Hydrogenation catalyst and method for preparing dimethyl succinate through dimethyl maleate hydrogenation
By encapsulating Cu into pure silicon molecular sieve pores, the problems of high price of palladium carbon catalysts and aggregation of active components are solved, and high stability and selectivity preparation of dimethyl succinate is achieved, which is extended. The catalyst life is improved and the preparation efficiency is improved.
Patent Information
- Application Number
- CN202310519924.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-05-09
AI Technical Summary
The existing catalysts for preparing dimethyl succinate with dimethyl maleate hydrogenation have high palladium carbon prices and the active components aggregate during the reaction, resulting in a decrease in hydrogenation effect and a short catalyst life.
By mixing the complexing agent with soluble copper salt and buffer solution, combining silicon source and molecular sieve template agent for hydrothermal treatment, Cu@S-1 hydrogenation catalyst is formed, and Cu is encapsulated with the pores of pure silicon molecular sieve to prevent its aggregation and achieve high Dispersion and stability.
It improves the stability and selectivity of the catalyst, extends the service life of the catalyst, and significantly improves the preparation efficiency of dimethyl succinate.
Smart Images

Figure CN118925783A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a hydrogenation catalyst, in particular to a catalyst for preparing dimethyl succinate by hydrogenating dimethyl maleate. Background Art
[0002] Dimethyl succinate (DMS) is an important synthetic flavoring, mainly used in the preparation of fruit and fruit wine flavors. It is also an important chemical intermediate, widely used in food, medicine, coatings, rubber, plastics and other industries. DMS can be used as a raw material for the synthesis of 1,4-butanediol, γ-butyrolactone, and tetrahydrofuran. At present, most industrial production methods of dimethyl succinate are obtained by esterification of succinic acid (SA) and methanol, but the catalyst of this technology is concentrated sulfuric acid, which has the disadvantages of many side reactions, low yield, high equipment requirements and environmental pollution.
[0003] CN101905160A discloses a method for preparing dimethyl succinate by hydrogenating dimethyl maleate (DMM) under the action of a Cu / ZnO / Al2O3 ternary catalyst. The method uses a fixed bed reactor. The raw material is diluted with methanol and enters the reactor together with H2. The active components of the catalyst are composed of copper, zinc oxide and aluminum oxide. The mass percentage of each component is: 30-60% copper, 10-50% zinc oxide, and 5-50% aluminum oxide.
[0004] CN103464153A discloses a hydrogenation catalyst for producing dimethyl succinate and a preparation method thereof. Resin-based spherical activated carbon is used as a carrier, palladium nitrate is loaded by a liquid phase sedimentation method, and then WO3 is loaded on the carrier, thereby increasing the life of the palladium-carbon catalyst used for preparing dimethyl succinate from dimethyl maleate.
[0005] However, in the above-mentioned method for preparing dimethyl succinate by hydrogenating dimethyl maleate, the palladium-carbon catalyst is expensive, and as the reaction proceeds, the active components Pd or Cu that play a hydrogenation role will aggregate, resulting in a decrease in the hydrogenation effect and a shortened catalyst life. Therefore, it is of great application significance to prevent the hydrogenation metal from aggregating during the reaction and to develop a long-life dimethyl maleate hydrogenation catalyst. Summary of the invention
[0006] In view of the shortcomings of the prior art, the present invention provides a hydrogenation catalyst and a method for producing dimethyl succinate by hydrogenating dimethyl maleate using the same. The catalyst not only has high stability, but also has high selectivity for the reaction.
[0007] The technical purpose of the first aspect of the present invention is to provide a method for preparing a hydrogenation catalyst, comprising the following steps:
[0008] (1) mixing a complexing agent, a soluble copper salt, a buffer solution and water to obtain a solution A;
[0009] (2) mixing a silicon source, an alkali, a molecular sieve template and water, and subjecting the mixture to hydrothermal treatment to obtain a solution B;
[0010] (3) Liquid A is added dropwise into liquid B. After the reaction, the mixture is transferred to a closed reactor for crystallization under autogenous pressure to obtain a Cu@S-1 hydrogenation catalyst.
