2S3-x@C structure provides a channel for the rapid diffusion of iodine molecules into the interior of the adsorbent structure, which is the reason why its adsorption equilibrium speed is significantly improved. In addition, the more surface defects and active sites in the amorphous structure in AC-Bi2S3-x@C make its surface have higher adsorption activity, which can more effectively adsorb gaseous molecules. In addition, the amorphous structure enhances the charge transfer between sulfur vacancies and iodine molecules, increases the iodine adsorption capacity of the adsorbent and the proportion of chemical adsorption in the iodine capture process. The sulfur vacancy defects in the amorphous structure are more involved in the iodine capture process, which is also an important reason why the adsorption performance of AC-Bi2S3-x@C is better than that of crystalline C-Bi2S3-x@C.

[0090] The microstructure, surface element composition and distribution of sintered glass components were studied by SEM-EDS. Fig.12 (a) Fig.12 (c) and Fig.12 (e) Fig.12 As shown in (g), a dense and smooth structure was observed on the surface of the glass solid (GAC) of AC-Bi2S3-x@C, while a small number of holes existed on the surface of the glass solid (GC) of C-Bi2S3-x@C, which may be attributed to the desorption of physically adsorbed iodine molecules during the sintering process. EDS spectra of GAC and GC ( Fig.12 (b) and Fig.12 (f)) shows that the sintered glass waste contains Zn, B, Bi, O, C, S and I elements, and the corresponding element distribution diagram is as follows: Fig.12 (d1)- Fig.12 (d7) shows that the above elements are evenly distributed on the surface of the glass sample, which indicates that the iodine-containing waste (I-AC-Bi2S3-x@C-1 and IC-Bi2S3-x@C-1) has been fixed in the Bi-Zn-B glass network.

[0091] XRD analysis was used to study the changes in the composition of the glass waste form before and after sintering. Fig. 9 As shown in (e), the characteristic diffraction peaks of BiI3 (JCPDS NO.76-1472) and stabilizer Bi2O3 (JCPDS NO.74-2351) were detected in both GAC and GC samples before sintering. The intensity of the characteristic peak belonging to BiI3 in the GAC sample is higher than that in the GC sample, which is attributed to the higher proportion of chemical adsorption in the iodine capture process of AC-Bi2O3-x@C. Fig. 9 In (f), after sintering, the characteristic peaks originally belonging to BiI3 in GAC and GC samples disappeared, and new characteristic peaks belonging to BiOI (JCPDS NO.73-2062) and Bi5O7I (JCPDS NO.38-0669) appeared, indicating that the iodine captured by BiI3 through chemical adsorption has been effectively converted into the more thermodynamically stable Bi after sintering. x O y I. In addition, the peak intensities of BiOI and Bi5O7I in the GAC sample are higher than those in GC, indicating that the high chemical adsorption ratio is conducive to the effective conversion of iodine-containing waste into BixOyI during the sintering process. Fig. 9 (g) It can be found that the density and Vickers hardness of the GAC sample are higher than those of the GC, which indicates that the chemically adsorbed BiI3 can be densely fixed in the glass matrix under the action of the stabilizer Bi2O3, while the physically adsorbed I2 is easily desorbed during the sintering process, which reduces the density and hardness of the glass component. In addition, the amorphous part in AC-Bi2S3-x@C can enhance the bonding force between glass particles, help form a dense glass structure, and improve the mechanical properties and durability of the solidified glass.

[0092] In order to further clarify the stable solidification mechanism of iodine during sintering, the retention rate of iodine in the form of sintered glass waste was investigated. Fig. 9 As shown in (h), the iodine retention rate in GAC is higher, reaching 92.3%, which may be attributed to the fact that BiI3 reacts more easily with the stabilizer Bi2O3 to form stable Bi x O y I. Although I2 can react with Bi2O3 to generate BiI3 or Bi x O y I, but it is easy to desorb at high temperature. The physical adsorption ratio in IC-Bi2O3-x@C is higher, which reduces the iodine retention rate.

