Cobalt-doped iron-based MOF catalyst and preparation and application thereof

By introducing cobalt atoms into iron-based MOF and using multi-stage solvothermal method, the Fe-O-Co asymmetric structure was constructed, which solved the OH-dominated problem of iron-based MOF catalysts in electron-rich organic matter treatment, and achieved high efficiency dominated by 1O2 Degradation and structural stability are improved, suitable for complex wastewater treatment.

CN118925807APending Publication Date: 2024-11-12ZHEJIANG SCI-TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411057268.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

When existing iron-based MOF catalysts treat electron-rich organic matter, OH dominates the degradation efficiency, and lack of structural stability and durability, making it difficult to adapt to complex industrial wastewater treatment.

Method used

By introducing cobalt atoms, the Fe-O-Co asymmetric structure is constructed, and the ligand coordination defect is reduced by using multi-stage solvothermal method, the electron density of the Fe site is enhanced, and a more stable cobalt-doped iron-based MOF catalyst is formed to promote 1O2 Generation and degradation of electron-rich organic matter.

Benefits of technology

It improves the degradation efficiency of cobalt-doped iron-based MOF catalysts to electron-rich organic matter, enhances structural stability and environmental tolerance, is suitable for deep treatment of complex printing and dyeing wastewater, and has wide pH adaptability and good reusability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925807A_ABST
    Figure CN118925807A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of catalyst synthesis, in particular to a cobalt-doped iron-based MOF catalyst and preparation and application thereof. The invention provides a preparation method of a cobalt-doped iron-based MOF (Metal Organic Framework) catalyst, and the cobalt-doped iron-based MOF catalyst is obtained by carrying out solvothermal reaction on N, N-dimethylformamide containing cobalt salt, iron salt and terephthalic acid and then drying, the solvothermal reaction is carried out at 50 DEG C for 20-30 minutes, then at 100 DEG C for 20-30 minutes, and then at 150 DEG C for 14-22 hours. According to the method for preparing the cobalt-doped Fe-MOFs through multi-stage solvothermal insulation, the ligand coordination defect degree in an iron-based MOF catalyst is reduced, the oxygen vacancy content in the structure is reduced, the surface Lewis acid site density is weakened, and ozone O-O bond breakage, decomposition and conversion are promoted to form < 1 > O2.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalyst synthesis, and in particular to a cobalt-doped iron-based MOF catalyst and a preparation and application thereof. Background Art

[0002] Heterogeneous catalytic ozonation (HCO) technology has attracted much attention due to its advantages such as fast reaction speed, no secondary pollution, and easy and clean oxygen source. It can be applied to the treatment of various polluted wastewaters.

[0003] The core of HCO technology lies in the use of solid catalysts, which provide an active center that can significantly enhance the ability of ozone to oxidize organic matter. The presence of catalysts not only improves the utilization rate of ozone and reduces ozone consumption, but also promotes the production of more strongly oxidizing ·OH, thereby more effectively degrading dyes and other organic pollutants in wastewater.

[0004] Metal organic framework materials (MOFs) have the characteristics of rich pore structure, unsaturated metal coordination, and modifiable structure design, which can provide a unique solution to the problem of active site exposure and mass transfer enrichment. Among them, iron-based MOFs (Fe-MOFs) have abundant Lewis acid sites, which can effectively catalyze the decomposition of ozone to generate ·OH, thereby enhancing the oxidative degradation ability of organic pollutants. 1 O2, as another main reactive group among reactive oxygen species (ROS), has a stronger degradation effect than ·OH on electron-rich organic matter containing unsaturated double bonds and benzene rings such as unsaturated alkanes and phenols.

[0005] Currently, electron-rich organic compounds such as phenols are commonly found in industrial wastewater, such as wastewater from the petrochemical, pharmaceutical, paper and textile industries. 1 O2, it can effectively treat wastewater from the petrochemical, pharmaceutical, paper and textile industries. Summary of the invention

[0006] The present invention provides a cobalt-doped iron-based MOF catalyst and its preparation and application. The present invention introduces heterogeneous metal Co atoms into the iron-oxygen cluster nodes by a mixed metal salt solvothermal method, constructs Fe-O-Co asymmetric structure doping, reduces the degree of ligand coordination defects of the iron-based MOF under the auxiliary effect of multi-stage solvothermal, reduces the oxygen vacancy content in the structure, and then weakens the total acid density of Lewis acid sites on the surface of the iron-based MOF, so that it is converted into 1 O2 dominates, thus adapting to the efficient degradation of electron-rich organic matter.

[0007] In order to achieve the above object, the present invention provides the following technical solutions:

[0008] The present invention provides a method for preparing a cobalt-doped iron-based MOF catalyst. The cobalt-doped iron-based MOF catalyst is obtained by subjecting N,N-dimethylformamide containing cobalt salt, iron salt and terephthalic acid to a solvent thermal reaction and then drying; the solvent thermal reaction is: 20 to 30 minutes at 50°C, then 20 to 30 minutes at 100°C, and then 14 to 22 hours at 150°C.

[0009] The present invention aims to change the dominant group in the iron-based MOF / ozone system from ·OH to 1 O2, thereby achieving directional catalysis of electron-rich organic matter, broadening the application of iron-based MOF in textile printing and dyeing wastewater treatment, and providing a multi-stage solvent thermal insulation method for preparing cobalt-doped Fe-MOFs.

[0010] First, during the nucleation and crystal growth process of Fe-MOFs, multi-stage solvent thermal is used to uniformly dope cobalt into the reconstructed coordination environment and electronic structure of the metal active center, resulting in an increase in the electron density of the Fe site, enhanced Fe-O bond binding force, and healing of some coordination defects. Among them, the growth rate of the crystal nucleus can be controlled during the gradient heating process, making the cobalt doping more uniform, and thus further strengthening the oxygen bridge bond between the Co atom and the Fe atom during multiple heating and insulation processes. The final cobalt-doped iron-based MOF catalyst has a stronger structural stability. The Fe site, as a Lewis acid site for adsorbing ozone, significantly enhances the adsorption capacity of ozone in the cobalt-doped structure, and continues to activate the ozone molecules to decompose and transform to form 1 O2. Finally, due to the cobalt doping 1 Efficient generation of O2 enhances the HCO process 1 Degradation and removal of electron-rich organic pollutants by O2.

[0011] In addition, Co and Fe belong to the fourth period, group VIII transition metals, with the same saturated coordination number, but slightly different electronegativity, atomic radius, and electronic configuration. The introduction of Co can moderately rearrange the electrons in the doped region and reconstruct the degree of d-band delocalization of the metal site. Due to the difference in oxidizability between Co(II) and Fe(III) in the Fe-O-Co asymmetric node structure, the doping of heterogeneous metal Co atoms with the assistance of multi-stage solvothermal treatment can regulate the microenvironment of the metal active center, increase the electron density of the Fe site, strengthen the binding between the ligand oxygen and the Fe atom, make the ligand difficult to leave, reduce the unsaturated coordination center, and finally weaken the total acid density of Lewis acid sites on the surface of MIL-53(Fe)-18H.

