Submarine instrument cabin shell and preparation method thereof

By using inorganic composite materials such as α-SiC and ultra-high molecular weight polyethylene, a subsea instrument cabin shell with strong pressure resistance and high buoyancy is prepared, which solves the contradiction between pressure resistance and buoyancy demand in deep-sea environments and achieves low cost. High yield solution.

CN118927654APending Publication Date: 2024-11-12SHANGHAI JINGWU SEA MATERIAL TECHNOLOGY DEVELOPMENT CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310525557.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art cannot meet the high pressure resistance and high buoyancy requirements of the subsea instrument cabin in a deep-sea environment, and has high production cost and low yield.

Method used

The shell of the subsea instrument cabin is prepared by inorganic composite materials composed of α-SiC, α-SiC fibers, β-SiC and silicon phases. The hollow container is formed by surface processing, and the shell is realized by using ultra-high molecular weight polyethylene fasteners and connecting rings. The fastening of the body, the elastic modulus and compressive strength of the material reach 390-410GPa and 3600-4000Mpa, combined with bevel processing and bonding technology, ensure the connection sealing of the shell.

Benefits of technology

It does not deform in the deep sea of ​​11,000 meters, provides high buoyancy, light weight, low cost and high yield, and is suitable for commercial applications at all sea depths.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118927654A_ABST
    Figure CN118927654A_ABST
Patent Text Reader

Abstract

The invention discloses a submarine instrument cabin shell and a preparation method thereof. The preparation method comprises the following steps: performing surface processing on at least two shells forming the submarine instrument cabin shell, performing plane butt joint to form a hollow container, vacuumizing the hollow container, and bonding the end surfaces of the plane butt joint. A shell forming the submarine instrument cabin shell comprises two hemispherical shells and N cylindrical shells, and N is larger than or equal to 0. The elastic modulus of the material of the shell is 390 to 410 GPa, and the compressive strength of the material of the shell is 3600 to 4000 Mpa; the surface machining comprises one or more of outer circle machining, end face machining and bevel angle machining. The submarine instrument cabin shell prepared by the method does not deform in deep sea and is large in buoyancy, low in preparation cost and high in yield and cost performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a submarine instrument cabin shell and a preparation method thereof. Background Art

[0002] All fixed and autonomous instruments used in ocean research activities have two important things in common: firstly, they require a pressure-resistant housing and secondly, they require buoyancy to bring the instrument safely to the surface.

[0003] Seafloor seismometers, deep-sea profile measurement devices, and data transmission buoys released in the deep sea are several relatively fixed underwater and underwater measurement equipment. Their operation areas and processes are controllable, and they can simultaneously observe multiple elements and are easy to recycle. Therefore, they have high utilization value for observations in specific sea areas. In order to resist the erosion of deep-sea pressure and seawater, instruments, batteries, etc. need to be placed in an instrument cabin composed of a pressure-resistant shell. When the instrument cabin is deployed, the buoyancy of the instrument can be changed to adjust the speed of the instrument's fall, so that the instrument can land on the seabed at a lower speed or float in the water at a specified depth. Especially when there are several instrument cabins, they are connected by wires and data cables (deep-sea cables) to achieve battery sharing. The instrument cabin is equipped with a hydroacoustic and control circuit board, and its built-in power management module can monitor the battery's power reserve in real time. When measuring on the seabed, the coupling degree between the instrument and the seabed can be adjusted by buoyancy. When recovering data, dual antenna communication of GPS and satellite communication is adopted. The stored data is sent to the data receiving center via satellite communication. At the same time, the location information and battery information of the instrument are reported, and the instrument recovery is arranged according to the remaining battery power. After the data transmission is completed, the instrument sinks automatically to continue data detection.