[0093] The solidified iodine-containing waste glass may be corroded by environmental factors such as groundwater and underground gas during geological disposal, and the dissolution of radioactive elements and other harmful substances will cause serious harm to the underground environment and human health. Therefore, the chemical durability of sintered glass waste forms was investigated in aqueous, acidic and alkaline solutions. Fig. 9 As shown in (i), the normalized iodine leaching rate of GAC is lower than that of GC. This is because the stable Bi in GAC x O y I accounts for a higher proportion. It is worth noting that the normalized iodine leaching rates of GAC and GC in aqueous solution are 4.63×10 -5 , and 13.78×10 - 5 g / (m 2 •d). Fig. 9 (i) and Table 5 show that GAC and GC are comparable to previously reported low-temperature cured glass samples in terms of iodine loading and chemical durability.

[0094] In this study, CAU-17 was used as the material to prepare sulfur vacancy-rich amorphous-crystalline AC-Bi2S3-x@C by solvothermal sulfurization. The amorphous-crystalline AC-Bi2S3-x@C showed better radioactive iodine vapor capture performance. Specifically, the amorphous structure enhances the charge transfer between sulfur vacancy defects and iodine molecules. In addition, the amorphous structure provides channels for iodine molecules to diffuse rapidly into the interior of the adsorbent and sufficient internal binding sites, promoting the adsorption of iodine molecules inside it. Based on the synergistic effect of amorphous structure and sulfur vacancy defects, AC-Bi2S3-x@C exhibits a fast adsorption equilibrium time (15min), outstanding iodine adsorption capacity (1763.9mg / g), a high chemical adsorption ratio (93.4%), and good thermal and irradiation stability. Subsequent iodine-containing waste glass solidification studies showed that I-AC-Bi2S3-x@C with a high chemical adsorption ratio showed a higher iodine retention rate. And the iodine captured by chemical adsorption in the form of BiI3 is easier to convert into more stable Bi x O y I is fixed in a commercial glass substrate. This study highlights the synergistic effect of amorphous structure and sulfur vacancy defects in iodine capture, providing a new idea for constructing materials that can efficiently and stably capture radioactive iodine.

[0095] It should be noted that the terms used in the present invention are only for describing specific embodiments, rather than limiting the scope of the present application. As shown in the present specification, unless the context clearly indicates an exception, the words "one", "a", "a kind of" and / or "the" do not specifically refer to the singular, but may also include the plural. The terms "include", "comprise" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method or device. In the absence of more restrictions, the elements defined by the sentence "include one..." do not exclude the presence of other identical elements in the process, method or device including the elements.

[0096] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the technical solutions of the embodiments of the present invention.