[0012] In summary, the total acid density of Lewis acid sites on the surface of the cobalt-doped iron-based MOF catalyst prepared by multi-stage solvent thermal reaction in the present invention is reduced, so that the total acid density of Lewis acid sites on the surface of the cobalt-doped iron-based MOF catalyst ... 1 O2 dominates, thus adapting to the efficient degradation of electron-rich organic matter.

[0013] Furthermore, the applicant conducted degradation tests on a variety of electron-rich organic matter, and found that the cobalt-doped iron-based MOF catalyst showed efficient degradation of a variety of electron-rich organic matter such as 4-AP, HQ, 4-CP, 4-CN, phenol and 4-NP. Among them, the removal rate of 4-CP, phenol, HQ and 4-AP exceeded 96% within 10 minutes. It is confirmed that the cobalt-doped iron-based MOF catalyst obtained under this scheme successfully achieved the regulation of ROS, making the cobalt-doped iron-based MOF catalyst more suitable for the degradation of electron-rich organic matter.

[0014] Preferably, the solvent thermal reaction is: 50°C for 30 min, then 100°C for 30 min, then 150°C for 16 to 20 h.

[0015] Further preferably, the solvent thermal reaction is: 30 min at 50°C, then 30 min at 100°C, then 18 h at 150°C.

[0016] Preferably, the molar ratio of cobalt to iron in the cobalt salt and the iron salt is 1:4.

[0017] Preferably, the iron salt is selected from any one of ferric nitrate, ferric chloride, ferric sulfate and ammonium ferric citrate.

[0018] Preferably, the cobalt salt is selected from any one of cobalt nitrate, cobalt sulfate and cobalt chloride.

[0019] Preferably, the ratio between the total molar amount of cobalt and iron in the cobalt salt and the iron salt and the molar amount of terephthalic acid is 1:1.

[0020] Preferably, the drying temperature is 80-120° C., and the drying time is 12-36 hours.

[0021] More preferably, the drying temperature is 100° C. and the drying time is 24 hours.

[0022] The present invention also provides a cobalt-doped iron-based MOF catalyst prepared by the above preparation method.

[0023] The present invention also provides the application of cobalt-doped iron-based MOF catalyst in the degradation of electron-rich organic pollutants.

[0024] Therefore, the present invention has the following beneficial effects:

[0025] (1) The present invention provides a method for preparing cobalt-doped Fe-MOFs by multi-stage solvent thermal insulation. The cobalt atoms and iron atoms are fully combined through oxygen bridge bonds to form more stable crystal nuclei by multi-stage heating. The growth rate of the crystal nuclei can be controlled during the gradient heating process to achieve uniform doping of cobalt atoms, thereby reducing the degree of ligand coordination defects in the iron-based MOF catalyst, reducing the oxygen vacancy content in the structure, weakening the surface Lewis acid site density, and promoting the ozone OO bond breakage decomposition transformation formation 1 O2.

[0026] (2) The cobalt-doped Fe-MOFs prepared in the present invention exhibit high selectivity for electron-rich organic pollutants and have outstanding degradation efficiency for electron-rich organic pollutants.

[0027] (3) The present invention is developed by 1 The O2-dominated cobalt-doped Fe-MOFs / ozone system has strong environmental tolerance and is suitable for deep treatment of printing and dyeing wastewater with high salt content, complex water quality components and variable matrix composition.

[0028] (4) The cobalt-doped Fe-MOFs obtained in the present invention have good structural stability, wide pH adaptability and good reusability. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 PXRD spectra before and after cobalt doping;

[0030] Figure 2 SEM images before and after cobalt doping, where a is MIL-53(Fe)-18H, b is MIL-53(FeCo)-18H, and c is the mapping image;

[0031] Figure 3 FT-IR images before and after cobalt doping, where a is the full spectrum and b is 400-800 cm -1 A magnified view of the range, c is the Raman spectrum;

[0032] Figure 4 BET diagrams before and after cobalt doping, where a is the nitrogen adsorption / desorption curve and b is the pore size distribution diagram;

[0033] Figure 5 The full XPS spectra before and after cobalt doping, where a is MIL-53(Fe)-18H and b is MIL-53(FeCo)-18H;

[0034] Figure 6 XPS spectra before and after cobalt doping, where a is C1s, b is O1s, c is Fe2p, and d is Co2p;

[0035] Figure 7 Py-FTIR spectra before and after cobalt doping, where a is MIL-53(Fe)-18H and b is MIL-53(FeCo)-18H;

[0036] Figure 8 Solid EPR spectra before and after cobalt doping, where a is MIL-53(Fe)-18H and b is MIL-53(FeCo)-18H;

[0037] Fig. 9 The electrochemical performance diagrams before and after cobalt doping, where a is the Tafel polarization curve, b is the LSV curve, and c is the EIS spectrum;

[0038] Fig.10 EPR spectra of different catalytic ozone systems, where a is the result of DMPO / ·OH and b is the result of DMPO / O2 ·- As a result, c is TEMP / 1 O2 results;

[0039] Fig.11 are the performance diagrams of different catalytic ozone systems, where a is the fluorescence spectrum of catalytic ozone oxidation of coumarin, b is the fluorescence spectrum of catalytic ozone oxidation of coumarin corresponding to different time points, c is the curve of the cumulative concentration of ·OH produced versus time, d is the degradation curve of oxidized MDE, e is the corresponding pseudo-first-order kinetic fitting curve, and f is 1 O2 steady-state concentration bar graph;

[0040] Fig.12 is the effect diagram of the quencher, where a is the effect of the quencher on the ozone degradation of 4-NP catalyzed by cobalt-doped MIL-53(Fe)-18H, and b is the k value corresponding to a;

[0041] Fig.13 The results of catalytic ozone degradation of phenol and 4-NP are shown in Figure 1, where a is the catalytic ozone degradation of phenol and the pseudo-first-order kinetic fitting results, b is the catalytic ozone degradation of 4-NP and the pseudo-first-order kinetic fitting results, and c is the k value corresponding to a and b;

[0042] Fig.14 The degradation effect of MIL-53(FeCo)-18H on different pollutants, where a is a schematic diagram of selective degradation of electron-rich organic pollutants, b is a curve of catalytic ozone degradation of various organic pollutants, and c is the linear fitting result of k value and IP value;

[0043] Fig.15 The catalytic ozone decomposition kinetics result diagram, where a is the ozone decomposition curve and b is the pseudo-first-order kinetic fitting curve;

[0044] Fig.16The effect of water matrix on the catalytic effect of catalyst, where a is inorganic salt (200 mg L -1 ) is the effect of HA on the catalytic ozone degradation of phenol by MIL-53(FeCo)-18H, b is the effect of HA on the catalytic ozone degradation of phenol by MIL-53(FeCo)-18H;

[0045] Fig.17 Figure 2 is the result diagram of catalyst stability and adaptability, where a is the effect of initial pH on ozone degradation of phenol, b is the k value corresponding to a, c is the repeated use performance diagram, d is the FT-IR spectrum before and after repeated use, and e is the PXRD spectrum before and after repeated use. DETAILED DESCRIPTION

[0046] The present invention is further described below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.

