Catalyst for catalytic pyrolysis of industrial organic waste salt as well as preparation method and application of catalyst

By using a carrier-loaded transition metal oxide catalyst in industrial waste salts for low-temperature catalytic pyrolysis, the problems of high-temperature treatment and incomplete organic matter removal are solved, and the deep removal of organic matter in industrial waste salts are achieved.

CN118925792APending Publication Date: 2024-11-12INSTITUTE OF PROCESS ENGINEERING CHINESE ACADEMY OF SCIENCES

Patent Information

Application Number
CN202410989301.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing industrial waste salt pyrolysis process has problems such as high treatment temperature, incomplete removal of organic matter, and high cost, and the catalyst cannot be reused, which affects the efficiency of resource utilization.

Method used

The catalysts with support are ceramics, activated alumina, silicon oxide or silicon alumina molecular sieve, and support transition metal oxides such as copper oxide, nickel oxide, cerium oxide, etc., and industrial organic waste salts are treated in an oxygen atmosphere through low-temperature catalytic pyrolysis process. Reduce the catalytic pyrolysis temperature and achieve deep removal of organic matter.

Benefits of technology

The deep removal of organic matter in industrial waste salt is achieved, production costs are reduced, melting phenomena and equipment failures are avoided, and the catalyst can be reused, improving the efficiency of resource utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a catalyst for catalytic pyrolysis of industrial organic waste salt as well as a preparation method and application of the catalyst. The catalyst comprises a carrier and a metal oxide loaded on the carrier; the carrier comprises any one or a combination of at least two of ceramic, activated aluminum oxide, silicon oxide or a silicon-aluminum molecular sieve; the metal oxide comprises any one or a combination of at least two of copper oxide, nickel oxide, cerium oxide, lanthanum oxide, zirconium oxide, cobalt oxide, manganese oxide, vanadium oxide or chromium oxide. According to the present invention, by designing the specific composition of the catalyst and the industrial organic waste salt catalytic pyrolysis method, the industrial organic waste salt can be subjected to catalytic pyrolysis at the low temperature by using the catalyst provided by the present invention, the catalyst preparation process conditions are mild, and the prepared catalyst can be repeatedly used; the production cost of catalytic pyrolysis of the industrial organic waste salt and the catalytic pyrolysis treatment temperature are reduced, and deep removal of organic matters in the industrial waste salt is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of industrial solid waste treatment and resource utilization, and specifically relates to a catalyst for catalytic pyrolysis of industrial organic waste salt, and a preparation method and application thereof. Background Art

[0002] In the production process of coal chemical, pharmaceutical, petrochemical and other industries, due to the demand for zero wastewater discharge, a large amount of waste salt containing organic matter (referred to as industrial waste salt) will inevitably be produced in the multi-effect evaporation process. Industrial waste salt has the characteristics of a wide variety, complex composition and high toxicity. If it cannot be properly handled and disposed, it will directly lead to environmental pollution and waste of resources. Therefore, the purification and recycling of industrial waste salt is of great significance to environmental management and enterprise development.

[0003] At present, the treatment methods for industrial waste salt containing high concentrations of organic matter include incineration and solidification landfill, which not only brings serious environmental safety hazards, but also wastes resources. In comparison, the recycling of waste salt is the most promising treatment method, but the deep removal of organic pollutants in waste salt is the main limiting factor for recycling. The removal of organic pollutants in waste salt includes thermal treatment and non-thermal treatment. Non-thermal treatment processes include advanced oxidation, membrane separation and recrystallization processes, all of which dissolve waste salt in aqueous solution for reprocessing. The treatment cost is high, and waste salt with a high organic content cannot be deeply purified. Thermal treatment is a common method for effectively removing organic pollutants from waste salt. It generally refers to placing waste salt in equipment such as rotary kilns or heating furnaces, calcining at above 800°C, so that the organic pollutants in the waste salt are decomposed and oxidized into gaseous components at high temperature. However, as the temperature increases, the waste salt will melt, making it difficult for the pyrolysis equipment to operate normally, and some organic matter in the molten salt is not completely removed, making it difficult to purify and reuse the waste salt. In addition, the higher pyrolysis temperature requires higher energy consumption, resulting in higher costs for pyrolysis purification of waste salt.

[0004] CN107662930A discloses a method for refining salt containing organic matter, which discloses that organic waste salt is passed into a rotary furnace for high-temperature cracking, so that the organic matter in the salt is cracked and carbonized, the salt after high-temperature cracking is dissolved in water, filtered to obtain transparent brine, and the brine is evaporated and crystallized to obtain salt without organic matter. However, this method is costly, easy to wear out equipment, and difficult to apply in practice.

[0005] CN111422886A discloses a method and application of low-temperature catalytic pyrolysis treatment of organic waste salt. A mixed solution of organic waste salt and ammonium salt catalyst is dried, ground and sieved, and then pyrolyzed at 300-700°C in an inert atmosphere. The solid after pyrolysis is dissolved in water, filtered, and the filtrate is evaporated and recrystallized to obtain inorganic salts. The filter residue is removed and freeze-dried, and a carbon nanomaterial that can be used for a supercapacitor or a battery negative electrode is obtained after high-temperature graphitization treatment. The ammonium salt catalyst used in this method is a disposable drug and cannot be recycled. In addition, the pyrolysis atmosphere is a nitrogen or argon atmosphere, and the operating cost is relatively high. When used in an actual production process, the investment cost needs to be fully evaluated.