[0004] Since the shape of the deep-sea pressure hull is mainly determined by the maximum design depth and the effective load (load capacity) acting on the hull, as well as the service life, spherical and combined spherical pressure hulls are generally advantageous for deep-sea equipment with a water depth of more than 800 meters; while cylindrical hulls are mostly used for working depths below 800 meters. However, in deep water environments (water depths greater than 1,500 meters), this cylindrical shell structure clearly exposes the problem of insufficient pressure resistance. If the cylindrical structure is still used, the thickness of the cylinder can only be increased, and the problems that follow are: the weight of the pressure-resistant cylinder of the instrument cabin is greatly increased, the buoyancy is seriously reduced, and the amount of material used is also increased, resulting in high costs. Glass spherical cabins used in full sea depths (11,000 meters) are currently only produced in a few places in the world. Due to the small elastic modulus and low hardness of the glass spherical cabin, it has been used several times at 10,000 meters, and many of them are used once, and the interface is damaged by peeling. Silicon nitride, aluminum oxide and silicon carbide ceramics used in the prior art shrink in volume by 15% to 22% during the shell preparation process, resulting in a very low yield rate, extremely poor cost performance, and almost impossible commercial application. Summary of the invention

[0005] In order to solve the problem in the prior art that the submarine instrument cabin cannot simultaneously meet the requirements of high pressure resistance and high buoyancy in a deep sea environment, the present invention proposes a submarine instrument cabin shell and a preparation method thereof. The submarine instrument cabin shell prepared by the present invention can remain unchanged in the deep sea and has high buoyancy, low preparation cost, high yield rate and high cost performance.

[0006] The present invention mainly adopts the following technical solutions to solve the above technical problems:

[0007] The present invention provides a method for preparing a subsea instrument cabin shell, which comprises the following steps:

[0008] After surface processing of at least two shells constituting the outer shell of the submarine instrument cabin, plane docking is performed to form a hollow container, and then the hollow container is evacuated, and the end faces of the plane docking are bonded; the shells constituting the outer shell of the submarine instrument cabin include 2 hemispherical shells and N cylindrical shells, wherein N≥0;

[0009] The elastic modulus of the material of the shell is 390-410GPa, and the compressive strength is 3600-4000Mpa;

[0010] The surface processing includes one or more of outer circle processing, end surface processing and bevel processing.

[0011] In the present invention, the material of the shell is preferably an inorganic composite material composed of four phases: α-SiC, α-SiC fiber, β-SiC and silicon phase.

[0012] In the present invention, the hardness of the material of the shell is preferably HRA85-93, for example, HRA90 or HRA92.

[0013] In the present invention, the density of the shell material is preferably 3-3.12 g / cm 3 , for example, 3.05 g / cm 3 or 3.10g / cm 3 .

[0014] In the present invention, the fracture toughness of the material of the shell is preferably 5-9 MPa·m 1 / 2 , for example 7MPa·m 1 / 2 .

[0015] In the present invention, the bending strength of the material of the shell is preferably 330-420 MPa, for example 350 MPa or 360 MPa.

[0016] In the present invention, the elastic modulus of the material of the shell is preferably 395 Gpa, 400 Gpa or 405 Gpa.

[0017] In the present invention, the compressive strength of the material of the shell is preferably 3800Mpa or 3900Mpa.

[0018] In the present invention, when the surface processing adopts beveling processing, the end faces of the hemispherical shell and the cylindrical shell are respectively processed to form a pair of mutually matching planes and a pair of mutually matching inclined surfaces, and the pair of planes and the pair of inclined surfaces together form the connecting surface of the hemispherical shell and the cylindrical shell.

[0019] Among them, those skilled in the art can conventionally understand that the meaning of the mutual matching is: the connecting surfaces of the hemispherical shell and the cylindrical shell respectively include a plane and an inclined surface connected to each other, wherein the width of the plane of the hemispherical shell is equal to the width of the plane of the planar cylindrical shell, and the angle formed between the inclined surfaces of the hemispherical shell and the inclined surfaces of the hemispherical shell is equal to the angle formed between the inclined surfaces of the cylindrical shell and the inclined surfaces of the cylindrical shell, so that the connecting surfaces of the hemispherical shell and the cylindrical shell fit together.

[0020] In the present invention, preferably, fasteners parallel to the axis and connecting rings perpendicular to the axis are provided around the container, and the fasteners and connecting rings are used to achieve fastening between the shells. The number of the fasteners and connecting rings can be determined according to the actual fixing conditions of the shell of the subsea instrument cabin.