[0047] [Example]

[0048] Example 1

[0049] Cobalt-doped MIL-53(Fe)-18H was prepared by a solvothermal method. The specific preparation method is as follows: at room temperature, a metal salt mixed with 16mmol FeCl3·6H2O and 4mmol CoCl2·6H2O and 20mmol terephthalic acid (H2BDC) were dissolved in 120mL N,N-dimethylformamide (DMF) to obtain a clear and transparent precursor solution, which was then transferred to a polytetrafluoroethylene reactor and kept at 50℃ for 30min, then heated to 100℃ for another 30min, and finally heated to 150℃ for 18h. After the reaction timer was terminated, the crude catalyst was obtained by centrifugation at 10000rpm for 5min after natural cooling, and then washed at least three times with 50mL DMF and 50mL ethanol respectively to completely remove the residual raw materials and impurities. Finally, the washed solid was placed in a vacuum oven at 100℃ and dried for 24h to obtain a yellow powder catalyst, which was marked as MIL-53(FeCo)-18H.

[0050] Comparative Example 1

[0051] MIL-53(Fe)-18H was prepared by a solvothermal method. The specific preparation method is as follows: at room temperature, 20mmolFeCl3·6H2O and 20mmolH2BDC were dissolved in 120mL DMF to obtain a clear and transparent precursor solution, and then the solution was transferred to a polytetrafluoroethylene reactor, kept at 50℃ for 30min, then heated to 100℃ for another 30min, and finally heated to 150℃ for 18h. After the reaction timer was terminated, the crude catalyst was obtained by centrifugation at 10000rpm for 5min after natural cooling, and then washed at least three times with 50mL DMF and 50mL ethanol respectively to completely remove the residual raw materials and impurities. Finally, the washed solid was placed in a vacuum oven at 100℃ and dried for 24h to obtain a yellow powder catalyst, which was marked as MIL-53(Fe)-18H.

[0052]

Performance test

[0053] 1. Structural characterization

[0054] ①Crystal structure

[0055] In order to explore the structural evolution caused by cobalt doping, the MIL-53(FeCo)-18H obtained in Example 1 and the MIL-53(Fe)-18H obtained in Comparative Example 1 were subjected to PXRD tests. The results are as follows: Figure 1 shown.

[0056] observe Figure 1 It can be seen that the PXRD spectrum of undoped MIL-53(Fe)-18H shows four obvious characteristic peaks at 2θ of 9.4°, 12.6°, 18.9° and 22.1°, while in the PXRD spectrum of cobalt-doped MIL-53(Fe)-18H, in addition to the above four characteristic peaks, there are two new characteristic peaks located at 2θ of 17.6° and 25.4°. In addition, it is found that the intensity ratio of the two characteristic peaks at 12.6° and 18.9° has increased significantly. This shows that cobalt doping will cause Co atoms to partially and evenly occupy the Fe atom position in the MIL-53(Fe)-18H ferroxene cluster node, causing the morphology and structure of MIL-53(Fe)-18H to change.

[0057] ② Appearance

[0058] In order to further verify the results of PXRD, the MIL-53(FeCo)-18H obtained in Example 1 and the MIL-53(Fe)-18H obtained in Comparative Example 1 were subjected to SEM test, and the results are as follows: Figure 2 shown.

[0059] observe Figure 2 It can be seen that: Figure 2a It can be observed that MIL-53(Fe)-18H presents a bipyramidal hexagonal prism morphology with a large number of cracks and the cone tip disappears. Figure 2 The MIL-53(FeCo)-18H crystal corresponding to b presents irregular fragment shape. Figure 1 As a result, the formation of Fe-O-Co asymmetric node structure leads to the accelerated evolution of the crystal structure of MIL-53(Fe)-18H, which may be due to the Co-O bond dissociation energy (397.4±8.7D o 298 / kJ mol -1 ) is slightly smaller than the Fe-O bond dissociation energy (407.0±1.0D o 298 / kJ mol -1 ), so the MIL-53(FeCo)-18H crystal is thermodynamically unstable due to the replacement of part of the Fe-O structure by the Co-O structure, and tends to break into irregular fragments.

[0060] ③Molecular structure

[0061] Furthermore, the organic linkers and iron oxide cluster structures of MIL-53(FeCo)-18H and MIL-53(Fe)-18H catalysts were comprehensively studied by FT-IR and Raman spectroscopy. Figure 3 shown.

[0062] observe Figure 3 a and Figure 3 bIt can be seen that: Figure 3 In a, the FT-IR spectra of both cobalt-doped and undoped MIL-53(Fe)-18H show a peak at 750 cm -1 、820cm -1 and 1016cm -1 The characteristic absorption peaks at left and right wave numbers are attributed to the deformation vibration of the CH bond on the benzene ring of the organic linker H2BDC; and the peaks at 1389cm -1 and 3429cm -1 The characteristic absorption peaks at left and right wavenumbers are respectively attributed to the symmetric stretching vibration of -COOH of H2BDC substituent and the OH stretching vibration of water molecules adsorbed on the catalyst surface or bound to the metal site. Figure 3 It can be observed in b that the relative position of MIL-53(Fe)-18H is 552 cm -1 The wave number is attributed to the characteristic absorption peak of Fe-O bond stretching vibration. The characteristic peak of MIL-53(FeCo)-18H is red-shifted to 544 cm -1This may be due to the partial replacement of Fe atoms in the Fe-O-Fe node structure by Co atoms to form a new Fe-O-Co node structure, which also shows that the heterogeneous metal Co atoms are successfully doped into the MIL-53(Fe)-18H structure.

[0063] In addition, observation Figure 3 The Raman results in c show that in the Raman spectra of undoped and cobalt-doped MIL-53(Fe)-18H, a -1 、1450cm -1 and 1426cm -1 The characteristic absorption peaks at left and right wave numbers correspond to the carboxyl groups in the H2BDC structure; -1 The characteristic peaks of the left and right wave numbers correspond to the C=O structure; the characteristic peak associated with the Fe-O(H)-Fe(Co) bridging group is located at 863 cm -1 At the same time, the characteristic absorption peak of Fe-O bond stretching vibration is located at 631cm -1 about.