[0006] Therefore, in view of the problems of high treatment temperature and incomplete removal of organic matter in the current process of pyrolysis of industrial waste salt to remove organic matter, it is necessary to develop more efficient catalytic materials and catalytic pyrolysis processes to further reduce the catalytic pyrolysis treatment temperature and achieve deep removal of organic matter in industrial waste salt. Summary of the invention

[0007] In view of the deficiencies of the prior art, the object of the present invention is to provide a catalyst for catalytic pyrolysis of industrial organic waste salts, and a preparation method and application thereof. In the present invention, by designing the specific composition of the catalyst and the method for catalytic pyrolysis of industrial organic waste salts, the catalyst provided by the present invention can be used to catalytically pyrolyze industrial organic waste salts at a relatively low temperature, and the process conditions for preparing the catalyst are relatively mild, and the prepared catalyst can be reused, thereby reducing the production cost and catalytic pyrolysis treatment temperature of the catalytic pyrolysis of industrial organic waste salts, and achieving deep removal of organic matter in industrial waste salts.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a catalyst for catalytic pyrolysis of industrial organic waste salt, the catalyst comprising a carrier and a metal oxide supported on the carrier;

[0010] The carrier comprises any one of ceramics, activated alumina, silicon oxide or silicon-alumina molecular sieve or a combination of at least two thereof;

[0011] The metal oxide includes any one or a combination of at least two of copper oxide (CuO), nickel oxide (NiO), cerium oxide (CeO2), lanthanum oxide (La2O3), zirconium oxide (ZrO2), cobalt oxide (Co2O3), manganese oxide (MnO), vanadium oxide (V2O5) or chromium oxide (Cr2O3).

[0012] In the present invention, by designing the specific composition of the catalyst and the method for catalytic pyrolysis of industrial organic waste salt, the industrial organic waste salt can be catalytically pyrolyzed at a relatively low temperature using the catalyst provided by the present invention, and the process conditions for preparing the catalyst are relatively mild. The prepared catalyst can be reused, thereby reducing the production cost of the catalytic pyrolysis of industrial organic waste salt and the catalytic pyrolysis treatment temperature, and achieving deep removal of organic matter in the industrial waste salt.

[0013] The method for catalytic pyrolysis of industrial organic waste salt provided by the present invention can not only reduce the COD of industrial solid waste salt to below 109 mg / Kg (waste salt), but also prevent the solid waste salt from melting and prevent the pyrolysis equipment from malfunctioning and affecting its normal operation.

[0014] Transition metal oxides are inexpensive, have good reducibility, high thermal stability and high anti-toxicity, and are extremely advantageous in low-temperature catalytic oxidation. Using transition metal oxides as the active component of the catalyst and loading them on a carrier material with a large specific surface area and a porous structure can promote the uniform dispersion of active sites and strengthen the chemical reaction process. As the temperature of the furnace body increases, the organic matter in the waste salt gradually gasifies or decomposes to produce volatile organic pollutants. The catalyst present in the gaps between the waste salt particles can adsorb and fix pollutant molecules and promote further decomposition of organic pollutants through surface active oxygen species. At the same time, the transition metal oxides are reduced and oxygen vacancies are generated on the surface. In an oxygen-rich atmosphere, oxygen vacancies are supplemented by oxygen in the gas phase, resulting in the reactivation of the adsorbed oxygen and the reoxidation of the reduced metal oxide. Oxygen vacancies in the active components of the catalyst play an important role in this process.

[0015] In the present invention, by selecting specific transition metal oxides, the catalytic pyrolysis treatment temperature of industrial organic waste salt is reduced, the deep removal effect of organic matter in industrial waste salt is improved, and the catalyst is made reusable, thereby reducing the production cost of catalytic pyrolysis of industrial organic waste salt.

[0016] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the objectives and beneficial effects of the present invention can be better achieved and realized.

[0017] As a preferred technical solution of the present invention, the carrier is a silicon-aluminum molecular sieve.

[0018] Preferably, the silicon-aluminum ratio of the silicon-aluminum molecular sieve is 20-1500 (for example, 50, 200, 300, 400, 500, 600, 800, 1000, 1200, 1400 or 1500, etc.), and more preferably 200-400.

[0019] In the present invention, by selecting a silicon-aluminum molecular sieve with a specific silicon-aluminum ratio as a catalyst carrier, the depth of removal of organic matter in industrial waste salt can be further improved. If the silicon-aluminum ratio of the silicon-aluminum molecular sieve is too large or too small, the depth of removal of organic matter in industrial waste salt will be poor.

[0020] Preferably, the metal oxide is selected from copper oxide and / or cobalt oxide, and more preferably is a combination of copper oxide and cobalt oxide.

[0021] Bimetallic oxide catalysts can construct more lattice defects and oxygen vacancies, which are more conducive to oxygen adsorption and activation, as well as organic matter adsorption, and enhance the catalytic degradation reaction of organic matter.

[0022] Preferably, the metal oxide is selected from a combination of copper oxide and cobalt oxide, and the mass ratio of Cu element to Co element in the metal oxide is (0.25-4):1, for example, it can be 0.25:1, 0.5:1, 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1 or 4:1, etc.

[0023] In the present invention, the deep removal effect of organic matter in industrial waste salt can be further improved by controlling the molar ratio of copper oxide to cobalt oxide within a specific range.