[0021] Wherein, the connecting ring preferably includes symmetrically arranged fastener positioning holes, and the fastener positioning holes are used to connect with the fasteners and fix the shell.

[0022] Wherein, the material of the fastener is preferably one or more of ultra-high molecular weight polyethylene, titanium alloy and stainless steel.

[0023] Wherein, the material of the connecting ring is preferably ultra-high molecular weight polyethylene.

[0024] Wherein, the molecular weight of the ultra-high molecular weight polyethylene is preferably greater than 1 million.

[0025] The density of the ultra-high molecular weight polyethylene is preferably less than 1 g / cm 3 .

[0026] In the present invention, ultra-high molecular weight polyethylene fasteners and connecting rings are used, and the material density is less than 1g / cm 3 , which has the advantage of not reducing the buoyancy of the instrument cabin underwater.

[0027] In the present invention, the method for preparing the shell preferably includes the following steps:

[0028] S1, uniformly mixing α-SiC fiber, α-SiC particles and phenolic resin to obtain a slurry, spray drying, and obtaining a spherical particle raw material; wherein the length of the α-SiC fiber is less than 300 μm and the diameter is ≤10 μm; the particle size of the α-SiC particles is 1-100 μm;

[0029] S2, pressing the spherical particle raw material into a green blank, and then curing the green blank;

[0030] S3, after the curing treatment, siliconizing treatment is performed to obtain a shell.

[0031] Wherein, in parts by weight, the preferred ratio of the α-SiC fiber, the α-SiC particles and the phenolic resin is (6-30): (60-84): 10.

[0032] Wherein, in step S1, the particle size of the α-SiC particles is preferably 10-100 μm, for example: the number of α-SiC particles with a particle size of 100 μm, 60 μm, and 10 μm each accounts for 33.3%; or, the number of α-SiC particles with a particle size of 15 μm, 5 μm, and 1 μm each accounts for 33.3%; or, the number of α-SiC particles with a particle size of 50 μm, 20 μm, and 10 μm each accounts for 33.3%.

[0033] The pressing and molding can be performed by selecting a mold according to the desired shapes of the hemispherical shell and the cylindrical shell.

[0034] The compression molding method may be conventional in the art, preferably isostatic pressing, slip injection or molding.

[0035] Wherein, the isostatic pressing method is preferably a dry bag method or a wet bag method.

[0036] Before the siliconizing treatment, it is preferred to further include a step of opening holes, the purpose of which is to provide holes for vacuuming, holes for sensors and holes for wires. The number of holes can be determined according to the needs during use, and when some of the holes are not used, the holes are sealed using sealing technology.

[0037] Wherein, the diameter of the opening is preferably 5-20 mm.

[0038] Wherein, after the siliconizing treatment, it is preferred to further include a surface desiliconization step, wherein the purpose of the surface desiliconization is to remove residual silicon on the surface of the spherical shell blank.

[0039] The surface desiliconization is preferably performed by sandblasting.

[0040] In the present invention, the processing is preferably performed using a diamond grinding wheel.

[0041] In the present invention, N is preferably 1-20, more preferably 1-4, for example 1 or 2.

[0042] In the present invention, when N≥2, the cylindrical shell is coaxially arranged on the axis between the two hemispherical shells.

[0043] In the present invention, the bonding is preferably carried out by drip irrigation.

[0044] In the present invention, after the bonding, the steps of drying and tape wrapping are preferably further included.

[0045] It is known to those skilled in the art that, in order to facilitate transportation and lifting, the guard plate generally includes a plurality of through holes and a plurality of ears.

[0046] In the present invention, it is known to those skilled in the art that in order to improve the sealing performance between the shells, a sealing ring can usually be provided between the shells.

[0047] Wherein, the sealing ring is preferably an O-ring or a planar sealing ring.

[0048] In a preferred embodiment of the present invention, the processing adopts outer circle processing and end surface processing, and no sealing ring is provided.

[0049] In a preferred embodiment of the present invention, the processing adopts bevel processing, and no sealing ring is provided.

[0050] In a preferred embodiment of the present invention, the processing adopts outer circle processing and end surface processing, and a plane sealing ring is arranged between the shells.