[0097] References: [1] JH Yang, HS Park, D.-H. Ahn, M.-S. Yim, Glass composite wasteforms for iodine confined in bismuth-embedded SBA-15, J. Nucl. Mater. 480(2016) 150–158. https: / / doi.org / 10.1016 / j.jnucmat.2016.08.001. [2]Y. Nan, LL Tavlarides, DW DePaoli, Adsorption of iodine onhydrogen-reduced silver-exchanged mordenite: Experiments and modeling, AIChEJ. 63 (2017) 1024–1035. https: / / doi.org / 10.1002 / aic.15432. [3]L. Wu, J.A. Sawada, D.B. Kuznicki, T. Kuznicki, S.M. Kuznicki,Iodine adsorption on silver-exchanged titania-derived adsorbents, J.Radioanal. Nucl. Chem. 302 (2014) 527–532. https: / / doi.org / 10.1007 / s10967-014-3252-5. [4]Z. Tian, T.-S. Chee, L. Zhu, T. Duan, X. Zhang, L. Lei, C. Xiao,Comprehensive comparison of bismuth and silver functionalized nickel foamcomposites in capturing radioactive gaseous iodine, J. Hazard. Mater. 417(2021) 125978. https: / / doi.org / 10.1016 / j.jhazmat.2021.125978. [5]Y. Xiong, Y. Ai, H. Wang, E. Wang, H. Dan, Y. Ding, High capacityadsorption of iodine gas by Ag0@C / SiO2 derived from rice husk: synergisticeffect between C / SiO2 supports and Ag0 sites, J. Radioanal. Nucl. Chem. 332(2023) 3059–3068. https: / / doi.org / 10.1007 / s10967-023-08973-7. [6]J. Zhou, T. Lan, T. Li, Q. Chen, P. Bai, F. Liu, Z. Yuan, W.Zheng, X. Luo, W. Yan, T. Yan, Highly efficient capture of iodine in spentfuel reprocessing off-gas by novelly porous copper-doped silica zeolites,Sep. Purif. Technol. 290 (2022) 120895. https: / / doi.org / 10.1016 / j.seppur.2022.120895. [7]Q. Zhao, C. Liao, G. Chen, R. Liu, Z. Wang, A. Xu, S. Ji, K. Shih,L. Zhu, T. Duan, In Situ Confined Synthesis of a Copper-EncapsulatedSilicalite-1 Zeolite for Highly Efficient Iodine Capture, Inorg. Chem. 61(2022) 20133–20143. https: / / doi.org / 10.1021 / acs.inorgchem.2c03582. [8]X. He, L. Chen, X. Xiao, Y. Gan, J. Yu, J. Luo, H. Dan, Y. Wang,Y. Ding, T. Duan, Improved utilization of Cu0 for efficient adsorption ofiodine in gas and solution by mesoporous Cu0-SBA-15 via solvothermalreduction method, Chem. Eng. J. 462 (2023) 142175. https: / / doi.org / 10.1016 / j.cej.2023.142175. [9]Y. Xiong, Y. Ai, H. Wang, Y. Zhang, X. He, H. Dan, Y. Ding, Facilesynthesis of novel Cu0@SiO2 adsorbents derived from rice husk for highlyefficient capture iodine gas, J. Sol-Gel Sci. Technol. 107 (2023) 503–511.https: / / doi.org / 10.1007 / s10971-023-06100-2.

[10] Z. Tian, T.-S. Chee, X. Zhang, L. Lei, C. Xiao, Novel bismuth-based electrospinning materials for highly efficient capture of radioiodine,Chem. Eng. J. 412 (2021) 128687. https: / / doi.org / 10.1016 / j.cej.2021.128687.

[11] H. Zou, F. Yi, M. Song, X. Wang, L. Bian, W. Li, N. Pan, X.Jiang, Novel synthesis of Bi-Bi2O3-TiO2-C composite for capturing iodine-129in off-gas, J. Hazard. Mater. 365 (2019) 81–87. https: / / doi.org / 10.1016 / j.jhazmat.2018.11.001.

[12] A. Al-Mamoori, M. Alsalbokh, S. Lawson, A.A. Rownaghi, F. Rezaei,Development of bismuth-mordenite adsorbents for iodine capture from off-gasstreams, Chem. Eng. J. 391 (2020) 123583. https: / / doi.org / 10.1016 / j.cej.2019.123583.

[13] S.W. Kang, J.-H. Yang, M.-S. Yim, Examining Practical ApplicationFeasibility of Bismuth-Embedded SBA-15 for Gaseous Iodine Adsorption, Nucl.Technol. 206 (2020) 1593–1606. https: / / doi.org / 10.1080 / 00295450.2020.1713680.

[14] Z. Tian, T.-S. Chee, R. Meng, Y. Hao, X. Zhou, B. Ma, L. Zhu, T.Duan, C. Xiao, Incipient wetness impregnation to prepare bismuth-modifiedall-silica beta zeolite for efficient radioactive iodine capture, Environ.Funct. Mater. 1 (2022) 92–104. https: / / doi.org / 10.1016 / j.efmat.2022.05.006.