[0064] ④Aperture

[0065] The porous structures of MIL-53(Fe)-18H and MIL-53(FeCo)-18H were evaluated using the BET technique. The test conditions were: degassing temperature 100°C. The results are shown in Figure 4 And as shown in Table 1.

[0066] observe Figure 4 It can be seen that: Figure 4 In a, both nitrogen adsorption / desorption curves have typical IV type isotherms and H3 type hysteresis loops, indicating that both doped and undoped MIL-53(Fe)-18H have mesoporous material properties. From the pore size distribution diagram, it can be seen that the pore sizes of both are mainly distributed between 2-10nm, further reflecting the porous structure of undoped and cobalt-doped MIL-53(Fe)-18H catalysts with mesopores as the main component. In addition, the latter is significantly more distributed in the pore size range of 2-10nm than the former, indicating that the pore structure of MIL-53(FeCo)-18H has changed, and it is predicted that MIL-53(FeCo)-18H has a larger pore volume and specific surface area.

[0067] Table 1 Pore structure information of undoped and cobalt-doped MIL-53(Fe)-18H

[0068]

[0069] ⑤Element composition and chemical state

[0070] Figure 2In c, the undoped and cobalt-doped MIL-53(Fe)-18H catalysts have been mapped. From the element distribution in the figure, it can be seen that Co does exist and the Co element is evenly distributed. Comparing the EDS results in Table 2, it can be intuitively found that the three elements of C, O, and Fe in MIL-53(Fe)-18H account for 55.98%, 33.74%, and 10.28%, respectively, and the Fe and Co elements in MIL-53(FeCo)-18H account for 9.81% and 0.65%, respectively, indicating that the experiment successfully prepared cobalt-doped MIL-53(Fe)-18H.

[0071] Table 2 EDS data information of undoped and cobalt-doped MIL-53(Fe)-18H

[0072] catalyst C(%) O(%) Fe(%) Co(%) MIL-53(Fe)-18H 55.98 33.74 10.28 - MIL-53(FeCo)-18H 57.91 31.63 9.81 0.65

[0073] In order to further analyze and verify the elemental composition and element valence state of undoped and cobalt-doped MIL-53(Fe)-18H, this application uses XPS technology to characterize the two catalysts, and the results are as follows: Figures 5-6 shown.

[0074] observe Figure 6 From the high-resolution C1sXPS spectrum of a, it can be found that the three peaks located near the binding energies of 284.6, 285.2, and 289.1 eV are respectively attributed to the carbon atoms in the CC / CH, CO, and C=O structures on the benzene ring of the organic ligand.

[0075] like Figure 6 c. In the high-resolution Fe 2p XPS spectra of MIL-53(Fe)-18H and MIL-53(FeCo)-18H, the two characteristic peaks at around 711 eV and 724 eV correspond to the Fe 2p 3 / 2 and Fe 2p 1 / 2 Meanwhile, the other two signal peaks located at 718eV and 731eV belong to the characteristic satellite peaks of Fe(Ⅲ), indicating that the Fe element mainly exists in the +3 valence state in both the undoped and cobalt-doped MIL-53(Fe)-18H catalysts. 1 / 2 and Fe 2p 3 / 2 The characteristic peaks show that their binding energy shifts from high to low, which is due to the weakening of the anchoring effect of Fe(III) on the outermost electrons, indicating that the electron density of Fe(III) in MIL-53(FeCo)-18H increases, indicating a decrease in the density of Lewis acid sites on its surface. Figure 6 In d, the characteristic peaks at 783.8 eV and 797.3 eV represent the Co 2p3 / 2 and Co 2p 1 / 2 The Co(II) in the region; the characteristic peaks at 789.3eV and 804.6eV belong to the oscillating satellite peaks of Co(II), indicating that the doped Co element mainly exists in the divalent form, and no other valence states are found. In the high-resolution O1sXPS spectrum of MIL-53(Fe)-18H, three different characteristic peaks appeared by fitting the peaks, indicating the existence of three different types of O, whose binding energies are located at 530.0, 531.9 and 533.3eV, respectively, and correspond to lattice oxygen (Olatt), surface hydroxyl groups (Oads) formed by oxygen vacancies adsorbed water molecules, and surface residual water molecules (Osurf). After cobalt doping, the area ratio of Oads to Olatt decreased from 5.56 to 4.55, which may be due to the reduction of low-coordinated metal sites, so the number of surface metal-hydroxyl (M-OH) adducts formed by adsorbed water molecules also decreased, indicating that cobalt doping reduced the oxygen vacancy content in the MIL-53(Fe)-18H catalyst structure.

[0076] ⑥Lewis acid site density

[0077] In the section "⑤ Element composition and chemical state", the applicant has found from the XPS results that the electron density of Fe(III) in MIL-53(Fe)-18H increases after cobalt doping, which reduces the Lewis acid site density on the surface of MIL-53(FeCo)-18H. On this basis, the applicant has conducted Py-FTIR technology measurement on MIL-53(Fe)-18H before and after doping, and the results are as follows: Figure 7 And as shown in Table 3.

[0078] like Figure 7 As shown in the figure, the unsaturated metal coordination center adsorbs and combines with the pyridine molecule to form the ν18a and ν12 vibration forms at 1070 cm -1 and 1040cm -1 Corresponding signal peaks appeared nearby, and the density of different acid site types on the surface of each catalyst was quantitatively calculated based on the ν18a signal peak area.

[0079] It can be seen from Table 3 that the total acid density of MIL-53(FeCo)-18H (1.76 mmol g -1 ) decreased compared with MIL-53(Fe)-18H (2.08mmol g -1 ) decreased by 15.4%, which is consistent with the prediction results of Fe 2p XPS spectrum analysis. At the same time, the density of neutral acid also decreased slightly from 0.68 mmol g -1 Reduced to 0.56 mmol g -1In addition, the weak acid density of MIL-53(Fe)-18H is significantly reduced, and the weak acid density of MIL-53(Fe)-18H is more than 10 times that of MIL-53(FeCo)-18H. However, the strong acid density of MIL-53(FeCo)-18H is improved compared with MIL-53(Fe)-18H, from 0.97mmol g -1 Increased to 1.15 mmol g -1 It can be seen that the introduction of Co in the ferrite cluster node changes the electronic structure of the Fe site, thereby affecting the composition type and density of Lewis acid sites on the surface of MIL-53(Fe)-18H.

[0080] Table 3 Surface Lewis acid site density of undoped and cobalt-doped MIL-53(Fe)-18H

[0081]

[0082] ⑦ Oxygen vacancies

[0083] This application uses solid EPR technology to characterize MIL-53(Fe)-18H before and after cobalt doping. The test conditions are: microwave frequency 9.85GHz, power 12.72mW. The results are as follows Figure 8 shown.