[0024] As a preferred technical solution of the present invention, taking the mass percentage of the catalyst as 100%, the mass percentage of the metal element in the catalyst is 2-10%, for example, it can be 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%.

[0025] It should be noted that the metal element in the catalyst refers to the metal element in the metal oxide in the catalyst, and the metal element is selected from any one of Cu, Ni, Ce, La, Zr, Co, Mn, V or Cr, or a combination of at least two thereof.

[0026] In the present invention, by controlling the content of metal oxide in the catalyst within a specific range, the removal effect of organic matter in industrial waste salt can be improved. If the content of metal oxide in the catalyst is too low, the removal effect of organic matter in industrial waste salt is poor; if the content of metal oxide in the catalyst is too high, it will cause waste of catalyst.

[0027] Preferably, the catalyst has a D 50 The particle size is 100nm~10μm.

[0028] In the present invention, by controlling the D 50 When the particle size is within a specific range, it can be fully mixed with industrial organic waste salt, thereby achieving deep removal of organic matter in industrial waste salt.

[0029] It should be noted that in the present invention, the catalyst is in the form of powder.

[0030] In a second aspect, the present invention provides a method for preparing a catalyst for catalytic pyrolysis of industrial organic waste salt as described in the first aspect, the preparation method comprising the following steps:

[0031] The metal inorganic salt and citric acid are dissolved in water, and the carrier is added thereto, mixed, dried, and calcined to obtain the catalyst.

[0032] It should be noted that the metal cation in the metal salt is selected from Cu 2+ 、Ni 2+ 、Ce 2+ ,La 3+ 、Zr 4+ 、Co 3+ , Mn 2+ 、V 3+ Cr 3+ Any one or a combination of at least two of; anions exemplarily include: Cl ˉ 、SO4 2- and NO3 ˉ . Metal oxides are formed by high-temperature calcination and decomposition of metal inorganic salts.

[0033] As a preferred technical solution of the present invention, the mass ratio of the metal inorganic salt to citric acid is 1:(0.5-2); for example, it can be 1:0.5, 1:0.6, 1:0.8, 1:1, 1:1.2, 1:1.4, 1:1.6, 1:1.8 or 1:2, etc.

[0034] Preferably, the mixing time is 12 to 24 hours, for example, it can be 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours or 24 hours.

[0035] Preferably, the drying temperature is 100-120°C (for example, it can be 100°C, 102°C, 104°C, 106°C, 108°C, 110°C, 112°C, 114°C, 116°C, 118°C or 120°C, etc.), and the drying time is 12-24h (for example, it can be 12h, 16h, 18h, or 24h, etc.).

[0036] Preferably, the calcination temperature is 400-600°C (for example, 400°C, 420°C, 450°C, 480°C, 500°C, 520°C, 540°C, 560°C, 580°C or 600°C, etc.), and the calcination time is 2-4h (for example, 2h, 2.5h, 3h, 3.5h or 4h, etc.).

[0037] As a preferred technical solution of the present invention, the method for preparing the catalyst for catalytic pyrolysis of industrial organic waste salt specifically comprises the following steps:

[0038] The metal inorganic salt and citric acid are dissolved in water, a carrier is added thereto, mixed for 12 to 24 hours, dried at 100 to 120° C. for 12 to 24 hours, and then calcined at 400 to 600° C. for 2 to 4 hours to obtain the catalyst;

[0039] The mass ratio of the metal inorganic salt to citric acid is 1:(0.5-2), and the mass percentage of the metal element in the catalyst is 2-10%.

[0040] It should be noted that the present invention does not have any special restrictions on the amount of solvent water used in preparing the above catalyst, and the commonly used amount range in the art is applicable.

[0041] In a third aspect, the present invention provides a method for catalytic pyrolysis of industrial organic waste salt, the method comprising the following steps:

[0042] (1) In an oxygen-containing atmosphere, industrial organic waste salt particles and the catalyst described in the first aspect are mixed and catalytically pyrolyzed;

[0043] (2) dissolving the solid after catalytic pyrolysis in water, filtering to obtain a filtrate and a filter residue, evaporating and crystallizing the filtrate to obtain a crystalline salt, thereby completing the catalytic pyrolysis of industrial organic waste salt.

[0044] As a preferred technical solution of the present invention, the oxygen-containing atmosphere includes air and / or oxygen.

[0045] Preferably, in the oxygen-containing atmosphere, the amount of oxygen introduced is 5 to 20 times the COD of the industrial organic waste salt particles, for example, it can be 5 times, 6 times, 7 times, 8 times, 9 times, 10 times, 11 times, 12 times, 13 times, 14 times, 15 times, 16 times, 17 times, 18 times, 19 times or 20 times, etc.

[0046] It should be noted that the degree of waste salt pollution is measured by the total organic carbon (TOC) or chemical oxygen demand (COD) value measured after the waste salt is prepared into brine. COD is an important indicator of water pollution. The greater the degree of water pollution, the higher the COD index; TOC is a comprehensive indicator of the total amount of organic matter in the water sample. Its measurement principle is to use platinum as a catalyst to oxidize and burn the water sample, and measure the increase in CO2 in it to determine the total carbon content in the water sample.

[0047] Preferably, the D of the industrial organic waste salt particles is 50The particle size is ≤300μm (for example, it can be 10μm, 20μm, 50μm, 70μm, 100μm, 120μm, 150μm, 180μm, 200μm, 220μm, 240μm, 250μm, 270μm or 300μm, etc.), preferably 150μm to 250μm.