[0051] In a preferred embodiment of the present invention, the processing adopts bevel processing, and an O-ring is arranged between the shells.

[0052] The present invention also provides a submarine instrument cabin shell produced by the above-mentioned production method.

[0053] The present invention also provides a submarine instrument cabin housing, which includes two hemispherical shells and N cylindrical shells, wherein N≥0;

[0054] The elastic modulus of the material of the shell is 390-410GPa, and the compressive strength is 3600-4000Mpa;

[0055] The material of the shell is an inorganic composite material composed of four phases: α-SiC, α-SiC fiber, β-SiC and silicon phase.

[0056] In the present invention, the hardness of the material of the shell is preferably HRA85-93, for example, HRA90 or HRA92.

[0057] In the present invention, the density of the shell material is preferably 3-3.12 g / cm 3 , for example, 3.05 g / cm 3 or 3.10g / cm 3 .

[0058] In the present invention, the fracture toughness of the material of the shell is preferably 5-9 MPa·m 1 / 2 , for example 7MPa·m 1 / 2 .

[0059] In the present invention, the bending strength of the material of the shell is preferably 330-420 MPa, for example 350 MPa or 360 MPa.

[0060] In the present invention, the elastic modulus of the material of the shell is preferably 395 Gpa, 400 Gpa or 405 Gpa.

[0061] In the present invention, the compressive strength of the material of the shell is preferably 3800Mpa or 3900Mpa.

[0062] In the present invention, the hemispherical shell preferably contains holes, wherein the number of the holes can be determined according to the needs during use, and when some of the holes are not in use, the holes are sealed using sealing technology.

[0063] In the present invention, N is preferably 1-20, more preferably 1-4, for example 1 or 2.

[0064] In the present invention, when N≥2, the cylindrical shell is coaxially arranged on the axis between the two hemispherical shells.

[0065] In the present invention, the wall thickness of the hemispherical shell is preferably 5-24 mm, such as 15 mm or 20 mm.

[0066] In the present invention, the outer diameter of the hemispherical shell is preferably 300-1200 mm, such as 650 mm or 1000 mm.

[0067] In the present invention, the length of the cylindrical shell is preferably 300-2000 mm, such as 1500 mm or 1800 mm.

[0068] In the present invention, the wall thickness of the cylindrical shell is preferably 18-32 mm.

[0069] In the present invention, the ratio of the wall thickness of the hemispherical shell to the wall thickness of the cylindrical shell is preferably 1:(1.1-4).

[0070] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.

[0071] The reagents and raw materials used in the present invention are commercially available.

[0072] The positive and progressive effects of the present invention are:

[0073] The subsea instrument cabin shell made of the inorganic composite material adopted in the present invention can remain unchanged in the deep sea at a depth of 11,000 meters, has strong pressure resistance, and can also provide great buoyancy and light weight, meeting the use requirements of the entire sea depth. The materials used are single and inexpensive, the shell wall thickness is small, and the transportation is convenient, so it can be used commercially.

[0074] The present invention can adopt a simpler processing method, and the preparation process is simple. Due to the advantages of the materials used in this application, the shell volume can shrink by less than 1% during the preparation process, which is conducive to the preparation of larger instrument cabin shells, with high yield rate and cost-effectiveness, and the yield rate can reach more than 95%. BRIEF DESCRIPTION OF THE DRAWINGS

[0075] Figure 1 This is a cross-sectional view of the seabed instrument cabin of Example 1.

[0076] Figure 2 This is a cross-sectional view of the seabed instrument cabin of Example 3.

[0077] Figure 3 This is a cross-sectional view of the seabed instrument cabin of Example 4.

[0078] Figure 4 This is the connection method of Example 1 in which the outer circle is machined, the end face is machined, and then the plane is butted together.

[0079] Figure 5 This is the connection method of Example 2 in which the planes are butt-jointed after beveling.

[0080] Figure 6 The connection method of Example 3 is that the planes are butted after bevel processing and are matched with an O-ring.

[0081] Figure 7 This is the connection method of Example 4 in which the outer circle is machined, the end face is machined, and then the planes are butt-jointed, and a plane sealing ring is used.