[0084] observe Figure 8 It can be seen that two symmetrical signal peaks belonging to oxygen vacancies at the nodes of ferrite clusters appear near the g value of 2.000, and the characteristic signal peak intensity of MIL-53(FeCo)-18H is weaker than that of MIL-53(Fe)-18H, indicating that the oxygen vacancy content in the former structure is less than that in the latter, that is, the ligand coordination defects are fewer, which is consistent with the XPS results.

[0085] In addition, the g value can be used to determine the coordination environment of the metal site, the Fe(III) center. Figure 8 The signal peak that appears symmetrically around g=2.02 belongs to the unsaturated tetracoordinated Fe(III) (the saturated coordination of Fe(III) is hexacoordinated). This confirms that the unsaturated coordination of MIL-53(Fe)-18H exists in the form of tetracoordinated [FeO4], and the tetracoordinate number of MIL-53(FeCo)-18H is lower than that of MIL-53(Fe)-18H.

[0086] ⑧Electrochemical performance

[0087] This application uses an electrochemical workstation to characterize the electrochemical properties of MIL-53(Fe)-18H before and after cobalt doping. The results are as follows: Fig. 9 shown.

[0088] observe Fig. 9It can be seen that compared with MIL-53(Fe)-18H, MIL-53(FeCo)-18H shows a relatively smaller arc radius in the EIS spectrum and a higher current density in the LSV curve, indicating that the MIL-53(FeCo)-18H catalyst has the ability to quickly transfer charge. In addition, according to the Tafel polarization curve, the corrosion current of the catalyst was calculated by the external cutting method, and it was found that the corrosion current of MIL-53(FeCo)-18H (8.61×10 -9 A) is MIL-53(Fe)-18H(3.47×10 -9 A), which further indicates that cobalt doping enhances the electron transfer ability of MIL-53(Fe)-18H catalyst, thereby potentially improving its catalytic ozone activity.

[0089] 2. Catalytic ozone oxidation degradation experiment

[0090] After a series of characterizations of the obtained MIL-53(Fe)-18H and MIL-53(FeCo)-18H, it was found that the surface of the cobalt-doped MIL-53(Fe)-18H showed a lower Lewis acid site density. The specific effect of the Lewis acid site density on the catalytic ability of MIL-53(FeCo)-18H needs further exploration. To this end, after obtaining the above results, the applicant explored the catalytic ozone degradation of MIL-53(Fe)-18H and MIL-53(FeCo)-18H.

[0091] The experimental conditions and procedures of this part are as follows:

[0092] Phenol and 4-NP were selected as the simulation objects of the main organic pollutants in the effluent of the secondary sedimentation tank of printing and dyeing wastewater to explore the ozone activation efficiency of MIL-53(FeCo)-18H catalyst. The specific experimental process is: 30 mg of powdered catalyst is evenly dispersed in 300 mL of 20 mg L -1 of phenol solution (or 50 mg L -1 4-NP solution) and then a concentration of 100 mg L -1 , flow rate 60 mL min -1 The HCO process was started with ozone gas. 1 mL of sample was taken with a syringe at given time intervals and filtered with a 0.22 μm aqueous PES filter. 30 μL of 0.1 mol L -1 Na2S2O3 solution was added to quench the residual ozone molecules and ROS. All oxidative degradation experiments were carried out in a water bath at 25°C and 30 rpm.

[0093] In addition to phenol and 4-NP, a series of benzene ring organic pollutants, including 4-AP, HQ, 4-CP and 4-CN, were screened to verify the selectivity of cobalt-doped MIL-53(Fe)-18H catalytic ozone degradation for organic pollutants. The degradation test concentration of these organic pollutants was 50 mg L -1 , and other conditions were consistent with the degradation of phenol and 4-NP. For the deep treatment of real printing and dyeing wastewater, except for sampling 10mL at 30 and 60min of reaction, other degradation experimental conditions were the same as those for the degradation of phenol and 4-NP.

[0094] The parameters in this section are determined as follows:

[0095] (1) Analysis of organic pollutant concentration

[0096] The peak intensities of phenol, 4-NP, 4-AP, HQ, 4-CP, 4-CN and MDE solution samples were detected by 1260 high performance liquid chromatograph from Agilent Technologies, USA. The stationary phase of the high performance liquid chromatography test was a ZORBAX Eclipse XDB-C18 column (3.5 mm, 4.6 × 150 mm), and other test conditions are shown in Table 4.

[0097] Table 4 HPLC test conditions

[0098]

[0099]

[0100] Degradation rate of organic pollutants (1-C t / C0) is calculated as follows:

[0101]

[0102] Where B0 is the peak intensity corresponding to the initial sample solution, B t is the peak intensity corresponding to the sample solution at time t.

[0103] (2) ROS determination

[0104] EPR technology, free radical quenching experiment and free radical probe method were used to analyze the ROS generated by ozone decomposition during catalytic ozone decomposition. In the EPR technology, DMPO was used as ·OH and O2 ·- Signal capture agent, in which water is used as solvent for the capture of OH, O2 ·- Methanol was used as the solvent for the capture; TEMP was used as 1The O2 signal capture agent, the solvent is water. The EPR spectrum of ROS generated by ozone decomposition and transformation was tested using the A300 electron spin resonance spectrometer of Bruker Company, USA. In the free radical quenching experiment, TBA and methanol were used as ·OH quenchers, and carbon tetrachloride and p-BQ were used as O2 ·- Quenchers, FFA and L-his as 1 O2 quencher, comparative quencher (2 g L -1 )’s inhibition degree on the catalytic degradation system is used to identify the contribution of ROS to the degradation of organic pollutants.

[0105] In the free radical probe method, coumarin (10 mM) was used as the ·OH probe to measure the cumulative concentration of ·OH in the system. 1 O2 probe, measuring system 1 O2 steady-state concentration, MDE and ozone, ·OH, 1 O2, O2 ·- The second-order reaction rate constants are k 1O2,MDE =1.5×10 8 M -1 s -1 , k ·OH,MDE =6×10 9 M -1 s -1 , k O3,MDE <1M -1 s -1 , k O2·-,MDE =0M -1 s -1 It can be seen that in the catalytic ozone system, MDE is mainly 1 O2 and ·OH oxidative degradation, so 20 mg L -1 The solvent composition was replaced by 50% water and 50% methanol to eliminate the reaction between OH and MDE, so that the concentration of MDE changed from 1 O2 dominated, and other reaction conditions were consistent with the catalytic ozone oxidation degradation experiment. 1 The steady-state concentration of O2 is determined by MDE and the relationship between ozone, OH, 1 O2, O2 ·- The second-order reaction rate constant is calculated by the following formula: 1 Take O2 as an example:

[0106] MDE+ 1 O2→Substrate (2)

[0107]