[0048] In the present invention, by controlling the D 50 Within a specific range of particle size, industrial organic waste salt with smaller particle size has a larger specific surface area, which facilitates subsequent thorough mixing with catalyst powder, and is beneficial for subsequent uniform distribution of organic pollutants in catalytic pyrolysis in the industrial organic waste salt particles, allowing for full contact and reaction with the catalyst.

[0049] Preferably, the industrial organic waste salt particles include any one of pesticide organic waste salt particles, pharmaceutical organic waste salt particles, printing and dyeing organic waste salt particles, lithium battery organic waste salt particles, and coal chemical organic waste salt particles, or a combination of at least two of them.

[0050] Preferably, the main components of the industrial organic waste salt particles are sodium chloride and / or sodium sulfate, and also include organic pollutants.

[0051] Preferably, the mass ratio of the industrial organic waste salt particles to the catalyst is ≤50:1 (for example, it may be 5:1, 10:1, 15:1, 20:1, 25:1, 30:1, 35:1, 40:1 or 50:1, etc.).

[0052] In the present invention, by controlling the mass ratio of industrial organic waste salt particles to the catalyst within a specific range, deep removal of organic matter in industrial waste salt can be achieved. If the mass ratio of industrial organic waste salt particles to the catalyst is too large, that is, the amount of the catalyst is too small, the removal effect of organic matter in industrial waste salt is poor; if the mass ratio of industrial organic waste salt particles to the catalyst is small, that is, the amount of the catalyst is too large, it will cause a waste of catalyst and increase the treatment cost.

[0053] Based on actual industrial production considerations, the mass ratio of the industrial organic waste salt particles to the catalyst may preferably be (10-50):1.

[0054] As a preferred technical solution of the present invention, the temperature of the catalytic pyrolysis is 350-550°C, for example, it can be 350°C, 370°C, 400°C, 420°C, 440°C, 460°C, 480°C, 500°C, 520°C, 540°C or 550°C.

[0055] Preferably, the catalytic pyrolysis time is 30 min to 90 min, for example, it can be 30 min, 40 min, 50 min, 60 min, 70 min, 80 min or 90 min.

[0056] Preferably, the catalytic pyrolysis method comprises using a heating furnace to perform catalytic pyrolysis.

[0057] The heating furnace is a rotary tube furnace or a rotary kiln.

[0058] Preferably, the heating rate of the heating furnace is 5 to 20°C / min, for example, it can be 5°C / min, 7°C / min, 8°C / min, 10°C / min, 12°C / min, 14°C / min, 16°C / min, 18°C / min or 20°C / min.

[0059] As a preferred technical solution of the present invention, a pretreatment step is also included before mixing the industrial organic waste salt particles and the catalyst.

[0060] The pretreatment method comprises: crushing and drying the industrial organic waste salt.

[0061] Preferably, the pulverizing method includes grinding and ball milling.

[0062] Preferably, the drying temperature is 90-120°C, for example, it may be 90°C, 92°C, 94°C, 96°C, 98°C, 100°C, 102°C, 105°C, 108°C, 111°C, 114°C, 117°C or 120°C, etc.

[0063] Preferably, the drying time is 12 h to 24 h, for example, it can be 12 h, 14 h, 16 h, 18 h, 20 h, 22 h or 24 h.

[0064] In the present invention, most of the water in the industrial organic waste salt can be removed by drying, so as to avoid the waste salt from sticking into blocks and hanging on the wall, which will affect the subsequent operation.

[0065] As a preferred technical solution of the present invention, the method for catalytic pyrolysis of industrial organic waste salt specifically comprises the following steps:

[0066] (1) After crushing the industrial organic waste salt, dry it at 90-120°C for 12h-24h to obtain D 50 Industrial organic waste salt particles with a particle size of ≤300μm;

[0067] In an oxygen-containing atmosphere, industrial organic waste salt particles and the catalyst according to any one of claims 1 to 3 are mixed at a mass ratio of ≤50:1, a heating furnace is used, the heating rate of the heating furnace is controlled to be 5 to 20°C / min, and catalytic pyrolysis is performed at 350 to 550°C for 30 to 90 minutes;

[0068] Among them, in the oxygen-containing atmosphere, the amount of oxygen introduced is 5 to 20 times the COD of the industrial organic waste salt particles;

[0069] (2) dissolving the solid after catalytic pyrolysis in water, filtering to obtain a filtrate and a filter residue, evaporating and crystallizing the filtrate to obtain a crystalline salt, thereby completing the catalytic pyrolysis of industrial organic waste salt.

[0070] Compared with the prior art, the present invention has the following beneficial effects:

[0071] (1) In the present invention, by designing the specific composition of the catalyst and the method for catalytic pyrolysis of industrial organic waste salt, the catalyst provided by the present invention can be used to catalytically pyrolyze industrial organic waste salt at a relatively low temperature, and the catalyst preparation process conditions are relatively mild. The production cost and catalytic pyrolysis treatment temperature of the industrial organic waste salt are relatively low, thereby achieving deep removal of organic matter in the industrial waste salt.

[0072] (2) Compared with catalytic pyrolysis treatment without using a catalyst, the present invention limits the specific selection of the catalyst, dissolves the mixture of waste salt after pyrolysis and the catalyst in deionized water, filters the catalyst, and prepares a brine with a salt content of 100 g / L. The COD content is measured to be less than 41.2 mg / L.