[0082] Figure 8 A schematic diagram of the structure of the connecting ring.

[0083] Fig. 9 Schematic diagram of the three-dimensional structure of the connecting ring.

[0084] Fig.10 A schematic diagram of a transport container including a subsea instrument compartment housing.

[0085] The following are the descriptions of the reference numerals:

[0086] 1-submarine instrument compartment housing, 2-hole, 3-connecting ring, 4-fastener, 5-processing part, 6-O-ring, 7-flat sealing ring, 8-fastener positioning hole, 9-transport container. DETAILED DESCRIPTION

[0087] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.

[0088] The structural diagram and three-dimensional structural diagram of the connecting ring 3 used in the embodiment of the present application are as follows Figure 8 and Fig. 9 As shown, the connecting ring 3 includes fastener positioning holes 8.

[0089] In the actual use of the submarine instrument cabin, in order to facilitate its transportation on the ground, the submarine instrument cabin shell 1 is usually placed in a transport container 9, and the transport container 9 can also serve as a protective barrier for the submarine instrument cabin shell 1 to prevent collision or impact in seawater. Fig.10 shown.

[0090] The inorganic composite materials used in Examples 1-4 were prepared by the following steps:

[0091] The α-SiC fiber, α-SiC particles and phenolic resin are uniformly mixed to obtain a slurry, which is spray-dried to obtain a spherical particle raw material; wherein the length of the α-SiC fiber is less than 300 μm and the diameter is ≤10 μm; the number of α-SiC particles with a particle size of 15 μm, 5 μm and 1 μm each accounts for 33.3%; the feed ratio of α-SiC fiber, α-SiC particles and phenolic resin is 25:65:10.

[0092] Example 1

[0093] This embodiment adopts the following steps to prepare the subsea instrument cabin housing 1:

[0094] S1, using the above inorganic composite material to prepare two hemispherical shells with a wall thickness of 11mm and an outer diameter of 535mm by a grouting method, and then punching a hole 2 on the dried hemispherical shell to obtain a hemispherical shell blank; after the hemispherical shell blank is cured, it is placed in a high-temperature furnace for siliconization treatment, and then a strong impact sandblasting process is used to remove residual silicon on the surface of the blank to obtain a shell;

[0095] S2, the shell is processed through outer circle and end surface, and then plane-jointed to obtain a container, such as Figure 4 As shown, the outer circle machining and end surface machining are performed at the machining location 5;

[0096] S3. After the container is evacuated, a low-viscosity adhesive is dripped into the end face seal, dried at room temperature, wrapped with adhesive tape, connected with fasteners 4 and connecting rings 3, and a protective plate is installed around the container to obtain a submarine instrument cabin shell 1; wherein the material of the fasteners 4 includes titanium alloy, and the material of the connecting ring 3 includes ultra-high molecular weight polyethylene.

[0097] The cross-sectional view of the submarine instrument cabin prepared in this embodiment is as follows Figure 1 As shown, its diameter is 532mm, suitable for 11000m water depth, and weight-to-displacement ratio is less than 0.4g / cm 3 , net buoyancy is greater than 55 kg.

[0098] Example 2

[0099] This embodiment adopts the following steps to prepare the subsea instrument cabin housing 1:

[0100] S1, using the above inorganic composite material to prepare two hemispherical shells with a wall thickness of 15mm and an outer diameter of 650mm by isostatic pressing, and then punching a hole 2 on the dried hemispherical shell to obtain a hemispherical shell blank; after the hemispherical shell blank is cured, it is placed in a high-temperature furnace for siliconization treatment, and then a strong impact sandblasting process is used to remove residual silicon on the surface of the blank to obtain a shell;

[0101] S2, the shell is processed at an angle and then flat-jointed to obtain a container, such as Figure 5 As shown, the bevel processing is performed at processing location 5;

[0102] S3. After the container is evacuated, a low-viscosity adhesive is dripped into the end face seal, dried at room temperature, wrapped with adhesive tape, connected with fasteners 4 and connecting rings 3, and a protective plate is installed around the container to obtain a submarine instrument cabin shell 1; wherein the material of the fasteners 4 includes titanium alloy, and the material of the connecting ring 3 includes ultra-high molecular weight polyethylene.