[0108] (3) Ozone concentration measurement

[0109] The indigo method was used to determine the ozone concentration in the solution. First, the concentration was 278.65 mg L -1 Prepare a phosphate buffer solution with a pH of 2 using the standard stock solution of sodium indigo disulfonate: weigh 7.1 g of anhydrous disodium hydrogen phosphate and 6.8 g of potassium dihydrogen phosphate, dissolve in water, and dilute to 1 L. Then, add 2.00 mL of sodium indigo disulfonate solution, 5.00 mL of phosphate buffer, and 5.00 mL of solution sample to a 50 mL colorimetric tube, and then dilute to 50 mL with water. Finally, use a Lambda35 UV-visible spectrophotometer from Perkin Elmer, USA, to measure the sample absorbance at λ=610 nm. The cuvette thickness is 1 cm. The mass concentration of ozone in the solution sample is calculated according to formula (6):

[0110]

[0111] Where: ρ is the mass concentration of ozone, g L -1 ; ε is the molar absorptivity of sodium indigo disulfonate, which is 0.193×10 4 Lmol -1 cm -1 ; b is the thickness of the cuvette, which is 1 cm; V 水样 is the volume of the water sample, mL; A0 is the absorbance of the blank sample; A1 is the absorbance of the sample; 48 is the molar mass of ozone, g mol -1 .

[0112] In order to analyze the consumption of ozone in the presence of catalyst, 50 mL of saturated ozone solution (the power of the ozone generator was controlled at 60% and the gas flow rate was 60 mL min -1 , water bath temperature is 25℃, keep continuous ventilation for more than 1h) add 5mg catalyst sample, place it in an intelligent constant temperature oscillator, control the temperature to 25℃, the speed is 50rpm, and take 5.00mL with a pipette at regular intervals, quickly add it to a 50mL colorimetric tube for absorbance determination. The ozone consumption rate in the solution is calculated according to formula (7):

[0113]

[0114] Where A is the ozone consumption rate; ρ0 is the initial sample ozone mass concentration, that is, the mass concentration of the ozone saturated solution, which is calculated to be 0.008 g L -1 ρ t is the ozone mass concentration of the sampled solution at time t, g L -1 .

[0115] ① Exploration of degradation pathways

[0116] (1) Identify ROS types

[0117] Ozone catalytic tests were conducted on MIL-53(Fe)-18H before and after cobalt doping. The ozone system without adding catalyst was used as the control group, and the degradation liquid was collected for EPR test. No pollutants were added in this part, and water was used as the solvent for testing. The rest of the experimental conditions were referred to the above part of "2. Catalytic ozone oxidation degradation experiment".

[0118] The results are as follows Fig.10 As shown, it can be observed that: Fig.10 In a, when DMPO is used as an efficient ·OH scavenger and water is used as a solvent, the EPR spectrum of the MIL-53(Fe)-18H / ozone system monitors the obvious quartet of characteristic peaks belonging to the DMPO-·OH adduct (signal intensity ratio is 1:2:2:1). However, the characteristic signal peak representing ·OH in the EPR spectrum of the MIL-53(FeCo)-18H / ozone system is very weak, indicating that the Fe site of the MIL-53(Fe)-18H catalyst tends to catalyze the dissociation of ozone into ·OH, while cobalt doping weakens the conversion efficiency of ozone → ·OH. At the same time, from Fig.10 b It can be seen that when methanol is used as the solvent instead of water and DMPO is still used as a free radical scavenger, the ·OH is quickly quenched by methanol and belongs to DMPO-O2 ·- The characteristic signal peaks of the adducts were detected in the EPR spectra of both the undoped and cobalt-doped MIL-53(Fe)-18H catalytic ozone systems, and the signal peak intensities of the two systems were almost equal, indicating that cobalt doping has an important effect on the catalytic ozone decomposition to produce O2 ·- In addition, no obvious 1:2:2:1 quadruple characteristic peaks and peaks representing O2 ·- The characteristic signal peaks indicate that ozone is difficult to decompose by itself to produce OH and O2 ·- In addition, from Fig.10 c It can be found that when TEMP is 1 When water was used as solvent, each system showed typical triple characteristic peaks with a signal intensity ratio of 1:1:1, which was attributed to TEMP- 1 Surprisingly, the strongest signal of O2 adduct was detected in the MIL-53(FeCo)-18H / ozone system. 1 The O2 signal peak indicates that cobalt doping enhances the selective generation of ozone by MIL-53(Fe)-18H 1 The effectiveness of O2.

[0119] The above results show that the cobalt doping method that changes the nucleation process of MIL-53(Fe)-18H crystals has the effect of inducing the selective conversion of ozone, which makes the ·OH produced by ozone decomposition turn to the production of1 O2 conversion.

[0120] (2) Quantification of ROS production concentration

[0121] In order to further evaluate the catalytic effect of cobalt-doped MIL-53(Fe)-18H on the production of ·OH 1 The experiment used coumarin and MDE as probes to quantify the cumulative concentration and 1 The steady-state concentration of O2 is used to quantify the generation of OH and 1 O2 concentration. No pollutants were added in this part, and water was used as the solvent for testing. The rest of the experimental conditions were referred to the aforementioned part of "2. Catalytic ozone oxidation degradation experiment".

[0122] like Fig.11 As shown in a, during the catalytic process, the ·OH produced by the activated ozone reacts with coumarin to produce heptahydroxycoumarin, which shows a typical fluorescence absorption peak at 450nm in the fluorescence spectrum. There is a great difference in the fluorescence absorption peak intensity between the undoped and cobalt-doped MIL-53(Fe)-18H / ozone systems, indicating that the two have different abilities to activate ozone to produce ·OH. After 30 minutes of reaction, the undoped MIL-53(Fe)-18H activated ozone to produce more ·OH than the cobalt-doped MIL-53(Fe)-18H. At the same time, Fig.11 b It can be observed intuitively that the amount of heptahydroxycoumarin generated by the reaction increases with the extension of reaction time. The result of calculating the cumulative concentration of OH based on the fluorescence absorption peak intensity of heptahydroxycoumarin is as follows Fig.11 As shown in Figure 3, the cumulative concentration of ·OH produced by the catalytic decomposition of ozone by undoped and cobalt-doped MIL-53(Fe)-18H increased steadily with the catalytic time, and there was a rapid growth process in the first 10 minutes, and then the growth rate slowed down. When the reaction lasted for 30 minutes, cobalt-doped MIL-53(Fe)-18H could activate ozone to accumulate and produce 23.45 μmol L -1 The concentration of ·OH was higher than that of undoped MIL-53(Fe)-18H (34.61 μmol L -1 ) weakened by 32.2%.