[15] Q. Xian, L. Chen, W. Fan, Y. Liu, X. He, H. Dan, L. Zhu, Y. Ding,T. Duan, Facile synthesis of novel Bi0-SBA-15 adsorbents by an improvedimpregnation reduction method for highly efficient capture of iodine gas, J.Hazard. Mater. 424 (2022) 127678. https: / / doi.org / 10.1016 / j.jhazmat.2021.127678.

[16] Q. Xian, Y. Gan, J. Yu, X. Xiao, Q. Chen, H. Dan, L. Zhu, Y.Ding, T. Duan, Scalable and economical Bi0-SiO2 for the high efficientcapture of iodine gas, J. Nucl. Mater. 567 (2022) 153849. https: / / doi.org / 10.1016 / j.jnucmat.2022.153849.

[17] H. Zou, J. Guo, M. Song, F. Yi, X. Wang, N. Pan, H. Li, W. Li, L.Bian, Bi2S3-reduced graphene oxide composite for gaseous radioiodine captureand its immobilization within glass composite material, Prog. Nucl. Energy135 (2021) 103705. https: / / doi.org / 10.1016 / j.pnucene.2021.103705.

[18] X. Li, X. Wang, L. Dong, Q. Zou, C. He, Y. Zhu, T. Fujita, C.Liao, C.-W. Kao, Y.-R. Lu, Combining Electrospinning and Hydrothermal Methodsto Prepare Bi2S3@SiO2 Nanostructure-Based Membranes for Enhanced CaptureCapacity of Off-Gas Iodine from a Nuclear Plant, ACS Appl. Nano Mater. 6(2023) 4328–4336. https: / / doi.org / 10.1021 / acsanm.2c05438.

[19] K. Chen, A. Gu, X. Zhou, P. Wang, C. Gong, P. Mao, Y. Jiao, K.Chen, Y. Yang, Core-shell structured Bi2S3-ZnS@C derived from ZIF-8 forefficient capture and reliable storage of volatile radioactive iodine, Sep.Purif. Technol. 322 (2023) 124380. https: / / doi.org / 10.1016 / j.seppur.2023.124380.

[20] K.-W. Chen, X.-Y. Zhou, X.-J. Dai, Y.-T. Chen, S.-X. Li, C.-H.Gong, P. Wang, P. Mao, Y. Jiao, K. Chen, Y. Yang, Sulfur vacancy-rich bismuthsulfide nanowire derived from CAU-17 for radioactive iodine capture incomplex environments: Performance and intrinsic mechanisms, J. Hazard. Mater.473 (2024) 134584. https: / / doi.org / 10.1016 / j.jhazmat.2024.134584.

[21] K. Yang, W. Zhu, S. Scott, Y. Wang, J. Wang, B.J. Riley, J.Vienna, J. Lian, Immobilization of cesium and iodine into Cs3Bi2I9perovskite-silica composites and core-shell waste forms with high wasteloadings and chemical durability, J. Hazard. Mater. 401 (2021) 123279.https: / / doi.org / 10.1016 / j.jhazmat.2020.123279.

[22] S. Chong, J.A. Peterson, B.J. Riley, D. Tabada, D. Wall, C.L.Corkhill, J.S. McCloy, Glass-bonded iodosodalite waste form forimmobilization of 129I, J. Nucl. Mater. 504 (2018) 109–121. https: / / doi.org / 10.1016 / j.jnucmat.2018.03.033.

[23] J.H. Yang, H.-S. Park, Y.-Z. Cho, Silver phosphate glasses forimmobilization of radioactive iodine, Ann. Nucl. Energy 110 (2017) 208–214.https: / / doi.org / 10.1016 / j.anucene.2017.06.042.

[24] C.W. Lee, J.-Y. Pyo, H.-S. Park, J.H. Yang, J. Heo,Immobilization and bonding scheme of radioactive iodine-129 in silvertellurite glass, J. Nucl. Mater. 492 (2017) 239–243. https: / / doi.org / 10.1016 / j.jnucmat.2017.05.024.