[0103] The cross-sectional view of the submarine instrument cabin prepared in this embodiment is as follows Figure 1 As shown, the seabed instrument cabin prepared in this embodiment is suitable for a water depth of 7000 meters.

[0104] Example 3

[0105] This embodiment adopts the following steps to prepare the subsea instrument cabin housing 1:

[0106] S1, using the above inorganic composite material to prepare two hemispherical shells with a wall thickness of 20mm and an outer diameter of 1000mm by isostatic pressing, and then punching 2 holes on the dried hemispherical shells to obtain a hemispherical shell blank, and preparing a cylindrical shell blank with a shell length of 1500mm and a wall thickness of 28mm by molding; the hemispherical shell blank and the cylindrical shell blank are placed in a high-temperature furnace for siliconization treatment after curing, and then the residual silicon on the surface of the blank is removed by a sandblasting process with strong impact force to obtain a shell;

[0107] S2, the above shells are butted against each other after beveling, and connected with O-ring 6 to obtain a container, such as Figure 6 As shown, the bevel processing is performed at processing location 5;

[0108] S3. After the container is evacuated, a low-viscosity adhesive is dripped into the end face seal, dried at room temperature, wrapped with adhesive tape, connected with fasteners 4 and connecting rings 3, and a protective plate is installed around the container to obtain a submarine instrument cabin shell 1; wherein the material of the fasteners 4 includes titanium alloy, and the material of the connecting ring 3 includes ultra-high molecular weight polyethylene.

[0109] The cross-sectional view of the submarine instrument cabin prepared in this embodiment is as follows Figure 2 As shown, it is suitable for water depth of 6000 meters.

[0110] Example 4

[0111] This embodiment adopts the following steps to prepare the subsea instrument cabin housing 1:

[0112] S1, using the above inorganic composite material to prepare two hemispherical shells with a wall thickness of 24mm and an outer diameter of 1200mm by a grouting method, and then punching 2 holes on the dried hemispherical shells to obtain hemispherical shell blanks, and preparing two cylindrical shell blanks with a shell length of 1800mm and a wall thickness of 32mm by a grouting method; after the hemispherical shell blanks and the cylindrical shell blanks are cured, they are placed in a high-temperature furnace for siliconization treatment, and then the residual silicon on the surface of the blanks is removed by a sandblasting process with strong impact force to obtain a shell;

[0113] S2, the shell is butted after the outer circle and end surface are processed, and connected with the plane sealing ring 7 to obtain a container, such as Figure 7 As shown, the outer circle machining and end surface machining are performed at the machining location 5;

[0114] S3. After the container is evacuated, a low-viscosity adhesive is dripped onto the end face seal, dried at room temperature, wrapped with adhesive tape, connected with fasteners 4 and connecting rings 3, and a protective plate is installed around the container to obtain a submarine instrument cabin shell 1; wherein the material of the fasteners 4 includes ultra-high molecular weight polyethylene, and the material of the connecting ring 3 includes ultra-high molecular weight polyethylene.

[0115] The cross-sectional view of the submarine instrument cabin prepared in this embodiment is as follows Figure 3 As shown, it is suitable for water depth of 4500 meters.

[0116] Effect Example 1

[0117] 1. Ultimate pressure 145MPa hydrostatic pressure test:

[0118] The subsea instrument cabin shell obtained in Example 1 is placed in a hydrostatic pressure test device for pressure increase, each time by 20 MPa until 100 MPa; after 100 MPa, the pressure is increased by 5 MPa each time, and the pressure is maintained for 1 min after each pressure increase until the pressure reaches 145 MPa. The pressure is maintained for 2 min at the highest pressure, and then the pressure is released to 0 MPa. The pressure release rate is not greater than 60 MPa / min. After the test, the subsea instrument cabin shell is taken out to observe whether there is any abnormality.