[0073] (3) In the present invention, by selecting a silicon-aluminum molecular sieve with a specific silicon-aluminum ratio as a carrier, copper oxide and cobalt oxide as active ingredients, and controlling the mass ratio of the Cu element and the Co element in the catalyst within a specific range, and controlling the mass ratio of the industrial organic waste salt and the catalyst within a specific range during the catalytic pyrolysis process, the catalyst can improve the removal effect of organic pollutants in the industrial waste salt particles. The mixture of industrial waste salt and the catalyst after catalytic pyrolysis was dissolved in deionized water, and after filtering the catalyst, it was prepared into a salt water with a salt content of 100g / L, and its COD content was measured to be 24.2mg / L. DETAILED DESCRIPTION

[0074] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0075] The sources of some components in the embodiments and comparative examples are as follows:

[0076] Industrial organic waste salt: The same batch of industrial organic waste salt is used in the following examples and comparative examples, and its main inorganic salt component is Na2SO4. When it is dissolved in pure water to prepare 100g / L brine, the COD content is measured to be 391.2±5mg / L. It should be noted that although the same batch of industrial waste salt is used in the following examples and comparative examples, the COD of the waste salt before catalytic pyrolysis is slightly different due to the experimental schedule and the influence of COD test errors, and the differences are all within the allowable error range.

[0077] The preparation method of the industrial organic waste salt particles used in the following examples and comparative examples is as follows:

[0078] The industrial organic waste salt was crushed by grinding and dried at 110°C for 24h to obtain D 50 Industrial organic waste salt particles with a particle size of 200μm.

[0079] The numbers following the silica-alumina molecular sieve as the carrier of the catalyst used in the following examples and comparative examples represent the silicon-alumina ratio, such as "ZSM" in ZSM-50 represents silica-alumina molecular sieve, and "50" represents the silicon-alumina ratio.

[0080] Example 1

[0081] This embodiment provides a method for catalytic pyrolysis of industrial organic waste salt, which is as follows:

[0082] (1) Catalyst preparation: 0.571 g Cu(NO3)3·9H2O, 0.493 g Co(NO3)2·6H2O and 0.827 g citric acid were weighed into 50 mL water, stirred until dissolved, and then 5 g of silica-alumina molecular sieve ZSM-50 was added. After stirring for 12 h, the mixture was dried at 110°C for 15 h and then taken out. Finally, the mixture was heated to 500°C in a muffle furnace at a rate of 5°C / min for 3 h to obtain a Co and Cu dual-doped catalyst. The mass ratio of Cu to Co in the catalyst was 3:2. Based on the mass percentage of the catalyst as 100%, the mass percentage of Cu and Co in the catalyst was 5%.

[0083] (2) In an air atmosphere, 5 g of industrial organic waste salt particles and the catalyst obtained in step (1) were mixed in a mass ratio of 10:1, catalytically pyrolyzed at 500° C. for 60 min, and then taken out after cooling;

[0084] (3) The mixture of the pyrolyzed catalyst and industrial organic waste salt is dissolved in deionized water to prepare a brine with a salt content of 100 g / L, and the inorganic salt is completely dissolved by magnetic stirring. The catalyst is filtered out to obtain a filtrate, and the filtrate is evaporated and crystallized to obtain crystalline salt, thereby completing the catalytic pyrolysis of the industrial organic waste salt.

[0085] Example 2

[0086] This embodiment provides a method for catalytic pyrolysis of industrial organic waste salt, which differs from Embodiment 1 only in that:

[0087] The catalyst carrier ZSM-50 in step (1) of Example 1 was replaced with an equal mass of ZSM-300;

[0088] Other conditions are the same as in Example 1.

[0089] Example 3

[0090] This embodiment provides a method for catalytic pyrolysis of industrial organic waste salt, which differs from Embodiment 1 only in that:

[0091] The catalyst carrier ZSM-50 in step (1) of Example 1 was replaced with an equal mass of ZSM-600;

[0092] Other conditions are the same as in Example 1.

[0093] Example 4

[0094] This embodiment provides a method for catalytic pyrolysis of industrial organic waste salt, which differs from Embodiment 1 only in that:

[0095] The catalyst carrier ZSM-50 in step (1) of Example 1 was replaced with an equal mass of ZSM-1500;

[0096] Other conditions are the same as in Example 1.

[0097] Example 5

[0098] This embodiment provides a method for catalytic pyrolysis of industrial organic waste salt, which differs from Embodiment 1 only in that:

[0099] The catalyst carrier ZSM-50 in step (1) of Example 1 was replaced with an equal mass of ZSM-30;

[0100] Other conditions are the same as in Example 1.

[0101] Example 6

[0102] This embodiment provides a method for catalytic pyrolysis of industrial organic waste salt, which differs from Embodiment 1 only in that:

[0103] The catalyst carrier ZSM-50 in step (1) of Example 1 was replaced with an equal mass of ZSM-2000;

[0104] Other conditions are the same as in Example 1.

[0105] Example 7

[0106] This embodiment provides a method for catalytic pyrolysis of industrial organic waste salt, which differs from Embodiment 2 only in that:

[0107] The catalyst used in this embodiment is a Co and Cu dual-doped catalyst, wherein the mass ratio of Cu to Co is 1:4. In step (1), the amounts of Cu(NO3)3·9H2O and Co(NO3)2·6H2O are 0.191 g and 0.986 g, respectively;

[0108] The other conditions are the same as those in Example 2.