[0011] Furthermore, the complexing agent in step (1) is selected from at least one of ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate and ethylenediamine; preferably, the complexing agent is disodium ethylenediaminetetraacetate. The soluble copper salt is selected from at least one of copper nitrate, copper sulfate and copper chloride; preferably, the soluble copper salt is copper nitrate. The buffer solution is at least one of a mixed solution of sodium carbonate and sodium bicarbonate, a mixed solution of disodium hydrogen phosphate and potassium dihydrogen phosphate, and a mixed solution of ammonium chloride and ammonia water; preferably, the buffer solution is a mixed solution of ammonium chloride and ammonia water, wherein the molar ratio of ammonium chloride to ammonia water is 0.1 to 10:1.
[0012] Furthermore, the molar ratio of each substance in the A solution of step (1) is: the sum of the conjugate acid and base in the buffer solution: Cu: H2O: complexing agent = (0.15-1.5): 1: (10-100): (0.2-20); preferably: the sum of the conjugate acid and base in the buffer solution: Cu: H2O: complexing agent = (0.3-1): 1: (20-80): (4-8).
[0013] Furthermore, in step (1), the substances in liquid A are stirred at 30 to 50° C. for 30 to 120 min to be fully mixed.
[0014] Further, the silicon source in step (2) is selected from at least one of fumed silica, water glass, silica sol and tetraethyl orthosilicate; preferably, the silicon source is tetraethyl orthosilicate. The base is selected from at least one of sodium hydroxide, potassium hydroxide, ammonia water and n-butylamine; preferably, the base is sodium hydroxide. The molecular sieve template is selected from at least one of n-butylamine, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrapropylammonium bromide and ammonia water; preferably, the molecular sieve template is tetrapropylammonium hydroxide.
[0015] Furthermore, in step (2), the silicon source in liquid B is calculated as SiO2, the base is calculated as OH-, and the molar ratio of each substance is SiO2:OH-:template:H2O=1:(0.1~15):(0.05~10):(5~30); preferably, SiO2:OH-:template:H2O=1:(0.15~3):(0.1~4):(10~20).
[0016] Furthermore, the temperature of the hydrothermal treatment in step (2) is 40 to 80° C., preferably 40 to 60° C., and the reaction time is 2 to 18 hours, preferably 4 to 8 hours.
[0017] Furthermore, in step (3), after liquid A is dripped into liquid B, the mixture is stirred and reacted at 40 to 80° C. for 4 to 36 hours.
[0018] Furthermore, in step (3), the temperature of the crystallization reaction is 120 to 190° C., preferably 155 to 170° C., and the time is 18 to 96 hours, preferably 48 to 72 hours.
[0019] Furthermore, liquid A and liquid B are mixed at a Cu:SiO2 mass ratio of 1:5 to 1:999, preferably 1:9 to 1:19.
[0020] Furthermore, after crystallization in step (3), the process also includes collecting, filtering, washing, drying and calcining the product to obtain the catalyst. The collection and post-processing process of the product after crystallization is familiar to those skilled in the art and will not be described in detail here. A specific product collection process that can be implemented in the present invention but is not limited to this is: after the crystallization is completed, the temperature of the reactor is cooled to room temperature by quenching with running water, the crystallized product is filtered or centrifuged, wherein the solid product is washed with deionized water to a pH value of 7 to 8, dried, heated to 400-600°C at a heating rate of 1 to 8°C / min and calcined for 2-10h to remove the template to obtain the catalyst.
[0021] The technical purpose of the second aspect of the present invention is to provide a hydrogenation catalyst prepared by the above method.
[0022] The Cu content in the above hydrogenation catalyst is 0.1-15.0 wt %; preferably, 5.0-10.0 wt %.
[0023] The present invention uses a complexing agent as a structure directing agent to encapsulate Cu in the form of metal clusters in the pores of pure silica zeolite, and prevents Cu from aggregating during the reaction process through the spatial restriction of the zeolite pores, so that it is always kept at a high dispersion to achieve hydrogenation and has high stability.
[0024] The technical purpose of the third aspect of the present invention is to provide a method for preparing dimethyl succinate by hydrogenating dimethyl maleate, wherein the Cu@S-1 hydrogenation catalyst is contacted with a raw material for reaction.
[0025] Furthermore, the hydrogenation catalyst is subjected to reduction treatment before use. The reduction method is well known to those skilled in the art. Generally, hydrogen is contacted with the catalyst at a certain reduction temperature. Commonly, nitrogen with a certain hydrogen content is contacted with the catalyst at 150-300° C. for 2-10 hours.