[0119] 2. 115MPa pressure 10 cycles test:

[0120] The subsea instrument cabin shell obtained in Example 1 is placed in a hydrostatic pressure test device for pressure increase, each time by 20 MPa until 100 MPa; after 100 MPa, the pressure is increased by 5 MPa each time, and the pressure is maintained for 1 minute after each pressure increase until the pressure reaches 115 MPa. The pressure is maintained for 2 minutes at the highest pressure, and then the pressure is released to 0 MPa. The pressure release rate is not greater than 60 MPa / min. The above pressure increase and pressure maintenance process is repeated 9 times. After the test, the subsea instrument cabin shell is taken out to observe whether there is any abnormality.

[0121] 3. Test under 115MPa pressure for 10 hours:

[0122] The subsea instrument cabin shell obtained in Example 1 is placed in a hydrostatic pressure test device for pressure increase, each time by 20 MPa until 100 MPa; after 100 MPa, the pressure is increased by 5 MPa each time, and the pressure is maintained for 1 minute after each pressure increase until the pressure reaches 115 MPa. The pressure is maintained for 10 hours at the highest pressure. If there is a pressure drop during the process, the equipment automatically replenishes the pressure and then releases the pressure to 0 MPa. The pressure release rate is not greater than 60 MPa / min. After the test, the subsea instrument cabin shell is taken out to observe whether there is any abnormality.

[0123] After the above tests, if the outer shell of the subsea instrument compartment has no cracks under a pressure of 115MPa and no water leakage during the test, it indicates that it is suitable for deep-sea operations at a depth of 11,000 meters.

[0124] After testing, the data of the subsea instrument cabin shell obtained in Example 1 are as follows:

[0125] After the completion of the three tests (1) 145 MPa ultimate pressure, (2) 10 cycles of 115 MPa pressure, and (3) 10 hours of testing under 115 MPa pressure, the outer shell of the subsea instrument cabin prepared in Example 1 was intact without cracks and no water leakage occurred during the test, indicating that the outer shell of the subsea instrument cabin of Example 1 has excellent pressure resistance (resistance to external pressure) strength and is suitable for deep-sea operations at a depth of 11,000 meters.

Claims

1. A method for preparing a submarine instrument cabin shell, characterized in that: The method comprises the following steps: performing surface processing on at least two shells constituting the outer shell of the submarine instrument cabin, then butting the two shells together to form a hollow container, evacuating the hollow container, and bonding the butted end surfaces together; The shell of the submarine instrument cabin includes two hemispherical shells and N cylindrical shells, where N is greater than or equal to 0; The elastic modulus of the material of the shell is 390-410GPa, and the compressive strength is 3600-4000Mpa; The surface processing includes one or more of outer circle processing, end surface processing and bevel processing.

2. The method for preparing the submarine instrument cabin shell according to claim 1, characterized in that: The shell is made of an inorganic composite material consisting of four phases: α-SiC, α-SiC fiber, β-SiC and silicon phase; and / or, the elastic modulus of the material of the housing is 395 GPa, 400 GPa or 405 GPa; And / or, the compressive strength of the material of the shell is 3800 MPa or 3900 MPa.

3. The method for preparing the submarine instrument cabin shell according to claim 1, characterized in that: The hardness of the material of the shell is HRA85-93, for example, HRA90 or HRA92; And / or, the density of the material of the shell is 3-3.12 g / cm 3 , for example 3.05 g / cm 3 or 3.10g / cm 3 ; And / or, the fracture toughness of the material of the shell is 5-9 MPa·m 1 / 2 , for example 7MPa·m 1 / 2 ; And / or, the bending strength of the material of the housing is 330-420 MPa, for example, 350 MPa or 360 MPa.

4. The method for preparing the submarine instrument cabin shell according to claim 1, characterized in that: A fastener parallel to the axis and a connecting ring perpendicular to the axis are further provided on the periphery of the container, and the fastener and the connecting ring are used to achieve fastening between the shells; wherein the connecting ring preferably includes symmetrically arranged fastener positioning holes, and the fastener positioning holes are used to connect with the fastener and fix the shell; wherein the material of the fastener is preferably one or more of ultra-high molecular weight polyethylene, titanium alloy and stainless steel, and the material of the connecting ring is preferably ultra-high molecular weight polyethylene; And / or, when the surface processing adopts beveling processing, the end faces of the hemispherical shell and the cylindrical shell are respectively processed to form a pair of mutually matching planes and a pair of mutually matching inclined surfaces, and the pair of planes and the pair of inclined surfaces together form the connecting surface of the hemispherical shell and the cylindrical shell.