[0109] Example 8

[0110] This embodiment provides a method for catalytic pyrolysis of industrial organic waste salt, which differs from Embodiment 2 only in that:

[0111] The catalyst used in this embodiment is a Co and Cu dual-doped catalyst, wherein the mass ratio of Cu and Co is 4:1, and the amounts of Cu(NO3)3·9H2O and Co(NO3)2·6H2O are 0.764g and 0.246g respectively;

[0112] The other conditions are the same as those in Example 2.

[0113] Example 9

[0114] This embodiment provides a method for catalytic pyrolysis of industrial organic waste salt, which differs from Embodiment 2 only in that:

[0115] The catalyst used in this embodiment is a Co and Cu dual-doped catalyst, the mass ratio of Cu and Co is 1:9, and the amounts of Cu(NO3)3·9H2O and Co(NO3)2·6H2O are 0.0955g and 1.11g respectively;

[0116] The other conditions are the same as those in Example 2.

[0117] Example 10

[0118] This embodiment provides a method for catalytic pyrolysis of industrial organic waste salt, which differs from Embodiment 2 only in that:

[0119] The catalyst used in this embodiment is a Co and Cu doped catalyst, wherein the mass ratio of Cu and Co is 6:1, and the amounts of Cu(NO3)3·9H2O and Co(NO3)2·6H2O are 0.859 g and 0.123 g respectively;

[0120] The other conditions are the same as those in Example 2.

[0121] Embodiment 11

[0122] This embodiment provides a method for catalytic pyrolysis of industrial organic waste salt, which differs from Embodiment 2 only in that:

[0123] Replace 0.493 g Co(NO3)2·6H2O in step (1) with an equal mass of Ni(NO3)2·6H2O;

[0124] The other conditions are the same as those in Example 2.

[0125] Example 12

[0126] This embodiment provides a method for catalytic pyrolysis of industrial organic waste salt, which differs from Embodiment 2 only in that:

[0127] Replace 0.571 g Cu(NO3)3·9H2O in step (1) with 0.743 g Ni(NO3)2·6H2O;

[0128] The other conditions are the same as those in Example 2.

[0129] Example 13

[0130] This embodiment provides a method for catalytic pyrolysis of industrial organic waste salt, which differs from Embodiment 2 only in that:

[0131] The metal oxide in the catalyst is CuO;

[0132] In step (1), Co(NO3)2·6H2O is not used, and the amount of Cu(NO3)3·9H2O used is 0.951 g, and the obtained catalyst is a Cu-doped catalyst; the mass percentage of Cu in the catalyst is 5%;

[0133] The other conditions are the same as those in Example 2.

[0134] Embodiment 14

[0135] This embodiment provides a method for catalytic pyrolysis of industrial organic waste salt, which differs from Embodiment 2 only in that:

[0136] The metal oxide in the catalyst is Co2O3

[0137] In step (1), no Cu(NO3)3·9H2O is used, and the amount of Co(NO3)2·6H2O used is 1.233 g, and the obtained catalyst is a Co-doped catalyst; the mass percentage of Co in the catalyst is 5%;

[0138] The other conditions are the same as those in Example 2.

[0139] Embodiment 15

[0140] This embodiment provides a method for catalytic pyrolysis of industrial organic waste salt, which differs from Embodiment 2 only in that:

[0141] In this embodiment, the mass ratio of industrial organic waste salt to catalyst is 5:1;

[0142] The other conditions are the same as those in Example 2.

[0143] Example 16

[0144] This embodiment provides a method for catalytic pyrolysis of industrial organic waste salt, which differs from Embodiment 2 only in that:

[0145] In this embodiment, the mass ratio of industrial organic waste salt to catalyst is 30:1;

[0146] The other conditions are the same as those in Example 2.

[0147] Embodiment 17

[0148] This embodiment provides a method for catalytic pyrolysis of industrial organic waste salt, which differs from Embodiment 2 only in that:

[0149] In this embodiment, the mass ratio of industrial organic waste salt to catalyst is 50:1;

[0150] The other conditions are the same as those in Example 2.

[0151] Embodiment 18

[0152] This embodiment provides a method for catalytic pyrolysis of industrial organic waste salt, which differs from Embodiment 2 only in that:

[0153] In this embodiment, the mass ratio of industrial organic waste salt to catalyst is 100:1;

[0154] The other conditions are the same as those in Example 2.

[0155] Comparative Example 1

[0156] This comparative example provides a method for pyrolysis of industrial organic waste salt, which is as follows:

[0157] (1) In an air atmosphere, 5 g of industrial organic waste salt was catalytically pyrolyzed at 500 °C for 60 min and then taken out after cooling;

[0158] (2) Dissolve the waste salt after pyrolysis in 50 mL of water, dissolve all the inorganic salts by magnetic stirring, filter to obtain a filtrate, and use a COD meter to test the organic matter content in the filtrate; evaporate the filtrate and crystallize to obtain crystalline salt.