[0123] Fig.11 d is the result of ozone oxidation degradation of MDE catalyzed by undoped MIL-53(Fe)-18H and cobalt-doped MIL-53(Fe)-18H. 1 O2, O2 ·- The second-order reaction rate constant of MDE can directly reflect the generation of ozone decomposition in the catalytic system when 50% methanol replaces 50% aqueous solution. 1 The effectiveness of O2. Fig.11 d and Fig.11 As shown in Figure e, the efficiency of MIL-53(FeCo)-18H in catalyzing ozone degradation of MDE is significantly higher than that of MIL-53(Fe)-18H / ozone system. The degradation rate of the former exceeds 50% at 5 min, and the k value is 0.165 min -1 The degradation rate of the latter is about 30%, and the k value is 0.070min -1 , indicating that cobalt doping produces more ozone activation than MIL-53(Fe)-18H 1 O2. In addition, according to the k value of degradation MDE 1 The results of O2 steady-state concentration are as follows Fig.11 As shown in f, it can be found that MIL-53(FeCo)-18H can activate ozone to stably produce 1.83*10 -5 μM concentration 1 O2, compared with MIL-53(Fe)-18H(7.78*10 -6 μM) increased by 135.2%.

[0124] In summary, the introduction of heterogeneous metal Co atoms induced a 32.2% decrease in the efficiency of MIL-53(Fe)-18H in catalytic ozone decomposition to produce ·OH. 1 The efficiency of O2 increased by 135.2%, greatly enhancing the selective production of catalytic ozone 1 The effectiveness of O2.

[0125] (3) Determine the dominant component of ROS

[0126] To confirm 1 O2 plays a leading role in the degradation of organic pollutants by ozone catalysis of cobalt-doped MIL-53(Fe)-18H. The dye intermediate, 4-NP, was used as a model pollutant in the experiment, and the ROS quenching technique was used to determine the leading component of 4-NP degradation. The rest of the experimental conditions refer to the aforementioned section "2. Catalytic ozone oxidation degradation experiment".

[0127] Methanol and TBA are both highly effective quenchers of ·OH. The former has a quenching effect on both surface-bound ·OH and ·OH free in the solution, while the latter can only remove ·OH in the solution. Fig.12 As shown in the figure, the addition of methanol or TBA can accelerate the degradation and removal of 4-NP, which may be due to the formation of fine bubbles leading to enhanced mass transfer. p-BQ is a common O2 ·- quencher, however, since p-BQ can also rapidly consume OH and 1 O2, which can easily lead to misjudgment of experimental results. Fig.12 As shown in the figure, the significant inhibitory effect of p-BQ on the degradation and removal of 4-NP may be due to ·OH and1 The quenching of O2 is the cause, not O2 ·- Therefore, carbon tetrachloride was used as O2 ·- Quencher. Fig.12 As shown in the figure, the effect of carbon tetrachloride on the degradation efficiency of 4-NP is negligible, indicating that O2 ·- FFA and L-his are often used as 1 O2 quencher, made from Fig.12 It can be seen that the presence of FFA and L-his can effectively inhibit the removal of 4-NP, indicating that 1 O2 is the main ROS in the ozone degradation of 4-NP by cobalt-doped MIL-53(Fe)-18H. After adding FFA, the removal rate of 4-NP dropped sharply by 79.8%, while after adding L-his, the removal rate of 4-NP dropped by 21.3%, which was significantly lower than the former. 1 In addition to O2, ozone (redox potential: 2.07 eV) can also directly oxidize 4-NP. In addition, FFA can consume part of the ozone and 1 The reaction activity of O2 is higher than that of L-his, so it is reasonable that there is a big difference in the inhibitory effect between FFA and L-his.

[0128] The quenching experimental results show that in the cobalt-doped MIL-53(Fe)-18H / ozone system, 1 O2 is the dominant ROS component that degrades 4-NP.

[0129] ② 1 Selective degradation in O2-dominated systems

[0130] In “① Exploration of degradation pathways”, it has been found that cobalt doping induces MIL-53(Fe)-18H to catalyze ozone decomposition to produce ·OH 1 O2 conversion, confirmed 1 O2 plays a dominant role in the degradation and removal of the model organic pollutant (4-NP). 1 O2 is electrophilic and tends to oxidize and destroy organic pollutants with multi-electron structure characteristics. 1 O2 selectively degrades organic pollutants, revealing 1 The behavioral characteristics and mechanism of O2 oxidation degradation of organic pollutants were studied. A series of organic pollutants were selected in the experiment to explore the degradation efficiency of the HCO process.

[0131] The experiment first selected typical phenolic organic compounds, phenol and 4-NP, as model pollutants. The former has more electrons than the latter. OH has strong oxidizing properties and is a non-selective oxidant. 1O2 has a moderate oxidation capacity and is highly effective in oxidizing and degrading electron-rich organic pollutants. 1 O2 oxidative degradation, and both are easily attacked by OH. Fig.13 As shown in the phenol degradation experiment, MIL-53(FeCo)-18H showed higher catalytic ozone degradation efficiency than MIL-53(Fe)-18H. The former degraded and removed 100% of phenol within 8 minutes, and the k value was 0.547min -1 , is the latter (0.277min -1 ). In addition, compared with undoped MIL-53(Fe)-18H, the introduction of Co had a negligible effect on the adsorption performance of phenol, but weakened the adsorption capacity of 4-NP. Interestingly, the degradation results of 4-NP were exactly the opposite of phenol. MIL-53(Fe)-18H had better catalytic ozone degradation efficiency than MIL-53(FeCo)-18H, which had a removal rate of 85.2% for 4-NP and a k value of 0.204min. -1 , which is significantly lower than the former (0.267min -1 Compared with undoped MIL-53(Fe)-18H, the outstanding degradation efficiency of cobalt-doped MIL-53(Fe)-18H catalyzed by ozone on electron-rich phenol and the inferior degradation efficiency on relatively electron-deficient 4-NP once again prove that the introduction of Co induces the selective conversion of catalytic ozone from decomposition to production of ·OH to production of 1 O2 conversion, and confirmed 1 Selective degradation of electron-rich organic pollutants by O2-dominated system.