[0026] Furthermore, the process conditions for preparing dimethyl succinate by hydrogenating dimethyl maleate are as follows: the catalyst is crushed into 20-40 meshes and loaded into a shell-and-tube reactor, and both ends are filled with quartz sand. Under a hydrogen atmosphere, the raw material dimethyl maleate is passed into the reaction tube through a horizontal flow pump, the reaction pressure is 0.5-5Mpa, the reaction temperature is 140-220°C, and the molar ratio of hydrogen to dimethyl maleate is 20-400.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] (1) In the preparation method of the present invention, a complexing agent is used to introduce Cu into the pores of a pure silicon molecular sieve. The pure silicon molecular sieve is not acidic and will not affect the hydrogenation reaction. The unique pore restriction effect of the pure silicon molecular sieve is used to prevent Cu from aggregating and growing during the reaction and affecting the hydrogenation effect, thereby making the catalyst more stable and improving the life of the catalyst.
[0029] (2) The Cu@S-1 hydrogenation catalyst prepared by the present invention catalyzes the production of dimethyl succinate from dimethyl maleate. Compared with the Cu-based catalyst prepared by the conventional preparation method, the catalyst of the present invention has a longer service life and significantly improved selectivity.
[0030] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 . XRD diffraction pattern of the catalyst Cu@S-1-1# prepared in Example 1;
[0032] Figure 2 . TEM image of the catalyst Cu@S-1-1# prepared in Example 1;
[0033] Figure 3 . STEM image of the catalyst Cu@S-1-1# prepared in Example 1;
[0034] Figure 4 .Ultraviolet-visible absorption spectra of reactants and products in the verification experiment of Example 1. DETAILED DESCRIPTION
[0035] The following non-limiting embodiments may enable a person skilled in the art to more fully understand the present invention, but are not intended to limit the present invention in any way.
[0036] Example 1
[0037] Preparation of catalyst Cu@S-1-1#:
[0038] (1) A buffer solution prepared from disodium ethylenediaminetetraacetate, copper nitrate, ammonium chloride and ammonia water and deionized water were mixed and stirred at 30° C. for 30 min, which was recorded as solution A. The molar composition of the solution was: the sum of the conjugate acid and base in the buffer solution: Cu:H2O:complexing agent = 1.5:1:10:0.2;
[0039] (2) Mixing tetraethyl orthosilicate, ammonia water, tetrapropylammonium hydroxide and deionized water to obtain liquid B, wherein the silicon source is calculated as SiO2, and the base is calculated as OH-, and the molar composition thereof is: SiO2:OH-:template:H2O=1:0.15:0.1:10, and subjecting the liquid B to hydrothermal treatment at 40°C for 4h;
[0040] (3) Liquid A was slowly added dropwise to liquid B. Liquid A and liquid B were mixed at a Cu:SiO2 mass ratio of 1:19, and then stirred at 40°C for 4 hours. The resulting mixture was transferred into a hydrothermal crystallization reactor with a polytetrafluoroethylene liner, and dynamically rotated crystallized at 170°C for 72 hours under autogenous pressure. After the crystallization, the temperature of the reactor was cooled to room temperature by running water. The crystallized product was filtered or centrifuged, and the solid product was washed with deionized water to a pH value of 7-8, then dried at 120°C, heated to 540°C at a heating rate of 3°C / min, and calcined for 6 hours to remove the template agent, thereby obtaining the catalyst Cu@S-1-#1. The Cu loading was 5.0wt% calculated based on the feed amount.
[0041] The XRD diffraction pattern of catalyst Cu@S-1-1# shows a typical MFI topological structure, such as Figure 1 As shown in the figure, the relative crystallinity is 99%, and no CuO diffraction peak is observed, indicating that the metal is well encapsulated and evenly dispersed, and there are no CuO metal agglomerate particles. The TEM and STEM images of the product are shown in the figure below. Figure 2 and Figure 3 As shown, it can be observed that the metal Cu nanoparticles are evenly distributed in the S-1 pores and have a uniform particle size of about 2 to 4 nm.
[0042] To further illustrate that Cu is encapsulated in the pores of pure silicon S-1 rather than deposited on the surface of pure silicon S-1, liquid phase hydrogenation experiments were used to verify this.