[0159] Comparative Example 2

[0160] This comparative example provides a method for catalytic pyrolysis of industrial organic waste salt, which is as follows:

[0161] (1) Catalyst preparation: 1.804 g of Fe(NO3)3·9H2O was weighed and stirred until dissolved, then 5 g of silica-alumina molecular sieve ZSM-300 was added, stirred for 12 h, dried at 110°C, and finally, the mixture was heated to 500°C in a muffle furnace at a rate of 5°C / min and calcined for 3 h to obtain an Fe-doped catalyst;

[0162] (2) In an air atmosphere, 5 g of industrial organic waste salt and the catalyst obtained in step (1) were mixed in a mass ratio of 10:1, subjected to catalytic pyrolysis at 500° C. for 60 min, and taken out after cooling;

[0163] (3) The mixture was dissolved in 50 mL of water, and the inorganic salt was completely dissolved by magnetic stirring. The mixture was filtered to obtain a filtrate, and the filtrate was evaporated and crystallized to obtain a crystalline salt.

[0164] Comparative Example 3

[0165] This comparative example provides a method for catalytic pyrolysis of industrial organic waste salt, which is as follows:

[0166] (1) Catalyst preparation: 0.571 g Cu(NO3)3·9H2O, 0.493 g Co(NO3)2·6H2O and 0.827 g citric acid were added to 50 mL water, stirred until dissolved, dried at 110°C for 3 h and then taken out; finally, the mixture was heated to 500°C in a muffle furnace at a rate of 5°C / min for 3 h to obtain a CuO-Co2O3 catalyst;

[0167] (2) In an air atmosphere, 5 g of industrial organic waste salt and the catalyst obtained in step (1) were mixed in a mass ratio of 10:1, subjected to catalytic pyrolysis at 500° C. for 60 min, and taken out after cooling;

[0168] (3) The mixture is dissolved in 50 mL of water, and the inorganic salt is completely dissolved by magnetic stirring, and filtered to obtain a filtrate. The organic matter content in the filtrate is tested using a COD meter; the filtrate is evaporated and crystallized to obtain a crystalline salt.

[0169] The industrial organic waste salts before and after catalytic pyrolysis in the above examples and comparative examples were used to prepare brine with a salt content of 100 g / L. After filtering the solid catalyst, the COD content was measured. The results are shown in Table 1 below.

[0170] Table 1

[0171]

[0172]

[0173] As can be seen from the contents of Table 1, in the present invention, by designing the specific composition of the catalyst and the method for catalytic pyrolysis of industrial organic waste salt, the industrial organic waste salt can be catalytically pyrolyzed at a relatively low temperature using the catalyst provided by the present invention, and the process conditions for preparing the catalyst are relatively mild, the production cost of the catalytic pyrolysis of industrial organic waste salt and the catalytic pyrolysis treatment temperature are relatively low, and the deep removal of organic matter in the industrial waste salt is achieved.

[0174] From the comparison of the relevant data of Examples 1-18 and Comparative Examples 1-3, it can be seen that the present invention significantly improves the removal effect of organic pollutants in industrial waste salt by designing the specific composition of the catalyst and further by designing the specific selection of metal oxides and carriers, so that the COD content in the filtrate obtained by dissolving the waste salt after catalytic pyrolysis is 41.2 mg / L.

[0175] It can be seen from Examples 1-6 that the present invention can further enhance the catalyst's removal effect on organic pollutants in industrial waste salt particles by selecting a molecular sieve with a specific silicon-aluminum ratio as a carrier, so that the COD content in the filtrate is 23.7 mg / L.

[0176] It can be seen from Example 2 and Examples 11-14 that the present invention selects two metal oxides as active ingredients in the catalyst, and further selects copper oxide and cobalt oxide as active ingredients in the catalyst, which can further enhance the catalyst's removal effect on organic pollutants in industrial waste salt particles, so that the COD content in the filtrate is 22.7 mg / L. Replacing one of the metal oxides with a Co, Cu dual-doped molecular sieve catalyst or using only one of the metal oxides as an active component will deteriorate the thermal decomposition treatment effect of waste salt.

[0177] It can be seen from Example 2 and Examples 7-10 that the present invention further improves the catalyst's removal effect on organic pollutants in industrial waste salt particles by controlling the mass ratio of Cu element and Co element in the catalyst to (0.25-4):1 (Example 2, Examples 7-8), so that the COD content in the filtrate after catalytic pyrolysis is 22.3 mg / L.

[0178] It can be seen from Examples 2 and 15-18 that the present invention improves the removal effect of the catalyst on organic pollutants in industrial waste salt particles by controlling the mass ratio of industrial organic waste salt particles and the catalyst to ≤50:1, so that the COD content in the filtrate after catalytic pyrolysis is 24.2 mg / L.

[0179] In summary, the present invention designs the specific composition of the catalyst and the method for catalytic pyrolysis of industrial organic waste salt. The catalyst provided by the present invention can be used to catalytically pyrolyze industrial organic waste salt at a relatively low temperature, thereby reducing the production cost and catalytic pyrolysis treatment temperature of the catalytic pyrolysis of industrial organic waste salt, and achieving deep removal of organic matter in industrial waste salt.

[0180] The applicant declares that the present invention illustrates the detailed process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A catalyst for catalytic pyrolysis of industrial organic waste salt, characterized in that: The catalyst comprises a carrier and a metal oxide supported on the carrier; The carrier comprises any one of ceramics, activated alumina, silicon oxide or silicon-alumina molecular sieve or a combination of at least two thereof; The metal oxide includes any one of copper oxide, nickel oxide, cerium oxide, lanthanum oxide, zirconium oxide, cobalt oxide, manganese oxide, vanadium oxide or chromium oxide, or a combination of at least two thereof.