[25] L. Campayo, A. Grandjean, A. Coulon, R. Delorme, D. Vantelon, D.Laurencin, Incorporation of iodates into hydroxyapatites: a new approach forthe confinement of radioactive iodine, J. Mater. Chem. 21 (2011) 17609–17611.https: / / doi.org / 10.1039 / C1JM14157K.

[26] J.H. Yang, J.M. Shin, J.J. Park, G.I. Park, Waste Form of SilverIodide (AgI) with Low-Temperature Sintering Glasses, Sep. Sci. Technol. 49(2014) 298–304. https: / / doi.org / 10.1080 / 01496395.2013.817424.

[27] E.R. Maddrell, E.R. Vance, C. Grant, Z. Aly, A. Stopic, T.Palmer, J. Harrison, D.J. Gregg, Silver iodide sodalite – Wasteform / Hipcanister interactions and aqueous durability, J. Nucl. Mater. 517 (2019) 71–79. https: / / doi.org / 10.1016 / j.jnucmat.2019.02.002.

[28] J.H. Yang, H.-S. Park, Y.-Z. Cho, Al2O3-containing silverphosphate glasses as hosting matrices for radioactive iodine, J. Nucl. Sci.Technol. 54 (2017) 1330–1337. https: / / doi.org / 10.1080 / 00223131.2017.1365025.

[29] Q. Xian, X. Xiao, J. Yu, Y. Gan, L. Chen, X. He, E. Wang, H. Dan,L. Zhu, Y. Ding, T. Duan, High Retention Immobilization of Iodine in B–Bi–ZnOxide Glass Using Bi2O3 as a Stabilizer under a N2 Atmosphere, Inorg. Chem.61 (2022) 19633–19641. https: / / doi.org / 10.1021 / acs.inorgchem.2c03601.

[30] S.-S. Shin, G.-Y. Kim, B. Lee, J.-H. Yang, Y.-S. Son, J.-H. Choi,J.-Y. Pyo, K.R. Lee, H.-S. Park, H.W. Kang, Silver tungstate–tellurite glassfor radioactive iodine immobilization, J. Non-Cryst. Solids 624 (2024)122728. https: / / doi.org / 10.1016 / j.jnoncrysol.2023.122728.

Claims

1. A bismuth sulfide nanocomposite material for radioactive iodine capture, characterized in that: The main body of the bismuth sulfide nanocomposite material is bismuth sulfide having both an amorphous structure and a crystal structure, and carbon is uniformly dispersed in the bismuth sulfide.

2. The bismuth sulfide nanocomposite material according to claim 1, characterized in that: The content of sulfur vacancies in the bismuth sulfide nanocomposite material is 29%-44%.

3. The bismuth sulfide nanocomposite material according to claim 1, characterized in that: The specific surface area of ​​the bismuth sulfide nanocomposite material is 40 m 2 / g-54m 2 / g.

4. The method for preparing the bismuth sulfide nanocomposite material according to any one of claims 1 to 3, characterized in that: The preparation method comprises: adding CAU-17 material into sodium sulfide solution, hydrothermal reaction, solid-liquid separation, washing and drying the separated solid product to obtain bismuth sulfide nanocomposite material.

5. The preparation method according to claim 4, characterized in that: The molar concentration of the sodium sulfide solution is 0.1M-0.3M.

6. The preparation method according to claim 4, characterized in that: The mass concentration of the CAU-17 material in the sodium sulfide solution is 100 mg / 30 mL.

7. The preparation method according to claim 4, characterized in that: The temperature of the hydrothermal heating is 80° C.-100° C., and the time of the hydrothermal heating is 23 h-25 h.

8. The preparation method according to claim 4, characterized in that: The specific method of washing includes washing with deionized water and ethanol in sequence at least three times.

9. The preparation method according to claim 4, characterized in that: The drying temperature is 50°C-70°C.

10. Use of the bismuth sulfide nanocomposite material according to any one of claims 1 to 3 in adsorbing iodide ions.