[0043] Dissolve 0.1g sodium borohydride in 3g aqueous solution, add 0.1g catalyst Cu@S-1-1#, and react for 30min. The purpose of this step is to reduce the hydrogenation active metal in the catalyst and provide hydrogen for the liquid phase hydrogenation reaction. Add 15mL 3-nitrotoluene and 7g water to the above solution and react for 1h in a sealed container. After the reaction is completed, the reactants and products are analyzed by UV-visible absorption spectroscopy in the range of 225-400nm. Figure 4 .Depend on Figure 4It can be seen that the raw material 3-nitrotoluene is not hydrogenated to 3-aminotoluene by Cu@S-1-1#, which proves that the hydrogenation active metal Cu is completely encapsulated in the pure silicon S-1. Since the molecular diameter of 3-nitrotoluene is larger than the pore diameter of S-1, it cannot enter the interior of S-1 and cannot undergo hydrogenation reaction to generate 3-aminotoluene.
[0044] Example 2
[0045] Preparation of catalyst Cu@S-1-2#:
[0046] The preparation process is the same as that of Example 1, except that the molar composition of liquid A is: the sum of the conjugate acid and base in the buffer solution: Cu:H2O: complexing agent = 1.2:1:40:6, the molar composition of the silicon source in liquid B, calculated as SiO2, and the base in liquid B, calculated as OH-, is: SiO2:OH-: template agent:H2O = 1:0.3:0.2:20, liquid A and liquid B are mixed at a Cu:SiO2 mass ratio of 1:9, and the theoretical loading amount of Cu is 10.0wt%.
[0047] Example 3
[0048] Preparation of catalyst Cu@S-1-3#:
[0049] The preparation process is the same as that of Example 1, except that the molar composition of liquid A is: the sum of the conjugate acid and base in the buffer solution: Cu:H2O: complexing agent = 0.8:1:50:6, the molar composition of the silicon source in liquid B, calculated as SiO2, and the base in liquid B, calculated as OH-, is: SiO2:OH-: template agent: H2O = 1:0.3:3:25, and liquid A and liquid B are mixed at a Cu:SiO2 mass ratio of 1:5.67, except that the theoretical loading amount of Cu is 15.0wt%.
[0050] Example 4
[0051] Preparation of catalyst Cu@S-1-4#:
[0052] (1) A buffer solution prepared by ethylenediamine, copper nitrate, sodium carbonate and sodium bicarbonate and deionized water were mixed and stirred at 50° C. for 120 min, which was recorded as solution A. The molar composition of the solution was: the sum of the conjugate acid and base in the buffer solution: Cu:H2O:complexing agent = 0.25:1:20:2;
[0053] (2) Mixing tetraethyl orthosilicate, ammonia water, tetrapropylammonium hydroxide and deionized water to obtain liquid B, wherein the silicon source is calculated as SiO2, and the base is calculated as OH-, and the molar composition thereof is: SiO2:OH-:template:H2O=1:0.6:0.4:20, and subjecting the liquid B to hydrothermal treatment at 60°C for 8h;
[0054] (3) Liquid A was slowly added dropwise to liquid B. Liquid A and liquid B were mixed at a Cu:SiO2 mass ratio of 1:9, and then stirred at 60°C for 12 hours. The resulting mixture was transferred into a hydrothermal crystallization reactor with a polytetrafluoroethylene liner, and dynamically rotated crystallized at 165°C for 56 hours under autogenous pressure. After the crystallization, the temperature of the reactor was cooled to room temperature by running water. The crystallized product was filtered or centrifuged, and the solid product was washed with deionized water to a pH value of 7-8, then dried at 120°C, heated to 540°C at a heating rate of 3°C / min, and calcined for 6 hours to remove the template, thereby obtaining the catalyst Cu@S-1-#4. The Cu loading was 10.0wt% based on the feed amount.
[0055] Example 5
[0056] Preparation of catalyst Cu@S-1-5#:
[0057] The preparation process is the same as that of Example 4, except that the soluble copper salt in step (1) is copper sulfate.
[0058] Example 6
[0059] Preparation of catalyst Cu@S-1-6#:
[0060] The preparation process is the same as that of Example 4, except that the silicon source in step (2) is fumed silica and the alkali is sodium hydroxide.