2. The catalyst for catalytic pyrolysis of industrial organic waste salt according to claim 1, characterized in that: The carrier is a silicon-aluminum molecular sieve; Preferably, the silicon-aluminum ratio of the silicon-aluminum molecular sieve is 20 to 1500, more preferably 200 to 400; Preferably, the metal oxide is selected from copper oxide and / or cobalt oxide, and more preferably is a combination of copper oxide and cobalt oxide; Preferably, the metal oxide is selected from a combination of copper oxide and cobalt oxide, and the mass ratio of the Cu element to the Co element in the metal oxide is (0.25-4):

1.

3. The catalyst for catalytic pyrolysis of industrial organic waste salt according to claim 1 or 2, characterized in that: Taking the mass percentage of the catalyst as 100%, the mass percentage of the metal element in the catalyst is 2 to 10%; Preferably, the catalyst has a D 50 The particle size is 100nm~10μm.

4. A method for preparing a catalyst for catalytic pyrolysis of industrial organic waste salts according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: The metal inorganic salt and citric acid are dissolved in water, and the carrier is added thereto, mixed, dried, and calcined to obtain the catalyst.

5. The preparation method according to claim 4, characterized in that: The mixing time is 12 to 24 hours; Preferably, the drying temperature is 100-120°C and the drying time is 12-24h; Preferably, the calcination temperature is 400-600° C. and the calcination time is 2-4 hours.

6. A method for catalytic pyrolysis of industrial organic waste salt, characterized in that: The method for catalytic pyrolysis of industrial organic waste salt comprises the following steps: (1) In an oxygen-containing atmosphere, industrial organic waste salt particles and the catalyst according to any one of claims 1 to 3 are mixed and catalytically pyrolyzed; (2) dissolving the solid after catalytic pyrolysis in water, filtering to obtain a filtrate and a filter residue, evaporating and crystallizing the filtrate to obtain a crystalline salt, thereby completing the catalytic pyrolysis of industrial organic waste salt.

7. The method for catalytic pyrolysis of industrial organic waste salt according to claim 6, characterized in that: The oxygen-containing atmosphere includes air and / or oxygen; Preferably, in the oxygen-containing atmosphere, the amount of oxygen introduced is 5 to 20 times the chemical oxygen demand contained in the industrial organic waste salt; Preferably, the D of the industrial organic waste salt particles is 50 The particle size is ≤300 μm, preferably 150 to 250 μm; Preferably, the industrial organic waste salt includes any one or a combination of at least two of pesticide organic waste salt, pharmaceutical organic waste salt, printing and dyeing organic waste salt, lithium battery organic waste salt particles, and coal chemical organic waste salt; Preferably, the mass ratio of the industrial organic waste salt to the catalyst is ≤50:

1.

8. The method for catalytic pyrolysis of industrial organic waste salt according to claim 6 or 7, characterized in that: The temperature of the catalytic pyrolysis is 350-550°C; Preferably, the catalytic pyrolysis time is 30 to 90 minutes; Preferably, the catalytic pyrolysis method comprises using a heating furnace to perform catalytic pyrolysis; Preferably, the heating furnace has a heating rate of 5 to 20° C. / min.

9. The method for catalytic pyrolysis of industrial organic waste salt according to any one of claims 6 to 8, characterized in that: The step of pre-treating the industrial organic waste salt particles before mixing the catalyst is also included; The pretreatment method comprises: crushing and drying the industrial organic waste salt; Preferably, the pulverizing method includes grinding and ball milling; Preferably, the drying temperature is 90-120°C; Preferably, the drying time is 12 to 24 hours.

10. The method for catalytic pyrolysis of industrial organic waste salt according to any one of claims 6 to 9, characterized in that: The method for catalytic pyrolysis of industrial organic waste salt specifically comprises the following steps: (1) After crushing the industrial organic waste salt, dry it at 90-120°C for 12-24h to obtain D 50 Industrial organic waste salt particles with a particle size of ≤300μm; In an oxygen-containing atmosphere, industrial organic waste salt particles and the catalyst according to any one of claims 1 to 3 are mixed at a mass ratio of ≤50:1, a heating furnace is used, the heating rate of the heating furnace is controlled to be 5 to 20°C / min, and catalytic pyrolysis is performed at 350 to 550°C for 30 to 90 minutes; Among them, in the oxygen-containing atmosphere, the mass of oxygen introduced is 5 to 20 times the mass of COD in the industrial organic waste salt; (2) dissolving the solid after catalytic pyrolysis in water, filtering to obtain a filtrate and a filter residue, evaporating and crystallizing the filtrate to obtain a crystalline salt, thereby completing the catalytic pyrolysis of industrial organic waste salt.

Citation Information

Patent Citations

  • Oxygen-bearing thermal decomposition and catalytic oxidization integration treatment method for chemical waste salts

    CN110107902A

  • Industrial abraum salt decomposition treatment device and method

    CN111774408A

  • System and method for treating industrial waste salt through circulating fluidized bed

    CN111957273A

  • Monolithic catalyst for catalyzing ozone to degrade VOCs as well as preparation and application of monolithic catalyst

    CN112827505A

  • Catalyst for catalytic ozonation of volatile organic compounds and preparation method thereof

    CN113145161A

Cited By

  • Catalyst for cracking and oxidizing organic flue gas generated by melting medical waste salt

    CN119746922A

  • Catalytic pyrolysis of organic waste salt aerogel catalyst and its preparation method and application

    CN122999198A