[0132] To further explore 1 The behavior characteristics and mechanism of O2 oxidation degradation of organic pollutants. In addition to phenol and 4-NP, four other organic pollutants were selected as degradation substrates according to the type of substituents on the benzene ring. A series of research objects with different electronic environments were constructed, including 4-AP, HQ, 4-CP and 4-CN. 1 The degradation and removal efficiency of the O2-dominated system MIL-53(FeCo)-18H / ozone on them. Fig.14 As shown in (b), the removal efficiencies of 4-CP, phenol, HQ, and 4-AP over MIL-53(FeCo)-18H catalyst exceeded 96% within 10 min, while the removal efficiencies of 4-NP and 4-NC were 85% and 77%, respectively. Fig.14 Figure c shows the k values ​​of six organic pollutants. The k value of (-NH2)4-AP with a strong electron-donating group is the highest, which is 0.512 min -1 , while the k value of 4-NP with strong electron-withdrawing group (-NO2) is 0.203min -1, the k value of 4-CN with two electron-withdrawing groups (-NO2 and -Cl) is the lowest, which is 0.152 min -1 , the order of the degradation efficiency of the six organic pollutants is: 4-AP > HQ > phenol > 4-CP > 4-NP > 4-CN. Thus, 1 The degradation efficiency of O2-dominated system for organic pollutants may be related to the electron-donating and electron-withdrawing groups of the pollutants. In the cobalt-doped MIL-53(Fe)-18H / ozone system, electron-rich organic pollutants (with -NH2, -OH, and -R as electron-donating groups) are more likely to be attacked by the ROS-dominant component - 1 O2. Therefore, the order of k values is consistent with the order of the electron-donating and electron-withdrawing abilities of the substituents of organic pollutants. In addition, taking the ionization energy (IP) of organic pollutants as an index to evaluate the electron-donating and electron-withdrawing ability, electron-rich organic compounds usually have higher IP values. On the contrary, relatively electron-deficient organic compounds usually have lower IP values. The order of the ionization energies of the six organic pollutants is: 4-AP < HQ < phenol < 4-CP < 4-NP < 4-CN. To further verify 1 the selective degradation of O2 to electron-rich organic pollutants, the linear relationship between the IP value and the k value of organic pollutants was experimentally explored, and the results are as Fig.14 shown in Fig.14 c. As can be seen from 2 c, there is an obvious linear relationship between the IP value and the k value. As the IP value increases, the k value decreases, and the linear index R 2 value is 0.974, indicating a good linear relationship, thus confirming 1 the outstanding degradation efficiency of the O2-dominated system for electron-rich organic pollutants.

[0133] ③ Catalytic ozone decomposition kinetics

[0134] Fig.15 For the decomposition of ozone in different systems, it can be seen that under normal temperature and pressure conditions, the decomposition and consumption rate of ozone in water is relatively slow, and the half-life is approximately around 20 min. In the presence of the MIL-53(Fe)-18H catalyst, the ozone decomposition rate is greatly enhanced (the k value is 0.707 min -1 ), and it is all consumed within 4 min, indicating that the Fe active center activates the rapid decomposition of ozone, and ozone is rapidly decomposed and transformed into ·OH, O2 ·- , 1 O2 and other ROS under the action of the active sites. In addition, in the presence of the MIL-53(FeCo)-18H catalyst, the decomposition rate of ozone is lower than that of the MIL-53(Fe)-18H system, and the k value is 0.142 min -1 , which may be because cobalt doping enhances the efficiency of ozone selectively generating 1 O2, and a large amount of1 Due to its relatively long lifespan, O2 participates in the decolorization of the indicator reagent sodium indigo disulfonate, creating the illusion that ozone consumption is slowing down.

[0135] ④Catalyst stability and adaptability

[0136] Fig.16 The degradation of MIL-53(FeCo)-18H catalyst in different inorganic salt systems / HA, including sodium sulfate, sodium bicarbonate, sodium carbonate, and sodium chloride. Fig.16 It can be seen that the degradation and removal efficiency of phenol was almost unaffected and could still be 100% degraded and removed within 10 minutes, indicating that the MIL-53(FeCo)-18H ozone catalyst has strong resistance to the inhibition caused by the coexistence of inorganic salt anions. However, the presence of a large amount of HA (0-7mM) inhibited the degradation rate of phenol. When the HA concentration increased from 0 to 1mM, the k value increased from 0.460min to 0.710min. -1 Down to 0.345min -1 However, when the HA concentration increased from 1 mM to 5 mM, the inhibitory effect of HA on the degradation of phenol decreased slightly; when the HA concentration further increased to 7 mM, the removal of phenol was inhibited by 10% and the k value dropped to 0.224 min. -1 It is worth noting that the "inhibitory effect" of high concentration HA on the catalytic ozone oxidation degradation efficiency of MIL-53(FeCo)-18H is weak, and the degradation rate of phenol is still as high as 88% even in the presence of 7 mM concentration of HA.

[0137] Fig.17 a~ Fig.17 b shows the degradation of MIL-53(FeCo)-18H catalyst at different pH values. Fig.17 a~ Fig.17 b It can be seen that when the initial pH value is 5.90 and 7.77, the removal rate of phenol by MIL-53(FeCo)-18H catalytic ozone process is faster, and the k value is 0.460min -1 and 0.513min -1 When the initial pH value was adjusted to strong acidity (2.27, 3.94) or strong alkalinity (10.08), the degradation and removal of phenol was slightly inhibited, and the k value dropped to 0.422min, -1 、0.431min -1 and 0.424min -1However, within 10 minutes, the degradation rate of phenol still reached 100%. It can be seen that with the change of initial pH, the degradation rate and k value of phenol are slightly different, indicating that the initial pH value of the MIL-53 (FeCo) -18H / ozone system has no significant effect on the degradation efficiency of phenol, indicating that the MIL-53 (FeCo) -18H ozone catalyst has a wide pH applicability.

[0138] Fig.17 c is the cyclic degradation diagram of MIL-53(FeCo)-18H catalyst. Fig.17 c It can be seen that the efficiency of MIL-53(FeCo)-18H in catalyzing the degradation of phenol by ozone remained at a high level during the four consecutive cycles. Furthermore, the FT-IR and PXRD characterization of MIL-53(FeCo)-18H before and after the cyclic degradation revealed that the results were as follows Fig.17 d~ Fig.17 As shown in e: No obvious changes were found in the two spectra, indicating that the MIL-53(FeCo)-18H catalyst has good structural stability.

Claims

1. A method for preparing a cobalt-doped iron-based MOF catalyst, characterized in that: The cobalt-doped iron-based MOF catalyst is obtained by solvent thermal reaction of N,N-dimethylformamide containing cobalt salt, iron salt and terephthalic acid and then drying; the solvent thermal reaction is: 20 to 30 minutes at 50°C, then 20 to 30 minutes at 100°C, and then 14 to 22 hours at 150°C.

2. The preparation method according to claim 1, characterized in that The molar ratio of cobalt to iron in the cobalt salt and the iron salt is 1:

4.

3. The preparation method according to claim 1 or 2, characterized in that: The iron salt is selected from any one of ferric nitrate, ferric chloride, ferric sulfate and ammonium ferric citrate.

4. The preparation method according to claim 1 or 2, characterized in that: The cobalt salt is selected from any one of cobalt nitrate, cobalt sulfate and cobalt chloride.

5. The preparation method according to claim 1 or 2, characterized in that: The ratio between the total molar amount of cobalt and iron in the cobalt salt and the iron salt and the molar amount of terephthalic acid is 1:

1.

6. The preparation method according to claim 1, characterized in that: The drying temperature is 80 to 120° C., and the drying time is 12 to 36 hours.

7. A cobalt-doped iron-based MOF catalyst prepared by the preparation method according to any one of claims 1 to 6.

8. Use of the cobalt-doped iron-based MOF catalyst as claimed in claim 7 in the degradation of electron-rich organic pollutants.