[0061] Example 7
[0062] Preparation of catalyst Cu@S-1-7#:
[0063] (1) A buffer solution prepared from disodium ethylenediaminetetraacetate, copper chloride, ammonium chloride and ammonia water and deionized water were mixed and stirred at 40° C. for 60 min, which was referred to as solution A. The molar composition of the solution was: the sum of the conjugate acid and base in the buffer solution: Cu:H2O:complexing agent = 0.75:1:30:4;
[0064] (2) mixing silica sol, ammonia water, tetrapropylammonium hydroxide and deionized water to obtain solution B, whose molar composition is: SiO2:OH-:template:H2O=1:0.3:0.3:15, and subjecting the solution B to hydrothermal treatment at 50°C for 12h;
[0065] (3) Liquid A was slowly added dropwise to liquid B. Liquid A and liquid B were mixed at a Cu:SiO2 mass ratio of 1:11.5, and then stirred at 50°C for 24 hours. The resulting mixture was transferred into a hydrothermal crystallization reactor with a polytetrafluoroethylene liner, and dynamically rotated crystallized at 160°C for 72 hours under autogenous pressure. After the crystallization, the temperature of the reactor was cooled to room temperature by running water. The crystallized product was filtered or centrifuged, and the solid product was washed with deionized water to a pH value of 7-8, then dried at 120°C, heated to 540°C at a heating rate of 3°C / min, and calcined for 6 hours to remove the template, thereby obtaining the catalyst Cu@S-1-#7. The Cu loading calculated based on the feed amount was 8.0wt%.
[0066] Example 8
[0067] Preparation of catalyst Cu@S-1-8#:
[0068] The preparation process is the same as that of Example 7, except that the buffer solution in step (1) is a mixture of disodium hydrogen phosphate and potassium dihydrogen phosphate, the molar composition of liquid A is: the sum of the conjugate acid and base in the buffer solution: Cu:H2O:complexing agent = 1.2:1:50:7, and liquid A and liquid B are mixed at a Cu:SiO2 mass ratio of 1:9.53. The Cu loading calculated based on the feed amount is 9.5wt%.
[0069] Example 9
[0070] Preparation of catalyst Cu@S-1-9#:
[0071] The preparation process is the same as in Example 7, except that the molar composition of solution B in step (2) is: SiO2:OH - : Template: H2O = 1:0.8:0.5:25, A solution and B solution are mixed at a Cu:SiO2 mass ratio of 1:7. The Cu loading calculated based on the feed amount is 12.5wt%.
[0072] Comparative Example 1
[0073] Preparation of Cu / SiO2:
[0074] In this comparative example, a Cu / SiO2 catalyst with a Cu content of 10.0 wt% was prepared by a conventional wet impregnation method.
[0075] The metal Cu precursor copper nitrate was dissolved in deionized water and stirred until dissolved; then the calcined SiO2 carrier was added thereto and stirred at room temperature for 8 hours. The mass ratio of Cu, SiO2 and H2O in the obtained mixture was 0.1:1:10. The obtained mixture was transferred to an oven and dried at 120°C for 24 hours. The product was taken out after cooling, ground, and calcined at 540°C for 6 hours to obtain a Cu / SiO2 catalyst prepared by traditional wet impregnation method, recorded as DB1.
[0076] Comparative Example 2
[0077] Cu-Zn-Al catalyst: A commercially available conventional Cu-Zn-Al catalyst was used, with a Cu content of 10 wt%, denoted as DB2.
[0078] Comparative Example 3
[0079] Cu-Al2O3 catalyst: A commercially available conventional Cu-Al2O3 catalyst with a Cu content of 10 wt% was used, denoted as DB3.
[0080] The metal contents in the catalysts obtained in various embodiments and comparative examples were characterized by XRF as shown in Table 1.
[0081] Table 1
[0082]
[0083]
[0084] Catalyst Evaluation
[0085] The catalyst was crushed into 20-40 meshes and loaded into a reaction tube of a micro-fixed bed reactor with an inner diameter of 10 mm. The catalyst was placed near the constant temperature section and filled with 20-40 mesh quartz sand at both ends.
[0086] Catalyst reduction, introduce 5% H2 + 95% N2 mixed gas, program temperature rise to 230°C, maintain for 5 hours, and then lower to reaction temperature.