5. The method for preparing the submarine instrument cabin shell according to claim 1, characterized in that: The method for preparing the shell comprises the following steps: S1, uniformly mixing α-SiC fibers, α-SiC particles, and phenolic resin to obtain a slurry, and spray drying the slurry to obtain a spherical particle raw material; wherein the α-SiC fibers have a length of less than 300 μm and a diameter of ≤10 μm; and the α-SiC particles have a particle size of 1-100 μm; S2, pressing the spherical particle raw material into a green billet, and then curing the green billet; S3, performing siliconization treatment after the curing treatment to obtain the shell.

6. The method for preparing the submarine instrument cabin shell according to claim 5, characterized in that: The compression molding method is one of isostatic pressing, slip casting or molding; And / or, preferably, a step of opening holes is further included before the siliconizing treatment; And / or, in parts by weight, the ratio of the α-SiC fiber, the α-SiC particles and the phenolic resin is preferably (6-30): (60-84): 10; And / or, the particle size of the α-SiC particles is 10-100 μm, for example: the number of α-SiC particles with a particle size of 100 μm, 60 μm, and 10 μm each accounts for 33.3%; or, the number of α-SiC particles with a particle size of 15 μm, 5 μm, and 1 μm each accounts for 33.3%; or, the number of α-SiC particles with a particle size of 50 μm, 20 μm, and 10 μm each accounts for 33.3%.

7. The method for preparing the submarine instrument cabin shell according to claim 1, characterized in that: The end surface is processed by a diamond grinding wheel; And / or, N is 1-20, preferably 1-4, for example 1 or 2; and / or, when N ≥ 2, the cylindrical shells are coaxially arranged on the axis between the two hemispherical shells; And / or, the bonding is performed by drip irrigation; And / or, a sealing ring is further provided between the housings; wherein the sealing ring is preferably an O-ring or a flat sealing ring; And / or, the processing adopts outer circle processing and end face processing, and no sealing ring is set; or, the processing adopts bevel processing, and no sealing ring is set; or, the processing adopts outer circle processing and end face processing, and a flat sealing ring is set between the shells; or, the processing adopts bevel processing, and an O-ring is set between the shells.

8. A submarine instrument cabin shell produced by the method for producing a submarine instrument cabin shell according to any one of claims 1 to 7.

9. A submarine instrument cabin housing, characterized in that: The shell of the outer shell includes two hemispherical shells and N cylindrical shells, where N is greater than or equal to 0; The elastic modulus of the material of the shell is 390-410GPa, and the compressive strength is 3600-4000Mpa; The shell is made of an inorganic composite material consisting of four phases: α-SiC, α-SiC fiber, β-SiC and silicon phase.

10. The submarine instrument compartment housing according to claim 9, characterized in that: Said N is 1-20, preferably 1-4, for example 1 or 2; And / or, the hardness of the material of the shell is HRA85-93, for example, HRA90 or HRA92; And / or, the density of the material of the shell is 3-3.12 g / cm 3 , for example 3.05 g / cm 3 or 3.10g / cm 3 ; And / or, the fracture toughness of the material of the shell is 5-9 MPa·m 1 / 2 , for example 7MPa·m 1 / 2 ; And / or, the bending strength of the material of the housing is 330-420 MPa, for example, 350 MPa or 360 MPa; And / or, the wall thickness of the hemispherical shell is 5-24 mm, for example 15 mm or 20 mm; And / or, the outer diameter of the hemispherical shell is 300-1200 mm, for example 650 mm or 1000 mm; And / or, the length of the cylindrical shell is 300-2000 mm, for example 1500 mm or 1800 mm; And / or, the wall thickness of the cylindrical shell is 18-32 mm; And / or, the ratio of the wall thickness of the hemispherical shell to the wall thickness of the cylindrical shell is 1:(1.1-4).

Citation Information

Cited By

  • Inorganic composite material as well as preparation method and application thereof

    CN118930295A