[0087] The reaction gas was switched to pure H2, and the raw material dimethyl maleate was introduced into the reaction tube through a horizontal flow pump. The reaction pressure was 1.0 MPa, the reaction temperature was 170°C, the molar ratio of hydrogen to dimethyl maleate was 200, and the feed volume space velocity LHSV was 0.2 h -1 The reaction product was condensed and analyzed by gas chromatography for its composition. The results are shown in Table 2.
[0088] Table 2
[0089]
[0090]
Claims
1. A method for preparing a hydrogenation catalyst, The following steps are involved: (1) Mixing a complexing agent, a soluble copper salt, a buffer solution and water to obtain solution A; (2) mixing a silicon source, an alkali, a molecular sieve template and water, and subjecting the mixture to hydrothermal treatment to obtain a solution B; (3) Liquid A was added dropwise into liquid B. After the reaction, the liquid was transferred to a closed reactor and crystallized under autogenous pressure to obtain a Cu@S-1 hydrogenation catalyst.
2. The preparation method according to claim 1, It is characterized in that The complexing agent in step (1) is selected from at least one of ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate and ethylenediamine; the soluble copper salt is selected from at least one of copper nitrate, copper sulfate and copper chloride; and the buffer solution is at least one of a mixed solution of sodium carbonate and sodium bicarbonate, a mixed solution of disodium hydrogen phosphate and potassium dihydrogen phosphate, and a mixed solution of ammonium chloride and aqueous ammonia.
3. The preparation method according to claim 1, It is characterized in that The molar ratio of each substance in solution A in step (1) is: the sum of the conjugate acid and base in the buffer solution: Cu:H 2 O: complexing agent = (0.15~1.5):1: (10~100): (0.2~20).
4. The preparation method according to claim 1, It is characterized in that The silicon source in step (2) is selected from at least one of fumed silica, water glass, silica sol and tetraethyl orthosilicate; the base is selected from at least one of sodium hydroxide, potassium hydroxide, ammonia water and n-butylamine; and the molecular sieve template is selected from at least one of n-butylamine, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrapropylammonium bromide and ammonia water.
5. The preparation method according to claim 1, It is characterized in that Step (2) The silicon source in solution B is SiO 2 The base is OH - The molar ratio of each substance is SiO 2 :OH - :Template:H 2 O=1:(0.1~15):(0.05~10):(5~30).
6. The preparation method according to claim 1, It is characterized in that The temperature of the hydrothermal treatment in step (2) is 40 to 80° C., and the reaction time is 2 to 18 hours.
7. The preparation method according to claim 1, It is characterized in that In step (3), after liquid A is added dropwise to liquid B, the mixture is stirred at 40-80° C. for 4-36 hours.
8. The preparation method according to claim 1, It is characterized in that The temperature of the crystallization reaction in step (3) is 120-190° C. and the time is 18-96 hours.
9. The preparation method according to claim 1, It is characterized in that A liquid and B liquid are Cu:SiO 2 The mass ratio is 1:5~1:
999.
10. The hydrogenation catalyst prepared by the preparation method according to any one of claims 1 to 9.
11. A method for preparing dimethyl succinate by hydrogenating dimethyl maleate, It is characterized in that The hydrogenation catalyst according to claim 10 is contacted with the raw material for reaction.
12. The method according to claim 11, It is characterized in that The hydrogenation catalyst is subjected to reduction treatment before use.
13. The method according to claim 11, It is characterized in that The process conditions for preparing dimethyl succinate by hydrogenation of dimethyl maleate are as follows: the catalyst is crushed into 20-40 meshes and loaded into a tubular reactor, and both ends are filled with quartz sand. Under a hydrogen atmosphere, the raw material dimethyl maleate is passed into the reaction tube through a horizontal flow pump, the reaction pressure is 0.5-5Mpa, the reaction temperature is 140-220°C, and the molar ratio of hydrogen to dimethyl maleate is 20-400.
Citation Information
Patent Citations
Catalyst for use in synthesis of dimethyl succinate and application thereof
CN101905160A
Method for preparing hydrogenation catalyst for producing dimethyl succinate
CN103464153A
Catalyst for preparing ethanol by virtue of acetate hydrogenation and preparation method thereof
CN102974382A
Process for preparing y-type high-si zeolite
CN1058358A
Zeolite molecular sieve supported metal catalyst as well as synthesis method and application thereof
CN113649064A